{"id":218012,"date":"2021-02-21T06:28:52","date_gmt":"2021-02-20T22:28:52","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=218012"},"modified":"2021-02-20T21:29:03","modified_gmt":"2021-02-20T13:29:03","slug":"%e8%83%bd%e5%88%b7%e7%88%86ns%e7%9a%84%e5%a4%9a%e5%b1%82%e8%bd%ac%e8%a7%92%e7%9f%b3%e5%a2%a8%e7%83%af%ef%bc%8c%e5%8f%af%e4%b8%8d%e6%ad%a2%e6%98%af%e6%9b%b9%e5%8e%9f%e4%b8%80%e5%ae%b6","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=218012","title":{"rendered":"\u80fd\u5237\u7206NS\u7684\u591a\u5c42\u8f6c\u89d2\u77f3\u58a8\u70ef\uff0c\u53ef\u4e0d\u6b62\u662f\u66f9\u539f\u4e00\u5bb6"},"content":{"rendered":"<p>\u725b\u5e74\u7684\u6700\u540e\u4e00\u4e2a\u4f11\u606f\u65e5\uff0c\u5927\u90e8\u5206\u793e\u755c\u8fd8\u6c89\u6d78\u5728\u5047\u671f\u5373\u5c06\u7ed3\u675f\u7684\u60b2\u75db\u4e2d&#8230;\u4e0e\u6b64\u540c\u65f6\uff0c\u5e74\u5ea6NS\u9489\u5b50\u6237\u8f6c\u89d2\u77f3\u58a8\u70ef\uff0c\u5b83\u5b83\u5b83\u53c8\u6765\u4e86\uff0c\u8fd9\u4e00\u6b21\u8fd8\u662fNature\u7684\u5c01\u9762\u3002<\/p>\n<p>\u8fd9\u7bc7\u6587\u7ae0\u5e76\u6ca1\u6709\u5728\u5fae\u4fe1\u516c\u4f17\u53f7\u4e0a\u5237\u51fa\u5927\u6c34\u82b1\uff0c\u4e00\u90e8\u5206\u539f\u56e0\u662f\u5b83\u5e76\u4e0d\u51fa\u81ea\u9b54\u89d2\u77f3\u58a8\u70ef\u5929\u624d\u5c11\u5e74\u66f9\u539f\uff0c\u800c\u662f\u6765\u81ea\u5df4\u897f\u7c73\u7eb3\u65af\u8054\u90a6\u5927\u5b66\u7684Ado Jorio\u548c\u7f8e\u56fd\u743c\u68ee\u00b7\u7f57\u5170\u79d1\u5b66\u4e2d\u5fc3\u7684Vincent Meunier\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-218015 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-1-11.png\" alt=\"\" width=\"600\" height=\"419\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-1-11.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-1-11-300x210.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u4e8b\u5b9e\u4e0a\uff0c\u5168\u7403\u8303\u56f4\u5185\u4ece\u4e8b\u77f3\u58a8\u70ef\u8f6c\u89d2\u7814\u7a76\u7684\u79d1\u5b66\u5bb6\u662f\u5f88\u591a\u7684\uff0c\u8fdc\u8fdc\u4e0d\u6b62\u66f9\u539f\u548c\u4ed6\u7684\u8001\u677fPablo Jarillo-Herrero\u3002\u8fdc\u7684\u4e0d\u8bf4\uff0c\u54b1\u4eec\u590d\u65e6\u5927\u5b66\u7269\u7406\u7cfb\u7684\u5f20\u8fdc\u6ce2\u6559\u6388\u4e5f\u7814\u7a76\u8fc7\u8fd9\u4e2a\u3002<\/p>\n<p>\u5728\u8fd9\u7bc7\u6587\u7ae0\u91cc\u9762\uff0c\u6211\u4eec\u5c31\u6765\u5520\u5520\u5565\u662f\u8f6c\u89d2\u77f3\u58a8\u70ef\uff0c\u5168\u7403\u8303\u56f4\u5185\u6709\u54ea\u4e9b\u5927\u5bb6\u5728\u641e\u8fd9\u4e2a\u3002<\/p>\n<p><strong>\u5565\u662f\u8f6c\u89d2\u77f3\u58a8\u70ef\uff1f<\/strong><\/p>\n<p>\u77f3\u58a8\u70ef\u8f6c\u89d2\u5c5e\u4e8e\u4e00\u4e2a\u65b0\u5174\u7684\u7814\u7a76\u9886\u57df\u2014\u2014twistronics\uff08\u4ece\u540d\u5b57\u4e0a\u770b\u51fa\u6765\u8fd9\u8d27\u662f\u626d\u66f2\u548c\u7535\u5b50\uff0c\u4fe9\u82f1\u6587\u5355\u8bcd\u7684\u7ed3\u5408\uff09\u3002\u7b80\u5355\u8bf4\u6765\uff0c\u5f53\u4e8c\u7ef4\u6750\u6599\u7247\u53d1\u751f\u626d\u66f2\u65f6\uff0c\u8fd9\u79cd\u626d\u66f2\u4f1a\u4f7f\u6750\u6599\u7684\u4e00\u4e9b\u7269\u7406\u884c\u4e3a\u53d1\u751f\u5de8\u5927\u7684\u6539\u53d8\u3002\u8fd9\u91cc\u7684\u7269\u7406\u884c\u4e3a\u5305\u62ec\u9ad8\u6e29\u8d85\u5bfc\u3001\u975e\u7ebf\u6027\u5149\u5b66\u548c\u7ed3\u6784\u8d85\u6da6\u6ed1\u6027\u7b49\u7b49\u3002<\/p>\n<p>\u66f9\u539f\u56e0\u4e3a\u505a\u51fa\u4e86\u8f6c\u89d2\u7ea6\u4e3a1.08<sup>o<\/sup>\u7684\u53cc\u5c42\u8f6c\u89d2\u77f3\u58a8\u70ef\uff0c\u5728Nature\u4e0a\u53d1\u8868\u4e862\u7bc7\u80cc\u9760\u80cc\u7684\u8bba\u6587\u800c\u5907\u53d7\u5173\u6ce8\u3002\u800c\u90a3\u4e2a\u795e\u5947\u76841.08<sup>o<\/sup>\u4e5f\u88ab\u79f0\u4e3a\u9b54\u89d2\u3002\u6240\u4ee5\u8bf4\uff0c\u9b54\u89d2\u77f3\u58a8\u70ef\u7684\u7814\u7a76\u662f\u8f6c\u89d2\u77f3\u58a8\u70ef\u7814\u7a76\u7684\u4e00\u90e8\u5206\u3002<\/p>\n<p>\u4e8b\u5b9e\u4e0a\uff0c\u56e0\u4e3a\u8fd9\u4e2a\u9886\u57df\u7684\u7814\u7a76\u5341\u5206\u706b\u7206\uff0c\u9876\u520a\u4e0a\u7684\u7814\u7a76\u6210\u679c\u66f4\u8fed\u662f\u975e\u5e38\u5730\u8fc5\u901f\u3002\u9664\u4e86\u53cc\u5c42\u8f6c\u89d2\u77f3\u58a8\u70ef\u88ab\u505a\u51fa\u6765\u4ee5\u5916\uff0c\u4e09\u5c42\u3001\u56db\u5c42\u7684\u8f6c\u89d2\u77f3\u58a8\u70ef\u4e5f\u662f\u6709\u7684\u3002\u4e16\u754c\u4e0a\u4ece\u4e8b\u8fd9\u4e2a\u9886\u57df\u7814\u7a76\u7684\u79d1\u5b66\u5bb6\u5f88\u591a\uff0c\u4ed6\u4eec\u4e5f\u5e94\u8be5\u50cf\u66f9\u539f\u4e00\u6837\u88ab\u4e2d\u56fd\u7684\u79d1\u7814\u7fa4\u4f17\u6240\u8ba4\u8bc6\uff1aHarvard\u5927\u5b66\u7684Philip Kim\u3001UC Berckley\u7684\u738b\u67ab\u6559\u6388\u7b49\u7b49\u3002<\/p>\n<p><strong><b>1.\u5df4\u897f\u7c73\u7eb3\u65af\u8054\u90a6\u5927\u5b66Ado Jorio&amp;\u7f8e\u56fd\u743c\u68ee\u00b7\u7f57\u5170\u79d1\u5b66\u4e2d\u5fc3Vincent Meunier Nature\uff1a\u4f4e\u89d2\u5ea6\u626d\u66f2\u53cc\u5c42\u77f3\u58a8\u70ef\u4e2d\u6676\u683c\u52a8\u529b\u5b66\u7684\u5c40\u57df\u5316<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-218016 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-2-10.png\" alt=\"\" width=\"600\" height=\"310\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-2-10.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-2-10-300x155.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u626d\u66f2\u7684\u53cc\u5c42\u77f3\u58a8\u70ef\u662f\u901a\u8fc7\u4f7f\u53cc\u5c42\u77f3\u58a8\u70ef\u4e2d\u7684\u4e24\u4e2a\u6676\u4f53\u7f51\u7edc\u5f7c\u6b64\u76f8\u5bf9\u65cb\u8f6c\u800c\u4ea7\u751f\u7684\u3002\u5bf9\u4e8e\u8f83\u5c0f\u7684\u626d\u66f2\u89d2\uff0c\u6750\u6599\u4f1a\u7ecf\u5386\u81ea\u7ec4\u7ec7\u7684\u6676\u683c\u91cd\u6784\uff0c\u4ece\u800c\u5bfc\u81f4\u5f62\u6210\u5468\u671f\u6027\u91cd\u590d\u7684\u7574\u3002\u4ea7\u751f\u7684\u8d85\u6676\u683c\u8c03\u8282\u6750\u6599\u4e2d\u7684\u632f\u52a8\u548c\u7535\u5b50\u7ed3\u6784\uff0c\u4ece\u800c\u5bfc\u81f4\u7535\u5b50-\u58f0\u5b50\u8026\u5408\u884c\u4e3a\u53d1\u751f\u53d8\u5316\uff0c\u5e76\u89c2\u5bdf\u5230\u5f3a\u76f8\u5173\u6027\u548c\u8d85\u5bfc\u7535\u6027\u3002\u4f46\u662f\uff0c\u6df1\u5165\u4e86\u89e3\u8fd9\u4e9b\u8c03\u5236\u5e76\u4e86\u89e3\u76f8\u5173\u6548\u679c\u5177\u6709\u6311\u6218\u6027\uff0c\u56e0\u4e3a\u5bf9\u4e8e\u5b9e\u9a8c\u6280\u672f\u800c\u8a00\uff0c\u8c03\u5236\u91cf\u592a\u5c0f\uff0c\u65e0\u6cd5\u51c6\u786e\u5730\u89e3\u6790\u76f8\u5173\u7684\u80fd\u7ea7\uff0c\u800c\u5bf9\u4e8e\u7406\u8bba\u6a21\u578b\u800c\u8a00\uff0c\u8c03\u5236\u91cf\u592a\u5927\uff0c\u65e0\u6cd5\u6b63\u786e\u5730\u63cf\u8ff0\u5c40\u90e8\u6548\u5e94\u3002<\/p>\n<p><strong><b>\u5df4\u897f\u7c73\u7eb3\u65af\u8054\u90a6\u5927\u5b66Ado Jorio&amp;\u7f8e\u56fd\u743c\u68ee\u00b7\u7f57\u5170\u79d1\u5b66\u4e2d\u5fc3Vincent Meunier<\/b><\/strong>\u62a5\u9053\u7531\u7eb3\u7c73\u62c9\u66fc\u5206\u5149\u955c\u4ea7\u751f\u7684\u9ad8\u5149\u8c31\u5149\u5b66\u56fe\u50cf\uff0c\u8be5\u56fe\u50cf\u662f\u91cd\u6784\u7684\uff08\u4f4e\u89d2\u5ea6\uff09\u626d\u66f2\u53cc\u5c42\u77f3\u58a8\u70ef\u4e2d\u7684\u6676\u4f53\u8d85\u6676\u683c\u3002\u7eb3\u7c73\u62c9\u66fc\u6280\u672f\u4f7f\u7528\u53ef\u89c1\u5149\u89c2\u5bdf\u6676\u4f53\u7ed3\u6784\u6210\u4e3a\u53ef\u80fd\uff0c\u8be5\u6280\u672f\u63ed\u793a\u4e86\u6676\u683c\u52a8\u529b\u5b66\u7684\u5c40\u90e8\u5316\uff0c\u5e76\u4e14\u5b58\u5728\u5e94\u53d8\u5b64\u5b50\u548c\u62d3\u6251\u70b9\uff0c\u5bfc\u81f4\u53ef\u68c0\u6d4b\u7684\u5149\u8c31\u53d8\u5316\u3002\u901a\u8fc7\u539f\u5b50\u6a21\u578b\u53ef\u4ee5\u4f7f\u7ed3\u679c\u5408\u7406\u5316\uff0c\u8be5\u6a21\u578b\u53ef\u4ee5\u8bc4\u4f30\u8d85\u6676\u683c\u7684\u7535\u5b50\u72b6\u6001\u548c\u632f\u52a8\u72b6\u6001\u7684\u5c40\u90e8\u5bc6\u5ea6\u3002\u8be5\u8bc4\u4f30\u7a81\u51fa\u4e86\u5b64\u5b50\u548c\u62d3\u6251\u70b9\u4e0e\u7ed3\u6784\u7684\u632f\u52a8\u548c\u7535\u5b50\u7279\u6027\u7684\u76f8\u5173\u6027\uff0c\u5c24\u5176\u662f\u5bf9\u4e8e\u8f83\u5c0f\u7684\u626d\u66f2\u89d2\u3002\u8fd9\u4e2a\u7ed3\u679c\u662f\u8fc8\u5411\u4e86\u89e3\u539f\u5b50\u548c\u7eb3\u7c73\u5c3a\u5ea6\u4e0a\u4e0e\u58f0\u5b50\u76f8\u5173\u7684\u6548\u5e94\uff08\u4f8b\u5982Jahn-Teller\u6548\u5e94\u548c\u5e93\u73c0\u7535\u5b50\u914d\u5bf9\uff09\u7684\u91cd\u8981\u4e00\u6b65\uff0c\u5e76\u4e14\u53ef\u80fd\u4f1a\u5728\u626d\u8f6c\u65cb\u7ffc\u6280\u672f\u8fc5\u731b\u53d1\u5c55\u7684\u80cc\u666f\u4e0b\u5e2e\u52a9\u6539\u5584\u5668\u4ef6\u7684\u7279\u6027\u3002<\/p>\n<p><strong><b>\u6587\u732e\u94fe\u63a5\uff1a<\/b><\/strong><\/p>\n<p><strong><b>Localization of lattice dynamics in low-angle twisted bilayer graphene.<\/b><\/strong><\/p>\n<p><strong><b>(<\/b><\/strong><strong><b>Nature<\/b><\/strong><strong><b>, 202<\/b><\/strong><strong><b>1<\/b><\/strong><strong><b>, DOI:10.1038\/s41586-021-03252-5)<\/b><\/strong><\/p>\n<p><strong><b>2.\u9ebb\u7701\u7406\u5de5Pablo Jarillo-Herrero&amp;\u66f9\u539fNature\uff1a\u9b54\u89d2\u626d\u66f2\u4e09\u5c42\u77f3\u58a8\u70ef\u4e2d\u53ef\u8c03\u8c10\u7684\u5f3a\u8026\u5408\u8d85\u5bfc<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-218017 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-3-10.png\" alt=\"\" width=\"600\" height=\"566\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-3-10.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-3-10-300x283.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u83ab\u5c14\u8d85\u6676\u683c\u6700\u8fd1\u5df2\u7ecf\u6210\u4e3a\u4e00\u4e2a\u5e73\u53f0\uff0c\u53ef\u4ee5\u5728\u6b64\u5e73\u53f0\u4e0a\u4ee5\u524d\u6240\u672a\u6709\u7684\u53ef\u8c03\u6027\u7814\u7a76\u76f8\u5173\u7684\u7269\u7406\u5b66\u548c\u8d85\u5bfc\u6027\u3002\u5c3d\u7ba1\u5728\u5176\u4ed6\u51e0\u79cd\u83ab\u5c14\u6761\u7eb9\u7cfb\u7edf\u4e2d\u4e5f\u89c2\u5bdf\u5230\u4e86\u76f8\u5173\u7684\u6548\u5e94\uff0c\u4f46\u9b54\u89d2\u626d\u66f2\u7684\u53cc\u5c42\u77f3\u58a8\u70ef\u4ecd\u7136\u662f\u552f\u4e00\u53ef\u91cd\u590d\u6d4b\u91cf\u51fa\u575a\u56fa\u7684\u8d85\u5bfc\u6027\u7684\u77f3\u58a8\u70ef\u3002<strong><b>\u9ebb\u7701\u7406\u5de5Pablo Jarillo-Herrero&amp;\u66f9\u539f<\/b><\/strong>\u5b9e\u73b0\u4e86\u9b54\u89d2\u626d\u66f2\u4e09\u5c42\u77f3\u58a8\u70ef\uff08MATTG\uff09\u4e2d\u7684\u83ab\u5c14\u6761\u7eb9\u8d85\u5bfc\u4f53\uff0c\u5176\u6bd4\u9b54\u89d2\u626d\u66f2\u53cc\u5c42\u77f3\u58a8\u70ef\u5177\u6709\u66f4\u597d\u7684\u7535\u5b50\u7ed3\u6784\u53ef\u8c03\u6027\u548c\u8d85\u5bfc\u6027\u80fd\u3002\u970d\u5c14\u6548\u5e94\u548c\u91cf\u5b50\u632f\u8361\u4f5c\u4e3a\u5bc6\u5ea6\u548c\u7535\u573a\u7684\u51fd\u6570\u7684\u6d4b\u91cf\u4f7f\u80fd\u591f\u786e\u5b9a\u6b63\u5e38\u91d1\u5c5e\u72b6\u6001\u4e0b\u7cfb\u7edf\u7684\u53ef\u8c03\u8c10\u76f8\u754c\u3002\u96f6\u78c1\u573a\u7684\u7535\u963b\u7387\u6d4b\u91cf\u8868\u660e\uff0c\u8d85\u5bfc\u7535\u6027\u7684\u5b58\u5728\u4e0e\u6bcf\u4e2a\u6469\u5c14\u5355\u5143\u683c\u4e2d\u4e24\u4e2a\u8f7d\u6d41\u5b50\u51fa\u73b0\u7684\u5bf9\u79f0\u5bf9\u79f0\u76f8\u7d27\u5bc6\u76f8\u5173\u3002\u8d85\u5bfc\u76f8\u88ab\u6291\u5236\u5e76\u9650\u5236\u5728\u90e8\u5206\u56f4\u7ed5\u5bf9\u79f0\u5bf9\u79f0\u76f8\u7684Van Hove\u5947\u5f02\u70b9\u4e0a\uff0c\u8fd9\u4e0e\u5f31\u8026\u5408Bardeen-Cooper-Schriefer\u7406\u8bba\u5f88\u96be\u534f\u8c03\u3002\u6b64\u5916\uff0c\u7cfb\u7edf\u5e7f\u6cdb\u7684\u539f\u4f4d\u53ef\u8c03\u6027\u4f7f\u80fd\u591f\u8fbe\u5230\u8d85\u5f3a\u8026\u5408\u72b6\u6001\uff0c\u5176\u7279\u5f81\u662fGinzburg-Landau\u76f8\u5e72\u957f\u5ea6\u8fbe\u5230\u4e86\u5e73\u5747\u7c92\u5b50\u95f4\u8ddd\u79bb\uff0c\u5e76\u4e14\u975e\u5e38\u5927\u7684TBKT\/TF\u503c\u8d85\u8fc70.1\u3002\u8fd9\u4e9b\u89c2\u5bdf\u7ed3\u679c\u8868\u660e\uff0cMATTG\u53ef\u4ee5\u5728\u5206\u9891\u9644\u8fd1\u88ab\u7535\u8c03\u8c10\u4e3a\u4e8c\u7ef4Bose-Einstein\u51b7\u51dd\u7269\u3002\u6587\u7ae0\u7ed3\u679c\u5efa\u7acb\u4e86\u53ef\u8c03\u8c10\u7684\u83ab\u5c14\u6761\u7eb9\u8d85\u5bfc\u4f53\u7cfb\u5217\uff0c\u5b83\u4eec\u6709\u53ef\u80fd\u5f7b\u5e95\u6539\u53d8\u5bf9\u5f3a\u8026\u5408\u8d85\u5bfc\u6027\u7684\u57fa\u672c\u7406\u89e3\u548c\u5e94\u7528\u3002<\/p>\n<p><strong><b>\u6587\u732e\u94fe\u63a5\uff1a<\/b><\/strong><\/p>\n<p><strong><b>Tunable strongly coupled superconductivity in magic-angle twisted trilayer graphene.<\/b><\/strong><\/p>\n<p><strong><b>(<\/b><\/strong><strong><b>Nature<\/b><\/strong><strong><b>, 202<\/b><\/strong><strong><b>1<\/b><\/strong><strong><b>, DOI:10.1038\/s41586-021-03192-0)<\/b><\/strong><\/p>\n<p><strong><b>3.\u54c8\u4f5b\u5927\u5b66Philip Kim&amp;Xiaomeng Liu Nature\uff1a\u53cc\u87ba\u65cb\u53cc\u5c42\u77f3\u58a8\u70ef\u4e2d\u53ef\u8c03\u8c10\u7684\u81ea\u65cb\u6781\u5316\u76f8\u5173\u6001<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-218018 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-4-10.png\" alt=\"\" width=\"600\" height=\"362\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-4-10.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-4-10-300x181.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u5c06\u6676\u683c\u4e2d\u7535\u5b50\u7684\u80fd\u91cf\u5e26\u5bbd\u51cf\u5c0f\u5230\u8fdc\u8ddd\u79bb\u5e93\u4ed1\u76f8\u4e92\u4f5c\u7528\u80fd\u4ee5\u4e0b\u53ef\u4fc3\u8fdb\u76f8\u5173\u6548\u5e94\u3002\u83ab\u5c14\u8d85\u6676\u683c-\u901a\u8fc7\u5c06Vander Waals\u5f02\u8d28\u7ed3\u6784\u5806\u53e0\u5728\u4e00\u8d77\u5e76\u63a7\u5236\u5176\u626d\u8f6c\u89d2\u800c\u5236\u6210-\u4f7f\u7535\u5b50\u80fd\u5e26\u7ed3\u6784\u7684\u5de5\u7a0b\u5316\u6210\u4e3a\u53ef\u80fd\u3002\u5916\u6765\u91cf\u5b50\u76f8\u53ef\u4ee5\u51fa\u73b0\u5728\u5de5\u7a0b\u83ab\u5c14\u6761\u7eb9\u4e2d\u3002\u9b54\u672f\u89d2\u626d\u66f2\u53cc\u5c42\u77f3\u58a8\u70ef\u8102\u80aa\u5e26\u4e2d\u76f8\u5173\u7684\u7edd\u7f18\u5b50\u6001\uff0c\u8d85\u5bfc\u6027\u548c\u91cf\u5b50\u5f02\u5e38\u970d\u5c14\u6548\u5e94\u7684\u6700\u65b0\u53d1\u73b0\u6fc0\u53d1\u4e86\u5176\u4ed6\u83ab\u5c14\u7cfb\u7edf\u4e2d\u76f8\u5173\u7535\u5b50\u6001\u7684\u63a2\u7d22\u3002\u8303\u5fb7\u534e\u83ab\u5c14\u6761\u7eb9\u8d85\u6676\u683c\u7684\u7535\u5b50\u6027\u8d28\u53ef\u4ee5\u901a\u8fc7\u8c03\u8282\u5c42\u95f4\u8026\u5408\u6216\u7ec4\u6210\u5c42\u7684\u80fd\u5e26\u7ed3\u6784\u6765\u8fdb\u4e00\u6b65\u8c03\u8282\u3002<strong><b>\u54c8\u4f5b\u5927\u5b66Philip Kim&amp;Xiaomeng Liu<\/b><\/strong>\u4f7f\u7528\u53cc\u53cc\u5c42\u77f3\u58a8\u70ef\uff08TDBG\uff09\u7684\u8303\u5fb7\u534e\u529b\u5f02\u8d28\u7ed3\u6784\uff0c\u8bc1\u660e\u4e86\u4e00\u4e2a\u8102\u80aa\u7535\u5b50\u80fd\u5e26\uff0c\u8be5\u7535\u5b50\u80fd\u5e26\u53ef\u4ee5\u5728\u4e00\u5b9a\u7684\u626d\u66f2\u89d2\u8303\u56f4\u5185\u901a\u8fc7\u5782\u76f4\u7535\u573a\u8fdb\u884c\u8c03\u8c10\u3002\u4e0e\u9b54\u89d2\u626d\u66f2\u7684\u53cc\u5c42\u77f3\u58a8\u70ef\u76f8\u4f3c\uff0cTDBG\u5728\u534a\u548c\u56db\u5206\u4e4b\u4e00\u8102\u80aa\u533a\u663e\u793a\u51fa\u80fd\u9699\uff0c\u8868\u660e\u51fa\u73b0\u4e86\u76f8\u5173\u7684\u7edd\u7f18\u4f53\u72b6\u6001\u3002\u8fd9\u4e9b\u7edd\u7f18\u4f53\u72b6\u6001\u7684\u95f4\u9699\u968f\u7740\u5e73\u9762\u5185\u78c1\u573a\u7684\u589e\u52a0\u800c\u589e\u52a0\uff0c\u8868\u660e\u94c1\u78c1\u987a\u5e8f\u3002\u63ba\u6742\u534a\u6210\u54c1\u7edd\u7f18\u5b50\u65f6\uff0c\u968f\u7740\u6e29\u5ea6\u964d\u4f4e\uff0c\u7535\u963b\u7387\u7a81\u7136\u4e0b\u964d\u3002\u8fd9\u79cd\u4e34\u754c\u884c\u4e3a\u4ec5\u9650\u4e8e\u5bc6\u5ea6-\u7535\u5730\u5e73\u9762\u4e2d\u7684\u4e00\u5c0f\u90e8\u5206\uff0c\u5e76\u4e14\u5f52\u56e0\u4e8e\u4ece\u6b63\u5e38\u91d1\u5c5e\u5230\u81ea\u65cb\u6781\u5316\u76f8\u5173\u6001\u7684\u76f8\u53d8\u3002\u7535\u573a\u53ef\u8c03TDBG\u4e2d\u81ea\u65cb\u6781\u5316\u76f8\u5173\u6001\u7684\u53d1\u73b0\u4e3a\u5de5\u7a0b\u76f8\u4e92\u4f5c\u7528\u9a71\u52a8\u7684\u91cf\u5b50\u76f8\u63d0\u4f9b\u4e86\u4e00\u6761\u65b0\u9014\u5f84\u3002<\/p>\n<p><strong><b>\u6587\u732e\u94fe\u63a5\uff1a<\/b><\/strong><\/p>\n<p><strong><b>Tunable spin-polarized correlated states in twisted double bilayer graphene.<\/b><\/strong><\/p>\n<p><strong><b>(<\/b><\/strong><strong><b>Nature<\/b><\/strong><strong><b>, 2020, DOI:10.1038\/s41586-020-2458-7)<\/b><\/strong><\/p>\n<p><strong><b>4.\u54c8\u4f5b\u5927\u5b66Philip Kim Science\uff1a\u4ea4\u66ff\u626d\u66f2\u9b54\u89d2\u4e09\u5c42\u77f3\u58a8\u70ef\u4e2d\u7684\u7535\u573a\u53ef\u8c03\u8d85\u5bfc<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-218019 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-5-5.png\" alt=\"\" width=\"600\" height=\"415\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-5-5.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-5-5-300x208.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u901a\u8fc7\u626d\u8f6c\u8303\u5fb7\u534e\uff08vdW\uff09\u5f02\u8d28\u7ed3\u6784\u4e2d\u7684\u5c42\u6765\u5de5\u7a0b\u5316\u83ab\u5c14\u8d85\u6676\u683c\u5df2\u7ecf\u53d1\u73b0\u4e86\u5404\u79cd\u5404\u6837\u7684\u91cf\u5b50\u73b0\u8c61\u3002<strong><b>\u54c8\u4f5b\u5927\u5b66Philip Kim<\/b><\/strong>\u6784\u5efa\u4e86\u4e00\u4e2a\u7531\u4e09\u4e2a\u77f3\u58a8\u70ef\u5c42\u7ec4\u6210\u7684vdW\u5f02\u8d28\u7ed3\u6784\uff0c\u8fd9\u4e9b\u77f3\u58a8\u70ef\u5c42\u4ee5\u4ea4\u66ff\u7684\u626d\u66f2\u89d2\u00b1\u03b8\u5806\u53e0\u3002\u5728\u5e73\u5747\u626d\u66f2\u89d2\u03b8\u301c1.56\u00b0\uff08\u7406\u8bba\u4e0a\u9884\u6d4b\u4e3a\u5f62\u6210\u5e73\u5766\u7535\u5b50\u5e26\u7684\u9b54\u89d2\uff09\u4e0b\uff0c\u89c2\u5bdf\u5230\u4f4d\u79fb\u573a\u53ef\u8c03\u8c10\u7684\u8d85\u5bfc\u6027\uff0c\u5176\u6700\u5927\u4e34\u754c\u6e29\u5ea6\u4e3a2.1K\u3002\u901a\u8fc7\u8c03\u6574\u63ba\u6742\u6c34\u5e73\u548c\u4f4d\u79fb\u573a\uff0c\u4f5c\u8005\u53d1\u73b0\u8d85\u5bfc\u673a\u5236\u4e0e\u83ab\u5c14\u5e26\u7684\u6781\u5316\u6781\u5316\u4e00\u8d77\u51fa\u73b0\uff0c\u5e76\u5728\u9ad8\u4f4d\u79fb\u573a\u53d7\u5230\u8303\u970d\u592b\u5947\u5f02\u6027\uff08vHS\uff09\u7684\u9650\u5236\u3002\u8fd9\u4e2a\u53d1\u73b0\u663e\u793a\u51fa\u4e0e\u5f31\u8026\u5408\u63cf\u8ff0\u7684\u4e0d\u4e00\u81f4\uff0c\u8fd9\u8868\u660e\u89c2\u5bdf\u5230\u7684\u83ab\u5c14\u8d85\u5bfc\u5177\u6709\u975e\u5e38\u89c4\u7684\u6027\u8d28\u3002<\/p>\n<p><strong><b>\u6587\u732e\u94fe\u63a5\uff1a<\/b><\/strong><\/p>\n<p><strong><b>Electric field tunable superconductivity in alternating twist magic-angle trilayer graphene.<\/b><\/strong><\/p>\n<p><strong><b>(<\/b><\/strong><strong><b>Science<\/b><\/strong><strong><b>, 202<\/b><\/strong><strong><b>1<\/b><\/strong><strong><b>, DOI:10.1126\/science.abg0399)<\/b><\/strong><\/p>\n<p><strong><b>5.\u52a0\u5dde\u5927\u5b66\u4f2f\u514b\u5229\u5206\u6821\u738b\u67ab\u3001Aaron Bostwick&amp;\u9996\u5c14\u5927\u5b66Jeil Jung Nature Physics\uff1a\u9b54\u672f\u89d2\u626d\u66f2\u9644\u8fd1\u7684\u53cc\u5c42\u77f3\u58a8\u70ef\u4e2d\u6241\u5e73\u7535\u5b50\u5e26\u7684\u53ef\u89c6\u5316<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-218020 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-6-7.png\" alt=\"\" width=\"600\" height=\"385\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-6-7.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-6-7-300x193.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u5982\u679c\u53cc\u5c42\u77f3\u58a8\u70ef\u4ee5\u7279\u5b9a\u7684\u626d\u66f2\u89d2\uff08\u79f0\u4e3a\u201c\u9b54\u89d2\u201d\uff09\u5806\u53e0\uff0c\u5219\u53ef\u4ee5\u9884\u6d4b\u53cc\u5c42\u77f3\u58a8\u70ef\u5c06\u5f62\u6210\u5e73\u5766\u5206\u6563\u7684\u83ab\u5c14\u6761\u7eb9\u5fae\u5e26\u3002\u6700\u8fd1\uff0c\u636e\u62a5\u9053\u5177\u6709\u9b54\u672f\u89d2\u626d\u66f2\u7684\u626d\u66f2\u53cc\u5c42\u77f3\u58a8\u70ef\uff08tBLG\uff09\u8868\u73b0\u51fa\u76f8\u5173\u7684\u7edd\u7f18\u72b6\u6001\u548c\u8d85\u5bfc\u6027\uff0c\u5728\u8be5\u4f53\u7cfb\u4e2d\uff0c\u6241\u5e73\u5fae\u5e26\u7684\u5b58\u5728\u88ab\u8ba4\u4e3a\u5bf9\u4e8e\u4f20\u8f93\u6d4b\u91cf\u4e2d\u8fd9\u4e9b\u6709\u5e8f\u76f8\u7684\u51fa\u73b0\u81f3\u5173\u91cd\u8981\u3002\u5c3d\u7ba1tBLG\u4e2d\u7684\u96a7\u9053\u5149\u8c31\u6cd5\u548c\u7535\u5b50\u53ef\u538b\u7f29\u6027\u6d4b\u91cf\u5df2\u53d1\u73b0\u4e0e\u5e73\u5766\u5fae\u578b\u5e26\u7684\u5b58\u5728\u4e00\u81f4\u7684van Hove\u5947\u5f02\u6027\uff0c\u4f46\u4ecd\u7f3a\u4e4f\u76f4\u63a5\u89c2\u5bdftBLG\u4e2d\u8fd9\u79cd\u83ab\u5c14\u6761\u7eb9\u5fae\u578b\u5e26\u5728\u52a8\u91cf\u7a7a\u95f4\u4e2d\u5e73\u5766\u5206\u6563\u7684\u89c2\u5bdf\u3002<strong><b>\u52a0\u5dde\u5927\u5b66\u4f2f\u514b\u5229\u5206\u6821\u738b\u67ab\u3001Aaron Bostwick&amp;\u9996\u5c14\u5927\u5b66Jeil Jung<\/b><\/strong>\u901a\u8fc7\u4f7f\u7528\u5177\u6709\u7eb3\u7c73\u7ea7\u5206\u8fa8\u7387\u7684\u89d2\u5ea6\u5206\u8fa8\u5149\u53d1\u5c04\u5149\u8c31\u6280\u672f\u62a5\u9053\u4e86\u8fd9\u79cd\u5e73\u5766\u7684\u83ab\u5c14\u6761\u7eb9\u5fae\u5e26\u7684\u53ef\u89c6\u5316\u3002\u8be5\u6280\u672f\u7684\u9ad8\u7a7a\u95f4\u5206\u8fa8\u7387\u4f7f\u5f97\u80fd\u591f\u6d4b\u91cftBLG\u7684\u5c40\u90e8\u7535\u5b50\u7ed3\u6784\u3002\u6d4b\u91cf\u7ed3\u679c\u8868\u660e\uff0c\u5728\u5ba4\u6e29\u4e0b\uff0ctBLG\u7684\u7535\u8377\u4e2d\u6027\u9644\u8fd1\u5b58\u5728\u63a5\u8fd1\u4e8e\u5e7b\u89d2\u7684\u5e73\u5766\u7684\u83ab\u5c14\u5e26\u3002<\/p>\n<p><strong><b>\u6587\u732e\u94fe\u63a5\uff1a<\/b><\/strong><\/p>\n<p><strong><b>Visualization of the flat electronic band in twisted bilayer graphene near the magic angle twist.<\/b><\/strong><\/p>\n<p><strong><b>(<\/b><\/strong><strong><b>Nature Physics<\/b><\/strong><strong><b>, 202<\/b><\/strong><strong><b>1<\/b><\/strong><strong><b>, DOI:10.1038\/s41567-020-0974-x)<\/b><\/strong><\/p>\n<p><strong><b>6.\u9b4f\u8328\u66fc\u79d1\u5b66\u7814\u7a76\u9662S. Ilani&amp;\u9ebb\u7701\u7406\u5de5Pablo Jarillo-Herrero Nature\uff1a\u9b54\u89d2\u77f3\u58a8\u70ef\u7684\u76f8\u53d8\u548c\u72c4\u62c9\u514b\u6062\u590d\u7684\u7ea7\u8054<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-218021 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-7-5.png\" alt=\"\" width=\"600\" height=\"316\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-7-5.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-7-5-300x158.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u9b54\u89d2\u9644\u8fd1\u626d\u66f2\u7684\u53cc\u5c42\u77f3\u58a8\u70ef\u5c55\u73b0\u51fa\u4e30\u5bcc\u7684\u7535\u5b50\u76f8\u5173\u7269\u7406\u7279\u6027\uff0c\u663e\u793a\u51fa\u7edd\u7f18\u3001\u78c1\u6027\u548c\u8d85\u5bfc\u76f8\u3002\u9884\u8ba1\u8be5\u7cfb\u7edf\u7684\u7535\u5b50\u5e26\u5728\u9b54\u672f\u89d2\u9644\u8fd1\u4f1a\u660e\u663e\u53d8\u7a84\uff0c\u4ece\u800c\u5bfc\u81f4\u5404\u79cd\u53ef\u80fd\u7834\u574f\u5bf9\u79f0\u7684\u57fa\u6001\u3002<strong><b>\u9b4f\u8328\u66fc\u79d1\u5b66\u7814\u7a76\u9662S. Ilani&amp;\u9ebb\u7701\u7406\u5de5Pablo Jarillo-Herrero<\/b><\/strong>\u4f7f\u7528\u5c40\u90e8\u7535\u5b50\u53ef\u538b\u7f29\u6027\u7684\u6d4b\u91cf\u7ed3\u679c\uff0c\u663e\u793a\u8fd9\u4e9b\u76f8\u5173\u7684\u76f8\u4f4d\u6e90\u81ea\u5177\u6709\u9ad8\u80fd\u6001\u4e14\u5177\u6709\u4e0d\u6b63\u5e38\u7684\u5e26\u72b6\u5206\u5e03\u5e8f\u5217\u3002\u5f53\u5c06\u8f7d\u6ce2\u6dfb\u52a0\u5230\u7cfb\u7edf\u4e2d\u65f6\uff0c\u5bf9\u5e94\u4e8e\u65cb\u8f6c\u548c\u8c37\u5e95\u81ea\u7531\u5ea6\u7684\u56db\u4e2a\u7535\u5b50\u201c\u504f\u7231\u201d\u5c31\u4e0d\u4f1a\u5e73\u7b49\u5730\u504f\u79bb\u3002\u76f8\u53cd\uff0c\u5b83\u4eec\u662f\u901a\u8fc7\u4e00\u7cfb\u5217\u5c16\u9510\u7684\u76f8\u53d8\u586b\u5145\u7684\uff0c\u8fd9\u4e9b\u76f8\u53d8\u8868\u73b0\u4e3a\u6469\u5c14\u7eb9\u6676\u683c\u6574\u6570\u9644\u8fd1\u7535\u5b50\u53ef\u538b\u7f29\u6027\u7684\u5f3a\u70c8\u4e0d\u5bf9\u79f0\u8df3\u8dc3\u3002\u5728\u6bcf\u6b21\u8f6c\u6362\u65f6\uff0c\u4e00\u4e2a\u81ea\u65cb\/\u8c37\u504f\u5411\u4f1a\u4f7f\u6240\u6709\u8f7d\u5b50\u4ece\u5176\u90e8\u5206\u7fbd\u7ffc\u7684\u540c\u4f34\u4e2d\u79fb\u51fa\uff0c\u201c\u91cd\u7f6e\u201d\u5230\u7535\u8377\u4e2d\u6027\u70b9\u9644\u8fd1\u3002\u7ed3\u679c\uff0c\u5728\u6bcf\u6b21\u6574\u6570\u7ffb\u8f6c\u4e4b\u540e\uff0c\u5728\u7535\u8377\u4e2d\u6027\u9644\u8fd1\u89c2\u5bdf\u5230\u7684\u7c7b\u4f3c\u72c4\u62c9\u514b\u7684\u7279\u5f81\u518d\u6b21\u51fa\u73b0\u3002\u5316\u5b66\u52bf\u9644\u8fd1\u7684\u5e73\u9762\u7535\u78c1\u573a\u4f9d\u8d56\u6027\u7684\u6d4b\u91cf\u63ed\u793a\u4e86\u5f88\u5927\u7684\u81ea\u53d1\u78c1\u5316\u5f3a\u5ea6\uff0c\u8fdb\u4e00\u6b65\u8bc1\u5b9e\u4e86\u5bf9\u79f0\u7834\u574f\u7ea7\u8054\u7684\u56fe\u666f\u3002\u5728\u8fdc\u9ad8\u4e8e\u8d85\u5bfc\u548c\u76f8\u5173\u7edd\u7f18\u72b6\u6001\u5f00\u59cb\u7684\u6e29\u5ea6\u4e0b\u89c2\u5bdf\u5230\u76f8\u53d8\u548c\u72c4\u62c9\u514b\u6062\u590d\u7684\u5e8f\u5217\u3002\u8fd9\u8868\u660e\u5728\u6b64\u62a5\u9053\u7684\u72b6\u6001\u5177\u6709\u5f3a\u70c8\u7834\u574f\u7684\u7535\u5b50\u504f\u597d\u5bf9\u79f0\u6027\u5e76\u6062\u590d\u4e86Dirac\u72b6\u7684\u7535\u5b50\u7279\u6027\uff0c\u5728\u9b54\u89d2\u77f3\u58a8\u70ef\u7684\u7269\u7406\u5b66\u4e2d\u5f88\u91cd\u8981\uff0c\u5f62\u6210\u4e86\u4e00\u79cd\u6bcd\u6001\uff0c\u5728\u8be5\u6bcd\u6001\u4e2d\uff0c\u8106\u6027\u66f4\u9ad8\u7684\u8d85\u5bfc\u548c\u76f8\u5173\u7edd\u7f18\u57fa\u6001\u51fa\u73b0\u3002<\/p>\n<p><strong><b>\u6587\u732e\u94fe\u63a5\uff1a<\/b><\/strong><\/p>\n<p><strong><b>Cascade of phase transitions and Dirac revivals in magic-angle graphene.<\/b><\/strong><\/p>\n<p><strong><b>(<\/b><\/strong><strong><b>Nature<\/b><\/strong><strong><b>, 2020, DOI:10.1038\/s41586-020-2373-y)<\/b><\/strong><\/p>\n<p><strong><b>7.\u9ebb\u7701\u7406\u5de5Pablo Jarillo-Herrero&amp;\u66f9\u539fNature\uff1a\u626d\u66f2\u7684\u53cc\u5c42-\u53cc\u5c42\u77f3\u58a8\u70ef\u4e2d\u7684\u53ef\u8c03\u8c10\u76f8\u5173\u72b6\u6001\u548c\u81ea\u65cb\u6781\u5316\u76f8<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-218022 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-8-7.png\" alt=\"\" width=\"600\" height=\"314\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-8-7.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-8-7-300x157.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u9b54\u89d2\u53cc\u7ede\u7ebf\u53cc\u5c42\u77f3\u58a8\u70ef\u4e2d\u76f8\u5173\u7edd\u7f18\u4f53\u72b6\u6001\u548c\u8d85\u5bfc\u6027\u7684\u6700\u65b0\u53d1\u73b0\u4f7f\u5f97\u80fd\u591f\u5bf9\u901a\u8fc7\u626d\u8f6c\u8303\u5fb7\u534e\u5f02\u8d28\u7ed3\u6784\u5b9e\u73b0\u7684\u53ef\u8c03\u5e26\u7cfb\u7edf\u4e2d\u7684\u7535\u5b50\u76f8\u5173\u6027\u8fdb\u884c\u5b9e\u9a8c\u7814\u7a76\u3002\u8fd9\u79cd\u65b0\u9896\u7684\u626d\u66f2\u89d2\u81ea\u7531\u5ea6\u548c\u63a7\u5236\u5ea6\u5e94\u8be5\u53ef\u4ee5\u63a8\u5e7f\u5230\u5176\u4ed6\u4e8c\u7ef4\u7cfb\u7edf\uff0c\u8fd9\u4e9b\u7cfb\u7edf\u53ef\u80fd\u8868\u73b0\u51fa\u76f8\u4f3c\u7684\u76f8\u5173\u7269\u7406\u884c\u4e3a\uff0c\u5e76\u4e14\u53ef\u4ee5\u4f7f\u6280\u672f\u80fd\u591f\u8c03\u8c10\u548c\u63a7\u5236\u7535\u5b50-\u7535\u5b50\u76f8\u4e92\u4f5c\u7528\u7684\u5f3a\u5ea6\u3002<strong><b>\u9ebb\u7701\u7406\u5de5Pablo Jarillo-Herrero&amp;\u66f9\u539f<\/b><\/strong>\u62a5\u9053\u4e86\u4e00\u4e2a\u57fa\u4e8e\u5c0f\u89d2\u5ea6\u626d\u66f2\u53cc\u5c42-\u53cc\u5c42\u77f3\u58a8\u70ef\uff08TBBG\uff09\u7684\u9ad8\u5ea6\u53ef\u8c03\u7684\u76f8\u5173\u7cfb\u7edf\uff0c\u8be5\u7cfb\u7edf\u7531\u4e24\u4e2a\u65cb\u8f6c\u7684\u4f2f\u7eb3\u5c14\u5806\u53e0\u7684\u53cc\u5c42\u77f3\u58a8\u70ef\u8584\u7247\u7ec4\u6210\u3002TBBG\u5177\u6709\u4e30\u5bcc\u7684\u76f8\u56fe\uff0c\u5177\u6709\u53ef\u8c03\u8c10\u7684\u76f8\u5173\u7edd\u7f18\u4f53\u72b6\u6001\uff0c\u5bf9\u626d\u66f2\u89d2\u548c\u7535\u4f4d\u79fb\u573a\u7684\u5e94\u7528\u90fd\u9ad8\u5ea6\u654f\u611f\uff0c\u7535\u4f4d\u79fb\u573a\u53ef\u4ee5\u6539\u53d8\u8d1d\u5c14\u7eb3\u5806\u53e0\u7684\u53cc\u5c42\u77f3\u58a8\u70ef\u7684\u56fa\u6709\u6781\u5316\u7387\u3002\u76f8\u5173\u7684\u7edd\u7f18\u4f53\u72b6\u6001\u53ef\u4ee5\u901a\u8fc7\u83ab\u5c14\u5355\u4f4d\u6676\u683c\u7684\u6240\u6709\u6574\u6570\u7535\u5b50\u7ffb\u8f6c\u5904\u7684\u4f4d\u79fb\u573a\u6765\u63a5\u901a\u548c\u65ad\u5f00\u3002\u8fd9\u4e9b\u76f8\u5173\u6001\u5bf9\u78c1\u573a\u7684\u54cd\u5e94\u8868\u660e\u81ea\u65cb\u6781\u5316\u7684\u57fa\u6001\u7684\u8bc1\u636e\uff0c\u4e0e\u9b54\u89d2\u626d\u66f2\u7684\u53cc\u5c42\u77f3\u58a8\u70ef\u5f62\u6210\u4e86\u9c9c\u660e\u7684\u5bf9\u6bd4\u3002\u6b64\u5916\uff0c\u5728\u8f83\u4f4e\u7684\u626d\u66f2\u89d2\u8303\u56f4\u5185\uff0cTBBG\u5728\u7535\u8377\u4e2d\u6027\u9644\u8fd1\u663e\u793a\u4e86\u591a\u7ec4\u5e26\uff0c\u5bfc\u81f4\u8bb8\u591a\u76f8\u5173\u72b6\u6001\u5bf9\u5e94\u4e8e\u8fd9\u4e9b\u5e26\u4e2d\u7684\u6bcf\u4e00\u4e2a\u7684\u534a\u7ffb\u8f6c\uff0c\u6240\u6709\u8fd9\u4e9b\u72b6\u6001\u4e5f\u90fd\u53ef\u4ee5\u901a\u8fc7\u4f4d\u79fb\u573a\u6765\u8c03\u8282\u3002\u8fd9\u4e2a\u7ed3\u679c\u53ef\u4ee5\u4f7f\u4eba\u4eec\u63a2\u7d22\u591a\u5e26\u626d\u66f2\u8d85\u6676\u683c\u4e2d\u626d\u66f2\u89d2\u548c\u7535\u573a\u63a7\u5236\u7684\u76f8\u5173\u76f8\u3002<\/p>\n<p><strong><b>\u6587\u732e\u94fe\u63a5\uff1a<\/b><\/strong><\/p>\n<p><strong><b>Tunable correlated states and spin-polarized phases in twisted bilayer<\/b><\/strong><strong><b>&#8211;<\/b><\/strong><strong><b>bilayer graphene.<\/b><\/strong><\/p>\n<p><strong><b>(<\/b><\/strong><strong><b>Nature<\/b><\/strong><strong><b>, 2020, DOI:10.1038\/s41586-020-2260-6)<\/b><\/strong><\/p>\n<p><strong><b>8.\u9b4f\u8328\u66fc\u79d1\u5b66\u7814\u7a76\u9662E. Zeldov&amp;\u9ebb\u7701\u7406\u5de5Pablo Jarillo-Herrero Nature\uff1a\u6620\u5c04\u9b54\u89d2\u77f3\u58a8\u70ef\u4e2d\u7684\u626d\u66f2\u89d2\u7d0a\u4e71\u548cLandau\u80fd\u7ea7<\/b><\/strong><\/p>\n<p><strong><b><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-218023 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-9-6.png\" alt=\"\" width=\"600\" height=\"604\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-9-6.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-9-6-150x150.png 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u7247-9-6-298x300.png 298w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\u6700\u8fd1\u53d1\u73b0\u7684\u7535\u5b50\u5e26\u4ee5\u53ca\u9b54\u672f\u89d2\u626d\u66f2\u53cc\u5c42\u77f3\u58a8\u70ef\uff08MATBG\uff09\u4e2d\u7684\u5f3a\u76f8\u5173\u548c\u8d85\u5bfc\u76f8\u81f3\u5173\u91cd\u8981\u5730\u53d6\u51b3\u4e8e\u5c42\u95f4\u626d\u66f2\u89d2\u03b8\u3002\u5c3d\u7ba1\u5df2\u7ecf\u8bc1\u660e\u4ee5\u5927\u7ea60.1\u5ea6\u7684\u7cbe\u5ea6\u63a7\u5236\u5168\u5c40\u03b8\uff0c\u4f46\u662f\u5173\u4e8e\u5c40\u90e8\u626d\u8f6c\u89d2\u7684\u5206\u5e03\u7684\u4fe1\u606f\u5f88\u5c11\u3002<strong><b>\u9b4f\u8328\u66fc\u79d1\u5b66\u7814\u7a76\u9662E. Zeldov&amp;\u9ebb\u7701\u7406\u5de5Pablo Jarillo-Herrero<\/b><\/strong>\u4f7f\u7528\u7eb3\u7c73\u7ea7\u5c16\u7aef\u626b\u63cf\u8d85\u5bfc\u91cf\u5b50\u5e72\u6d89\u88c5\u7f6e\uff08SQUID-on-tip\uff09\u83b7\u5f97\u5904\u4e8e\u91cf\u5b50\u970d\u5c14\u72b6\u6001\u7684Landau\u80fd\u7ea7\u7684\u65ad\u5c42\u56fe\u50cf\uff0c\u5e76\u7ed8\u5236\u516d\u65b9\u6c2e\u5316\u787c\uff08hBN\uff09\u5c01\u88c5\u7684MATBG\u4e2d\u7684\u5c40\u90e8\u03b8\u53d8\u5316\u56fe\u3002\u76f8\u5bf9\u7cbe\u5ea6\u4f18\u4e8e0.002\u5ea6\u4e14\u7a7a\u95f4\u5206\u8fa8\u7387\u53ea\u6709\u51e0\u4e2a\u83ab\u5c14\u5468\u671f\u7684\u8bbe\u5907\u3002\u4f5c\u8005\u53d1\u73b0\u4e86\u03b8\u7d0a\u4e71\u7a0b\u5ea6\u4e0eMATBG\u4f20\u8f93\u7279\u6027\u7684\u8d28\u91cf\u4e4b\u95f4\u7684\u76f8\u5173\u6027\uff0c\u5e76\u8868\u660e\u5373\u4f7f\u662f\u6700\u5148\u8fdb\u7684\u8bbe\u5907\uff0c\u5728\u03b8\u4e0a\u4e5f\u5b58\u5728\u76f8\u5f53\u5927\u7684\u5c40\u90e8\u53d8\u5316\uff0c\u6700\u9ad8\u53ef\u8fbe0.1\u5ea6\uff0c\u8868\u73b0\u51fa\u660e\u663e\u7684\u68af\u5ea6\u548c\u8df3\u8dc3\u7f51\u7edc\uff0c\u53ef\u80fd\u5305\u542b\u6ca1\u6709\u672c\u5730MATBG\u884c\u4e3a\u7684\u533a\u57df\u3002\u4f5c\u8005\u89c2\u5bdf\u5230MATBG\u4e2d\u7684\u76f8\u5173\u72b6\u6001\u76f8\u5bf9\u4e8e\u626d\u66f2\u89d2\u5f02\u5e38\u7279\u522b\u8106\u5f31\u3002\u6587\u7ae0\u8fd8\u8bc1\u660e\u4e86\u03b8\u7684\u68af\u5ea6\u4f1a\u4ea7\u751f\u5927\u7684\u6805\u6781\u53ef\u8c03\u9762\u5185\u7535\u573a\uff0c\u5373\u4f7f\u5728\u91d1\u5c5e\u533a\u57df\u4e5f\u4e0d\u4f1a\u88ab\u5c4f\u853d\uff0c\u8fd9\u4f1a\u901a\u8fc7\u5728\u6837\u54c1\u7684\u5927\u90e8\u5206\u533a\u57df\u4e2d\u5f62\u6210\u8fb9\u7f18\u901a\u9053\u800c\u6df1\u523b\u6539\u53d8\u91cf\u5b50\u970d\u5c14\u6001\uff0c\u5e76\u4e14\u53ef\u80fd\u4f1a\u5f71\u54cd\u76f8\u56fe\u548c\u8d85\u5bfc\u72b6\u6001\u3002\u56e0\u6b64\uff0c\u4f5c\u8005\u786e\u7acb\u4e86\u03b8\u7d0a\u4e71\u4f5c\u4e3a\u4e00\u79cd\u975e\u5e38\u89c4\u7c7b\u578b\u7684\u7d0a\u4e71\u7684\u91cd\u8981\u6027\uff0c\u80fd\u591f\u5c06\u626d\u66f2\u89d2\u68af\u5ea6\u7528\u4e8e\u5e26\u72b6\u7ed3\u6784\u5de5\u7a0b\uff0c\u5b9e\u73b0\u76f8\u5173\u73b0\u8c61\u4ee5\u53ca\u7528\u4e8e\u8bbe\u5907\u5e94\u7528\u7684\u95e8\u53ef\u8c03\u5185\u7f6e\u5e73\u9762\u7535\u573a\u3002<\/p>\n<p><strong><b>\u6587\u732e\u94fe\u63a5\uff1a<\/b><\/strong><\/p>\n<p><strong><b>Mapping the twist-angle disorder and Landau levels in magic-angle graphene.<\/b><\/strong><\/p>\n<p><strong><b>(<\/b><\/strong><strong><b>Nature<\/b><\/strong><strong><b>, 2020, DOI:10.1038\/s41586-020-2255-3)<\/b><\/strong><\/p>\n<p>\u672c\u6587\u7531tt\u4f9b\u7a3f\u3002<\/p>\n<p>\u672c\u5185\u5bb9\u4e3a\u4f5c\u8005\u72ec\u7acb\u89c2\u70b9\uff0c\u4e0d\u4ee3\u8868\u6750\u6599\u4eba\u7f51\u7acb\u573a\u3002<\/p>\n<p>\u672a\u7ecf\u5141\u8bb8\u4e0d\u5f97\u8f6c\u8f7d\uff0c\u6388\u6743\u4e8b\u5b9c\u8bf7\u8054\u7cfbkefu@cailiaoren.com\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1: tougao@cailiaoren.com.<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaorenVIP\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u725b\u5e74\u7684\u6700\u540e\u4e00\u4e2a\u4f11\u606f\u65e5\uff0c\u5927\u90e8\u5206\u793e\u755c\u8fd8\u6c89\u6d78\u5728\u5047\u671f\u5373\u5c06\u7ed3\u675f\u7684\u60b2\u75db\u4e2d&#8230;\u4e0e\u6b64\u540c\u65f6\uff0c\u5e74\u5ea6NS\u9489\u5b50\u6237\u8f6c\u89d2\u77f3\u58a8\u70ef\uff0c\u5b83\u5b83\u5b83\u53c8\u6765\u4e86\uff0c\u8fd9\u4e00\u6b21\u8fd8\u662fNature\u7684\u5c01\u9762\u3002 \u8fd9\u7bc7&#8230;<\/p>\n","protected":false},"author":11454,"featured_media":218014,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[1187],"tags":[],"class_list":["post-218012","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-zhuanlan"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/218012"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/11454"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=218012"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/218012\/revisions"}],"predecessor-version":[{"id":218025,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/218012\/revisions\/218025"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/218014"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=218012"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=218012"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=218012"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}