{"id":225626,"date":"2021-08-07T06:30:38","date_gmt":"2021-08-06T22:30:38","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=225626"},"modified":"2021-08-06T16:16:31","modified_gmt":"2021-08-06T08:16:31","slug":"%e5%8d%97%e4%ba%ac%e5%b7%a5%e4%b8%9a%e5%a4%a7%e5%ad%a6%e5%90%b4%e5%ae%87%e5%b9%b3%e6%95%99%e6%8e%88%e8%af%be%e9%a2%98%e7%bb%84eem-%e5%8d%95%e5%8e%9f%e5%ad%90mo%e9%94%9a%e5%ae%9a%e7%a3%b7%e7%82%b9","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=225626","title":{"rendered":"\u5357\u4eac\u5de5\u4e1a\u5927\u5b66\u5434\u5b87\u5e73\u6559\u6388\u8bfe\u9898\u7ec4EEM: \u5355\u539f\u5b50Mo\u951a\u5b9a\u78f7\u70b9\u7f3a\u9677\u5355\u5c42\u78f7\u5316\u787c\u4f5c\u4e3a\u6c2e\u8fd8\u539f\u53cd\u5e94\u7684\u9ad8\u6027\u80fd\u7535\u50ac\u5316\u5242\u7684\u8ba1\u7b97\u8bbe\u8ba1"},"content":{"rendered":"<p data-mpa-powered-by=\"yiban.io\"><strong>\u6210\u679c\u7b80\u4ecb<\/strong><\/p>\n<section>\n<section>\n<section>\n<section data-tools=\"135\u7f16\u8f91\u5668\" data-id=\"98545\" data-color=\"#374aae\">\n<section>\n<section>\n<section data-autoskip=\"1\">\n<section>\n<p>\u8fd1\u65e5\uff0c<strong>\u5357\u4eac\u5de5\u4e1a\u5927\u5b66\u5434\u5b87\u5e73\u6559\u6388\u8bfe\u9898\u7ec4\u548c\u6b66\u6c49\u7406\u5de5\u5927\u5b66\u7684\u8d75\u7131\u6559\u6388\u8bfe\u9898\u7ec4<\/strong>\u5728<em><strong>Energy &amp; Environmental Materials<\/strong><\/em>\u4e0a\u53d1\u8868\u9898\u4e3a\u201c<em><strong>Computational Design of Single Mo Atom Anchored Defective Boron Phosphide Monolayer as a High-performance Electrocatalyst for the Nitrogen Reduction Reaction<\/strong><\/em><strong>\u201d<\/strong>\u7684\u7814\u7a76\u8bba\u6587\u3002\u8be5\u8bba\u6587\u5229\u7528\u7b2c\u4e00\u6027\u539f\u7406\u548cDFT\u8ba1\u7b97\u7b5b\u9009\u51fa\u5177\u6709\u6700\u4f73\u50ac\u5316\u6027\u80fd\u7684Mo\u5355\u539f\u5b50\u951a\u5b9a\u7684\u5177\u6709\u78f7\u70b9\u7f3a\u9677\u7684\u5355\u5c42BP\uff08Mo\/BP\uff09\uff0c\u8be5Mo\/BP\u7684\u56fa\u6c2e\u53cd\u5e94\u8def\u5f84\u4f18\u9009\u4fc3\u9176\u673a\u5236\u548c\u8fde\u7eed\u673a\u5236\uff1b\u7535\u8377\u5e03\u5c45\u5206\u6790\u8868\u660e\uff0cMo-B<sub>3<\/sub>\u57fa\u56e2\u5728\u8fd8\u539f\u8fc7\u7a0b\u4e2d\u4f5c\u4e3a\u7535\u8377\u4f20\u9012\u4f53\u4e2d\u5fc3\u548c\u50ac\u5316\u6d3b\u6027\u4e2d\u5fc3\uff1b\u6b64\u5916\uff0cMo\/BP\u7684\u91d1\u5c5e\u7279\u6027\u6709\u5229\u4e8e\u5feb\u901f\u7535\u5b50\u8f6c\u79fb\uff0c\u63d0\u9ad8\u7535\u50ac\u5316\u53cd\u5e94\u7684\u6548\u7387\u3002\u8bc1\u660e\u4e86Mo\/BP\u662f\u4e00\u79cd\u5f88\u6709\u524d\u9014\u7684\u5355\u539f\u5b50\u56fa\u5b9aN<sub>2<\/sub>\u50ac\u5316\u5242\u3002\u8fd9\u9879\u7814\u7a76\u6709\u671b\u6fc0\u53d1\u5b9e\u9a8c\u548c\u7406\u8bba\u7684\u7ed3\u5408\uff0c\u8fdb\u4e00\u6b65\u63a2\u7d22\u66f4\u6709\u6f5c\u529b\u7684\u5355\u539f\u5b50\u7535\u50ac\u5316\u5242\u5728\u5408\u6210NH<sub>3<\/sub>\u4e2d\u7684\u5e94\u7528\u3002<\/p>\n<\/section>\n<\/section>\n<\/section>\n<\/section>\n<\/section>\n<\/section>\n<\/section>\n<\/section>\n<p><strong>\u5f15\u8a00<\/strong><\/p>\n<p>\u50ac\u5316\u8fd8\u539f\u6c2e\u6c14(N<sub>2<\/sub>)\u5236\u6c28(NH<sub>3<\/sub>)\u662f\u6700\u91cd\u8981\u548c\u6700\u5177\u6311\u6218\u6027\u7684\u5de5\u4e1a\u53cd\u5e94\u4e4b\u4e00\u3002\u4eba\u4eec\u666e\u904d\u8ba4\u4e3a\u7535\u5316\u5b66\u8fd8\u539f\u56fa\u6c2e\u662f\u6709\u6f5c\u529b\u66ff\u4ee3\u4f20\u7edf\u7684Haber-Bosch\u6cd5\u7684\u6280\u672f\u3002\u7136\u800c\uff0c\u8be5\u8fc7\u7a0b\u9700\u8981\u9ad8\u6548\u7684\u50ac\u5316\u5242\u6765\u8fdb\u884cN<sub>2<\/sub>\u8fd8\u539f\u53cd\u5e94(NRR)\u3002\u78f7\u5316\u787c(BP)\u5177\u6709\u8f83\u9ad8\u7684\u5bfc\u70ed\u6027\u3001\u5316\u5b66\u7a33\u5b9a\u6027\u3001\u7535\u8377\u8fc1\u79fb\u7387\u548c\u673a\u68b0\u5f3a\u5ea6\uff0c\u88ab\u8bc1\u660e\u662f\u4e00\u79cd\u9ad8\u6548\u7684\u7535\u5316\u5b66\u5408\u6210NH<sub>3<\/sub>\u7684\u50ac\u5316\u5242\u3002\u672c\u6587\u901a\u8fc7\u91c7\u7528\u7b2c\u4e00\u6027\u539f\u7406\u8ba1\u7b97\uff0c\u7cfb\u7edf\u5730\u7b5b\u9009\u4e86\u591a\u79cd\u5177\u6709\u50ac\u5316\u6f5c\u529b\u7684\u8fc7\u6e21\u91d1\u5c5e\uff08TM\uff09\u5355\u539f\u5b50\u951a\u5b9a\u7684\u5177\u6709\u78f7\u7f3a\u9677\u7684\u5355\u5c42\u78f7\u5316\u787c\u3002\u5229\u7528\u78f7\u70b9\u7f3a\u9677\u7684\u5355\u5c42BP\u5206\u5b50\u4e2d\u7684\u4e0d\u9971\u548cB\u539f\u5b50\u6765\u56fa\u5b9a\u5355TM\u539f\u5b50\u6765\u6fc0\u6d3b\u60f0\u6027N<sub>2<\/sub>\u5206\u5b50\u3002DFT\u8ba1\u7b97\u8868\u660e\uff0c\u5355TM\u539f\u5b50\u5728BP\u5355\u5c42\u4e2d\u6709\u826f\u597d\u7684\u7a33\u5b9a\u6027\uff0c\u53ef\u4ee5\u951a\u5b9a\u5728\u5355P\u7a7a\u4f4d\u4e0a\u3002\u6b64\u5916\uff0c\u951a\u5b9a\u5728BP\u5355\u5206\u5b50\u5c42\u4e0a\u7684Mo\u539f\u5b50\u5728\u6d3b\u5316N<sub>2<\/sub>\u5206\u5b50\u548c\u964d\u4f4e*NNH\u751f\u6210\u80fd\u5792\u7684\u540c\u65f6\uff0c\u5177\u6709\u826f\u597d\u7684N<sub>2<\/sub>\u8fd8\u539f\u50ac\u5316\u6d3b\u6027\u3002\u5728\u6b64\u57fa\u7840\u4e0a\uff0c\u8fdb\u4e00\u6b65\u7814\u7a76\u4e86Mo\/BP\u50ac\u5316N<sub>2<\/sub>\u5438\u9644\u8fc7\u7a0b\u548c\u7535\u5316\u5b66\u8f6c\u5316\u4e3aNH<sub>3<\/sub>\u76844\u79cd\u8be6\u7ec6\u673a\u7406\u3002\u7ed3\u679c\u8868\u660e\uff0c\u9176\u4fc3\u673a\u5236\u548c\u8fde\u7eed\u673a\u5236\u662fMo\/BP\u56fa\u5b9aN<sub>2<\/sub>\u7684\u6700\u4f18\u53cd\u5e94\u9014\u5f84\uff0c\u5176\u8fc7\u7535\u4f4d\u4e3a0.52 V\u3002\u56e0\u6b64\uff0c\u8bc1\u660e\u4e86Mo\u5355\u539f\u5b50\u951a\u5b9a\u7684\u5177\u6709P\u7a7a\u4f4d\u7f3a\u9677\u7684BP\u5355\u5206\u5b50\u5c42\u662f\u4e00\u79cd\u5f88\u6709\u524d\u9014\u7684NRR\u50ac\u5316\u5242\u3002\u672c\u7814\u7a76\u4e3a\u8bbe\u8ba1\u5355\u539f\u5b50\u7535\u50ac\u5316\u5242\u7528\u4e8e\u5408\u6210NH<sub>3<\/sub>\u63d0\u4f9b\u4e86\u4e00\u6761\u65b0\u7684\u9014\u5f84\u3002<\/p>\n<section><strong>\u56fe\u6587\u5bfc\u8bfb<\/strong><\/section>\n<section><\/section>\n<section>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-225636\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/1-4.png\" alt=\"\" width=\"600\" height=\"142\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/1-4.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/1-4-300x71.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<section><strong>\u56fe1.<\/strong>\u00a0a) H\u548cN<sub>2<\/sub>\u7684\u81ea\u7531\u80fd\u3002b) \u8ba1\u7b97\u7684*NNH\u548c*NH<sub>2<\/sub>\u7684\u5438\u9644\u80fd\u548cc) p\u70b9\u7f3a\u9677\u5355\u5c42BP\u4e0a\u4e0d\u540c\u5355\u539f\u5b50\u7b2c\u4e00\u6b65(*NN\u5230*NNH)\u7684\u53cd\u5e94\u81ea\u7531\u80fd\u3002<\/section>\n<section><\/section>\n<section>\u9996\u5148\uff0c\u6211\u4eec\u6839\u636e\u4ee5\u4e0b\u4e09\u4e2a\u6807\u51c6\u6765\u7b5b\u9009\u5408\u9002\u7684\u50ac\u5316\u5242\uff1a1\uff09\u5bf9N<sub>2<\/sub>\u5206\u5b50\u7684\u6355\u83b7\u80fd\u529b\u548c\u5bf9HER\u548cNRR\u53cd\u5e94\u7684\u4f18\u5148\u9009\u62e9\u6027\uff1b2)\u7a33\u5b9a*NNH\uff1b3) \u4e0d\u7a33\u5b9a*NH<sub>2<\/sub>\u7269\u79cd\u3002\u867d\u7136N<sub>2<\/sub>\u7684\u5438\u9644\u662f\u975e\u7535\u5316\u5b66\u8fc7\u7a0b\uff0c\u4f46\u5982\u679cN<sub>2<\/sub>\u4e0d\u80fd\u88ab\u5145\u5206\u6355\u83b7\uff0c\u5219\u5f88\u96be\u8fdb\u884c\u4e0b\u4e00\u6b65\u7684\u52a0\u6c22\u53cd\u5e94\u5e76\u83b7\u5f97\u8f83\u9ad8\u7684NRR\u9009\u62e9\u6027\u3002\u4ece<strong>\u56fe1<\/strong>\uff08a\uff09\u4e2d\u53ef\u4ee5\u770b\u51fa\uff0c\u6240\u6709\u7684\u5355\u4e00\u91d1\u5c5e\u5bf9N<sub>2<\/sub>\u7684\u5438\u9644\u6027\u5f88\u597d\uff0c\u5c24\u5176\u662fFe\u3001Mo\u548cTi\u8fd9\u4e09\u79cd\u91d1\u5c5e\uff0cN<sub>2<\/sub>\u5206\u5b50\u5728\u8fd9\u4e09\u79cd\u91d1\u5c5e\u4e0a\u7684\u5316\u5b66\u5438\u9644\u0394G\u503c\u5747\u4e3a\u8d1f\u3002\u53e6\u4e00\u65b9\u9762\uff0c\u5f53H\u5438\u9644\u6bd4N<sub>2<\/sub>\u5438\u9644\u66f4\u53d7\u6b22\u8fce\u65f6\uff0c\u5927\u591a\u6570\u91d1\u5c5e\u8868\u9762\u4f1a\u88ab*H\u8986\u76d6\uff0c\u88ab\u5438\u9644\u7684*H\u4e0d\u4ec5\u963b\u65ad\u4e86NRR\u7684\u6d3b\u6027\u4f4d\u70b9\uff0c\u8fd8\u4f1a\u53d1\u751f\u4e0d\u5fc5\u8981\u7684HER\u8fc7\u7a0b\uff0c\u964d\u4f4eNRR\u53cd\u5e94\u7684\u6cd5\u62c9\u7b2c\u6548\u7387\u3002\u4e3a\u6bd4\u8f83MTs\/BP\u4e0aNRR\u53cd\u5e94\u76f8\u5bf9\u4e8eHER\u53cd\u5e94\u7684\u4f18\u5148\u9009\u62e9\u6027\uff0c\u8fd8\u8ba1\u7b97\u4e86*H\u7684\u5438\u9644\u81ea\u7531\u80fd(\u0394GH)\u3002\u5bf9\u4e8e\u5927\u591a\u6570TMs\/BP\u50ac\u5316\u5242\uff0cN<sub>2<\/sub>\u7684\u7ed3\u5408\u6bd4H\u7684\u7ed3\u5408\u66f4\u5f3a\uff0c\u8fd9\u8bf4\u660e\u53cd\u5e94\u6709\u5229\u4e8e\u5411NRR\u53cd\u5e94\u8fdb\u4e00\u6b65\u53d1\u5c55\u3002\u53ea\u6709\u5c11\u6570\u51e0\u79cd\u91d1\u5c5e\u7684\u0394GH\u503c\u5927\u4e8eN<sub>2<\/sub>\uff0c\u5982Cu\/BP\u3001Mn\/BP\u3001Ru\/BP\u548cFe\/BP\uff0c\u8fd9\u5c31\u53ef\u4ee5\u6392\u9664\u4e86\u8fd9\u51e0\u79cd\u6750\u6599\u4f5c\u4e3aNRR\u50ac\u5316\u5242\u7684\u53ef\u80fd\u6027\u3002\u6839\u636e\u6807\u51c62\u548c3\uff0c\u5408\u9002\u7684\u50ac\u5316\u5242\u5e94\u8be5\u7a33\u5b9a*NNH\uff0c\u4f46\u4e0d\u7a33\u5b9a*NH<sub>2<\/sub>\u3002\u5982\u56fe1b\u6240\u793a\uff0c\u5728\u8fd9\u4e9bTMs\/BP\u50ac\u5316\u5242\u4e2d\uff0cMo\/BP\u662f\u6700\u7b26\u5408\u6761\u4ef6\u7684\u50ac\u5316\u5242\uff0c\u8bf4\u660eMo\/BP\u50ac\u5316\u5242\u53ef\u80fd\u5177\u6709\u826f\u597d\u7684\u56faN<sub>2<\/sub>\u6027\u80fd\u3002\u5bf9\u4e8e\u5927\u591a\u6570\u5355\u539f\u5b50\u50ac\u5316\u5242\u6765\u8bf4\uff0c\u7535\u4f4d\u51b3\u5b9a\u6b65\u9aa4(PDS)\u662f*NNH\u5f62\u6210\u7684\u7b2c\u4e00\u4e2a\u8d28\u5b50\u5316\u6b65\u9aa4\u6216*NH<sub>3<\/sub>\u5f62\u6210\u7684\u6700\u540e\u4e00\u4e2a\u8d28\u5b50\u5316\u6b65\u9aa4\u3002\u4e00\u822c\u60c5\u51b5\u4e0b\uff0c\u5982\u679c\u7b2c\u4e00\u4e2a\u8d28\u5b50\u5316\u6b65\u9aa4\u7684\u53cd\u5e94\u81ea\u7531\u80fd\u53d8\u5316\u8d85\u8fc70.8 eV\uff0c\u5219\u540e\u7eed\u53cd\u5e94\u6b65\u9aa4\u4e0d\u4f1a\u8fdb\u884c\u3002\u56e0\u6b64\uff0c\u6211\u4eec\u7ee7\u7eed\u901a\u8fc7\u7814\u7a76\u7b2c\u4e00\u8d28\u5b50\u81ea\u7531\u80fd\u53d8\u5316\u5c0f\u4e8e0.8 eV\u7684SACs\u6765\u786e\u5b9a\u6700\u7406\u60f3\u7684TM\/BP\u50ac\u5316\u5242\u3002\u56fe1c\u603b\u7ed3\u4e86BP\u7eb3\u7c73\u7247\u8868\u9762\u8d1f\u8f7d\u7684SACs\u5f62\u6210*NNH\u7684\u53cd\u5e94\u81ea\u7531\u80fd\u3002\u7ed3\u679c\u8868\u660e\uff0cMo\/BP\u7eb3\u7c73\u7247\u5f62\u6210*NNH\u7684\u7b2c\u4e00\u8d28\u5b50\u81ea\u7531\u80fd\u4e3a0.68 eV\uff0c\u662f\u6bd4\u8f83\u7406\u60f3\u7684\u50ac\u5316\u5242\u3002\u56e0\u6b64\uff0c\u7ed3\u5408\u4e09\u4e2a\u6807\u51c6\u548c*NNH\u7684\u5f62\u6210\uff0c\u9009\u62e9Mo\/BP\u7eb3\u7c73\u7247\u4f5c\u4e3a\u7814\u7a76\u7684\u6700\u5408\u9002\u7684\u7535\u50ac\u5316\u5242\u3002<\/section>\n<\/section>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-225637\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/2-4.png\" alt=\"\" width=\"600\" height=\"302\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/2-4.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/2-4-300x151.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<section><strong>\u56fe2.\u00a0<\/strong>a)\u4f18\u5316\u540e\u7684Mo\/BP\u539f\u5b50\u7ed3\u6784\u7684\u9876\u89c6\u56fe\u548c\u4fa7\u89c6\u56fe\uff1bb) \u5438\u9644\u7684\u5355\u4e2aMo\u539f\u5b50\u4ece\u7f3a\u9677\u7ed3\u5408\u4f4d\u70b9\u6269\u6563\u5230\u76f8\u90bb\u7684\u7a7a\u5fc3\u4f4d\u70b9\u7684\u6700\u5c0f\u80fd\u91cf\u8def\u5f84(MEP)\u548c\u539f\u5b50\u7ed3\u6784\u3002<\/section>\n<p>\u8ba1\u7b97\u5f97\u5230\u7684Mo\u951a\u5b9a\u7684\u5177\u6709P\u70b9\u7f3a\u9677\u7684\u5355\u5c42BP\u7684\u539f\u5b50\u7ed3\u6784\u5982<strong>\u56fe2<\/strong>a\u6240\u793a\u3002\u5355\u539f\u5b50\u4e0e\u6750\u6599\u7684\u7ed3\u5408\u8d8a\u5f3a\uff0c\u5176\u7a33\u5b9a\u6027\u8d8a\u597d\uff0c\u8fd9\u6837\u53ef\u4ee5\u66f4\u6709\u6548\u5730\u9632\u6b62\u5176\u5728\u5408\u6210\u548c\u5b9e\u9645\u5e94\u7528\u4e2d\u53d1\u751f\u805a\u96c6\uff0c\u4ece\u800c\u4fdd\u6301\u957f\u671f\u6709\u6548\u7684\u50ac\u5316\u6d3b\u6027\u3002\u5728\u52a8\u529b\u5b66\u4e0a\uff0c\u8ba1\u7b97\u4e86\u5438\u9644\u7684Mo\u539f\u5b50\u4eceP\u7a7a\u4f4d\u5411\u76f8\u90bb\u7a7a\u4f4d\u7684\u8fc1\u79fb\u3002\u5bf9\u4e8e\u5982\u56fe2b\u6240\u793a\u7684\u9ad8\u6269\u6563\u52bf\u5792(4.62 eV)\uff0c\u8fd9\u79cd\u8fc1\u79fb\u8fc7\u7a0b\u51e0\u4e4e\u662f\u4e0d\u53ef\u80fd\u7684\uff0c\u8bf4\u660eMo\/BP\u5177\u6709\u5f88\u597d\u7684\u7a33\u5b9a\u6027\uff0c\u5728\u5408\u6210\u548c\u5b9e\u9645\u5e94\u7528\u4e2d\uff0c\u5f88\u96be\u53d1\u751f\u805a\u96c6\uff0c\u4ece\u800c\u80fd\u591f\u4fdd\u6301\u9ad8\u6548\u7684\u50ac\u5316\u6d3b\u6027\u3002<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-225638\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/3-4.png\" alt=\"\" width=\"600\" height=\"187\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/3-4.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/3-4-300x94.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe3.<\/strong>a) Mo\/BP\u8868\u9762N<sub>2<\/sub>\u5438\u9644\u539f\u5b50\u6784\u578b\u7684\u7aef\u90e8\u548c\u4fa7\u90e8\u3002<\/p>\n<p>\u4f5c\u4e3aNRR\u521d\u59cb\u5316\u7684\u7b2c\u4e00\u6b65\uff0cN<sub>2<\/sub>\u5728\u50ac\u5316\u5242\u8868\u9762\u7684\u5438\u9644\u65b9\u5f0f\u5728\u540e\u7eed\u53cd\u5e94\u9014\u5f84\u4e2d\u8d77\u7740\u91cd\u8981\u4f5c\u7528\u3002\u5982<strong>\u56fe3<\/strong>\u6240\u793a\uff0c\u5728\u7f3a\u9677\u7684BP\u5355\u5206\u5b50\u5c42\u4e0a\u7684Mo\u539f\u5b50\uff0c\u7aef\u90e8\u548c\u4fa7\u90e8\u7684N<sub>2<\/sub>\u5438\u9644\u6784\u578b\u5728\u80fd\u91cf\u4e0a\u90fd\u662f\u6709\u5229\u7684\u3002\u5bf9\u4e8e\u7aef\u90e8\u5438\u9644\u6765\u8bf4\uff0cMo\u548cN<sub>2<\/sub>\u4e4b\u95f4\u7684Mo-N\u952e\u957f\u4e3a2.16\u00c5\uff1b\u4fa7\u8fb9\u6784\u578b\u4e2d\u7684Mo-N\u952e\u957f\u4e3a2.27 \u00c5\u548c2.44 \u00c5\u3002\u7535\u8377\u5bc6\u5ea6\u5dee\u8868\u660e\uff0c\u7535\u8377\u4ea4\u6362\u548c\u8f6c\u79fb\u4e3b\u8981\u53d1\u751f\u5728Mo\u539f\u5b50\u548cN<sub>2<\/sub>\u4e4b\u95f4\u3002<\/p>\n<section><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-225639\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/4-4.png\" alt=\"\" width=\"600\" height=\"390\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/4-4.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/4-4-300x195.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/section>\n<section><\/section>\n<section><strong>\u65b9\u68481.\u00a0<\/strong>\u5728Mo\/BP\u8868\u9762N<sub>2<\/sub>\u8fd8\u539f\u6210NH<sub>3<\/sub>\u7684\u8fdc\u7aef\u3001\u4ea4\u66ff\u3001\u9176\u4fc3\u548c\u8fde\u7eed\u673a\u5236\u793a\u610f\u56fe\u3002<\/section>\n<p>\u5bf9\u4e8e\u4e0d\u540c\u7684\u7535\u50ac\u5316\u5242\uff0cNRR\u8fc7\u7a0b\u8868\u73b0\u51fa\u4e0d\u540c\u7684\u673a\u7406\u3002\u4e00\u822c\u6765\u8bf4\uff0c\u7535\u5316\u5b66\u8fd8\u539fN<sub>2<\/sub>\u4e3aNH<sub>3<\/sub>\u7684\u53ef\u80fd\u53cd\u5e94\u9014\u5f84\u53ef\u5206\u4e3a\u8fdc\u7aef\u3001\u4ea4\u66ff\u3001\u9176\u4fc3\u548c\u8fde\u7eed\u673a\u5236\u3002\u56e0\u6b64\uff0c\u6211\u4eec\u9075\u5faa\u8fd9\u56db\u4e2a\u673a\u5236\u6765\u8bc4\u4f30Mo\/BP\u4f5c\u4e3a\u7535\u50ac\u5316\u5242\u7684\u6574\u4f53\u6027\u80fd\u3002N<sub>2<\/sub>\u7684\u6d3b\u5316\u4ee5\u53ca\u8fd8\u539f\u8fc7\u7a0b\uff0c\u5982<strong>\u65b9\u68481<\/strong>\u6240\u793a\u3002\u5728\u8fde\u7eed\u516d\u4e2a\u8d28\u5b50\u5316\u8fc7\u7a0b\u4e2d\uff0c\u6bcf\u4e00\u6b65\u90fd\u52a0\u5165\u4e00\u4e2a\u6c22\u539f\u5b50\uff0c\u5e76\u8fdb\u884c\u57fa\u4e8eDFT\u7684\u8ba1\u7b97\u6765\u5bfb\u627e\u6700\u5c0f\u80fd\u91cf\u914d\u7f6e\u3002<\/p>\n<section><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-225640\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/5-3.png\" alt=\"\" width=\"600\" height=\"326\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/5-3.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/5-3-300x163.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/section>\n<p><strong>\u56fe4<\/strong>.\u00a0\u5728Mo\/BP\u4e0a\uff0c\u8fdc\u7aef\u3001\u4ea4\u66ff\u3001\u9176\u4fc3\u548c\u8fde\u7eed\u673a\u5236\u4e0b\uff0cN<sub>2<\/sub>\u7535\u8fd8\u539f\u5230NH<sub>3<\/sub>\u8fc7\u7a0b\u4e2d\u5404\u79cd\u4e2d\u95f4\u4f53\u7684\u539f\u5b50\u7ed3\u6784\u3002<\/p>\n<section><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-225641\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/6-1.png\" alt=\"\" width=\"600\" height=\"353\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/6-1.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/6-1-300x177.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/section>\n<p><strong>\u56fe5<\/strong>.<strong>\u00a0<\/strong>Mo\/BP\u57280 eV\u548c\u4e0d\u540c\u5e94\u7528\u7535\u4f4d\u4e0b\uff0c\u901a\u8fc7a)\u8fdc\u7aef\u3001b)\u4ea4\u66ff\u3001c)\u9176\u4fc3\u548cd)\u8fde\u7eed\u673a\u5236\u4e0b\u50ac\u5316NRR\u7684\u81ea\u7531\u80fd\u3002<\/p>\n<p><strong>\u56fe4<\/strong>\u6240\u793a\u4e3aMo\/BP\u8868\u9762\u56db\u79cd\u53ef\u884c\u53cd\u5e94\u9014\u5f84\u5404\u57fa\u672c\u6b65\u9aa4\u4e0b\u4e0d\u540c\u72b6\u6001\u7684\u4f18\u5316\u51e0\u4f55\u7ed3\u6784\uff1b<strong>\u56fe5<\/strong>\u4e3a\u4e0d\u540c\u50ac\u5316\u53cd\u5e94\u8def\u5f84\u4e0b\u5404\u4e2a\u8fc7\u7a0b\u7684\u81ea\u7531\u80fd\u3002\u5728\u8fdc\u7aef\u673a\u5236\u4e0b\uff0c\u901a\u8fc7\u6dfb\u52a0\u4e00\u4e2a\u8d28\u5b50\u548c\u4e00\u4e2a\u7535\u5b50\u8f6c\u79fb\uff0c\u5438\u9644\u7684N<sub>2<\/sub>\u9996\u5148\u53d1\u751f\u6c22\u5316\u53cd\u5e94\uff0c\u5f62\u6210\u4e00\u4e2a*NNH\u7269\u79cd\u5438\u9644\u5728Mo\u4f4d\u70b9\u4e0a\u3002DFT\u8ba1\u7b97\u7ed3\u679c\u8868\u660e\uff0c\u8be5\u8f6c\u6362\u8fc7\u7a0b\u6240\u9700\u7684\u80fd\u91cf\u4e3a1.10 eV\uff0c\u5982\u56fe5a\u6240\u793a\u3002\u5728\u63a5\u4e0b\u6765\u7684\u6b65\u9aa4\u4e2d\uff0c*NNH\u5206\u5b50\u7684\u8fdc\u7aefN\u539f\u5b50\u4e0e(H<sup>+<\/sup>\u00a0+ e)\u7ed3\u5408\u5f62\u6210\u65b0\u7684*NNH<sub>2<\/sub>\u5206\u5b50\uff0c\u5409\u5e03\u65af\u81ea\u7531\u80fd\u964d\u4f4e0.13 eV\u3002\u968f\u540e\uff0c*NNH<sub>2<\/sub>\u57fa\u7684\u8fdc\u7aefN\u539f\u5b50\u7ee7\u7eed\u53d7\u5230\u7b2c\u4e09\u4e2a(H<sup>+<\/sup>\u00a0+ e)\u7684\u653b\u51fb\uff0c\u7b2c\u4e00\u4e2aNH<sub>3<\/sub>\u5f97\u4ee5\u91ca\u653e\u3002\u7136\u540e\uff0c\u4e00\u4e2aN\u539f\u5b50\u7559\u5728Mo\/BP\u8868\u9762\uff0c\u5b83\u5c06\u88ab\u53e6\u5916\u4e09\u4e2a\u4e0e\u7535\u5b50\u8026\u5408\u7684\u8d28\u5b50\u8fdb\u4e00\u6b65\u6c22\u5316\uff0c\u751f\u6210\u7b2c\u4e8c\u4e2aNH<sub>3<\/sub>\u5206\u5b50\u3002\u7531\u4e8e\u8fd9\u4e09\u4e2a\u57fa\u672c\u6b65\u9aa4\u90fd\u662f\u653e\u70ed\u7684\uff0c\u0394G\u503c\u5206\u522b\u4e3a0.39\u30010.84\u548c0.26 eV\uff0c\u56e0\u6b64\u7b2c\u4e8c\u4e2aNH<sub>3<\/sub>\u5f88\u5bb9\u6613\u751f\u6210\u3002\u5728\u4ea4\u66ff\u673a\u5236\u65b9\u9762\uff0c\u5373\u4f7f\u4e24\u4e2aN\u539f\u5b50\u4e4b\u95f4\u4ea4\u66ff\u53d1\u751f\u8d28\u5b50\u5316\uff0c*NN\u7b2c\u4e00\u6b21\u52a0\u6c22\u751f\u6210*NNH\u7684\u81ea\u7531\u80fd\u4ecd\u7136\u6700\u9ad8\uff0c\u5bfc\u81f4\u8d77\u59cb\u7535\u4f4d\uff081.10V\uff09\u4e0e\u8fdc\u7aef\u8def\u5f84\u76f8\u540c\uff08\u56fe5b\uff09\u3002\u56e0\u6b64\uff0c\u5728Mo\/BP\u5355\u5206\u5b50\u5c42\u8868\u9762\u901a\u8fc7\u8fd9\u4e24\u79cd\u673a\u5236\u5f88\u96be\u8fdb\u884c\u7684NRR\u8fc7\u7a0b\u3002\u5728\u9176\u4fc3\u673a\u5236\u4e0b, \u7b2c\u4e00\u4e2aNH<sub>3<\/sub>\u5c06\u5728\u7b2c\u516d\u6b65\u88ab\u91ca\u653e\uff0c\u56e0\u4e3a\u4e24\u4e2aN\u539f\u5b50\u4e4b\u95f4\u7684\u8d28\u5b50\u5316\u4ea4\u66ff\u53d1\u751f\u3002\u5982\u56fe5 c\u6240\u793a\uff0c\u9664\u4e86\u7b2c\u4e00\u4e2a\u53cd\u5e94(*NN + H<sup>+<\/sup>\u00a0+ e = *NNH)\u5916\uff0c\u540e\u7eed\u6b65\u9aa4\u90fd\u662f\u653e\u70ed\u7684\u3002\u8fd9\u4e2a\u57fa\u672c\u53cd\u5e94\u7684\u53d1\u751f\u53ea\u9700\u8981\u514b\u670d0.68 eV\u7684\u80fd\u91cf\u52bf\u5792\u5c31\u53ef\u4ee5\u4e86\uff0c\u8d77\u59cb\u7535\u4f4d\u5f88\u4f4e\uff080.68 V\uff09\u3002\u5728\u8fde\u7eed\u53cd\u5e94\u673a\u5236\u4e2d\uff0c*NN\u7b2c\u4e00\u6b21\u52a0\u6c22\u751f\u6210*NNH\u7684\u81ea\u7531\u80fd\u4ecd\u7136\u6700\u9ad8\uff0c\u5bfc\u81f4\u4e0e\u9176\u4fc3\u673a\u5236\u76f8\u540c\u7684\u8d77\u59cb\u7535\u4f4d\uff080.68 V\uff09(\u56fe5c)\uff0c\u8fdc\u4f4e\u4e8e\u8fdc\u7aef\u548c\u4ea4\u66ff\u673a\u5236\uff081.10 V\uff09\u3002<\/p>\n<section><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-225642\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/7-1.png\" alt=\"\" width=\"600\" height=\"476\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/7-1.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/7-1-300x238.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/section>\n<p><strong>\u56fe6<\/strong>.\u00a0Mo\/BP\u4e09\u4e2a\u57fa\u56e2\u7684\u7535\u8377\u53d8\u5316\u3002<\/p>\n<p>\u4e3a\u4e86\u66f4\u597d\u5730\u7814\u7a76Mo\/BP\u7684NRR\u50ac\u5316\u6548\u679c\uff0c\u8fdb\u884c\u4e86Hirshfeld\u7535\u8377\u5e03\u5c45\u5206\u6790\u3002\u5982<strong>\u56fe6<\/strong>\u6240\u793a\uff0c\u6cbf\u7740\u6709\u5229\u4e8e\u9176\u4fc3\u9014\u5f84\uff0c\u89c2\u5bdf\u5230\u4e86\u539f\u5b50\u7535\u8377\u7684\u6ce2\u52a8\u3002\u6839\u636e\u4ee5\u5f80\u7684\u7814\u7a76\uff0c\u6bcf\u4e00\u6b65\u90fd\u88ab\u5206\u4e3a\u4e09\u4e2a\u57fa\u56e2\uff0c\u5305\u62ecBP\u5355\u5206\u5b50\u5c42\uff08\u90e8\u52061\uff09\u3001Mo-B<sub>3<\/sub>\u7684\u50ac\u5316\u5242\u4e2d\u5fc3\uff08\u90e8\u52062\uff09\u3001\u548c\u5438\u9644\u53cd\u5e94\u4e2d\u95f4\u4f53N<sub>x<\/sub>H<sub>y<\/sub>\uff08\u90e8\u52063\uff09\u3002\u8ba1\u7b97\u7ed3\u679c\u8868\u660e\uff0c\u5728N<sub>2<\/sub>\u56fa\u5b9a\u8fc7\u7a0b\u4e2d\uff0c\u4e09\u4e2a\u4e2d\u95f4\u4f53\u7684\u7535\u8377\u90fd\u6709\u660e\u663e\u7684\u6ce2\u52a8\u3002\u4f8b\u5982\uff0c\u5728Mo\/BP\u5355\u5206\u5b50\u5c42\u8868\u9762\u8fdb\u884cN<sub>2<\/sub>\u5438\u9644\u540e\uff0cBP\u5355\u5206\u5b50\u5c42\u5206\u522b\u5411N<sub>2<\/sub>\u5206\u5b50\u548cMoB<sub>3<\/sub>\u5206\u5b50\u63d0\u4f9b\u4e86\u7ea60.06\u548c0.13\u4e2a\u7535\u5b50\u3002\u5f53(H<sup>+<\/sup>\u00a0+ e)\u4e0e*NN\u4ea4\u4e92\u5f62\u6210\u65b0\u7684*NNH\u7269\u79cd\uff0c*NNH\u548cMoB<sub>3<\/sub>\u53ef\u4ee5\u4eceBP\u5355\u5c42\u83b7\u5f970.01\u548c0.11\u7535\u5b50\u3002\u5728\u7b2c\u56db\u6b65\u4e2d\uff0cBP\u5355\u5206\u5b50\u5c42\u548cMoB<sub>3<\/sub>\u90e8\u5206\u5206\u522b\u4ece*NH2-*NH\u83b7\u5f97\u7ea60.05\u548c0.06\u4e2a\u7535\u5b50\u3002\u56e0\u6b64\uff0cMoB<sub>3<\/sub>\u57fa\u56e2\u4e0d\u4ec5\u662f\u5438\u9644\u53cd\u5e94\u4e2d\u95f4\u4f53NxHy\u4e0eBP\u5355\u5206\u5b50\u5c42\u5e95\u7269\u4e4b\u95f4\u7684\u6d3b\u6027\u4e2d\u5fc3\uff0c\u8fd8\u662f\u7535\u8377\u8f6c\u79fb\u7684\u4f20\u9012\u5668\u3002\u91cd\u8981\u7684\u662f\uff0cMo\/BP\u7684\u91d1\u5c5e\u6027\u8d28\u786e\u4fdd\u4e86\u9ad8\u6548\u7684\u7535\u8377\u8f6c\u79fb\uff0c\u8fdb\u4e00\u6b65\u8bc1\u660eMo\/BP\u662f\u4e00\u79cd\u5f88\u6709\u524d\u666f\u7684\u56fa\u5b9aN<sub>2<\/sub>\u7684\u7535\u50ac\u5316\u5242\u3002<\/p>\n<p><strong>\u603b\u7ed3\u4e0e\u5c55\u671b<\/strong><\/p>\n<section>\n<p>\u7efc\u4e0a\u6240\u8ff0\uff0c\u5229\u7528\u7b2c\u4e00\u6027\u539f\u7406\u8ba1\u7b97\uff0c\u6211\u4eec\u7cfb\u7edf\u5730\u7814\u7a76\u548c\u7b5b\u9009\u4e86\u591a\u79cd\u5355\u4e2a\u8fc7\u6e21\u91d1\u5c5e\u539f\u5b50\u951a\u5b9a\u5728\u5355\u78f7\u70b9\u7f3a\u9677\u7684\u5355\u5c42\u78f7\u5316\u787c(TMs\/BP)\u5728\u5408\u6210NH<sub>3<\/sub>\u7684\u4e2d\u50ac\u5316\u6027\u80fd\u3002\u8ba1\u7b97\u53d1\u73b0Mo\u5355\u539f\u5b50\u951a\u5b9a\u7684\u5177\u6709\u78f7\u70b9\u7f3a\u9677\u7684\u5355\u5c42BP\uff08Mo\/BP\uff09\u5177\u6709\u6700\u4f73\u50ac\u5316\u6027\u80fd\u7684\u3002\u8be5Mo\/BP\u7684\u56fa\u6c2e\u53cd\u5e94\u8def\u5f84\u4f18\u9009\u9176\u4fc3\u673a\u5236\u548c\u8fde\u7eed\u673a\u5236\uff1b\u7535\u8377\u5e03\u5c45\u5206\u6790\u8868\u660e\uff0cMo-B<sub>3<\/sub>\u57fa\u56e2\u5728\u8fd8\u539f\u8fc7\u7a0b\u4e2d\u4f5c\u4e3a\u7535\u8377\u4f20\u9012\u4f53\u4e2d\u5fc3\u548c\u50ac\u5316\u6d3b\u6027\u4e2d\u5fc3\uff1b\u6b64\u5916\uff0cMo\/BP\u7684\u91d1\u5c5e\u7279\u6027\u6709\u5229\u4e8e\u5feb\u901f\u7535\u5b50\u8f6c\u79fb\uff0c\u63d0\u9ad8\u7535\u50ac\u5316\u53cd\u5e94\u7684\u6548\u7387\u3002\u8bc1\u660e\u4e86Mo\/BP\u662f\u4e00\u79cd\u5f88\u6709\u524d\u9014\u7684\u5355\u539f\u5b50\u56fa\u5b9aN<sub>2<\/sub>\u50ac\u5316\u5242\u3002\u8fd9\u9879\u7814\u7a76\u6709\u671b\u6fc0\u53d1\u5b9e\u9a8c\u548c\u7406\u8bba\u7684\u7ed3\u5408\uff0c\u8fdb\u4e00\u6b65\u63a2\u7d22\u66f4\u6709\u6f5c\u529b\u7684\u5355\u539f\u5b50\u7535\u50ac\u5316\u5242\u5728\u5408\u6210NH<sub>3<\/sub>\u4e2d\u7684\u5e94\u7528\u3002<\/p>\n<section>\n<section>\n<section>\n<section>\n<section data-role=\"paragraph\">\n<section data-role=\"paragraph\">\n<section data-role=\"paragraph\">\n<section data-tools=\"135\u7f16\u8f91\u5668\" data-id=\"97590\" data-color=\"#374aae\">\n<section>\n<p><strong>\u6587\u732e\u94fe\u63a5<\/strong><\/p>\n<section>\n<p>Zaichun Liu,\u00a0Ting Huang,\u00a0Huhu Chang,\u00a0Faxing Wang,\u00a0Juan Wen,\u00a0Haodong Sun,\u00a0Masud Hossain,\u00a0Qingji Xie,\u00a0Yan Zhao*,\u00a0Yuping Wu*.Computational Design of Single Mo Atom Anchored Defective Boron Phosphide Monolayer as a High-performance Electrocatalyst for the Nitrogen Reduction Reaction.\u00a0<em>Energy\u00a0Environ. Mater<\/em>.\u00a0<strong>2021<\/strong>,\u00a0<em>4<\/em>, 222-228.<\/p>\n<p><span style=\"line-height: 1.5;\">DOI: 10.1002\/eem2.12120.<\/span><\/p>\n<p><span style=\"line-height: 1.5;\">https:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/eem2.12120<\/span><\/p>\n<\/section>\n<\/section>\n<section>\n<section>\n<section>\n<section><strong style=\"line-height: 1.5;\">\u4f5c\u8005\u7b80\u4ecb<\/strong><\/section>\n<\/section>\n<\/section>\n<\/section>\n<\/section>\n<\/section>\n<\/section>\n<\/section>\n<\/section>\n<\/section>\n<\/section>\n<\/section>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-225643\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/8-1.png\" alt=\"\" width=\"180\" height=\"211\" \/><\/p>\n<section>\n<p><strong>\u5434\u5b87\u5e73<\/strong>\uff0c\u7537\uff0c\u6559\u6388\uff0c\u535a\u58eb\u751f\u5bfc\u5e08\uff0c\u73b0\u4efb\u5357\u4eac\u5de5\u4e1a\u5927\u5b66\u80fd\u6e90\u79d1\u5b66\u4e0e\u5de5\u7a0b\u5b66\u9662\u9662\u957f\u30021997\u5e746\u6708\u6bd5\u4e1a\u4e8e\u4e2d\u56fd\u79d1\u5b66\u9662\u5316\u5b66\u7814\u7a76\u6240\uff0c\u83b7\u535a\u58eb\u5b66\u4f4d\uff0c\u6b64\u540e\u5206\u522b\u5728\u6e05\u534e\u5927\u5b66\u3001\u65e5\u672c\u65e9\u7a3b\u7530\u5927\u5b66\u548c\u5fb7\u56fd\u5f00\u59c6\u5c3c\u5179\u5de5\u4e1a\u5927\u5b66\u5de5\u4f5c\u54042\u5e74\uff0c2003\u5e748\u6708\u4f5c\u4e3a\u4f18\u79c0\u4eba\u624d\u5f15\u8fdb\u5230\u590d\u65e6\u5927\u5b66\u4efb\u6559\u6388\uff0c2015\u5e745\u6708\u4f5c\u4e3a\u7b2c\u4e8c\u5c42\u6b21\u4eba\u624d\u8c03\u5230\u5357\u4eac\u5de5\u4e1a\u5927\u5b66\u80fd\u6e90\u79d1\u5b66\u4e0e\u5de5\u7a0b\u5b66\u9662\u30022004\u5e74\u30012007\u5e74\u83b7\u4e0a\u6d77\u5e02\u79d1\u59d4\u201c\u79d1\u6280\u542f\u660e\u661f\u201d\uff0c2014\u5e74\u83b7\u56fd\u5bb6\u6770\u51fa\u9752\u5e74\u57fa\u91d1\uff0c2015\u88ab\u6c64\u68ee\u8def\u900f\u8bc4\u4e3a\u201c\u9ad8\u88ab\u5f15\u79d1\u5b66\u5bb6\u201d\u3002\u4e3b\u8981\u4ece\u4e8b\u9502\u79bb\u5b50\u7535\u6c60\u53ca\u5176\u5173\u952e\u6750\u6599\u3001\u8d85\u7ea7\u7535\u5bb9\u5668\u3001\u65b0\u578b\u50a8\u80fd\u4f53\u7cfb\u4e0e\u5668\u4ef6\u3001\u592a\u9633\u80fd\u5236\u6c22\u7b49\u65b9\u9762\u7684\u7814\u7a76\u3002\u8fd1\u51e0\u5e74\u5728Angew. Chem. Int. Edi.\u3001Adv. Mater.\u3001Adv. Energy Mater.\u3001Nano Lett.\u3001Prog. Mater. Sci.\u3001Nano Energy\u3001Chem. Mater.\u3001Chem. Commun.\u3001J Mater. Chem. A\u7b49\u56fd\u9645\u77e5\u540d\u6742\u5fd7\u53d1\u8868\u8bba\u6587220\u591a\u7bc7\u60c5\u51b5\uff0c\u8bba\u6587\u5f15\u75288000\u591a\u6b21\uff0cH-\u6307\u657053\u3002\u51fa\u7248\u4e2d\u6587\u8457\u4f5c4\u672c\u548c\u82f1\u6587\u8457\u4f5c1\u672c\uff0c\u53e6\u67096\u7ae0\u82f1\u6587\u548c2\u7ae0\u8282\u4e2d\u6587\u3002\u6388\u6743\u53d1\u660e\u4e13\u522921\u9879\u3002\u62c5\u4efbElectrochem. Commun. (2007-2013)\u7b49\u520a\u7269\u7684\u7f16\u59d4\uff0c\u81ea2006\u5e74\u8d77\u62c5\u4efbIUPAC\u56fd\u9645\u65b0\u578b\u6750\u6599\u53ca\u5176\u5236\u5907\u5b66\u672f\u4f1a\u8bae\u7684\u5171\u540c\u4e3b\u5e2d\u3002<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-225644\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/9-1.png\" alt=\"\" width=\"180\" height=\"297\" \/><\/p>\n<p>\u8d75\u7131\uff0c\u6e56\u5317\u7701\u201c\u767e\u4eba\u8ba1\u5212\u201d\u4e13\u5bb6\uff0c\u6b66\u6c49\u7406\u5de5\u5927\u5b66\u7845\u9178\u76d0\u5efa\u7b51\u6750\u6599\u56fd\u5bb6\u91cd\u70b9\u5b9e\u9a8c\u5ba4\u9996\u5e2d\u6559\u6388\uff0c\u6b66\u6c49\u5927\u5b66\u5de5\u4e1a\u79d1\u5b66\u7814\u7a76\u9662\u4e8c\u7ea7\u6559\u6388\uff0c\u535a\u5bfc\u3002\u4e3b\u8981\u4ece\u4e8b\u8ba1\u7b97\u5316\u5b66\u3001\u7eb3\u7c73\u6750\u6599\u6a21\u62df\u3001\u65b0\u80fd\u6e90\u6750\u6599\u5f00\u53d1\u548c3D\u6253\u5370\u7684\u7814\u7a76\u5de5\u4f5c\uff0c\u8d75\u7131\u662f\u7f8e\u56fd\u60e0\u666e\u516c\u53f83D\u6253\u5370\u6280\u672f\u7684\u4e3b\u521b\u4eba\u5458\u4e4b\u4e00\uff0c\u83b7\u7f8e\u56fd\u548c\u56fd\u9645\u4e13\u522925\u9879\uff0c\u5728\u5176\u7814\u7a76\u9886\u57df\u7684\u56fd\u9645\u6743\u5a01\u520a\u7269\u4e0a\u53d1\u8868\u9ad8\u6c34\u5e73\u7814\u7a76\u8bba\u658780\u4f59\u7bc7\uff0cSCI\u5f15\u7528\u8d85\u8fc736000\u4f59\u6b21\uff0c\u5176\u4e2d\u4e00\u7bc7\u8bba\u6587\u5355\u7bc7\u5f15\u7528\u8d85\u8fc712000\u6b21\uff0cH\u56e0\u5b50\u4e3a50\uff0c10\u5e74\u6765\u7684\u9ad8\u88ab\u5f15\u6587\u7ae0(Highly Cited Papers)\u4e3a9\u7bc7\uff0c2014-2017\u8fde\u7eed4\u5e74\u90fd\u88ab\u7f8e\u56fd\u6c64\u68ee\u8def\u900f\u96c6\u56e2\u548c\u79d1\u777f\u552f\u5b89\u516c\u53f8\u5217\u5165\u5168\u7403\u9ad8\u88ab\u5f15\u79d1\u5b66\u5bb6\u540d\u5355\u3002<\/p>\n<\/section>\n<\/section>\n<section data-role=\"paragraph\">\n<section data-role=\"outer\">\n<section>\n<section>\n<section>\n<section>\n<section data-autoskip=\"1\">\n<section>\n<section>\n<section>\n<section><strong style=\"line-height: 1.5;\">\u5173\u4e8e\u671f\u520a<\/strong><\/section>\n<\/section>\n<\/section>\n<\/section>\n<p>Energy &amp; Environmental Materials\uff08EEM\uff09\u662f\u7531\u90d1\u5dde\u5927\u5b66\u548cJohn Wiley &amp; Sons\uff0cInc. \u8054\u5408\u51fa\u7248\u7684\u80fd\u6e90\u4e0e\u73af\u5883\u6750\u6599\u7c7b\u5b63\u520a\uff0c\u4e3b\u8981\u62a5\u9053\u5148\u8fdb\u80fd\u6e90\u4e0e\u73af\u5883\u6750\u6599\u76f8\u5173\u7684\u6700\u65b0\u9ad8\u6c34\u5e73\u79d1\u7814\u6210\u679c\uff0c\u5728 Wiley Online Library \u4e0a\u53ef\u514d\u8d39\u83b7\u53d6\u5168\u6587\uff0c\u76ee\u524d\u514d\u6536\u7248\u9762\u8d39\u3002EEM\u5165\u90092017\u5e74\u4e2d\u56fd\u79d1\u6280\u671f\u520a\u56fd\u9645\u5f71\u54cd\u529b\u63d0\u5347\u8ba1\u5212\u9879\u76eeD\u7c7b\u652f\u6301\uff0c\u5df2\u88ab<strong>Science Citation Index Expanded (SCIE)<\/strong>\u3001<strong>Scopus<\/strong>\u3001<strong>EI<\/strong>\u3001Environment Index (EBSCO publishing)\u548cINSPECT(IET)\u6536\u5f55\u30022021\u5e74\u5165\u9009\u4e2d\u56fd\u79d1\u5b66\u5f15\u6587\u6570\u636e\u5e93\uff08Chinese Science Citation Database\uff0cCSCD\uff09\u6838\u5fc3\u5e93\uff0c\u6750\u6599\u79d1\u5b66\u7efc\u5408\u7c7bT1\u533a\u671f\u520a\uff0c<strong>\u9996\u4e2a\u5f71\u54cd\u56e0\u5b5015.122<\/strong>\uff0cJCR\u5206\u533aQ1\u533a\u3002EEM\u4e00\u76f4\u6267\u884c\u4e25\u683c\u7684\u56fd\u9645\u540c\u884c\u8bc4\u5ba1\u673a\u5236\uff0c\u6587\u7ae0\u5f55\u7528\u540e\u5c06\u5373\u65f6in press\u5728\u7ebf\u3002<\/p>\n<section><\/section>\n<\/section>\n<\/section>\n<\/section>\n<\/section>\n<\/section>\n<\/section>\n<\/section>\n","protected":false},"excerpt":{"rendered":"<p>\u6210\u679c\u7b80\u4ecb \u8fd1\u65e5\uff0c\u5357\u4eac\u5de5\u4e1a\u5927\u5b66\u5434\u5b87\u5e73\u6559\u6388\u8bfe\u9898\u7ec4\u548c\u6b66\u6c49\u7406\u5de5\u5927\u5b66\u7684\u8d75\u7131\u6559\u6388\u8bfe\u9898\u7ec4\u5728Energy &amp; Environmental Materials\u4e0a\u53d1\u8868\u9898\u4e3a\u201c&#8230;<\/p>\n","protected":false},"author":11454,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-225626","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/225626"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/11454"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=225626"}],"version-history":[{"count":3,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/225626\/revisions"}],"predecessor-version":[{"id":225647,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/225626\/revisions\/225647"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=225626"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=225626"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=225626"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}