{"id":219300,"date":"2021-03-19T06:52:31","date_gmt":"2021-03-18T22:52:31","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=219300"},"modified":"2021-03-18T20:52:56","modified_gmt":"2021-03-18T12:52:56","slug":"%e9%a6%99%e6%b8%af%e5%9f%8e%e5%b8%82%e5%a4%a7%e5%ad%a6%e5%bc%a0%e5%8d%8e%e5%9b%a2%e9%98%9fjacs%ef%bc%9a%e5%9c%a82h-fcc%e5%bc%82%e7%9b%b8%e9%87%91%e7%ba%b3%e7%b1%b3%e7%89%87%e4%b8%8a%e9%80%89%e6%8b%a9","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=219300","title":{"rendered":"\u9999\u6e2f\u57ce\u5e02\u5927\u5b66\u5f20\u534e\u56e2\u961fJACS\uff1a\u57282H\/fcc\u5f02\u76f8\u91d1\u7eb3\u7c73\u7247\u4e0a\u9009\u62e9\u6027\u5916\u5ef6\u751f\u957fRh\u7eb3\u7c73\u68d2\uff0c\u5f62\u62101D\/2D Rh-Au\u5f02\u8d28\u7ed3\u6784\u5b9e\u73b0\u9ad8\u6548\u6790\u6c22  \u00a0"},"content":{"rendered":"<p><strong><b>\u3010\u5f15\u8a00\u3011<\/b><\/strong><\/p>\n<p>\u5177\u6709\u7cbe\u786e\u5b9a\u4e49\u7684\u6210\u5206\u3001\u7ed3\u6784\u548c\u754c\u9762\u7684\u91d1\u5c5e\u5f02\u8d28\u7ed3\u6784\u5728\u50ac\u5316\u3001\u7b49\u79bb\u6fc0\u5143\u5b66\u7b49\u65b9\u9762\u62e5\u6709\u5e7f\u9614\u7684\u5e94\u7528\u524d\u666f\u3002\u5728\u5408\u6210\u91d1\u5c5e\u5f02\u8d28\u7ed3\u6784\u7684\u7b56\u7565\u4e2d\uff0c\u5916\u5ef6\u6a21\u677f\/\u79cd\u5b50\u751f\u957f\u6cd5\u80fd\u591f\u5728\u751f\u957f\u4e8c\u6b21\u91d1\u5c5e\u4e4b\u524d\u8bbe\u8ba1\u6a21\u677f\/\u79cd\u5b50\u3002\u901a\u8fc7\u8bbe\u8ba1\u6a21\u677f\/\u79cd\u5b50\uff0c\u4f7f\u5176\u5177\u6709\u7279\u5b9a\u5916\u9732\u9762\u6216\u9ad8\u80fd\u4f4d\u70b9\uff08\u5982\u5806\u579b\u5c42\u9519\u548c\u5b6a\u6676\u8fb9\u754c\u3001\u5c16\u89d2\u548c\u8fb9\u7f18\uff09\uff0c\u4e8c\u6b21\u91d1\u5c5e\u7684\u5404\u5411\u5f02\u6027\u751f\u957f\u53ef\u4ee5\u5728\u5176\u7279\u5b9a\u9762\u6216\u4f4d\u70b9\u4e0a\u89e6\u53d1\uff0c\u4ece\u800c\u5f62\u6210\u9ad8\u5ea6\u63a7\u5236\u7684\u91d1\u5c5e\u5f02\u8d28\u7ed3\u6784\u3002\u7136\u800c\uff0c\u76ee\u524d\u4e3a\u6b62\uff0c\u51e0\u4e4e\u6240\u6709\u7528\u4f5c\u5916\u5ef6\u751f\u957f\u7684\u6a21\u677f\/\u79cd\u5b50\u7eb3\u7c73\u6676\u90fd\u9650\u4e8e\u5176\u70ed\u529b\u5b66\u7a33\u5b9a\u76f8\u3002\u7eb3\u7c73\u6750\u6599\u76f8\u5de5\u7a0b\uff08PEN\uff09\u4f7f\u5408\u6210\u5177\u6709\u975e\u70ed\u529b\u5b66\u7a33\u5b9a\u76f8\u7684\u91d1\u5c5e\u7eb3\u7c73\u6676\u6210\u4e3a\u53ef\u80fd\u3002\u8fd9\u4e9b\u975e\u5e38\u89c4\u76f8\u91d1\u5c5e\u7eb3\u7c73\u6676\u53ef\u8fdb\u4e00\u6b65\u88ab\u7528\u4f5c\u6a21\u677f\uff0c\u6765\u6784\u5efa\u91d1\u5c5e\u5f02\u8d28\u7ed3\u6784\u3002\u7136\u800c\uff0c\u6b64\u7c7b\u975e\u5e38\u89c4\u76f8\u91d1\u5c5e\u7eb3\u7c73\u6676\u901a\u5e38\u5177\u6709\u7279\u6b8a\u7684\u7ed3\u6784\uff0c\u5f53\u88ab\u7528\u4e3a\u6a21\u677f\u65f6\uff0c\u5176\u7279\u6b8a\u7ed3\u6784\u901a\u5e38\u4f1a\u5f71\u54cd\u4e8c\u6b21\u91d1\u5c5e\u7684\u6210\u6838\u4e0e\u751f\u957f\uff0c\u6b64\u79cd\u5f71\u54cd\u4ecd\u9700\u7cfb\u7edf\u7814\u7a76\u3002<\/p>\n<p><strong><b>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/b><\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong><b>\u9999\u6e2f\u57ce\u5e02\u5927\u5b66\u5f20\u534e<\/b><\/strong><strong><b>\u6559\u6388\uff08\u901a\u8baf\u4f5c\u8005\uff09<\/b><\/strong>\u56e2\u961f\u62a5\u9053\u4e86\u4e00\u79cd\u5168\u65b0\u7684\u6e7f\u5316\u5b66\u4e00\u9505\u6cd5\u6765\u5236\u5907\u5177\u6709\u975e\u5e38\u89c42H\/\u9762\u5fc3\u7acb\u65b9(fcc)\u5f02\u76f8\u7684\u3001\u8fd1\u4f3c\u65b9\u5f62\u7684Au\u7eb3\u7c73\u7247\u3002\u8fd9\u79cd\u8fd1\u4f3c\u65b9\u5f62\u76842H\/fcc \u5f02\u76f8Au\u7eb3\u7c73\u7247\u5177\u6709\u72ec\u7279\u7684\u7ed3\u6784\uff0c\u5373\u4e24\u4e2a\u5bf9\u8fb9\u5177\u67092H\/fcc\u5f02\u76f8\u5e76\u4e14\u5bcc\u542b\u7f3a\u9677\uff0c\u53e6\u5916\u4e24\u4e2a\u5bf9\u8fb9\u5177\u6709\u57fa\u672c\u65e0\u7f3a\u9677\u7684fcc\u76f8\uff0c\u4e0a\u4e0b\u4e24\u4e2a\u57fa\u9762\u5177\u67092H\/fcc\u5f02\u76f8\u5e76\u4e14\u5bcc\u542b\u7f3a\u9677\u3002\u57fa\u4e8e\u6b64\uff0c2H\/fcc\u5f02\u76f8Au\u7eb3\u7c73\u7247\u88ab\u7528\u4f5c\u6a21\u677f\uff0c\u7cfb\u7edf\u7814\u7a76\u4e86\u5982\u4f55\u5728Au\u6a21\u677f\u7684\u4e0d\u540c\u533a\u57df\u7684\u4e0d\u540c\u6676\u76f8\u4e0a\u9009\u62e9\u6027\u751f\u957f\u4e8c\u6b21\u91d1\u5c5eRh\u7eb3\u7c73\u68d2\u3002\u901a\u8fc7\u8c03\u63a7\u53cd\u5e94\u6761\u4ef6\uff0cRh\u7eb3\u7c73\u68d2\u5916\u5ef6\u751f\u957f\u57282H\/fcc\u5f02\u76f8Au\u7eb3\u7c73\u7247\u4e0a\uff0c\u5f62\u6210\u4e86\u4e09\u79cd\u7c7b\u578b\u76841D\/2D Rh-Au\u5f02\u8d28\u7ed3\u6784\u3002\u5728A\u578b\u5f02\u6784\u4e2d\uff0cRh\u7eb3\u7c73\u68d2\u53ea\u751f\u957f\u5728\u4e24\u4e2a2H\/fcc\u5bf9\u8fb9\u76842H\u76f8\u533a\u57df\u548cfcc\u76f8\u7684\u5c42\u9519\/\u5b6a\u6676\u533a\u57df\uff0c\u5448\u73b0\u9ad8\u7684\u4f4d\u70b9\u9009\u62e9\u6027\u548c\u4f4e\u7684\u751f\u957f\u5bc6\u5ea6\u3002\u5728B\u578b\u5f02\u8d28\u7ed3\u6784\u4e2d\uff0cRh\u7eb3\u7c73\u68d2\u751f\u957f\u5728\u4e24\u4e2a2H\/fcc\u5bf9\u8fb9\u548c\u4e24\u4e2a2H\/fcc\u57fa\u9762\u76842H\u76f8\u533a\u57df\u548cfcc\u76f8\u7684\u5c42\u9519\/\u5b6a\u6676\u533a\u57df\uff0c\u5448\u73b0\u4e2d\u7b49\u7a0b\u5ea6\u7684\u4f4d\u70b9\u9009\u62e9\u6027\u548c\u751f\u957f\u5bc6\u5ea6\u3002\u5728C\u578b\u5f02\u6784\u4e2d\uff0cRh\u7eb3\u7c73\u68d2\u751f\u957f\u5728Au\u7eb3\u7c73\u7247\u7684\u56db\u4e2a\u8fb9\u548c\u4e24\u4e2a\u57fa\u9762\u7684\u6240\u6709\u7ed3\u6784\u4f4d\u70b9\u4e0a\uff0c\u4e0d\u5177\u6709\u4f4d\u70b9\u9009\u62e9\u6027\uff0c\u4f46\u5177\u6709\u5f88\u9ad8\u7684\u751f\u957f\u5bc6\u5ea6\u3002\u6b64\u5916\uff0cC\u578b\u5f02\u8d28\u7ed3\u6784\u88ab\u7528\u4f5c\u9178\u6027\u4ecb\u8d28\u4e2d\u7535\u5316\u5b66\u6790\u6c22\u53cd\u5e94\uff08HER\uff09\u7684\u50ac\u5316\u5242\uff0c\u8868\u73b0\u51fa\u826f\u597d\u7684\u6027\u80fd\u3002\u8be5\u6210\u679c\u4ee5\u9898\u4e3a<strong><b>\u201cSelective Epitaxial Growth of Rh Nanorods on 2H\/fcc Heterophase Au Nanosheets to Form 1D\/2D Rh<\/b><\/strong><strong><b>&#8211;<\/b><\/strong><strong><b>Au Heterostructures for Highly Efficient Hydrogen Evolution\u201d<\/b><\/strong>\u53d1\u8868\u5728\u4e86<strong><b>JACS<\/b><\/strong>\u4e0a\u3002<\/p>\n<p><strong><b>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/b><\/strong><\/p>\n<p><strong><b>\u56fe1 \u4ee52H\/fcc\u5f02\u76f8Au\u7eb3\u7c73\u7247\u4e3a\u6a21\u677f\u6784\u5efa\u4e09\u79cd1D\/2D Rh-Au\u5f02\u8d28\u7ed3\u6784<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-219301\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/03\/1-5.png\" alt=\"\" width=\"600\" height=\"407\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/03\/1-5.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/03\/1-5-300x204.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u56fe2 2H\/fcc\u5f02\u76f8Au\u7eb3\u7c73\u7247\u7684\u7ed3\u6784\u8868\u5f81<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-219302\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/03\/2-5.png\" alt=\"\" width=\"600\" height=\"719\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/03\/2-5.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/03\/2-5-250x300.png 250w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff092H\/fcc Au\u7eb3\u7c73\u7247\u7684TEM\u56fe\u50cf\u3002<\/p>\n<p>\uff08b\uff09\u5178\u578b\u76842H\/fcc Au\u7eb3\u7c73\u7247\u7684STEM\u56fe\u50cf\u3002<\/p>\n<p>\uff08c\uff09\u6cbf[110]<sub>h<\/sub>\/[101]<sub>f<\/sub>\u5e26\u8f74\u7684SAED\u56fe\u3002<\/p>\n<p>\uff08d-f\uff09\u00a02H\/fcc\u8fb9\u7f18\uff08d\uff09\u30012H\/fcc\u57fa\u9762\uff08e\uff09\u548cfcc\u8fb9\u7f18\uff08f\uff09\u7684\u539f\u5b50\u5206\u8fa8\u7387HAADF-STEM\u56fe\u50cf\u3002<\/p>\n<p>\uff08g\uff09\uff08e\uff09\u4e2d\u9752\u7eff\u8272\u865a\u7ebf\u77e9\u5f62\u533a\u57df\u7684\u653e\u5927\u7684\u539f\u5b50\u5206\u8fa8\u7387HAADF-STEM\u56fe\u50cf\u3002<\/p>\n<p>\uff08h-j\uff09\u5206\u522b\u4ece\uff08d-f\uff09\u4e2d\u7684\u865a\u7ebf\u6b63\u65b9\u5f62\u751f\u6210\u7684FFT\u56fe\u3002<\/p>\n<p><strong><b>\u56fe3 A\u578b1D\/2D Rh-Au\u5f02\u8d28\u7ed3\u6784\u7684\u7ed3\u6784\u8868\u5f81<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-219303\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/03\/3-5.png\" alt=\"\" width=\"600\" height=\"750\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/03\/3-5.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/03\/3-5-240x300.png 240w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u5178\u578bA\u578b\u5f02\u8d28\u7ed3\u6784\u7684TEM\u56fe\u50cf\u3002<\/p>\n<p>\uff08b-d\uff092H\/fcc\u8fb9\u7f18\uff08b\uff09\u30012H\/fcc\u57fa\u9762\uff08c\uff09\u548cfcc\u8fb9\u7f18\uff08d\uff09\u7684\u9ad8\u500d\u7387TEM\u56fe\u50cf\u3002<\/p>\n<p>\uff08e\uff09\u5178\u578bA\u578b\u5f02\u8d28\u7ed3\u6784\u7684STEM\u56fe\u50cf\u3002<\/p>\n<p>\uff08f-h\uff09\u00a02H\/fcc\u8fb9\u7f18\uff08f\uff09\u30012H\/fcc\u57fa\u9762\uff08g\uff09\u548cfcc\u8fb9\u7f18\uff08h\uff09\u7684\u539f\u5b50\u5206\u8fa8\u7387HAADF-STEM\u56fe\u50cf\u3002<\/p>\n<p>\uff08i-l\uff09\u4ece\uff08f-h\uff09\u4e2d\u7684\u865a\u7ebf\u6b63\u65b9\u5f62\u751f\u6210\u7684FFT\u56fe\u3002<\/p>\n<p>\uff08m\uff0cn\uff09\u5178\u578bA\u578b\u5f02\u8d28\u7ed3\u6784\u76842H\/fcc\u8fb9\u7f18\uff08m\uff09\u548cfcc\u8fb9\u7f18\uff08n\uff09\u7684STEM\u56fe\u50cf\u548c\u76f8\u5e94\u7684EDS\u5143\u7d20\u5206\u5e03\u56fe\u3002<\/p>\n<p><strong><b>\u56fe4 B\u578b1D\/2D Rh-Au\u5f02\u8d28\u7ed3\u6784\u7684\u7ed3\u6784\u8868\u5f81<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-219304\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/03\/4-5.png\" alt=\"\" width=\"600\" height=\"600\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/03\/4-5.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/03\/4-5-150x150.png 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/03\/4-5-300x300.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u5178\u578bB\u578b\u5f02\u8d28\u7ed3\u6784\u7684TEM\u56fe\u50cf\u3002<\/p>\n<p>\uff08b-d\uff092H\/fcc\u8fb9\u7f18\uff08b\uff09\u30012H\/fcc\u57fa\u9762\uff08c\uff09\u548cfcc\u8fb9\u7f18\uff08d\uff09\u7684\u9ad8\u500d\u7387TEM\u56fe\u50cf\u3002<\/p>\n<p>\uff08e\uff09\u5178\u578bB\u578b\u5f02\u8d28\u7ed3\u6784\u7684STEM\u56fe\u50cf\u3002<\/p>\n<p>\uff08f-h\uff09\u00a02H\/fcc\u8fb9\u7f18\uff08f\uff09\u30012H\/fcc\u57fa\u9762\uff08g\uff09\u548cfcc\u8fb9\u7f18\uff08h\uff09\u7684\u539f\u5b50\u5206\u8fa8\u7387HAADF-STEM\u56fe\u50cf\u3002<\/p>\n<p>\uff08i-l\uff09\u4ece\uff08f-h\uff09\u4e2d\u7684\u865a\u7ebf\u6b63\u65b9\u5f62\u751f\u6210\u7684FFT\u56fe\u3002<\/p>\n<p>\uff08m\uff09\u5178\u578bB\u578b\u5f02\u8d28\u7ed3\u6784\u7684STEM\u56fe\u50cf\u548c\u76f8\u5e94\u7684EDS\u5143\u7d20\u5206\u5e03\u56fe\u3002<\/p>\n<p><strong><b>\u56fe5 C\u578b1D\/2D Rh-Au\u5f02\u8d28\u7ed3<\/b><\/strong><strong><b>\u6784<\/b><\/strong><strong><b>\u7684\u7ed3\u6784\u8868\u5f81<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-219305\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/03\/5-5.png\" alt=\"\" width=\"600\" height=\"600\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/03\/5-5.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/03\/5-5-150x150.png 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/03\/5-5-300x300.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u5178\u578bC\u578b\u5f02\u8d28\u7ed3\u6784\u7684TEM\u56fe\u50cf\u3002<\/p>\n<p>\uff08b-d\uff092H\/fcc\u8fb9\u7f18\uff08b\uff09\u30012H\/fcc\u57fa\u9762\uff08c\uff09\u548cfcc\u8fb9\u7f18\uff08d\uff09\u7684\u9ad8\u500d\u7387TEM\u56fe\u50cf\u3002<\/p>\n<p>\uff08e\uff09\u5178\u578bC\u578b\u5f02\u8d28\u7ed3\u6784\u7684STEM\u56fe\u50cf\u3002<\/p>\n<p>\uff08f-h\uff09\u00a02H\/fcc\u8fb9\u7f18\uff08f\uff09\u30012H\/fcc\u57fa\u9762\uff08g\uff09\u548cfcc\u8fb9\u7f18\uff08h\uff09\u7684\u539f\u5b50\u5206\u8fa8\u7387HAADF-STEM\u56fe\u50cf\u3002<\/p>\n<p>\uff08i\uff0cj\uff09\u4ece\uff08f\uff09\u4e2d\u7684\u865a\u7ebf\u6b63\u65b9\u5f62\u751f\u6210\u7684FFT\u56fe\u3002<\/p>\n<p>\uff08k\uff0cl\uff09\u4ece\uff08h\uff09\u4e2d\u7684\u865a\u7ebf\u6b63\u65b9\u5f62\u751f\u6210\u7684FFT\u56fe\u3002<\/p>\n<p>\uff08m\uff09\u5178\u578bC\u578b\u5f02\u8d28\u7ed3\u6784\u7684STEM\u56fe\u50cf\u548c\u76f8\u5e94\u7684EDS\u5143\u7d20\u5206\u5e03\u56fe\u3002<\/p>\n<p><strong><b>\u56fe6 \u9178\u6027\u4ecb\u8d28\u4e2dC\u578bRh-Au\u5f02\u8d28\u7ed3\u6784\u7684HER<\/b><\/strong><strong><b>\u50ac\u5316<\/b><\/strong><strong><b>\u6027\u80fd<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-219306\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/03\/6-5.png\" alt=\"\" width=\"600\" height=\"366\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/03\/6-5.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/03\/6-5-300x183.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09C\u578bRh-Au\u5f02\u8d28\u7ed3\u6784\u3001Rh\/C\uff0cPt\/C\u548c2H\/fcc Au\u7eb3\u7c73\u7247\u57280.5 M H<sub>2<\/sub>SO<sub>4<\/sub>\u6c34\u6eb6\u6db2\u4e2d\u7684\u6781\u5316\u66f2\u7ebf\u3002<\/p>\n<p>\uff08b\uff09C\u578bRh-Au\u5f02\u8d28\u7ed3\u6784\u3001Rh\/C\u548cPt\/C\u572810 mA cm<sup>&#8211;<\/sup><sup>2<\/sup>\u65f6\u7684\u8fc7\u7535\u4f4d\uff08\u5de6\u8f74\uff09\u548c30 mV\u65f6\u7684TOF\u503c\uff08\u53f3\u8f74\uff09\u7684\u6bd4\u8f83\u3002<\/p>\n<p>\uff08c\uff0cd\uff09C\u578bRh-Au\u5f02\u8d28\u7ed3\u6784\u3001Rh\/C\u548cPt\/C\u7684Tafel\u56fe\uff08c\uff09\u548cTOF\u56fe\uff08d\uff09\u3002<\/p>\n<p>\uff08e\uff09C\u578bRh-Au\u5f02\u8d28\u7ed3\u6784\u7684\u7a33\u5b9a\u6027\u6d4b\u8bd5\u3002<\/p>\n<p>\uff08f\uff09\u6bd4\u8f83C\u578bRh-Au\u5f02\u8d28\u7ed3\u6784\u4e0e\u4e00\u4e9b\u5df2\u62a5\u9053\u7684Rh\u57faHER\u7535\u50ac\u5316\u5242\u5728\u9178\u6027\u4ecb\u8d28\u4e2d\u7684HER\u6027\u80fd\u3002<\/p>\n<p><strong><b>\u3010\u5c0f\u7ed3\u3011<\/b><\/strong><\/p>\n<p>\u7efc\u4e0a\u6240\u8ff0\uff0c\u8be5\u5de5\u4f5c\u7cfb\u7edf\u7814\u7a76\u4e862H\/fcc Au\u7eb3\u7c73\u7247\u7684\u4e0d\u540c\u533a\u57df\u53ca\u4e0d\u540c\u6676\u76f8\u5bf9Rh\u7eb3\u7c73\u68d2\u4e8c\u6b21\u751f\u957f\u7684\u5f71\u54cd\u3002\u901a\u8fc7\u8c03\u63a7\u53cd\u5e94\u6761\u4ef6\uff0c\u6784\u5efa\u4e86A\u578b\u3001B\u578b\u548cC\u578b1D\/2D Rh-Au\u5f02\u8d28\u7ed3\u6784\uff0c\u5176\u4e2dRh\u7eb3\u7c73\u68d2\u7684\u751f\u957f\u5bc6\u5ea6\u4f9d\u6b21\u589e\u52a0\uff0c\u4f46\u4f4d\u70b9\u9009\u62e9\u6027\u4f9d\u6b21\u964d\u4f4e\u3002\u5177\u6709\u9ad8\u8868\u9762\u80fd\u7684fcc\u5c42\u9519\/\u5b6a\u6676\u533a\u57df\u548c2H\u7ed3\u6784\u63d0\u4f9b\u4e86\u57fa\u7840\uff0c\u800c\u5bf9\u53cd\u5e94\u6761\u4ef6\u7684\u7cbe\u786e\u8c03\u63a7\u4fdd\u8bc1\u4e86\u5408\u6210\u7684\u6210\u529f\u3002\u5229\u75281D\/2D\u51e0\u4f55\u7ed3\u6784\u548c\u5177\u6709\u4e30\u5bcc\u7f3a\u9677\u76842H\/fcc\u5f02\u76f8\u7ed3\u6784\uff0cC\u578b1D\/2D Rh-Au\u5f02\u8d28\u7ed3\u6784\u5bf9\u9178\u6027\u4ecb\u8d28\u4e2d\u7684\u7535\u5316\u5b66HER\u8868\u73b0\u51fa\u826f\u597d\u7684\u50ac\u5316\u6027\u80fd\u3002\u8be5\u5de5\u4f5c\u4e3a\u5408\u6210\u5177\u6709\u975e\u5e38\u89c4\u76f8\u7684\u91d1\u5c5e\u7eb3\u7c73\u6750\u6599\u4ee5\u53ca\u5982\u4f55\u5229\u7528\u6a21\u677f\u7684\u7ed3\u6784\u7279\u6b8a\u6027\u6765\u6784\u5efa\u5177\u6709\u7279\u6b8a\u7ed3\u6784\u7684\u91d1\u5c5e\u5f02\u8d28\u7ed3\u7eb3\u7c73\u6750\u6599\u63d0\u4f9b\u4e86\u65b0\u7684\u601d\u8def\u3002<\/p>\n<p><strong><b>\u6587\u732e\u94fe\u63a5\uff1a<\/b><\/strong><a href=\"https:\/\/pubs.acs.org\/doi\/abs\/10.1021\/jacs.1c00612\"><u>Selective Epitaxial Growth of Rh Nanorods on 2H\/fcc Heterophase Au Nanosheets to Form 1D\/2D Rh<\/u><u>&#8211;<\/u><u>Au Heterostructures for Highly Efficient Hydrogen Evolution<\/u><\/a>\uff08JACS\uff0c2021\uff0cDOI: 10.1021\/jacs.1c00612\uff09<\/p>\n<p><strong><b>\u5171\u540c\u7b2c\u4e00\u4f5c\u8005<\/b><\/strong><strong><b>\uff1a<\/b><\/strong>\u5218\u4f73\u73ae\uff0c\u725b\u6587\u65b0\uff0c\u5218\u8d35\u9ad8<\/p>\n<p><strong><b>\u901a\u8baf\u4f5c\u8005\uff1a<\/b><\/strong>\u5f20\u534e<\/p>\n<p><strong><b>\u901a\u8baf\u5355\u4f4d\uff1a<\/b><\/strong>\u9999\u6e2f\u57ce\u5e02\u5927\u5b66<\/p>\n<p><strong><b>\u3010<\/b><\/strong><strong><b>\u8bfe\u9898\u7ec4\u4ecb\u7ecd<\/b><\/strong><strong><b>\u3011<\/b><\/strong><\/p>\n<p>\u5f20\u534e\uff0c1992\u548c1995\u5e74\u5206\u522b\u83b7\u5357\u4eac\u5927\u5b66\u5b66\u58eb\u548c\u7855\u58eb\u5b66\u4f4d\uff0c1998\u5e74\u83b7\u5317\u4eac\u5927\u5b66\u535a\u58eb\u5b66\u4f4d(\u5bfc\u5e08\uff1a\u5218\u5fe0\u8303\u9662\u58eb)\u30021999\u548c2001\u5e74\u5206\u522b\u8d74\u6bd4\u5229\u65f6\u9c81\u6c76\u5927\u5b66Prof. Frans C. De Schryver\u8bfe\u9898\u7ec4\u548c\u7f8e\u56fd\u897f\u5317\u5927\u5b66Prof. Chad A. Mirkin\u8bfe\u9898\u7ec4\u4ece\u4e8b\u535a\u58eb\u540e\u7814\u7a76\u30022003\u548c2005\u5e74\u5206\u522b\u5728\u7f8e\u56fdNanoInk\u516c\u53f8\u548c\u65b0\u52a0\u5761\u751f\u7269\u5de5\u7a0b\u4e0e\u7eb3\u7c73\u6280\u672f\u7814\u7a76\u9662\u5de5\u4f5c\u30022006\u5e74\u52a0\u5165\u65b0\u52a0\u5761\u5357\u6d0b\u7406\u5de5\u5927\u5b66\u6750\u6599\u79d1\u5b66\u4e0e\u5de5\u7a0b\u5b66\u9662\u4efb\u52a9\u7406\u6559\u6388\uff0c\u5206\u522b\u4e8e2011\u30012013\u5e74\u664b\u5347\u4e3a\u526f\u6559\u6388\u3001\u6559\u6388\u30022019\u5e74\uff0c\u5168\u804c\u52a0\u76df\u9999\u6e2f\u57ce\u5e02\u5927\u5b66\u5316\u5b66\u7cfb\uff0c\u73b0\u4efb\u80e1\u6653\u660e\u8bb2\u5ea7\u6559\u6388\uff08\u7eb3\u7c73\u6750\u6599\uff09\u3002 \u00a0<\/p>\n<p>\u5f20\u534e\u6559\u6388\u7684\u7814\u7a76\u9886\u57df\u6db5\u76d6\u591a\u4e2a\u524d\u6cbf\u4ea4\u53c9\u5b66\u79d1\u3002\u76ee\u524d\u7684\u7814\u7a76\u805a\u7126\u4e8e\u7eb3\u7c73\u6750\u6599\u76f8\u5de5\u7a0b\uff08PEN\uff09\u3001\u7cbe\u7ec6\u591a\u7ea7\u7ed3\u6784\u7684\u53ef\u63a7\u5916\u5ef6\u751f\u957f\u7b49\uff1b\u5177\u4f53\u5de5\u4f5c\u4e3b\u8981\u5305\u62ec\u4ee5\u4e0b\u51e0\u4e2a\u65b9\u9762\uff1a\u8d85\u8584\u4e8c\u7ef4\u7eb3\u7c73\u6750\u6599\uff08\u5982\u91d1\u5c5e\u7eb3\u7c73\u7247\u3001\u91d1\u5c5e\u786b\u5316\u7269\u3001\u77f3\u58a8\u70ef\u3001\u91d1\u5c5e\u6709\u673a\u9aa8\u67b6\u3001\u5171\u4ef7\u6709\u673a\u6846\u67b6\u7b49\uff09\u3001\u65b0\u578b\u91d1\u5c5e\u76f8\u548c\u534a\u5bfc\u4f53\u7eb3\u7c73\u6750\u6599\u3001\u65b0\u578b\u65e0\u5b9a\u5f62\u7eb3\u7c73\u6750\u6599\uff0c\u53ca\u5176\u591a\u529f\u80fd\u7eb3\u7c73\u590d\u5408\u6750\u6599\u7684\u5236\u5907\uff0c\u4ee5\u53ca\u5728\u50ac\u5316\u3001\u6e05\u6d01\u80fd\u6e90\u3001\u5149\u7535\u5668\u4ef6\u3001\u7eb3\u7c73\u4e0e\u751f\u7269\u4f20\u611f\u3001\u73af\u5883\u6c34\u6c61\u67d3\u5904\u7406\u7b49\u65b9\u9762\u7684\u5e94\u7528\u7814\u7a76\u3002<\/p>\n<p>\u8fc4\u4eca\u4e3a\u6b62\uff0c\u5f20\u534e\u6559\u6388\u5df2\u7533\u8bf7\u4e8670\u4f59\u9879\u4e13\u5229\uff08\u5305\u62ec\u6388\u67431\u9879\u4e2d\u56fd\u4e13\u5229\u300110\u9879\u7f8e\u56fd\u4e13\u5229\u30011\u9879\u6b27\u6d32\u4e13\u5229\u548c1\u9879\u65b0\u52a0\u5761\u4e13\u5229\uff09\uff0c\u53d1\u8868\u4e86520\u4f59\u7bc7\u5b66\u672f\u8bba\u6587\u3002\u622a\u6b62\u4e8e2021\u5e743\u6708\uff0c\u57fa\u4e8eWeb of Science\u548c\u8c37\u6b4c\u5b66\u672f\u7684\u7edf\u8ba1\u6570\u636e\uff0c\u5f20\u534e\u6559\u6388\u7684\u6587\u7ae0\u5206\u522b\u88ab\u5f1585,000\u4f59\u6b21\uff08H\u56e0\u5b50\u4e3a143\uff09\u548c99,700\u4f59\u6b21\uff08H\u56e0\u5b50\u4e3a153\uff09\u3002\u5f20\u534e\u6559\u6388\u4e8e2020\u5e74\u5f53\u9009\u6b27\u6d32\u79d1\u5b66\u9662\u5916\u7c4d\u9662\u58eb (Foreign Fellow of European Academy of Sciences)\uff0c2015\u5e74\u5f53\u9009\u4e9a\u592a\u6750\u6599\u5b66\u9662\u9662\u58eb (Academician of the Asia Pacific Academy of Materials)\uff0c2014\u5e74\u5f53\u9009\u82f1\u56fd\u7687\u5bb6\u5316\u5b66\u4f1a\u4f1a\u58eb (Fellow of the Royal Society of Chemistry)\u3002<\/p>\n<p>\u5f20\u534e\u6559\u6388\u6240\u83b7\u5f97\u5b66\u672f\u8363\u8a89\u548c\u5956\u9879\u5305\u62ec\uff1a\u5165\u9009\u201c\u5168\u7403\u6700\u6709\u5f71\u54cd\u529b\u79d1\u5b66\u601d\u60f3\u540d\u5f55\uff08the World&#8217;s Most Influential Scientific Minds\uff09\u201d\u548c\u201c\u9ad8\u88ab\u5f15\u79d1\u5b66\u5bb6\u540d\u5355\u201d(2014\u5e74\u201c\u6750\u6599\u79d1\u5b66\u201d\uff0c2015-2020\u201c\u5316\u5b66\u201d\u548c\u201c\u6750\u6599\u79d1\u5b66\u201d\uff1b\u6c64\u68ee\u8def\u900f\/\u79d1\u777f\u552f\u5b89), 2014\u548c2015\u5e74\u5206\u522b\u5165\u9009\u5168\u740317\u548c19\u4f4d\u70ed\u95e8\u79d1\u5b66\u5bb6\u699c\u5355 (Hottest Researchers of Today\uff0c\u6c64\u68ee\u8def\u900f)\uff0c\u8363\u83b7\u6fb3\u5927\u5229\u4e9a\u4f0d\u9f99\u8d21\u5927\u5b66\u6821\u957f\u56fd\u9645\u5b66\u8005\u5956 (Vice-Chancellor&#8217;s International Scholar Award\uff0c2016)\uff0c\u7f8e\u56fd\u5316\u5b66\u5b66\u4f1aACS Nano Lectureship\u5956 (2015), \u4e16\u754c\u6587\u5316\u7406\u4e8b\u4f1a(WCC)\u7279\u522b\u8868\u5f70\u5956 (Special Recognition Award\uff0c2013), \u5e0c\u814aONASSIA Foundation Lectureship (2013), SMALL\u9752\u5e74\u521b\u65b0\u5956 (Wiley-VCH, 2012)\uff0c\u5357\u6d0b\u6770\u51fa\u7814\u7a76\u5956 (2011)\uff0c\u7b49\u3002<\/p>\n<p>\u5f20\u534e\u6559\u6388\u76f8\u5173\u5b66\u672f\u7f51\u9875\uff1a<\/p>\n<p>https:\/\/www.cityu.edu.hk\/chem\/profile\/hzhang.html<\/p>\n<p>https:\/\/scholars.cityu.edu.hk\/en\/persons\/hua-zhang(8f4e048e-884d-4f19-b2b4-ca4d3d53c515).html<\/p>\n<p>https:\/\/publons.com\/researcher\/1434653\/hua-zhang\/publications\/<\/p>\n<p>http:\/\/orcid.org\/0000-0001-9518-740X<\/p>\n<p>https:\/\/scholar.google.com\/citations?user=Cgo45S8AAAAJ&amp;hl=en \u00a0\u00a0<\/p>\n<p>\u672c\u6587\u7531<strong><b>\u6728\u6587\u97ec<\/b><\/strong>\u7ffb\u8bd1\uff0c\u6750\u6599\u725b\u6574\u7406\u7f16\u8f91\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c<u>\u6295\u7a3f\u90ae\u7bb1<\/u><u>tougao@cailiaoren.com<\/u>\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u5177\u6709\u7cbe\u786e\u5b9a\u4e49\u7684\u6210\u5206\u3001\u7ed3\u6784\u548c\u754c\u9762\u7684\u91d1\u5c5e\u5f02\u8d28\u7ed3\u6784\u5728\u50ac\u5316\u3001\u7b49\u79bb\u6fc0\u5143\u5b66\u7b49\u65b9\u9762\u62e5\u6709\u5e7f\u9614\u7684\u5e94\u7528\u524d\u666f\u3002\u5728\u5408\u6210\u91d1\u5c5e\u5f02\u8d28\u7ed3\u6784\u7684\u7b56\u7565\u4e2d\uff0c\u5916\u5ef6\u6a21\u677f\/\u79cd\u5b50\u751f\u957f\u6cd5\u80fd\u591f\u5728\u751f\u957f\u4e8c\u6b21&#8230;<\/p>\n","protected":false},"author":2109,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[116,3575,2639],"class_list":["post-219300","post","type-post","status-publish","format-standard","hentry","category-jiedu","tag-catalyst","tag-3575","tag-2639"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/219300"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/2109"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=219300"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/219300\/revisions"}],"predecessor-version":[{"id":219420,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/219300\/revisions\/219420"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=219300"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=219300"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=219300"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}