{"id":218332,"date":"2021-02-26T06:11:13","date_gmt":"2021-02-25T22:11:13","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=218332"},"modified":"2021-02-25T21:11:44","modified_gmt":"2021-02-25T13:11:44","slug":"%e4%b8%ad%e7%a7%91%e9%99%a2%e5%8c%96%e5%ad%a6%e6%89%80%e9%99%88%e5%bb%ba%e6%af%85%e5%88%98%e4%ba%91%e5%9c%bb%e5%9b%a2%e9%98%9fadv-mater-%e4%bb%8b%e8%b4%a8%e8%a1%ac%e5%ba%95%e4%b8%8a%e6%99%b6","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=218332","title":{"rendered":"\u4e2d\u79d1\u9662\u5316\u5b66\u6240\u9648\u5efa\u6bc5&#038;\u5218\u4e91\u573b\u56e2\u961fAdv. Mater.:\u4ecb\u8d28\u886c\u5e95\u4e0a\u6676\u5706\u7ea72D\u534a\u5bfc\u4f53MOF\u8584\u819c\u7684\u9762\u5bf9\u9762\u751f\u957f"},"content":{"rendered":"<p><strong><b>\u3010\u5f15\u8a00\u3011<\/b><\/strong><\/p>\n<p>\u591a\u5b54\u6750\u6599\u5728\u81ea\u7136\u754c\u4e2d\u65e0\u5904\u4e0d\u5728\uff0c\u5305\u62ec\u65e0\u673a\u548c\u6709\u673a\u591a\u5b54\u7ed3\u6784\uff0c\u5982\u8702\u7a9d\u3001\u6d77\u7ef5\u3001\u591a\u5b54\u9676\u74f7\u3001\u6728\u6750\u7b49\u3002\u8fd9\u4e9b\u6750\u6599\u5728\u6c14\u4f53\u5206\u79bb\u3001\u5fae\u7535\u5b50\u7b49\u9886\u57df\u5177\u6709\u91cd\u8981\u7684\u5e94\u7528\u524d\u666f\u3002\u5728\u5206\u5b50\u6c34\u5e73\u4e0a\uff0c\u591a\u5b54\u9aa8\u67b6\u6750\u6599\u53ef\u5206\u4e3a\u6709\u673a\u805a\u5408\u7269\u7f51\u7edc\u3001\u5171\u4ef7\u6709\u673a\u6846\u67b6\uff08COFs\uff09\u6216\u91d1\u5c5e\u6709\u673a\u6846\u67b6\uff08MOFs\uff09\u3002\u4e0eCOF\u6750\u6599\u76f8\u6bd4\uff0cMOFs\u662f\u4e00\u7c7b\u5728\u6e29\u548c\u7684\u5408\u6210\u6761\u4ef6\u4e0b\uff0c\u6709\u673a\u914d\u4f53\u4e0e\u91d1\u5c5e\u79bb\u5b50\u4e4b\u95f4\u901a\u8fc7\u914d\u4f4d\u952e\u8fde\u63a5\u7684\u591a\u5b54\u6676\u4f53\u6750\u6599\u3002\u7136\u800c\uff0c\u7531\u4e8eMOF\u6750\u6599\u672c\u5f81\u8f83\u4f4e\u7684\u5bfc\u7535\u6027\u751a\u81f3\u662f\u7edd\u7f18\u7684\uff0c\u5176\u5e94\u7528\u53d7\u5230\u4e00\u5b9a\u9650\u5236\u3002\u5f88\u591a\u5de5\u4f5c\u90fd\u662f\u901a\u8fc7\u63ba\u6742\u5ba2\u4f53\u5206\u5b50\u6765\u63d0\u9ad8MOF\u6750\u6599\u7684\u5bfc\u7535\u6027\u3002\u8fd1\u5e74\u6765\uff0c\u4eba\u4eec\u5408\u6210\u4e86\u4e00\u7cfb\u5217\u5bfc\u7535MOF\u8584\u819c\uff0c\u5e76\u5c06\u5176\u5e94\u7528\u4e8e\u4f20\u611f\u5668\u3001\u7535\u6c60\u7535\u6781\u3001\u8d85\u5bfc\u4f53\u7b49\u7535\u5b50\u6d3b\u6027\u5c42\u3002\u636e\u6211\u4eec\u6240\u77e5\uff0c\u6700\u6210\u719f\u7684\u4e8c\u7ef4\u5bfc\u7535MOFs\u662f\u5229\u7528\u8fc7\u6e21\u91d1\u5c5e\u79bb\u5b50\u548c\u542b\u6709\u2013OH\u3001\u2013NH<sub>2<\/sub>\u548c\u2013SH\u7b49\u5b98\u80fd\u56e2\u7684\u5e73\u9762\u5171\u8f6d\u82b3\u9999\u914d\u4f53\u5728\u65b9\u5f62\u5e73\u9762\u51e0\u4f55\u4e2d\u8fdb\u884c\u914d\u4f4d\u6784\u5efa\u7684\u3002\u4e8c\u7ef4\u5bfc\u7535MOF\u8584\u819c\u4f5c\u4e3a\u4e00\u79cd\u65b0\u578b\u591a\u5b54\u6676\u4f53\u6750\u6599\uff0c\u5728\u7535\u5b50\u5668\u4ef6\u4e2d\u5177\u6709\u5e7f\u9614\u7684\u5e94\u7528\u524d\u666f\u3002\u4e3a\u6b64\uff0c\u4eba\u4eec\u5f00\u53d1\u4e86\u51e0\u79cd\u5408\u6210\u65b9\u6cd5\u6765\u5236\u59072D MOF\u8584\u819c\u3002\u7531\u4e8e2D\u5927\u9aa8\u67b6\u6750\u6599\u8f83\u5dee\u7684\u6eb6\u89e3\u6027\uff0c\u4ee5\u65cb\u6d82\u6cd5\u4e3a\u4ee3\u8868\u7684\u4f20\u7edf\u8584\u819c\u52a0\u5de5\u6280\u672f\u6548\u679c\u5e76\u4e0d\u7406\u60f3\u3002Makiura\u7b49\u4eba\u62a5\u9053\u4e86\u4e00\u79cd\u81ea\u4e0b\u800c\u4e0a\u7684\u754c\u9762\u5236\u9020\u65b9\u6cd5\uff0c\u968f\u540e\u5176\u4ed6\u7814\u7a76\u5c0f\u7ec4\u4e5f\u5f00\u53d1\u4e86\u4e00\u4e9b\u6539\u826f\u8def\u7ebf\u3002\u8fd9\u4e9b\u5305\u62ec\u5728\u6c14-\u6db2\u6216\u6db2-\u6db2\u754c\u9762\u4e0a\u5408\u62102D MOF\u8584\u819c\uff0c\u7136\u540e\u901a\u8fc7Langmuir-Schaefer\uff08LS\uff09\u65b9\u6cd5\u6216\u5b9a\u5236\u7684\u7279\u6c1f\u9686\u53cd\u5e94\u5668\u8f6c\u79fb\u5230\u4ecb\u8d28\u886c\u5e95\u4e0a\u3002\u53e6\u5916\uff0c\u5728\u4ecb\u8d28\u886c\u5e95\u4e0a\u76f4\u63a5\u751f\u957f2D\u5bfc\u7535MOF\u8584\u819c\u5728\u534a\u5bfc\u4f53\u5de5\u4e1a\u4e2d\u662f\u7531\u524d\u666f\u7684\uff0c\u56e0\u4e3a\u5728\u7535\u5b50\u5668\u4ef6\u5236\u4f5c\u8fc7\u7a0b\u4e2d\u9700\u8981\u7edd\u7f18\u5c42\u5c06\u6676\u4f53\u7ba1\u6805\u6781\u548c\u6c9f\u9053\u5206\u5f00\uff0c\u540c\u65f6\u539f\u4f4d\u751f\u957f\u907f\u514d\u4e86\u590d\u6742\u7684\u540e\u8f6c\u79fb\u8fc7\u7a0b\u3002\u8fc4\u4eca\u4e3a\u6b62\uff0c\u4eba\u4eec\u5df2\u7ecf\u505a\u4e86\u5f88\u591a\u5de5\u4f5c\u6765\u63a2\u7d22\u5728\u4ecb\u8d28\u886c\u5e95\u4e0a\u76f4\u63a5\u751f\u957fMOF\u8584\u819c\u3002<\/p>\n<p><strong><b>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/b><\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c\u5728<strong><b>\u4e2d\u56fd\u79d1\u5b66\u9662\u5316\u5b66\u7814\u7a76\u6240<\/b><\/strong><strong><b>\u9648\u5efa\u6bc5\u7814\u7a76\u5458<\/b><\/strong><strong><b>\u548c<\/b><\/strong><strong><b>\u5218\u4e91\u573b\u9662\u58eb<\/b><\/strong><strong><b>\u56e2\u961f<\/b><\/strong><strong><b>\u7b49\u4eba<\/b><\/strong>\u5e26\u9886\u4e0b\uff0c\u53d7\u6bdb\u7ec6\u7ba1\u73b0\u8c61\u7684\u542f\u53d1\uff0c\u63d0\u51fa\u4e86\u4e00\u79cd\u5728\u4ecb\u8d28\u886c\u5e95\u4e0a\u751f\u957f2D Cu<sub>2<\/sub>(TCPP) (TCPP=\u95f4\u56db(4-\u7fa7\u57fa\u82ef\u57fa)\u535f\u5549)MOF\u5bfc\u7535\u8584\u819c\u7684\u9762\u5bf9\u9762\u9650\u57df\u751f\u957f\u65b9\u6cd5\u3002\u5229\u7528\u6bdb\u7ec6\u7ba1\u529b\u5c06\u5fae\u91cf\u4f4e\u6d53\u5ea6\u7684Cu<sup>2+<\/sup>\u548cTCPP\u6eb6\u6db2\u5faa\u73af\u6cf5\u5165\u5fae\u5b54\u754c\u9762\u4e2d\u3002Cu<sup>2+<\/sup>\u4f1a\u9996\u5148\u951a\u5b9a\u5230\u2013OH\u529f\u80fd\u5316\u7684\u4ecb\u7535\u5c42\u8868\u9762\uff0c\u5e76\u4e0e\u540e\u7eed\u6cf5\u5165\u7684TCPP\u914d\u4f53\u53d1\u751f\u914d\u4f4d\u53cd\u5e94\u3002\u5f85\u6c34\u5206\u5b50\u88ab\u7f13\u6162\u79fb\u9664\u540e\uff0cCu<sub>2<\/sub>(TCPP)\u5219\u88ab\u951a\u70b9\u5728\u4ecb\u7535\u5c42\u8868\u9762\u3002\u8be5MOF\u8584\u819c\u7684\u6676\u4f53\u7ed3\u6784\u901a\u8fc7\u591a\u79cd\u8868\u5f81\u6280\u672f\u5f97\u5230\u8bc1\u5b9e\uff0c\u5305\u62ec\u9ad8\u5206\u8fa8\u7387\u539f\u5b50\u529b\u663e\u5fae\u955c\u548c\u4f4e\u6e29\u900f\u5c04\u7535\u5b50\u663e\u5fae\u955c\uff08Cryo-TEM\uff09\u3002Cu<sub>2<\/sub>(TCPP) MOF\u8584\u819c\u7684\u7535\u5bfc\u7387\u4e3a\u22480.007 S cm<sup>-1<\/sup>\uff0c\u6bd4\u5176\u4ed6\u7fa7\u9178\u57faMOF\u6750\u6599\uff0810<sup>-6<\/sup>\u00a0S cm<sup>-1<\/sup>\uff09\u9ad8\u8fd14\u4e2a\u6570\u91cf\u7ea7\u3002\u8be5\u7b56\u7565\u540c\u6837\u4e5f\u9002\u7528\u4e8e\u5236\u5907\u5176\u4ed6\u6676\u5706\u7ea7\u5bfc\u7535MOF\u8584\u819c\u5982M<sub>3<\/sub>(HHTP)<sub>2<\/sub>(M=Cu\u3001Co\u548cNi\uff1bHHTP=2,3,6,7,10,11-\u4e09\u4e9a\u82ef\u57fa\u5df1\u9187)\uff0c\u8868\u660e\u8be5\u65b9\u6cd5\u5177\u6709\u5e7f\u6cdb\u7684\u5e94\u7528\u6f5c\u529b\u3002\u8be5\u6210\u679c\u4ee5\u9898\u4e3a<strong><b>\u201cFace-to-Face Growth of Wafer-Scale 2D Semiconducting MOF Films on Dielectric Substrates\u201d<\/b><\/strong>\u53d1\u8868\u5728\u4e86<strong><b>Adv. Mater.<\/b><\/strong>\u4e0a\u3002\u672c\u8bba\u6587\u7b2c\u4e00\u4f5c\u8005<strong><b>\u5218\u53cb\u661f<\/b><\/strong>\u3002<\/p>\n<p><strong><b>\u00a0<\/b><\/strong><strong><b>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/b><\/strong><\/p>\n<p><strong><b>\u56fe1 <\/b><\/strong><strong><b>MOF\u8584\u819c\u751f\u957f\u53ca\u6676\u5706\u7ea7\u8584\u819c\u5236\u5907\u793a\u610f\u56fe<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-218333\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/1-15.jpg\" alt=\"\" width=\"600\" height=\"402\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/1-15.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/1-15-300x201.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>a)\u5728\u4ecb\u8d28\u886c\u5e95\u4e0a\u751f\u957f\u7684MOF\u8584\u819c\u793a\u610f\u56fe\u3002<\/p>\n<p>b) \u6676\u5706\u7ea72D MOF\u8584\u819c\u5236\u5907\u793a\u610f\u56fe\u3002<\/p>\n<p>c) TCPP\u4e0eCu<sup>2+<\/sup>\u7684\u914d\u4f4d\u53cd\u5e94\u793a\u610f\u56fe\u3002<\/p>\n<p><strong><b>\u56fe2 <\/b><\/strong><strong><b>Cu<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>(TCPP) MOF\u8584\u819c\u7684\u5149\u5b66\u8868\u5f81<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-218334\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/2-15.jpg\" alt=\"\" width=\"600\" height=\"342\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/2-15.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/2-15-300x171.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>a) 4\u82f1\u5bf8\u77f3\u82f1\u73bb\u7483\u7167\u7247\u3002<\/p>\n<p>b) 4\u82f1\u5bf8\u6676\u5706\u7ea7Cu<sub>2<\/sub>(TCPP) MOF\u8584\u819c\u7167\u7247\u3002<\/p>\n<p>c)\u91c7\u7528\u6eb6\u6db2\u6cd5\u548c\u9762\u5bf9\u9762\u9650\u57df\u751f\u957f\u6cd5\u5236\u5907\u7684Cu<sub>2<\/sub>(TCPP) MOFs\u7684\u7d2b\u5916-\u53ef\u89c1\u5438\u6536\u5149\u8c31\u3002<\/p>\n<p>d)\u4e0d\u540c\u5faa\u73af\u6b21\u6570\u4e0bCu<sub>2<\/sub>(TCPP) MOF\u8584\u819c\u7684\u7d2b\u5916-\u53ef\u89c1\u5438\u6536\u5149\u8c31\u3002<\/p>\n<p>e) Cu<sub>2<\/sub>(TCPP) MOF\u8584\u819c\u7684\u6700\u5927\u5438\u5149\u5ea6\u968f\u5faa\u73af\u6570\u7684\u53d8\u5316\u66f2\u7ebf\u3002<\/p>\n<p>f) Cu<sub>2<\/sub>(TCPP) MOF\u8584\u819c\u7684\u7d2b\u5916-\u53ef\u89c1\u5438\u6536\u4e8c\u7ef4\u8f6e\u5ed3\u56fe\u3002<\/p>\n<p><strong><b>\u56fe3 <\/b><\/strong><strong><b>Cu<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>(TCPP) MOF\u8584\u819c\u7684\u5fae\u89c2\u8868\u5f81<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-218335\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/3-16.jpg\" alt=\"\" width=\"600\" height=\"361\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/3-16.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/3-16-300x181.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>a)\u57fa\u4e8eA-A\u5806\u79ef\u7684Cu<sub>2<\/sub>(TCPP) MOFs\u7684\u6a21\u62df\u5206\u5b50\u7ed3\u6784\u3002<\/p>\n<p>b)\u5b9e\u9a8c(\u7ea2\u8272)\u548c\u6a21\u62df(\u9ed1\u8272)PXRD\u56fe\u8c31\u3002<\/p>\n<p>c) Cu<sub>2<\/sub>(TCPP) MOF\u8584\u819c\u7684HRAFM\u76f8\u4f4d\u56fe\u50cf\u3002\u6bd4\u4f8b\u5c3a\uff1a4nm\u3002<\/p>\n<p>d) Cu<sub>2<\/sub>(TCPP) MOF\u8584\u819c(100)\u6676\u9762\u7684HRCryo-TEM\u56fe\u50cf\u3002\u6bd4\u4f8b\u5c3a\uff1a5nm\u3002<\/p>\n<p>e) Cu<sub>2<\/sub>(TCPP)\u8584\u819c(001)\u6676\u9762\u7684HRCryo-TEM\u56fe\u50cf\u3002\u6bd4\u4f8b\u5c3a\uff1a5 nm\u3002<\/p>\n<p><strong><b>\u56fe4 <\/b><\/strong><strong><b>Cu<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>(TCPP)MOF\u8584\u819c\u5668\u4ef6\u7684\u793a\u610f\u56fe<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-218336\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/4-15.jpg\" alt=\"\" width=\"600\" height=\"449\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/4-15.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/4-15-300x225.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>a)Cu<sub>2<\/sub>(TCPP)MOF\u8584\u819c\u5668\u4ef6\u7684\u793a\u610f\u56fe\u3002<\/p>\n<p>b)Cu<sub>2<\/sub>(TCPP)MOF\u8584\u819c\u5668\u4ef6\u5728N<sub>2<\/sub>\u6c14\u6c1b\u4e0b\u7684I<sub>ds<\/sub>-V<sub>G<\/sub>\u66f2\u7ebf\uff08V<sub>ds<\/sub>=2 V\uff09\u3002<\/p>\n<p>c) \u5668\u4ef6\u5728N<sub>2<\/sub>\u6c14\u6c1b\u4e0b\u7684I<sub>ds<\/sub>-V<sub>ds<\/sub>\u66f2\u7ebf\u3002<\/p>\n<p>d)\u51b7\u5374\u8fc7\u7a0b\u4e2d\u5f52\u4e00\u5316\u7535\u5bfc(\u03c3)\u4e0e1000T<sup>-1<\/sup>\u7684\u5173\u7cfb\uff0c\u63d2\u56fe\u4e3aln(\u03c3)\u4e0e1000T<sup>-1<\/sup>\u7684\u51fd\u6570\u5173\u7cfb\u3002<\/p>\n<p>e)\u5347\u964d\u6e29\u8fc7\u7a0b\u4e2d\u5668\u4ef6\u7684\u5f52\u4e00\u5316\u7535\u5bfc(\u03c3)\u53d8\u5316\uff08A\uff1a\u6e29\u5ea6\/K\uff1bB\uff1a\u51b7\u5374\u8fc7\u7a0b\uff1bC\uff1a\u52a0\u70ed\u8fc7\u7a0b\uff09\u3002<\/p>\n<p>f) MOF\/\u77f3\u58a8\u70ef\u5f02\u8d28\u7ed3\u5668\u4ef6\u7684\u793a\u610f\u56fe\u3002<\/p>\n<p>g) MOF\/\u77f3\u58a8\u70ef\u5f02\u8d28\u7ed3\u5668\u4ef6\u5728\u9ed1\u6697\u4e2d\u548c420nm\u6fc0\u5149\u7167\u5c04\u4e0b\u22480.5W cm<sup>-2<\/sup>\u7684J-V\u66f2\u7ebf\u3002<\/p>\n<p>h) MOF BHJ-OPD\u5668\u4ef6\u7684\u80fd\u7ea7\u56fe\u3002<\/p>\n<p>i) MOF BHJ-OPD\u5668\u4ef6\u5728420nm\u6fc0\u5149\u22480.5 W cm<sup>&#8211;<\/sup><sup>2<\/sup>\u7167\u5c04\u4e0b\u7684J-V\u66f2\u7ebf\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>5<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>\u6676\u5706\u7ea7Cu<\/b><\/strong><strong><sub><b>3<\/b><\/sub><\/strong><strong><b>(HHTP)<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>\u3001Co<\/b><\/strong><strong><sub><b>3<\/b><\/sub><\/strong><strong><b>(HHTP)<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>\u548cNi<\/b><\/strong><strong><sub><b>3<\/b><\/sub><\/strong><strong><b>(HHTP)<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>\u8584\u819c\u7684XRD\u548cHRCryo-TEM\u8868\u5f81<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-218337\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/5-11.jpg\" alt=\"\" width=\"600\" height=\"466\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/5-11.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/02\/5-11-300x233.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>a-c)\u5206\u522b\u4e3a\u6676\u5706\u7ea7\u7684a)Cu<sub>3<\/sub>(HHTP)<sub>2<\/sub>\u3001b)Co<sub>3<\/sub>(HHTP)<sub>2<\/sub>\u548cc)Ni<sub>3<\/sub>(HHTP)<sub>2<\/sub>\u8584\u819c\u7684\u7167\u7247\u3002<\/p>\n<p>d-f)\u5206\u522b\u4e3ad)Cu<sub>3<\/sub>(HHTP)<sub>2<\/sub>\u3001e)Co<sub>3<\/sub>(HHTP)<sub>2<\/sub>\u548cf)Ni<sub>3<\/sub>(HHTP)<sub>2<\/sub>\u8584\u819c\u7684\u5b9e\u9a8c(\u7ea2\u8272)\u548c\u6a21\u62df(\u84dd\u8272)XRD\u56fe\u3002<\/p>\n<p>g-i)\u5206\u522b\u4e3ag)Cu<sub>3<\/sub>(HHTP)<sub>2<\/sub>\u3001h)Co<sub>3<\/sub>(HHTP)<sub>2<\/sub>\u548ci)Ni<sub>3<\/sub>(HHTP)<sub>2<\/sub>\u8584\u819c\u7684HRCryo-TEM\u56fe\u50cf\uff0c\u63d2\u56fe\u663e\u793a\u4e86\u5b83\u4eec\u7684SAED\u6a21\u5f0f\u3002\u6bd4\u4f8b\u5c3a\uff1a5 nm\u3002<\/p>\n<p>\u3010<strong><b>\u5c0f\u7ed3<\/b><\/strong>\u3011<\/p>\n<p>\u7efc\u4e0a\u6240\u8ff0\uff0c\u672c\u5de5\u4f5c\u5f00\u53d1\u4e86\u4e00\u79cd\u57fa\u4e8e\u6bdb\u7ec6\u7ba1\u529b\u7684\u9762\u5bf9\u9762\u9650\u57df\u751f\u957f\u65b9\u6cd5\uff0c\u7528\u4e8e\u5236\u5907\u5927\u89c4\u6a21\u7684\u4e8c\u7ef4MOF\u8584\u819c\u3002\u2013OH\u529f\u80fd\u5316\u7684\u4ecb\u7535\u5c42\u5806\u53e0\u5f15\u8d77\u7684\u6bdb\u7ec6\u529b\u9a71\u52a8\u5fae\u91cfCu<sup>2+<\/sup>\u548cHHTP\u6eb6\u6db2\u8fdb\u5165\u5fae\u5b54\u754c\u9762\uff0c\u5e76\u5b9e\u73b0\u8868\u9762\u951a\u5b9aMOF\u8584\u819c\u7684\u81ea\u7ec4\u88c5\u3002\u8be5\u7b56\u7565\u53ef\u4ee5\u5b9e\u73b0\u5728\u77f3\u82f1\u3001\u84dd\u5b9d\u77f3\u3001SiO<sub>2<\/sub>\/Si\u7b49\u4ecb\u7535\u5c42\u57fa\u5e95\u4e0a\u751f\u957f\u4e86\u6676\u5706\u7ea7Cu<sub>2<\/sub>(TCPP)\u00a0MOF\u8584\u819c\uff0c\u5e76\u4f5c\u4e3a\u6d3b\u6027\u5c42\u5e94\u7528\u4e8e\u5404\u79cd\u7535\u5b50\u8bbe\u5907\u3002\u901a\u8fc7PXRD\u3001GIWAS\u3001HRAFM\u548cHRCryo-TEM\u5bf9\u8584\u819c\u8fdb\u884c\u8868\u5f81\uff0c\u8bc1\u5b9e\u4e86Cu<sub>2<\/sub>(TCPP) MOF\u8584\u819c\u5177\u6709\u9ad8\u5ea6\u7ed3\u6676\u76f8\u3002\u8be5\u751f\u957f\u7b56\u7565\u88ab\u5e94\u7528\u4e8e\u5408\u6210\u4e86Cu<sub>3<\/sub>(HHTP)<sub>2<\/sub>\u3001Co<sub>3<\/sub>HHTP)<sub>2<\/sub>\u3001Ni<sub>3<\/sub>(HHTP)<sub>2<\/sub>\u7b49\u5bfc\u7535MOF\u8584\u819c\u3002\u8fd9\u9879\u5de5\u4f5c\u63d0\u51fa\u4e86\u4e00\u79cd\u9650\u5236\u751f\u957f\u7b56\u7565\uff0c\u5b9e\u73b0\u4e86\u4ecb\u8d28\u886c\u5e95\u4e0a2D MOF\u8584\u819c\u7684\u5de5\u4e1a\u89c4\u6a21\u5316\u751f\u4ea7\u3002\u672c\u8bba\u6587\u7684\u7b2c\u4e00\u4f5c\u8005\u662f2019\u7ea7\u535a\u58eb\u751f\u5218\u53cb\u661f\uff0c\u901a\u8baf\u4f5c\u8005\u4e3a\u9648\u5efa\u6bc5\u7814\u7a76\u5458\u548c\u5218\u4e91\u573b\u9662\u58eb\u3002<\/p>\n<p><strong><b>\u6587\u732e\u94fe\u63a5\uff1a<\/b><\/strong><a href=\"https:\/\/0-onlinelibrary.wiley.com.carlson.utoledo.edu\/doi\/10.1002\/adma.202007741\" target=\"_blank\" rel=\"noopener\"><u>Face-to-Face Growth of Wafer-Scale 2D Semiconducting MOF Films on Dielectric Substrates<\/u><\/a>\uff08Adv. Mater.\uff0c 2021\uff0cDOI:10.1002\/adma.202007741\uff09<\/p>\n<p>\u3010<strong><b>\u56e2\u961f\u53ca\u6210\u679c\u4ecb\u7ecd<\/b><\/strong>\u3011<\/p>\n<p>\uff081\uff09\u56e2\u961f\u4ecb\u7ecd<\/p>\n<p>\u5218\u4e91\u573b\u7814\u7a76\u5458\uff0c\u4e2d\u56fd\u79d1\u5b66\u9662\u9662\u58eb\uff0c\u7b2c\u4e09\u4e16\u754c\u79d1\u5b66\u9662\u9662\u58eb\u3002\u7269\u7406\u5316\u5b66\u5bb6\u3002\u4e3b\u8981\u7814\u7a76\u9886\u57df\u5305\u62ec\u4e8c\u7ef4\u6750\u6599\uff08\u77f3\u58a8\u70ef\u3001BN\u8584\u819c\u3001TMD\u3001\u4e8c\u7ef4MOF\u3001COF\u8584\u819c\u7b49\uff09\u7684\u5236\u5907\u53ca\u8868\u5f81\u3001\u5206\u5b50\u6750\u6599\u7684\u8bbe\u8ba1\u4e0e\u5408\u6210\u3001\u6709\u673a\/\u805a\u5408\u7269\u6750\u6599\u53d1\u5149\u4e8c\u6781\u7ba1\u3001\u6709\u673a\u573a\u6548\u5e94\u6676\u4f53\u7ba1\u548c\u6c14\u4f53\u4f20\u611f\u5668\u7b49\u3002\u76ee\u524d\u5df2\u00a0\u53d1\u8868SCI\u8bba\u6587500\u4f59\u7bc7(\u5176\u4e2d130\u4f59\u7bc7\u53d1\u8868\u5728\u5f71\u54cd\u56e0\u5b50\u5927\u4e8e10\u7684\u671f\u520a\u4e0a)\uff0c\u4ed6\u4eba\u5f15\u75284\u4e07\u4f59\u6b21\uff0ch\u56e0\u5b50\u5927\u4e8e100\uff0c\u83b7\u6388\u6743\u4e2d\u56fd\u53d1\u660e\u4e13\u522970\u9879\uff0c\u51fa\u7248\u4e13\u8457\u4e00\u90e8\u53ca19\u7ae0\u8282\uff0c\u5728\u56fd\u5185\u5916\u5b66\u672f\u4f1a\u8bae\u4e0a\u505a\u5927\u4f1a\/\u9080\u8bf7\u62a5\u544a100\u4f59\u6b21\u30022007\uff0c2016\uff0c2019\u5e74\u83b7\u56fd\u5bb6\u81ea\u7136\u79d1\u5b66\u4e8c\u7b49\u5956\u5404\u4e00\u9879\uff0c2017\u5e74\u5ea6\u83b7\u5317\u4eac\u5e02\u81ea\u7136\u79d1\u5b66\u4e00\u7b49\u5956\u30022014-2020\u5e74\u5165\u9009\u6c64\u68ee\u8def\u900f\u5168\u7403&#8221;\u9ad8\u88ab\u5f15\u79d1\u5b66\u5bb6&#8221;\u76ee\u5f55\u3002\u73b0\u4e3a\u79d1\u6280\u90e8\u56fd\u5bb6\u91cd\u70b9\u57fa\u7840\u7814\u7a76\u53d1\u5c55\u8ba1\u5212\uff08973\u8ba1\u5212\uff09\u91cd\u5927\u79d1\u5b66\u524d\u6cbf\u9886\u57df\u7b2c\u56db\u5c4a\u4e13\u5bb6\u54a8\u8be2\u7ec4\u526f\u7ec4\u957f\u3001\u4e2d\u56fd\u5316\u5b66\u4f1a\u7406\u4e8b\u3001\u4e2d\u79d1\u9662\u5316\u5b66\u6240\u6709\u673a\u56fa\u4f53\u4e13\u4e1a\u59d4\u5458\u4f1a\u526f\u4e3b\u4efb\uff0c\u548c\u62c5\u4efb<em><i>Scientific Reports, Nanoscale, Flexible Printed Electronics\uff0cACS Materials Letter<\/i><\/em>\u7b496\u79cd\u671f\u520a\u7684\u7f16\u59d4\/\u987e\u95ee\u59d4\u5458\u4f1a\u6210\u5458\u3002<\/p>\n<p>\u9648\u5efa\u6bc5\u7814\u7a76\u5458\uff0c\u4e2d\u79d1\u9662\u767e\u4eba\u3002\u4e3b\u8981\u7814\u7a76\u5174\u8da3\u5305\u62ec\u77f3\u58a8\u70ef\u6750\u6599\u4e0e\u5668\u4ef6\u3001\u00a0\u6709\u673a\u4e8c\u7ef4\u539f\u5b50\u6676\u4f53\u7684\u8bbe\u8ba1\u4e0e\u5408\u6210\u3001\u4e8c\u7ef4MOF\u3001COF\u3001TMD\u7684\u5408\u6210\u53ca\u8868\u5f81\u7b49\u3002\u76ee\u524d\u5df2\u5728PNAS, Adv. Mater., Adv. Funct. Mater., Angew. Chem. Int. Ed., JACS, Adv. Sci., Phys. Rev. Lett., Chem. Mater. ACS nano, Small, Nano Res.\u7b49\u671f\u520a\u4e0a\u53d1\u8868\u6570\u5341\u7bc7\u7814\u7a76\u8bba\u6587\u3002<\/p>\n<p>\uff082\uff09\u56e2\u961f\u5728\u8be5\u9886\u57df\u5de5\u4f5c\u6c47\u603b<\/p>\n<p>[1] Y.\u00a0Liu\uff0cY.\u00a0Wei\uff0cM.\u00a0Liu\uff0cY.\u00a0Bai\uff0cX.\u00a0Wang\uff0cS.\u00a0Shang\uff0cJ.\u00a0Chen*\uff0cY.\u00a0Liu*\uff0cElectrochemical Synthesis of Large Area Two\u2010Dimensional Metal\u2013Organic Framework Films on Copper Anodes\uff0c<em><i>Angew. Chem. Int. Ed. <\/i><\/em><strong><b>2021,\u00a0<\/b><\/strong>133, 2923<\/p>\n<p>[2] X.\u00a0Du, J.\u00a0Zhang, H.\u00a0Wang, Z.\u00a0Huang, A.\u00a0Guo, L.\u00a0Zhao, Y.\u00a0Niu, I.\u00a0Li, B.\u00a0Wu* and Y.\u00a0Liu*,\u00a0Solid-solid interface growth of conductive metal-organic framework nanowire arrays and their supercapacitor application,\u00a0<em><i>Mater. Chem. Front.<\/i><\/em>\u00a0<strong><b>2020<\/b><\/strong>,\u00a0<strong><b>4<\/b><\/strong>, 243-251.<\/p>\n<p>[3] X.\u00a0Chen,# H.\u00a0Yang,# B.\u00a0Wu,* L.\u00a0Wang, Q.\u00a0Fu, and Y.\u00a0Liu*, Epitaxial Growth of h-BN on Templates of Various Dimensionalities in h-BN\u2013graphene Material Systems,\u00a0<em><i>Adv<\/i><\/em><em><i>.<\/i><\/em><em><i>\u00a0Mater<\/i><\/em><em><i>.<\/i><\/em><strong><b>\u00a02019, <\/b><\/strong>31<strong><b>,<\/b><\/strong>\u00a01805582.<\/p>\n<p>[4] L.\u00a0Fu, D.\u00a0Hu, Rafael G. Mendes, Mark H. R\u00fcmmeli, Q.\u00a0Dai, B.\u00a0Wu,* L.\u00a0Fu,* and Y.\u00a0Liu,* Highly Organized Epitaxy of Dirac Semimetallic PtTe2 Crystals with Extrahigh Conductivity and Visible Surface Plasmons at Edges,\u00a0<strong><b>ACS<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>Nano<\/b><\/strong>,\u00a0<strong><b>2018<\/b><\/strong>, 12, 9405-9411.<\/p>\n<p>[5] L.\u00a0Fu, F.\u00a0Wang, B.\u00a0Wu,* N.\u00a0Wu, W.\u00a0Huang, H.\u00a0Wang, C.\u00a0Jin, L.\u00a0Zhuang, J.\u00a0He, L.\u00a0Fu,* and Y.\u00a0Liu*\u00a0Van der Waals Epitaxial Growth of Atomic Layered HfS2 Crystals for Ultrasensitive Near-Infrared Phototransistors,<em><i>\u00a0<\/i><\/em><em><i>Adv<\/i><\/em><em><i>.<\/i><\/em><em><i>\u00a0Mater<\/i><\/em><em><i>.<\/i><\/em>\u00a0<strong><b>2017<\/b><\/strong>, 29, 1700439.<\/p>\n<p>\uff083\uff09 \u76f8\u5173\u4f18\u8d28\u6587\u732e\u63a8\u8350<\/p>\n<p>[1] X. Song, X. Wang, Y. Li, C. Zheng, B. Zhang, C.-a. Di, F. Li, C. Jin, W. Mi, L. Chen, W. Hu, 2D Semiconducting Metal-Organic Framework Thin Films for\u00a0Organic Spin Valves, <em><i>Angew. Chem. Int. Ed.<\/i><\/em>\u00a0<strong><b>2020<\/b><\/strong>, 59, 1118.<\/p>\n<p>[2] M.-S. Yao, X.-J. Lv, Z.-H. Fu, W.-H. Li, W.-H. Deng, G.-D. Wu, G. Xu, Layer-by-Layer Assembled Conductive Metal\u2013Organic Framework\u00a0Nanofilms for Room-Temperature Chemiresistive Sensing, <em><i>Angew. Chem. Int. Ed.<\/i><\/em>\u00a0<strong><b>2017<\/b><\/strong>, 56, 16510.<\/p>\n<p>[3] Vitalie Stavila, \u00a0Joanne Volponi, \u00a0Aaron M. Katzenmeyer, \u00a0\u00a0Matthew C. Dixonb, Mark D. Allendorf, Kinetics and mechanism of metal\u2013organic framework thin film growth: systematic investigation of HKUST-1 deposition on QCM electrodes, <em><i>Chem. Sci.<\/i><\/em>\u00a0<strong><b>2012<\/b><\/strong>,3, 1531.<\/p>\n<p>[4] Monica C. So, Shengye Jin, Ho-Jin Son, Gary P. Wiederrecht, Omar K. Farha, Joseph T. Hupp, Layer-by-Layer Fabrication of Oriented Porous Thin Films Based on Porphyrin-Containing Metal\u2212Organic Frameworks,<em><i>\u00a0J. Am. Chem. Soc.<\/i><\/em>\u00a0<strong><b>2013<\/b><\/strong>, 135, 42, 15698<\/p>\n<p>[5] Jinxuan Liu, Christof W\u00f6ll, Surface-supported metal\u2013organic framework thin films: fabrication methods, applications, and challenges,<em><i>\u00a0Chem. Soc. Rev.<\/i><\/em>\u00a0<strong><b>2017<\/b><\/strong>,46, 5730.<\/p>\n<p>\u672c\u6587\u7531<strong><b>\u6728\u6587\u97ec<\/b><\/strong>\u7ffb\u8bd1\uff0c\u6750\u6599\u725b\u6574\u7406\u7f16\u8f91\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c<a href=\"mailto:\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\"><u>\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com<\/u><\/a>\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u591a\u5b54\u6750\u6599\u5728\u81ea\u7136\u754c\u4e2d\u65e0\u5904\u4e0d\u5728\uff0c\u5305\u62ec\u65e0\u673a\u548c\u6709\u673a\u591a\u5b54\u7ed3\u6784\uff0c\u5982\u8702\u7a9d\u3001\u6d77\u7ef5\u3001\u591a\u5b54\u9676\u74f7\u3001\u6728\u6750\u7b49\u3002\u8fd9\u4e9b\u6750\u6599\u5728\u6c14\u4f53\u5206\u79bb\u3001\u5fae\u7535\u5b50\u7b49\u9886\u57df\u5177\u6709\u91cd\u8981\u7684\u5e94\u7528\u524d\u666f\u3002\u5728\u5206\u5b50\u6c34\u5e73\u4e0a\uff0c&#8230;<\/p>\n","protected":false},"author":2109,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[4270,2598],"class_list":["post-218332","post","type-post","status-publish","format-standard","hentry","category-jiedu","tag-mof","tag-2598"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/218332"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/2109"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=218332"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/218332\/revisions"}],"predecessor-version":[{"id":218410,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/218332\/revisions\/218410"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=218332"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=218332"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=218332"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}