{"id":218239,"date":"2021-02-23T12:00:48","date_gmt":"2021-02-23T04:00:48","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=218239"},"modified":"2021-02-23T11:03:47","modified_gmt":"2021-02-23T03:03:47","slug":"%e3%80%90%e5%b7%b2%e5%9b%9e%e5%a4%8d%e3%80%91adv-mater-%ef%bc%9a%e9%9d%a2%e5%90%91%e5%ba%94%e7%94%a8%e7%9a%84%e9%ab%98%e9%9d%a2%e5%ae%b9%e9%87%8f%e6%b0%b4%e7%b3%bb%e9%94%8c%e7%a6%bb%e5%ad%90%e7%94%b5","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=218239","title":{"rendered":"Adv. Mater.\uff1a\u9762\u5411\u5e94\u7528\u7684\u9ad8\u9762\u5bb9\u91cf\u6c34\u7cfb\u950c\u79bb\u5b50\u7535\u6c60\uff1a\u91cf\u5316\u6c22\u7684\u9038\u51fa\u91cf\u548c\u7528\u4e8e\u7a33\u5b9a\u950c\u8d1f\u6781\u7684\u56fa\u4f53\u79bb\u5b50\u5bfc\u4f53"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u950c\uff08Zn\uff09\u8d1f\u6781\u6709\u671b\u5e94\u7528\u4e8e\u9ad8\u5b89\u5168\u6027\u548c\u4f4e\u6210\u672c\u7684\u6c34\u7cfb\u7535\u6c60\u3002\u7136\u800c\uff0cZn\u5728\u6c34\u6027\u73af\u5883\u4e2d\u70ed\u529b\u5b66\u4e0d\u7a33\u5b9a\u3002\u56e0\u6b64\uff0c\u5373\u4f7f\u5728\u95f2\u7f6e\u65f6\uff0cZn\u7535\u6781\u4f1a\u5206\u89e3\u6c34H<sub>2<\/sub>O\u4ea7\u751f\u6c22\u6c14\u3002\u8fd9\u4e2a\u957f\u671f\u4ee5\u6765\u88ab\u5ffd\u89c6\u7684\u95ee\u9898\u5c06\u663e\u7740\u5f71\u54cd\u7535\u6c60\u7684\u5bff\u547d\u3002Zn\u7535\u6c60\u7535\u5316\u5b66\u8fc7\u7a0b\u4e2d\uff0c\u6c22\u7684\u751f\u6210\u8fd8\u6ca1\u6709\u7cbe\u786e\u5b9a\u91cf\u5316\u3002\u91cf\u5316Zn\u6c89\u79ef\u8fc7\u7a0b\u4e2d\u7535\u6781\u4e0a\u4ea7\u751f\u7684\u6c22\u662f\u4e86\u89e3\u5bfc\u81f4\u5bb9\u91cf\u635f\u5931\u548c\u7535\u6c60\u6545\u969c\u7684\u673a\u7406\u7684\u5173\u952e\u3002\u53e6\u4e00\u65b9\u9762\uff0c\u6790\u6c22\u51fa\u53cd\u5e94\u5f15\u8d77\u7684Zn\u7a81\u8d77\u5c06\u5728\u7535\u5316\u5b66\u5faa\u73af\u8fc7\u7a0b\u4e2d\u7684\u96c6\u4e2d\u7535\u573a\u4e0b\u5438\u5f15\u66f4\u591a\u7684Zn<sup>2+<\/sup>\uff08\u201c\u5c16\u7aef\u201d\u6548\u5e94\uff09\uff0c\u4ece\u800c\u52a0\u901f\u4e86Zn\u679d\u6676\u7684\u5782\u76f4\u751f\u957f\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u9999\u6e2f\u57ce\u5e02\u5927\u5b66\u7684\u652f\u6625\u4e49\u6559\u6388\u3001\u674e\u6768\u6768\u6559\u6388<\/strong>\u548c<strong>\u9999\u6e2f\u7406\u5de5\u5927\u5b66\u7684\u9ec4\u6d77\u6d9b\u6559\u6388\uff08\u5171\u540c\u901a\u8baf\u4f5c\u8005\uff09<\/strong>\u7b49\u4eba\u91c7\u7528\u539f\u4f4d\u7535\u6c60-\u6c14\u76f8\u8272\u8c31-\u8d28\u8c31\u5206\u6790\u7cbe\u786e\u7684\u6d4b\u91cf\u4e86Zn\u7535\u6c60\u4e2d\u7684\u6c22\u6c14\u91ca\u653e\u91cf\u3002\u5728Zn\/\/Zn\u5bf9\u79f0\u7535\u6c60\u4e2d\uff0c\u6c22\u901a\u91cf\u8fbe\u52303.76 mmol h<sup>-1<\/sup> cm<sup>-2<\/sup>\uff0c\u800c\u5728Zn\/\/MnO<sub>2<\/sub>\u7535\u6c60\u4e2d\uff0c\u6c22\u901a\u91cf\u8fbe\u52307.70 mmol h<sup>-1<\/sup> cm<sup>-2<\/sup>\u3002\u56e0\u6b64\uff0c\u6784\u5efa\u5177\u6709\u9ad8Zn<sup>2+<\/sup>\u8f6c\u79fb\u6570\uff080.65\uff09\u7684\u9ad8\u5ea6\u7535\u7edd\u7f18\uff080.11 mS cm<sup>-1<\/sup>\uff09\u540c\u65f6\u5177\u6709\u9ad8Zn<sup>2+<\/sup>\u79bb\u5b50\u5bfc\u7535\u6027\uff0880.2 mS cm<sup>-1<\/sup>\uff09ZnF<sub>2<\/sub>\u56fa\u4f53\u79bb\u5b50\u5bfc\u4f53\uff0c\u4ee5\u5c06Zn\u4e0e\u6db2\u4f53\u7535\u89e3\u8d28\u9694\u79bb\u3002\u8fd9\u4e0d\u4ec5\u9632\u6b62\u4ea7\u751f\u8d85\u8fc799.2\uff05\u7684\u6c22\uff0c\u4e5f\u53ef\u5f15\u5bfc\u5747\u5300\u7684Zn\u7535\u6c89\u79ef\u3002\u7cbe\u786e\u6d4b\u91cf\u540e\uff0cZn@ZnF<sub>2<\/sub>\/\/Zn@ZnF<sub>2<\/sub>\u7535\u6c60\u4ec5\u4ea7\u751f0.02 mmol h<sup>-1<\/sup> cm<sup>-2<\/sup>\u7684\u6c22\uff08\u5360Zn\/\/Zn\u6c60\u76840.53\uff05\uff09\u3002\u53e6\u5916\uff0c\u9ad8\u9762\u5bb9\u91cf\u7684Zn@ZnF<sub>2<\/sub>\/\/MnO<sub>2<\/sub>\uff08~3.2 mAh cm<sup>-2<\/sup>\uff09\u5145\u6ee1\u7535\u65f6\uff0c\u4ec5\u4ea7\u751f0.06 mmol h<sup>-1<\/sup> cm<sup>-2<\/sup>\u7684\u6700\u5927\u6c22\u901a\u91cf\uff08\u5360Zn\/\/Zn\u7535\u6c60\u76840.78\uff05\uff09\u3002\u540c\u65f6\uff0cZn@ZnF<sub>2<\/sub>\/\/Zn@ZnF<sub>2<\/sub>\u5bf9\u79f0\u7535\u6c60\u5728590\u5c0f\u65f6\uff08285\u4e2a\u5faa\u73af\uff09\u5185\u5728\u8d85\u9ad8\u7535\u6d41\u5bc6\u5ea6\u548c\u9762\u5bb9\u91cf\uff0810 mA cm<sup>-2<\/sup>\u300110 mAh cm<sup>-2<\/sup>\uff09\u4e0b\u8868\u73b0\u51fa\u51fa\u8272\u7684\u7a33\u5b9a\u6027\uff0c\u8fdc\u80dc\u8fc7\u5df2\u62a5\u9053\u7684\u6c34\u6027\u4f53\u7cfb\u4e2d\u7684\u5176\u7684Zn\u8d1f\u6781\u3002\u76f8\u5173\u6210\u679c\u4ee5<strong>\u201c<\/strong><strong>Toward Practical High-Areal-Capacity Aqueous Zinc-Metal Batteries: Quantifying Hydrogen Evolution and a Solid-Ion Conductor for Stable Zinc Anodes<\/strong>\u201d\u53d1\u8868\u5728<strong>Advanced Materials<\/strong>\u4e0a\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe<\/strong><strong> 1 <\/strong><strong>\u5728<\/strong><strong>2 M ZnSO<sub>4<\/sub><\/strong><strong>\u6c34\u6eb6\u6db2\u4e2d\uff0c<\/strong><strong>Zn<\/strong><strong>\u7535\u6781\u7684\u7ed3\u6784\u8868\u5f81<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-218244\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/1-13.jpg\" alt=\"\" width=\"600\" height=\"447\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/1-13.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/1-13-300x224.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u901a\u8fc7\u7535\u6c60-\u6c14\u76f8\u8272\u8c31-\u8d28\u8c31\uff08GC-MS\uff09\u539f\u4f4d\u76d1\u6d4b\u6d78\u51652 M ZnSO<sub>4<\/sub>\u6c34\u6eb6\u6db2\u4e2d\u7684Zn\u7535\u6781\u7684\u6c22\u9038\u51fa\uff1b<\/p>\n<p>\uff08b\uff09\u5c06Zn\u7535\u6781\u6d78\u51652 M ZnSO<sub>4<\/sub>\u7535\u89e3\u8d28\u4e2d\u7684\u539f\u4f4dXRD\u56fe\u8c31\uff1b<\/p>\n<p>\uff08c\u2013f\uff09Zn\u7535\u6781\u548c\u6d78\u51652 M ZnSO<sub>4<\/sub>\u6c34\u6eb6\u6db2\u4e2d\uff0c2\uff0c5\u548c10\u5929\u540e\u7684Zn\u7535\u6781\u7684SEM\u56fe\u50cf\uff1b<\/p>\n<p>\uff08g\uff09\u5728Zn\u7b94\u4e0a\u7684Zn\u6c89\u79ef\u793a\u610f\u56fe\uff1b<\/p>\n<p>\uff08h\uff09\u5728Zn@ZnF<sub>2<\/sub>\u7b94\u4e0a\u7684Zn\u6c89\u79ef\u793a\u610f\u56fe\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong> 2 Zn<\/strong><strong>\u548c<\/strong><strong>Zn@ZnF<sub>2<\/sub><\/strong><strong>\u7684\u7ed3\u6784\u5206\u6790<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-218243\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/2-13.jpg\" alt=\"\" width=\"600\" height=\"467\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/2-13.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/2-13-300x234.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09Zn\u548cZn@ZnF<sub>2<\/sub>\u7b94\u7684XRD\u56fe\u8c31\uff1b<\/p>\n<p>\uff08b\uff09Zn@ZnF<sub>2<\/sub>\u7b94\u7684SEM\u56fe\u50cf\uff1b<\/p>\n<p>\uff08c\uff09Zn@ZnF<sub>2<\/sub>\u7b94\u7684\u9ad8\u5206\u8fa8\u7387Zn 2p\u5149\u8c31\uff1b<\/p>\n<p>\uff08d\uff09Zn\u7b94\u7684\u9ad8\u5206\u8fa8\u7387Zn 2p\u5149\u8c31\uff1b<\/p>\n<p>\uff08e\uff09Zn@ZnF<sub>2<\/sub>\u7b94\u7684F 1s\u5149\u8c31\uff1b<\/p>\n<p>\uff08f\uff0cg\uff09Zn@ZnF<sub>2<\/sub>\u754c\u9762\u7684\u7535\u8377\u5bc6\u5ea6\u5206\u5e03\u56fe\uff0c\u4ee5\u53ca\u76f8\u5e94\u7684\u4e8c\u7ef4\u7b49\u9ad8\u7ebf\u56fe\uff1b<\/p>\n<p>\uff08h\uff09ZnF<sub>2<\/sub>\uff08002\uff09\u8868\u9762\u548cZnF<sub>2<\/sub>\u4f53\u5185Zn<sup>2+<\/sup>\u7684\u6269\u6563\u80fd\u5792\u56fe\uff1b<\/p>\n<p>\uff08i\uff09ZnF<sub>2<\/sub>\uff0cZn@ZnF<sub>2<\/sub>\u8868\u9762\u548cZn\uff08002\uff09\u8868\u9762\u4e0a\u5355\u4e2aZn\u539f\u5b50\u7684\u63d2\u5165\u80fd\u5792\u63d2\u56fe\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong> 3 Zn\/\/Cu<\/strong><strong>\u7535\u6c60\u548c<\/strong><strong>Zn@ZnF<sub>2<\/sub>\/\/Cu<\/strong><strong>\u7535\u6c60\u7684\u6027\u80fd\u5206\u6790<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-218242\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/3-14.jpg\" alt=\"\" width=\"600\" height=\"481\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/3-14.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/3-14-300x241.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09ZnF<sub>2<\/sub>\u5c42\u548c\u5e38\u89c4GF\u9694\u819c\u6d78\u67092 M ZnSO<sub>4<\/sub>\u7535\u89e3\u8d28\u7684\u79bb\u5b50\u7535\u5bfc\u7387\uff1b<\/p>\n<p>\uff08b\uff09ZnF<sub>2<\/sub>\u5c42\u548cZn\u7684\u7535\u5b50\u7535\u5bfc\u7387\uff1b<\/p>\n<p>\uff08c\uff09\u57281\u30012\u548c5 mA cm<sup>-2<\/sup>\uff08\u5bb9\u91cf\u4e3a1 mAh cm<sup>-2<\/sup>\uff09\u4e0b\uff0cZn\/\/Zn\u5bf9\u79f0\u7535\u6c60\u548cZn@ZnF<sub>2<\/sub>\/\/Zn@ZnF<sub>2<\/sub>\u5bf9\u79f0\u7535\u6c60\u7684\u5faa\u73af\u7a33\u5b9a\u6027\u6bd4\u8f83\u56fe\uff1b<\/p>\n<p>\uff08d\uff09\u500d\u7387\u6027\u80fd\u56fe\uff1b<\/p>\n<p>\uff08e\uff09\u572810 mA cm<sup>-2<\/sup>\u548c10 mAh cm<sup>-2<\/sup>\u4e0b\uff0cZn\/\/Zn\u5bf9\u79f0\u7535\u6c60\u548cZn@ZnF<sub>2<\/sub>\/\/Zn@ZnF<sub>2<\/sub>\u5bf9\u79f0\u7535\u6c60\u7684\u5faa\u73af\u7a33\u5b9a\u6027\uff1b<\/p>\n<p>\uff08f\uff09\u8fd9\u9879\u5de5\u4f5c\u4e0e\u5df2\u62a5\u9053\u7684\u5de5\u4f5c\u7684\u4e0d\u540c\u7535\u6d41\u5bc6\u5ea6\u4e0b\u7684\u53ef\u9006\u5bb9\u91cf\u5bf9\u6bd4\u56fe\uff1b<\/p>\n<p>\uff08g\uff0ch\uff0950\u6b21\u5faa\u73af\u540e\u7684Zn@ZnF<sub>2<\/sub>\u548cZn\u7684SEM\u56fe\u50cf\uff1b<\/p>\n<p>\uff08i\uff0cj\uff09\u57281 mAh cm<sup>-2<\/sup>\u548c2 mA cm<sup>-2<\/sup>\u65f6\uff0cZn\u6eb6\u89e3\u5ea6\u548cZn@ZnF<sub>2<\/sub>\u5728\u7684\u950c\u6c89\u79ef\u7684\u6a2a\u622a\u9762SEM\u56fe\u50cf\uff1b<\/p>\n<p>\uff08k\uff09\u57281 mA cm<sup>-2<\/sup>\u548c1 mAh cm<sup>-2<\/sup>\u65f6\uff0cZn\/\/Cu\u7535\u6c60\u548cZn@ZnF<sub>2<\/sub>\/\/Cu\u7535\u6c60\u5d4c\u5165\/\u8131\u51fa\u950c\u7684\u5e93\u4f26\u6548\u7387\uff1b<\/p>\n<p>\uff08l\uff09Zn@ZnF<sub>2<\/sub>\/\/Cu\u7535\u6c60\u5728\u7b2c1\u30015\u300110\u3001100\u3001500\u548c1000\u5708\u7684\u5bb9\u91cf-\u7535\u538b\u66f2\u7ebf\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong> 4 <\/strong><strong>Zn\/\/Zn<\/strong><strong>\u5bf9\u79f0\u7535\u6c60\u548c<\/strong><strong>Zn@ZnF<sub>2<\/sub>\/\/Zn@ZnF<sub>2<\/sub><\/strong><strong>\u7535\u6c60\u7684\u539f\u4f4d\u6790\u6c22\u5206\u6790<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-218241\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/4-13.jpg\" alt=\"\" width=\"600\" height=\"373\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/4-13.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/4-13-300x187.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff0cb\uff09Zn\u7b94\u548cZn@ZnF<sub>2<\/sub>\u7b94\u7684\u9540\u950c\u884c\u4e3a\u7684\u539f\u4f4d\u5149\u5b66\u53ef\u89c6\u5316\u89c2\u5bdf\uff1b<\/p>\n<p>\uff08c\uff0cd\uff09\u539f\u4f4d\u6d4b\u91cfZn\/\/Zn\u5bf9\u79f0\u7535\u6c60\u548cZn@ZnF<sub>2<\/sub>\/\/Zn@ZnF<sub>2<\/sub>\u5bf9\u79f0\u7535\u6c60\u7684\u6790\u6c22\u901a\u91cf\uff1b<\/p>\n<p>\uff08e\uff0cf\uff09\u9ad8\u9762\u5bb9\u91cfZn\/\/MnO<sub>2<\/sub>\u7535\u6c60\u548cZn@ZnF<sub>2<\/sub>\/\/MnO<sub>2<\/sub>\u7535\u6c60\u7684\u6c22\u6c14\u91ca\u653e\u901a\u91cf\uff1b<\/p>\n<p>\uff08g\uff09\u5728Zn@ZnF<sub>2<\/sub>\u754c\u9762\u548cZn\uff08002\uff09\u4e0a\u53d1\u751f\u6c22\u91ca\u653e\u53cd\u5e94\u7684\u5409\u5e03\u65af\u81ea\u7531\u80fd\u56fe\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong> 5<\/strong> <strong>Zn\/\/MnO<sub>2<\/sub><\/strong><strong>\u548c<\/strong><strong>Zn@ZnF<sub>2<\/sub>\/\/MnO<sub>2<\/sub><\/strong><strong>\u7535\u6c60\u7684\u6027\u80fd\u8868\u5f81<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-218240\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/5-9.jpg\" alt=\"\" width=\"600\" height=\"476\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/5-9.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/5-9-300x238.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09Zn@ZnF<sub>2<\/sub>\/\/MnO<sub>2<\/sub>\u7535\u6c60\u5728\u7b2c1\u3001100\u3001500\u548c1000\u5708\u5faa\u73af\u7684\u6052\u7535\u6d41\u5145\/\u653e\u7535\u66f2\u7ebf\uff1b<\/p>\n<p>\uff08b\uff09Zn\/MnO<sub>2<\/sub>\u7535\u6c60\u5728\u7b2c1\uff0c100\uff0c200\u548c300\u5708\u5faa\u73af\u7684\u6052\u7535\u6d41\u5145\u7535\/\u653e\u7535\u66f2\u7ebf\uff1b<\/p>\n<p>\uff08c\uff09Zn\/\/MnO<sub>2<\/sub>\u548cZn@ZnF<sub>2<\/sub>\/\/MnO<sub>2<\/sub>\u7535\u6c60\u7684\u5faa\u73af\u7a33\u5b9a\u6027\uff1b<\/p>\n<p>\uff08d\uff0ce\uff09Zn@ZnF<sub>2<\/sub>\/\/MnO<sub>2<\/sub>\u7535\u6c60\u6d4b\u8bd5\u540e\u7684Zn@ZnF<sub>2<\/sub>\u7b94\u7684SEM\u56fe\u50cf\u548cZn\/\/MnO<sub>2<\/sub>\u7535\u6c60\u7684Zn\u7b94\u7684SEM\u56fe\u50cf\uff1b<\/p>\n<p>\uff08f\uff0cg\uff09\u5faa\u73af\u6d4b\u8bd5\u540e\uff0cZn\/\/MnO<sub>2<\/sub>\u548cZn@ZnF<sub>2<\/sub>\/\/MnO<sub>2<\/sub>\u7535\u6c60\u7684\u5149\u5b66\u7167\u7247\uff1b<\/p>\n<p>\uff08h\uff09\u5728850 mAh\u7684\u5927\u5bb9\u91cf\u4e0b\uff0cZn\/\/MnO<sub>2<\/sub>\u548cZn@ZnF<sub>2<\/sub>\/\/MnO<sub>2<\/sub>\u7535\u6c60\u7684\u5faa\u73af\u7a33\u5b9a\u6027\u3002<\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u603b\u4e4b\uff0c\u672c\u6587\u901a\u8fc7\u539f\u4f4d\u7535\u6c60-\u6c14\u76f8\u8272\u8c31-\u8d28\u8c31\u5206\u6790\u6cd5\u5b9a\u91cf\u8bc4\u4f30\u4e86Zn\u6c89\u79ef\u8fc7\u7a0b\u4e2d\u7684\u6c22\u653e\u51fa\u901a\u91cf\uff0c\u5305\u62ecZn\/\/Zn\u4e0d\u5bf9\u79f0\u7535\u6c60\u548cZn\/\/MnO<sub>2<\/sub>\u7535\u6c60\u3002\u5728Zn\/\/Zn\u7535\u6c60\u7684\u6bcf\u4e2a\u5faa\u73af\u4e2d\uff0c\u6790\u6c22\u901a\u91cf\u8fbe\u52303.76 mmol h<sup>-1<\/sup> cm<sup>-2<\/sup>\uff0c\u800c\u5728Zn\/\/MnO<sub>2<\/sub>\uff08~3.2 mAh cm<sup>-2<\/sup>\uff09\u7535\u6c60\u4e2d\uff0c\u6c22\u6c14\u91ca\u653e\u901a\u91cf\u6700\u5927\u4e3a7.70 mmol h<sup>-1<\/sup> cm<sup>-2<\/sup>\u3002\u672c\u6587\u5236\u5907\u4e86\u56fa\u6001ZnF<sub>2<\/sub>\u7684Zn<sup>2+<\/sup>\u79bb\u5b50\u5bfc\u4f53\u3002\u4e0eZn\u7535\u6781\u76f8\u6bd4\uff0cZn@ZnF<sub>2<\/sub>\u7535\u6781\u663e\u793a\u51fa\u8f83\u5f3a\u7684\u6c22\u6291\u5236\u80fd\u529b\uff08\u5bf9\u79f0\u7535\u6c60\u4e2d\u4e3a3.76 <em>vs<\/em>. 0.02 mmol h<sup>-1<\/sup> cm<sup>-2<\/sup>\uff1b\u5145\u6ee1\u7535\u6c60\u4e2d\u4e3a7.70 <em>vs<\/em>. 0.06 mmol h<sup>-1<\/sup> cm<sup>-2<\/sup>\uff09\u3002\u540c\u65f6\uff0cZn@ZnF<sub>2<\/sub>\u7ed3\u6784\u53ef\u8c03\u8282Zn\u6c89\u79ef\u5e76\u4fc3\u8fdbZn<sup>2+<\/sup>\u6269\u6563\u3002\u56e0\u6b64\uff0c\u57285 mA cm<sup>-2<\/sup>\u65f6\uff0cZn@ZnF<sub>2<\/sub>\/\/Zn@ZnF<sub>2<\/sub>\u5bf9\u79f0\u6027\u7535\u6c60\u57282500 h\u5185\u8868\u73b0\u51fa\u9ad8\u5ea6\u53ef\u9006\u7684Zn\u5faa\u73af\uff1b\u572810 mA cm<sup>-2<\/sup>\uff0c10 mAh cm<sup>-2<\/sup>\u7684\u9ad8\u9762\u5bb9\u91cf\u548c\u4f4e56.4 mV\u603b\u8fc7\u7535\u4f4d\u4e0b\uff0c\u5177\u6709\u8f83\u597d\u7684\u5faa\u73af\u6027\u80fd\u3002\u7ed3\u679c\u8868\u9762\uff1a~3.2 mAh cm<sup>-2<\/sup>\u7684\u9ad8\u9762\u5bb9\u91cf\u7684Zn@ZnF<sub>2<\/sub>\/\/MnO<sub>2<\/sub>\u7535\u6c60\u53ef\u4ee5\u8fd0\u884c1000\u5708\uff0c\u5bb9\u91cf\u4fdd\u6301\u7387\u4e3a\u521d\u59cb\u5bb9\u91cf\u768493.63\uff05\u3002\u6700\u540e\uff0c4\u00d76 cm<sup>2<\/sup>\u7684850 mAh\u5927\u5bb9\u91cfZn@ZnF<sub>2<\/sub>\/\/MnO<sub>2<\/sub>\u7535\u6c60\u53ef\u4ee5\u5728160\u4e2a\u5faa\u73af\uff08800\u5c0f\u65f6\uff09\u5185\u53ef\u9006\u5730\u5de5\u4f5c\uff0c\u4ecd\u4fdd\u7559\u4e8693.17\uff05\u7684\u521d\u59cb\u5bb9\u91cf\u3002\u8fd9\u79cd\u5177\u6709\u9ad8\u53ef\u9006\u6027\u548c\u663e\u7740\u6291\u5236\u526f\u53cd\u5e94\u7684\u5148\u8fdbZn\u91d1\u5c5e\u8d1f\u6781\u7684\u7b56\u7565\u4e3a\u5b9e\u73b0\u9ad8\u9762\u5bb9\u91cf\u7684Zn\u91d1\u5c5e\u7535\u6c60\u63d0\u4f9b\u4e86\u4e00\u6761\u9014\u5f84\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5<\/strong><a href=\"https:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/adma.202007406\" target=\"_blank\" rel=\"noopener\"><strong>Toward Practical High-Areal-Capacity Aqueous Zinc-Metal Batteries: Quantifying Hydrogen Evolution and a Solid-Ion Conductor for Stable Zinc Anodes<\/strong><\/a>\uff08Advanced Materials DOI: 10.1002\/adma.202007406\uff09\u3002<\/p>\n<p><strong>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1a<\/strong><strong>cailiaokefu<\/strong><strong>\uff0c\u6211\u4eec\u4f1a\u9080\u8bf7\u5404\u4f4d\u8001\u5e08\u52a0\u5165\u4e13\u5bb6\u7fa4\u3002<\/strong><\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u950c\uff08Zn\uff09\u8d1f\u6781\u6709\u671b\u5e94\u7528\u4e8e\u9ad8\u5b89\u5168\u6027\u548c\u4f4e\u6210\u672c\u7684\u6c34\u7cfb\u7535\u6c60\u3002\u7136\u800c\uff0cZn\u5728\u6c34\u6027\u73af\u5883\u4e2d\u70ed\u529b\u5b66\u4e0d\u7a33\u5b9a\u3002\u56e0\u6b64\uff0c\u5373\u4f7f\u5728\u95f2\u7f6e\u65f6\uff0cZn\u7535\u6781\u4f1a\u5206\u89e3\u6c34H2O\u4ea7\u751f\u6c22\u6c14\u3002\u8fd9\u4e2a\u957f\u671f\u4ee5&#8230;<\/p>\n","protected":false},"author":7035,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[4580,2978],"class_list":["post-218239","post","type-post","status-publish","format-standard","hentry","category-jiedu","tag-4580","tag-2978"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/218239"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/7035"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=218239"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/218239\/revisions"}],"predecessor-version":[{"id":218266,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/218239\/revisions\/218266"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=218239"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=218239"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=218239"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}