{"id":218311,"date":"2021-02-25T06:30:50","date_gmt":"2021-02-24T22:30:50","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=218311"},"modified":"2021-03-03T11:47:16","modified_gmt":"2021-03-03T03:47:16","slug":"%e4%b8%8a%e5%b8%88%e5%a4%a7acs-nano%ef%bc%9a%e6%8f%90%e9%ab%98mxene%e5%9c%a8%e6%9c%89%e6%9c%ba%e6%ba%b6%e5%89%82%e7%9a%84%e5%88%86%e6%95%a3%e5%ba%a6","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=218311","title":{"rendered":"\u4e0a\u5e08\u5927ACS NANO\uff1a\u63d0\u9ad8MXene\u5728\u6709\u673a\u6eb6\u5242\u7684\u5206\u6563\u5ea6"},"content":{"rendered":"<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-218314 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72471-13.png\" alt=\"\" width=\"600\" height=\"203\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72471-13.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72471-13-300x102.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u3010\u6587\u7ae0\u4fe1\u606f\u3011<\/b><\/strong><\/p>\n<p>High Concentration of Ti<sub>3<\/sub>C<sub>2<\/sub>T<sub>x<\/sub>\u00a0MXene in\u00a0Organic Solvent<\/p>\n<p>\u7b2c\u4e00\u4f5c\u8005\uff1a\u5f20\u5e86\u8427<\/p>\n<p>\u901a\u8baf\u4f5c\u8005\uff1a\u674e\u8f89*<\/p>\n<p>\u5355\u4f4d\uff1a\u4e0a\u6d77\u5e08\u8303\u5927\u5b66<\/p>\n<p><strong><b>\u3010\u89c6\u9891\u4fe1\u606f\u3011<\/b><\/strong><\/p>\n<p>\u4ece\u591a\u5c42MXene\u6750\u6599\u5230\u5355\u5c42MXene\u6750\u6599\u7684\u5206\u6563\uff0c\u53ef\u4ee5\u6709\u591a\u901f\u5ea6\uff1f\u89c6\u9891\u544a\u8bc9\u4f60\uff0c\u53ea\u9700\u89815\u79d2\uff01\uff08\u9644\uff1a\u9664\u5b57\u5e55\u5916\uff0c\u5168\u7a0b\u65e0\u526a\u8f91\uff09<\/p>\n<div style=\"width: 368px;\" class=\"wp-video\"><!--[if lt IE 9]><script>document.createElement('video');<\/script><![endif]-->\n<video class=\"wp-video-shortcode\" id=\"video-218311-1\" width=\"368\" height=\"640\" preload=\"metadata\" controls=\"controls\"><source type=\"video\/mp4\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/797937d7994ee94f146a62851c53926e.mp4?_=1\" \/><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/797937d7994ee94f146a62851c53926e.mp4\">http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/797937d7994ee94f146a62851c53926e.mp4<\/a><\/video><\/div>\n<p><strong><b>\u3010\u5f15\u8a00\u3011<\/b><\/strong><\/p>\n<p>MXene\u662f\u5f53\u524d\u6700\u70ed\u95e8\u7684\u4e8c\u7ef4\u6750\u6599\u4e4b\u4e00\u3002\u4f46\u662f\uff0c\u5982\u4f55\u83b7\u5f97\u9ad8\u5728\u6709\u673a\u6eb6\u5242\u4e2d\u9ad8\u5ea6\u5206\u6563\u7684MXene\u6750\u6599\u4ecd\u7136\u662f\u5f53\u524d\u7814\u7a76\u7684\u4e00\u4e2a\u5de8\u5927\u6311\u6218\u3002\u76ee\u524d\u6587\u732e\u62a5\u9053\u7684\u5e38\u89c4\u65b9\u6848\u5236\u5907\u7684MXene\u6750\u6599\u7684\u6eb6\u89e3\u5ea6\u5f80\u5f80\u4e0d\u8db30.5 mg\/ml\u3002\u73b0\u6709\u7684\u4e24\u79cd\u5236\u5907\u9ad8\u6d53\u5ea6MXene\u6709\u673a\u6eb6\u5242\u7684\u5206\u6563\u6db2\u7684\u624b\u6bb5\u65e0\u6cd5\u6ee1\u8db3\u79d1\u7814\u5de5\u4f5c\u8005\u7684\u9700\u6c42\uff0c\u6eb6\u5242\u7f6e\u6362\u6cd5\u64cd\u4f5c\u590d\u6742\u3001\u4ea7\u7387\u4f4e\uff0c\u9020\u6210\u4e86\u6750\u6599\u6d6a\u8d39\uff1b\u8868\u9762\u4fee\u9970\u6cd5\u5f80\u5f80\u9700\u8981\u7528\u5230\u5927\u91cf\u7684\u8868\u9762\u4fee\u9970\u5242\uff0c\u4e14\u4e0d\u6613\u53bb\u9664\u3002\u800c\u5728\u590d\u5408\u6750\u6599\u548c\u5f88\u591a\u5bf9\u6c34\u654f\u611f\u7684\u5e94\u7528\u9886\u57df\uff0c\u6d01\u51c0\u3001\u9ad8\u6d53\u5ea6\u7684MXene\u6709\u673a\u6eb6\u5242\u5206\u6563\u6db2\u7684\u5236\u5907\u96be\u9898\u662f\u963b\u788d\u8be5\u9886\u57df\u53d1\u5c55\u7684\u4e00\u4e2a\u4e9f\u5f85\u89e3\u51b3\u7684\u79d1\u5b66\u95ee\u9898\u3002<\/p>\n<p><strong><b>\u3010\u6210\u679c\u4ecb\u7ecd\u3011<\/b><\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c\u4e0a\u6d77\u5e08\u8303\u5927\u5b66\u7684\u674e\u8f89\u6559\u6388\u5e26\u9886\u8bfe\u9898\u7ec4\uff0c\u5728\u56fd\u9645\u77e5\u540d\u671f\u520aACS Nano\u4e0a\u53d1\u8868\u9898\u4e3a\u201cHigh Concentration of Ti<sub>3<\/sub>C<sub>2<\/sub>T<sub>x<\/sub>\u00a0MXene in Organic Solvent\u201d\u7684\u7814\u7a76\u8bba\u6587\u3002\u672c\u7bc7\u6587\u7ae0\u5c55\u793a\u4e86\u674e\u8f89\u6559\u6388\u7684\u5728\u9ad8\u6d53\u5ea6MXene\u6709\u673a\u6eb6\u5242\u5206\u6563\u6db2\u65b9\u9762\u7684\u5de5\u4f5c\u3002\u6587\u7ae0\u8be6\u7ec6\u7684\u4ecb\u7ecd\u4e86\u8868\u9762\u5fae\u73af\u5883\u4fee\u9970\u6cd5\uff08TMM\uff09\u5236\u5907\u9ad8\u6d53\u5ea6\u6709\u673a\u6eb6\u5242\u7684\u65b9\u6848\uff0c\u5e76\u5bf9\u5408\u6210\u673a\u7406\u8fdb\u884c\u4e86\u6df1\u5165\u63a2\u8ba8\uff0c\u540c\u65f6\u8be5\u65b9\u6848\u5b8c\u7f8e\u7684\u89e3\u51b3\u4e86MXene\u7684\u6c27\u5316\u95ee\u9898\u3002\u672c\u6587\u4e3a\u672a\u6765MXene\u7684\u7814\u7a76\u63d0\u4f9b\u9ad8\u6548\u7684\u5236\u5907\u8def\u5f84\uff0c\u6709\u52a9\u4e8e\u52a0\u901fMXene\u6750\u6599\u9886\u57df\u7684\u7814\u7a76\u53ca\u5b9e\u9645\u5e94\u7528\u3002<\/p>\n<p><strong><b>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/b><\/strong><\/p>\n<p>\u53d7\u9650\u4e8eMXene\u7684\u4eb2\u6c34\u6027\uff0c\u5982\u4f55\u5236\u5907\u9ad8\u6d53\u5ea6MXene\u6709\u673a\u6eb6\u5242\u4e00\u76f4\u662f\u60ac\u800c\u672a\u51b3\u7684\u95ee\u9898\u3002\u65e9\u57282017\u5e74\uff0cYury Gogotsi\u6559\u6388\u7b49\u4eba\u5c31\u7cfb\u7edf\u7814\u7a76\u4e86Ti<sub>3<\/sub>C<sub>2<\/sub>T<sub>x<\/sub>\u5728\u6709\u673a\u6eb6\u5242\u4e2d\u7684\u5206\u6563\u6027\uff0c\u6700\u7ec8\u5236\u5907\u7684MXene\u5728\u6709\u673a\u6eb6\u5242\u4e2d\u7684\u6700\u9ad8\u6d53\u5ea6\u4ec5\u4ec5\u4e0d\u8db30.5 mg\/mL\u3002\u968f\u540e\u53d1\u5c55\u7684\u8868\u9762\u4fee\u9970\u6cd5\u4e5f\u9700\u8981\u5927\u91cf\u7684\u8868\u9762\u4fee\u9970\u5242\uff0c\u5f80\u5f80\u9700\u8981\u4e0eMXene\u540c\u7b49\u6570\u91cf\u7ea7\u7684\u8868\u9762\u4fee\u9970\u5242\uff0c\u5927\u5927\u963b\u788d\u4e86MXene\u7684\u7814\u7a76\u8fdb\u5c55\u3002\u4e3a\u4e86\u89e3\u51b3\u4e0a\u8ff0\u95ee\u9898\uff0c\u4f5c\u8005\u53d1\u5c55\u4e86TMM\u6cd5\u5236\u5907\u9ad8\u6d53\u5ea6MXene\u6709\u673a\u6eb6\u5242\uff08\u56fe1-2\uff09\u3002\u672c\u65b9\u6848\u53ef\u4ee5\u5feb\u901f\u9ad8\u6548\u7684\u5236\u5907\u6eb6\u89e3\u4e8eDMF\u3001DMAc\u3001PC\u7684\u9ad8\u6d53\u5ea6MXene\u5206\u6563\u6db2\u3002\u6587\u7ae0\u652f\u6491\u89c6\u9891\u5c55\u793a\u4e86\u591a\u5c42MXene\u5728PC\u6eb6\u5242\u4e2d\u7684\u5feb\u901f\u5206\u6563\uff0c\u8be5\u8fc7\u7a0b\u53ea\u9700\u89815s\u7684\u7b80\u5355\u624b\u6447\u5373\u53ef\u5b9e\u73b0\u3002<\/p>\n<p>\u901a\u8fc7\u5b9e\u9a8c\u63a2\u7a76\u53d1\u73b0\uff0cTMM\u6cd5\u7684\u4f18\u52bf\u5728\u4e8e\u9633\u79bb\u5b50\u7684\u63d2\u5c42\u548c\u5bf9\u6750\u6599\u8868\u9762\u4eb2\u758f\u6c34\u6027\u7684\u6539\u53d8\uff0c\u540c\u65f6\u4e5f\u4f9d\u8d56\u4e8e\u5408\u9002\u7684\u6eb6\u5242\u6027\u8d28\u4ee5\u5206\u6563MXene\u7eb3\u7c73\u7247\u3002\u4f5c\u8005\u4ece\u6eb6\u5242\u6027\u8d28\u548cMXene\u6750\u6599\u8868\u9762\u53d8\u5316\u4e24\u4e2a\u65b9\u9762\uff0c\u7cfb\u7edf\u6df1\u5165\u7684\u7814\u7a76\u4e86\u5982\u4f55\u63d0\u9ad8MXene\u5728\u6709\u673a\u6eb6\u5242\u4e2d\u7684\u5206\u6563\u6027\u3002\u5f97\u51fa\u5982\u4e0b\u7ed3\u8bba\uff0c1\uff0c\u5c11\u91cfTBA+\u7684\u4fee\u9970\u548c\u5bf9Ti3C2Tx\u8868\u9762\u7684\u6539\u6027\u4f7f\u5f97MXene\u7684\u4eb2\u758f\u6c34\u6027\u53d1\u751f\u4e86\u53d8\u5316\uff08\u56fe2\uff09\u30022\uff0c\u7ecf\u8fc7\u8ba1\u7b97\uff0c Ti3C2Tx\u7684Hansen\u6eb6\u5ea6\u53c2\u6570\u7684\u7ea6\u4e3a18.05 MPa<sup>1\/2<\/sup>\uff0c14.48 MPa<sup>1\/2<\/sup>\u548c8.76 MPa<sup>1\/2<\/sup>\u3002\uff08\u56fe3\uff09\u8fd9\u4e3a\u8fdb\u4e00\u6b65\u5bfb\u627e\u9002\u5408MXene\u7684\u6709\u673a\u6eb6\u5242\u5206\u6563\u6db2\u63d0\u4f9b\u66f4\u5177\u4f53\u7684\u53c2\u8003\u3002\u8be5\u65b9\u6848\u5355\u5c42\u6750\u6599\u7684\u5265\u79bb\u4ea7\u7387\u53ef\u4ee5\u8fbe\u523090%\u4ee5\u4e0a\uff0c\u4f7f\u7528\u8be5\u65b9\u6cd5\u53ef\u4ee5\u4e00\u9505\u5265\u79bb30 g\u591a\u5c42Ti3C2Tx\u539f\u6599\u3002\u5265\u79bb\u5f97\u5230\u7684Ti3C2Tx\u7eb3\u7c73\u7247\u8868\u9762\u6e05\u6d01\uff0c\u539a\u5ea6\u5747\u5300\uff0c\u5177\u6709\u8f83\u5927\u7684\u5c3a\u5bf8\u3002Ti<sub>3<\/sub>C<sub>2<\/sub>T<sub>x<\/sub>\u00a0MXene\u7684\u6709\u673a\u6eb6\u5242\u5206\u6563\u6db2\u5373\u4f7f\u5728\u5e38\u6e29\u6709\u6c27\u6761\u4ef6\u4e0b\uff0c\u4e5f\u5177\u6709\u5353\u8d8a\u7684\u6297\u6c27\u5316\u6027\u80fd\u3002\uff08\u56fe4\uff09<\/p>\n<p>\u5c06\u9ad8\u5206\u6563\u5728DMF\u6eb6\u6db2\u4e2d\u7684Ti<sub>3<\/sub>C<sub>2<\/sub>T<sub>x<\/sub>\u4e0ePAN\u6df7\u5408\u6db2\u8fdb\u884c\u4e86\u6e7f\u6cd5\u7eba\u4e1d\uff0c\u53ef\u4ee5\u5236\u5f97\u5177\u6709\u4f18\u5f02\u7535\u5bfc\u7387\u7684\u590d\u5408\u6750\u6599\uff08\u56fe5\uff09\u3002\u6700\u540e\uff0c\u591a\u79cd\u7c7b\u578b\u7684MXene\u90fd\u53ef\u4ee5\u91c7\u7528TMM\u6cd5\u5236\u5907\u9ad8\u6d53\u5ea6\u6709\u673a\u6eb6\u5242\u5206\u6563\u6db2\uff0c\u4f8b\u5982\uff1aNb<sub>2<\/sub>CT<sub>x<\/sub>\uff0cNb<sub>4<\/sub>C<sub>3<\/sub>T<sub>x<\/sub>\uff0cMo<sub>2<\/sub>Ti<sub>2<\/sub>C<sub>3<\/sub>T<sub>x<\/sub>\uff0c\u8bc1\u660e\u4e86\u8be5\u65b9\u6cd5\u7684\u666e\u9002\u6027\u3002\u8fd9\u9879\u5de5\u4f5c\u5c06\u4e3aMXene\u6750\u6599\u5bb6\u65cf\u7684\u7814\u7a76\u5e26\u6765\u65b0\u7684\u673a\u9047\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-218315 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72472-13.png\" alt=\"\" width=\"600\" height=\"443\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72472-13.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72472-13-300x222.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u56fe1.<\/b><\/strong><strong><b>\u00a0<\/b><\/strong>\u9ad8\u6d53\u5ea6MXene\u6709\u673a\u6eb6\u5242\u6750\u6599\u7684\u5236\u5907\u65b9\u6848\u548c\u4e0d\u540c\u6eb6\u5242\u4e2dTi3C2Tx\u7eb3\u7c73\u7247\u7684SEM\u56fe\u50cf\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-218316 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72473-13.png\" alt=\"\" width=\"600\" height=\"353\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72473-13.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72473-13-300x177.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>2<\/b><\/strong><strong><b>\uff1a <\/b><\/strong>\uff08a\uff09TMM\u6cd5\u5236\u5907\u9ad8\u6d53\u5ea6MXene\u6709\u673a\u6eb6\u5242\u5206\u6563\u6db2\u7684\u6d41\u7a0b\u793a\u610f\u56fe\uff08b\uff09S-Ti<sub>3<\/sub>C<sub>2<\/sub>T<sub>x<\/sub>-H<sub>2<\/sub>O; \uff08c\uff09S-Ti<sub>3<\/sub>C<sub>2<\/sub>T<sub>x<\/sub>-PC\uff1b\uff08d\uff09\u00a0S-Ti<sub>3<\/sub>C<sub>2<\/sub>T<sub>x<\/sub>-DMAc ; \uff08e\uff09S-Ti<sub>3<\/sub>C<sub>2<\/sub>T<sub>x<\/sub>-DMF\uff1b\uff08f\uff09H<sub>2<\/sub>O-M \uff0c\uff08g\uff09PC-M\uff0c\uff08h\uff09\u00a0DMAc-M\u548c\uff08i\uff09DMF-M\u7684SEM\u56fe\u50cf\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-218317 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72474-11.png\" alt=\"\" width=\"600\" height=\"452\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72474-11.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72474-11-300x226.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>3<\/b><\/strong><strong><b>. <\/b><\/strong>TMM\u6cd5\u5236\u5907\u9ad8\u6d53\u5ea6MXene\u6709\u673a\u6eb6\u5242\u5206\u6563\u6db2\u7684\u6d53\u5ea6\u4e0e\uff08a\uff09\u8868\u9762\u548c\uff08b\uff09\u6cb8\u70b9\u7684\u51fd\u6570\u62df\u5408\uff1b\uff08c\uff09\u6587\u7ae0\u4e2d\u6240\u7528\u5230\u7684\u6eb6\u5242\u53c2\u6570\uff08d\uff09\u4e0e\u6587\u732e\u76f8\u6bd4\uff0c\u53ef\u9ad8\u5206\u6563MXene\u6709\u673a\u6eb6\u5242\u7684\u6027\u8d28\u5bf9\u6bd4\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-218318 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72475-7.png\" alt=\"\" width=\"600\" height=\"323\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72475-7.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72475-7-300x162.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>4<\/b><\/strong><strong><b>.<\/b><\/strong>\u00a0\u76f8\u540c\u6d53\u5ea6\u4e0bTMM\u6cd5\u5236\u5907\u7684MXene\u6709\u673a\u6eb6\u5242\u4e0eMILD\u6cd5\u5236\u5907\u7684\u6c34\u6eb6\u6db2\u7684\u6c27\u5316\u7a33\u5b9a\u6027\u6d4b\u8bd5\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-218319 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72476-7.png\" alt=\"\" width=\"600\" height=\"364\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72476-7.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72476-7-300x182.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>5<\/b><\/strong><strong><b>.<\/b><\/strong><strong><b>\u00a0<\/b><\/strong>(a\uff09\u6e7f\u6cd5\u7eba\u4e1d\u7684\u6d41\u7a0b\u793a\u610f\u56fe\uff08b\uff09\u5236\u5907\u7684\u4e0d\u540cMXene\u542b\u91cf\u7684Ti3C2Tx\/PAN\u7ea4\u7ef4\u7684\u7167\u7247; \uff08c\uff09\u5236\u5907\u7684\u4e0d\u540cMXene\u542b\u91cf\u7684Ti3C2Tx\/PAN\u7ea4\u7ef4\u7684i-t\u66f2\u7ebf\uff1b\uff08d\uff09\u00a0\u5236\u5907\u7684\u4e0d\u540cMXene\u542b\u91cf\u7684Ti3C2Tx\/PAN\u7ea4\u7ef4\u7684\u7535\u5bfc\u7387\u5bf9\u6bd4\u00a0; \uff08e\uff09\u5bf9\u6bd4\u6587\u732e\u6bd4\u8f83\u4e0d\u540cMXene\u542b\u91cf\u4e0b\u7535\u5bfc\u7387\u7684\u5bf9\u6bd4\u3002<\/p>\n<p><strong><b>\u3010\u5c0f\u7ed3\u3011<\/b><\/strong><\/p>\n<p>\u7efc\u4e0a\u6240\u8ff0\uff0c\u8be5\u7814\u7a76\u901a\u8fc7\u8868\u9762\u5fae\u73af\u5883\u4fee\u9970\uff0c\u5b9e\u73b0\u4e86Ti<sub>3<\/sub>C<sub>2<\/sub>T<sub>x<\/sub>\u7b49MXene\u5728\u6709\u673a\u6eb6\u5242\u4e2d\u7684\u9ad8\u5ea6\u5206\u6563\u3002\u5265\u79bb\u5f97\u5230\u7684Ti3C2Tx\u7eb3\u7c73\u7247\u8868\u9762\u6e05\u6d01\uff0c\u539a\u5ea6\u5747\u5300\uff0c\u5177\u6709\u8f83\u5927\u7684\u5c3a\u5bf8\u3002\u540c\u65f6\u8be5\u65b9\u6848\u7b80\u5355\u9ad8\u6548\u3001\u6613\u4e8e\u91cd\u590d\uff0c\u8fd9\u9879\u5de5\u4f5c\u5c06\u4e3aMXene\u6750\u6599\u5bb6\u65cf\u7684\u7814\u7a76\u5e26\u6765\u65b0\u7684\u673a\u9047\u3002\u8be5\u5de5\u4f5c\u4e8e2021\u5e744\u670823\u65e5\u5728ACS nano\u53d1\u8868online\u3002<\/p>\n<p><strong><b>\u3010\u6587\u7ae0\u94fe\u63a5\u3011<\/b><\/strong><\/p>\n<p>High Concentration of Ti<sub>3<\/sub>C<sub>2<\/sub>T<sub>x<\/sub>\u00a0MXene in\u00a0Organic Solvent<\/p>\n<p>https:\/\/pubs.acs.org\/doi\/10.1021\/acsnano.0c10671<\/p>\n<p><strong><b>\u3010\u56e2\u961f\u4ecb\u7ecd\u3011<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><\/p>\n<p><strong><b><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-218320 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72477-6.png\" alt=\"\" width=\"250\" height=\"374\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72477-6.png 250w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/\u56fe\u72477-6-201x300.png 201w\" sizes=\"(max-width: 250px) 100vw, 250px\" \/><\/b><\/strong><\/p>\n<p><strong>\u674e\u8f89\u6559\u6388\uff1a<\/strong>2001\u5e74\u535a\u58eb\u6bd5\u4e1a\u4e8e\u590d\u65e6\u5927\u5b66\u5316\u5b66\u7cfb\u83b7\u535a\u58eb\u5b66\u4f4d\uff0c\u5e08\u4ece\u7269\u7406\u5316\u5b66\u5bb6\uff0c\u5316\u5b66\u6559\u80b2\u5bb6\u9093\u666f\u53d1\u9662\u58eb\u3002\u73b0\u62c5\u4efb\u4e0a\u6d77\u9ad8\u6821\u5316\u5b66\u9ad8\u539f\u5b66\u79d1(I\u7c7b)\u5efa\u8bbe\u8d1f\u8d23\u4eba\u3001\u4e0a\u6d77\u5e08\u8303\u5927\u5b66\u79d1\u6280\u5904\u5904\u957f\u3001\u4e0a\u6d77\u5e08\u8303\u5927\u5b66\u6821\u5b66\u672f\u59d4\u5458\u4f1a\u59d4\u5458\u548c\u4e0a\u6d77\u5e02\u7a00\u571f\u529f\u80fd\u6750\u6599\u91cd\u70b9\u5b9e\u9a8c\u5ba4\u526f\u4e3b\u4efb\u3002\u5148\u540e\u4e3b\u6301\u4e86\u79d1\u6280\u90e8973\u8ba1\u5212\u524d\u671f\u7814\u7a76\u4e13\u9879\u3001\u56fd\u5bb6\u81ea\u7136\u79d1\u5b66\u57fa\u91d1\u9752\u5e74\u79d1\u5b66\u57fa\u91d1\u9879\u76ee\u548c\u9762\u4e0a\u9879\u76ee(2\u9879)\uff0c\u4e0a\u6d77\u5e02\u79d1\u59d4\u57fa\u7840\u7814\u7a76\u91cd\u70b9\u9879\u76ee(3\u9879)\u3001\u4e0a\u6d77\u5e02\u7eb3\u7c73\u79d1\u6280\u4e13\u9879\u8bfe\u9898(2\u9879)\u53ca\u4f01\u4e1a\u59d4\u6258\u9879\u76ee\u7b49\u3002\u53d1\u8868SCI\u8bba\u658760\u4f59\u7bc7\u3002\u4e3b\u7f16\u4e2d\u6587\u4e13\u84571\u90e8\uff0c\u53c2\u7f16\u82f1\u6587\u4e13\u84571\u90e8\u3002\u6388\u6743\u4e2d\u56fd\u53d1\u660e\u4e13\u522913\u4ef6\uff0c\u8f6c\u8ba91\u4ef6\u3002\u5165\u9009\u6559\u80b2\u90e8\u65b0\u4e16\u7eaa\u4f18\u79c0\u4eba\u624d\u652f\u6301\u8ba1\u5212(2011\u5e74\u5ea6)\u3001\u4e0a\u6d77\u5e02\u6559\u59d4\u66d9\u5149\u8ba1\u5212(2010\u5e74\u5ea6)\u3001\u4e0a\u6d77\u5e02\u9752\u5e74\u79d1\u6280\u542f\u660e\u661f\u8ba1\u5212(2005\u5e74\u5ea6)\u548c\u4e0a\u6d77\u4eba\u624d\u53d1\u5c55\u8d44\u91d1\u8d44\u52a9\u8ba1\u5212(2012\u5e74\u5ea6)\u3002\u83b72012\u5e74\u5ea6\u4e0a\u6d77\u5e02\u81ea\u7136\u79d1\u5b66\u4e8c\u7b49\u5956(\u7b2c\u56db)\u3002<\/p>\n<p><strong><b>\u5f20\u5e86\u8427<\/b><\/strong>\uff1a\u4e0a\u6d77\u5e08\u8303\u5927\u5b662019\u7ea7\u535a\u58eb\u7814\u7a76\u751f\uff0c\u7814\u7a76\u91cd\u70b9\u662f\u4e8c\u7ef4MXene\u6750\u6599\u7684\u50ac\u5316\u5e94\u7528\u3002<\/p>\n<p>\u672c\u6587\u7531\u4f5c\u8005\u6295\u7a3f\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u6587\u7ae0\u4fe1\u606f\u3011 High Concentration of Ti3C2Tx\u00a0MXene in\u00a0Organic Solvent \u7b2c\u4e00\u4f5c\u8005\uff1a\u5f20\u5e86\u8427 \u901a\u8baf\u4f5c\u8005\uff1a\u674e\u8f89* &#8230;<\/p>\n","protected":false},"author":11454,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-218311","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/218311"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/11454"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=218311"}],"version-history":[{"count":4,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/218311\/revisions"}],"predecessor-version":[{"id":218323,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/218311\/revisions\/218323"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=218311"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=218311"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=218311"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}