{"id":225731,"date":"2021-08-10T06:30:58","date_gmt":"2021-08-09T22:30:58","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=225731"},"modified":"2021-08-09T16:40:51","modified_gmt":"2021-08-09T08:40:51","slug":"%e5%b9%bf%e4%b8%9c%e5%b7%a5%e4%b8%9a%e5%a4%a7%e5%ad%a6%e5%bc%a0%e6%b5%b7%e7%87%95%e5%9b%a2%e9%98%9fmrl%ef%bc%9a%e9%9d%99%e7%94%b5%e7%ba%ba%e4%b8%9d%e6%b3%95%e5%88%b6%e5%a4%87%e9%92%a0%e7%a6%bb","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=225731","title":{"rendered":"\u5e7f\u4e1c\u5de5\u4e1a\u5927\u5b66\u5f20\u6d77\u71d5\u56e2\u961fMRL\uff1a\u9759\u7535\u7eba\u4e1d\u6cd5\u5236\u5907\u94a0\u79bb\u5b50\u7535\u6c60\u9633\u6781MoP\/TiO2\u5f02\u6784\u6750\u6599"},"content":{"rendered":"<p><strong><b>\u6587\u732e\u94fe\u63a5<\/b><\/strong><\/p>\n<p>Facile Preparation of MoP\/TiO<sub>2<\/sub> Composite by Electrospinning Method for Sodium Ion Battery Anode, Materials Research Letters, 9:9, 382-390.<strong><b>\u00a0<\/b><\/strong>(<a href=\"https:\/\/doi.org\/10.1080\/21663831.2021.1949401\"><u>https:\/\/doi.org\/10.1080\/21663831.2021.1949401<\/u><\/a>)<\/p>\n<p><strong><b>\u3010\u80cc\u666f\u4ecb\u7ecd\u3011<\/b><\/strong><\/p>\n<p>\u8fd1\u5e74\u6765\uff0c\u6027\u80fd\u4f18\u5f02\u7684\u9502\u79bb\u5b50\u7535\u6c60\u5728\u4fbf\u643a\u5f0f\u7535\u5b50\u8bbe\u5907\u3001\u7535\u52a8\u6c7d\u8f66\u7b49\u9886\u57df\u5f97\u5230\u5927\u529b\u63a8\u5e7f\u3002\u968f\u7740\u9502\u79bb\u5b50\u7535\u6c60\u7684\u5e7f\u6cdb\u5e94\u7528\uff0c\u6709\u9650\u7684\u9502\u8d44\u6e90\u53ca\u5176\u4e0d\u65ad\u6500\u5347\u7684\u9700\u6c42\u548c\u4ef7\u683c\u4f7f\u5f97\u4eba\u4eec\u7684\u5173\u6ce8\u70b9\u9010\u6e10\u8f6c\u5411\u6f5c\u5728\u7684\u66ff\u4ee3\u50a8\u80fd\u4f53\u7cfb\u3002\u7531\u4e8e\u94a0\u6210\u672c\u4f4e\uff0c\u50a8\u91cf\u4e30\u5bcc\u7684\u4f18\u52bf\uff0c\u94a0\u79bb\u5b50\u7535\u6c60\u6210\u4e3a\u9502\u79bb\u5b50\u7535\u6c60\u5728\u50a8\u80fd\u5668\u4ef6\u65b9\u9762\u7684\u8865\u5145\u3002\u94a0\u79bb\u5b50\u7535\u6c60\u4e0e\u9502\u79bb\u5b50\u7535\u6c60\u5de5\u4f5c\u673a\u7406\u76f8\u4f3c\uff0c\u5747\u901a\u8fc7\u5de5\u4f5c\u79bb\u5b50\u5728\u6b63\u8d1f\u6781\u95f4\u6765\u56de\u7a7f\u68ad\u800c\u5b9e\u73b0\u80fd\u91cf\u7684\u5b58\u50a8\u4e0e\u8f6c\u6362\uff0c\u5e76\u4e14\u94a0\u4e0e\u9502\u7684\u7535\u6781\u7535\u4f4d\u76f8\u8fd1\u3002\u4f46\u94a0\u79bb\u5b50\u76f8\u5bf9\u8f83\u5927\u7684\u79bb\u5b50\u534a\u5f84\u4f7f\u5176\u5728\u5d4c\u5165\u8131\u51fa\u8fc7\u7a0b\u4e2d\u4f1a\u9762\u4e34\u66f4\u5927\u7684\u963b\u529b\uff0c\u5bb9\u6613\u9020\u6210\u9897\u7c92\u7684\u7834\u788e\u7c89\u5316\u4ee5\u53ca\u76f8\u5e94\u7684\u6027\u80fd\u8870\u51cf\uff0c\u56e0\u800c\u66f4\u96be\u4ee5\u9009\u62e9\u5408\u9002\u7684\u7535\u6781\u6750\u6599\u3002<\/p>\n<p>\u5177\u6709\u9ad8\u7406\u8bba\u5bb9\u91cf\u548c\u4f4e\u53cd\u5e94\u7535\u4f4d\u7684\u78f7\u57fa\u8d1f\u6781\u6750\u6599\u6210\u4e3a\u7406\u60f3\u7684\u5019\u9009\u8005\uff0c\u800c\u91d1\u5c5e\u78f7\u5316\u7269\u5728\u7535\u5316\u5b66\u5faa\u73af\u8fc7\u7a0b\u4e2d\u5f62\u6210\u7684\u8fc7\u6e21\u4e2d\u95f4\u76f8Na<sub>x<\/sub>M\/Na<sub>x<\/sub>P\u80fd\u6709\u6548\u7f13\u89e3\u4f53\u79ef\u81a8\u80c0\u3002\u5176\u4e2d\uff0c\u78f7\u5316\u94bc(MoP)\u6750\u6599\u7531\u4e8e\u5176\u4f18\u5f02\u7684\u7535\u5b50\u5bfc\u7535\u6027\u548c\u826f\u597d\u7684\u78b1\u91d1\u5c5e\u79bb\u5b50\u50a8\u80fd\u7684\u7535\u5316\u5b66\u6d3b\u6027\u800c\u53d7\u5230\u5e7f\u6cdb\u5173\u6ce8\u3002\u4e0e\u5176\u4ed6\u8f6c\u6362\u53cd\u5e94\u578b\u6750\u6599\u76f8\u4f3c\u7684\u662f\uff0cMoP\u4e5f\u5b58\u5728\u5faa\u73af\u7a33\u5b9a\u6027\u5dee\u548c\u5185\u90e8\u8f83\u5dee\u7684\u79bb\u5b50\u6269\u6563\u52a8\u529b\u5b66\u7279\u5f81\u7b49\u7f3a\u9677\u3002<strong><b>\u6784\u5efa\u5bfc\u7535\u78b3\u7f51\u7edc\u4ee5\u53ca\u7ed3\u5408\u7eb3\u7c73\u6676\u5f62\u6210\u5f02\u8d28\u7ed3\u6784\u662f\u63d0\u5347\u7535\u5316\u5b66\u6027\u80fd\u7684\u6709\u6548\u6750\u6599\u6539\u6027\u624b\u6bb5\u3002<\/b><\/strong>\u4e00\u7ef4\u7eb3\u7c73\u6750\u6599\u5177\u6709\u9ad8\u53cd\u5e94\u6d3b\u6027\uff0c\u9ad8\u5f62\u53d8\u8010\u53d7\u529b\uff0c\u8f83\u77ed\u7684\u79bb\u5b50\u6269\u6563\u8def\u5f84\u7b49\u4f18\u52bf\u3002\u4f5c\u4e3a\u4e00\u79cd\u7b80\u5355\u4e14\u901a\u7528\u7684\u4e00\u7ef4\u7eb3\u7c73\u6750\u6599\u5408\u6210\u65b9\u5f0f\uff0c\u9759\u7535\u7eba\u4e1d\u6cd5\u5236\u5907\u5f97\u5230\u7684\u524d\u9a71\u4f53\u7ecf\u60f0\u6027\u6c14\u6c1b\u78b3\u5316\u540e\u80fd\u591f\u5f62\u6210\u7a33\u5b9a\u7684\u78b3\u7ea4\u7ef4\u9aa8\u67b6\u3002\u9897\u7c92\u7684\u7eb3\u7c73\u5316\u5219\u80fd\u6709\u6548\u7f13\u89e3\u5728\u5145\u653e\u7535\u8fc7\u7a0b\u4e2d\u4f53\u79ef\u81a8\u80c0\u9020\u6210\u7684\u7ed3\u6784\u5e94\u529b\u3002\u8fc7\u6e21\u91d1\u5c5e\u79bb\u5b50\u548c\u6709\u673a\u914d\u4f53\u901a\u8fc7\u914d\u4f4d\u952e\u81ea\u7ec4\u88c5\u5f62\u6210\u7684\u6709\u673a-\u65e0\u673a\u6742\u5316\u6750\u6599\u5982MOF\uff08\u91d1\u5c5e-\u6709\u673a\u6846\u67b6\u6750\u6599\uff09\u7ecf\u8fc7\u7145\u70e7\u540e\u5728\u5b9e\u73b0\u7eb3\u7c73\u5316\u7684\u540c\u65f6\uff0c\u80fd\u591f\u6709\u6548\u907f\u514d\u9897\u7c92\u95f4\u7684\u56e2\u805a\u3002<\/p>\n<p><strong><b>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/b><\/strong><\/p>\n<p>\u8fd1\u671f\uff0c\u5e7f\u4e1c\u5de5\u4e1a\u5927\u5b66\u5f20\u6d77\u71d5\u6559\u6388\u56e2\u961f\u63d0\u4f9b\u4e86\u4e00\u79cd\u82ef\u80fa\u8f85\u52a9\u7684\u9759\u7535\u7eba\u4e1d\u6cd5\u5236\u5907MoP\u7684\u5de5\u827a\u8def\u7ebf\u3002\u9009\u62e9\u690d\u9178\u4f5c\u4e3a\u73af\u5883\u53cb\u597d\u578b\u78f7\u6e90\uff0c\u907f\u514d\u4e86\u8fc7\u91cf\u4f7f\u7528\u6b21\u78f7\u9178\u94a0\u7684\u6c14\u76f8\u78f7\u5316\u7684\u8def\u7ebf\u3002\u9009\u53d6\u78f7\u94bc\u9178\u4f5c\u4e3a\u94bc\u6e90\u548c\u805a\u5408\u53cd\u5e94\u5f15\u53d1\u5242\uff0c\u539f\u4f4d\u751f\u6210\u7684\u78f7\u94bc\u9178-\u805a\u82ef\u80fa\u524d\u9a71\u4f53\u501f\u52a9\u78f7\u94bc\u9178\u8d1f\u7535\u8377\u5c42\u7684\u6392\u65a5\u4f5c\u7528\u80fd\u591f\u6709\u6548\u6291\u5236\u9897\u7c92\u7684\u56e2\u805a\uff0c\u5e76\u4e14\u6709\u5229\u4e8e\u540e\u7eed\u5f15\u5165\u949b\u6e90\uff0c\u5f62\u6210\u5f02\u8d28\u7ed3\u6784\u4ece\u800c\u6709\u6548\u63d0\u5347\u5faa\u73af\u7a33\u5b9a\u6027\u548c\u754c\u9762\u7535\u5b50\u4f20\u8f93\u3002\u76f8\u5173\u8bba\u6587\u4ee5\u9898\u4e3a\u201c<strong><b>Facile Preparation of MoP\/TiO<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>\u00a0Composite by Electrospinning Method for Sodium Ion Battery Anode<\/b><\/strong>\u201d\u4e8e\u8fd1\u65e5\u53d1\u8868\u5728\u300aMaterial Research Letters\u300b\u4e0a\u3002<\/p>\n<p><strong><b>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/b><\/strong><\/p>\n<p><strong><b> <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-225734\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/\u56fe\u7247-2-6.png\" alt=\"\" width=\"600\" height=\"889\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/\u56fe\u7247-2-6.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/\u56fe\u7247-2-6-202x300.png 202w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p style=\"text-align: center;\"><strong><b>\u56fe1<\/b><\/strong><strong><b>. <\/b><\/strong>\u6750\u6599\u5408\u6210\u793a\u610f\u56fe\u53ca\u626b\u63cf\u7535\u955c\u548c\u900f\u5c04\u7535\u955c\u8868\u5f81<\/p>\n<p><strong><b><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-225735\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/\u56fe\u7247-3-6.png\" alt=\"\" width=\"600\" height=\"682\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/\u56fe\u7247-3-6.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/\u56fe\u7247-3-6-264x300.png 264w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p style=\"text-align: center;\"><strong><b>\u56fe<\/b><\/strong><strong><b>2<\/b><\/strong><strong><b>. <\/b><\/strong>\u7535\u5316\u5b66\u6027\u80fd\u8868\u5f81<\/p>\n<p><strong><b><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-225733\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/\u56fe\u7247-1-4.png\" alt=\"\" width=\"600\" height=\"584\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/\u56fe\u7247-1-4.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/08\/\u56fe\u7247-1-4-300x292.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p style=\"text-align: center;\"><strong><b>\u56fe<\/b><\/strong><strong><b>3. <\/b><\/strong>\u5faa\u73af\u540e\u7535\u6781\u6750\u6599\u9897\u7c92\u65e0\u5b9a\u578b\u5316\uff0c\u9897\u7c92\u5c3a\u5bf8\u57fa\u672c\u65e0\u53d8\u5316\uff0c\u6781\u5316\u51cf\u5c0f<\/p>\n<p><strong><b>\u3010\u7ed3\u8bba\u3011<\/b><\/strong><\/p>\n<p>\u603b\u7684\u6765\u8bf4\uff0cMoP\/TiO<sub>2<\/sub>\u78b3\u7ea4\u7ef4\u590d\u5408\u6750\u6599<strong><b>\u5177\u6709\u72ec\u7279\u7684\u7ed3\u6784\u4f18\u70b9\uff1a<\/b><\/strong>\uff081\uff09\u8f83\u5c0f\u7684\u9897\u7c92\u5c3a\u5bf8\u80fd\u591f\u6709\u6548\u7f13\u89e3\u5145\u653e\u7535\u8fc7\u7a0b\u4e2d\u7684\u4f53\u79ef\u6548\u5e94\uff0c\uff082\uff09\u524d\u9a71\u4f53\u70ed\u89e3\u5f62\u6210\u7684\u78b3\u7ea4\u7ef4\u5c01\u88c5\u548c\u5f15\u5165\u7684\u4e8c\u6c27\u5316\u949b\u63d0\u4f9b\u4e86\u53cc\u91cd\u7f13\u51b2\u4f5c\u7528\uff0c\u5927\u5e45\u5ea6\u63d0\u5347\u5faa\u73af\u7a33\u5b9a\u6027\uff0c\uff083\uff09\u5f62\u6210\u7684\u5f02\u8d28\u7ed3\u6784\u6709\u6548\u63d0\u5347\u754c\u9762\u7535\u5b50\u4f20\u8f93\u3002\u6240\u5236\u5907\u7684MoP\/TiO<sub>2<\/sub>\u590d\u5408\u6750\u6599\u5177\u6709\u826f\u597d\u7684\u7a33\u5b9a\u6027\uff0c1 A\/g\u7684\u7535\u6d41\u5bc6\u5ea6\u4e0b\u5faa\u73af4000\u6b21\u51e0\u4e4e\u6ca1\u6709\u5bb9\u91cf\u8870\u51cf\u3002\u5c06\u5faa\u73af\u540e\u7684\u7535\u6c60\u62c6\u89e3\u901a\u8fc7\u900f\u5c04\u7535\u955c\u89c2\u5bdf\uff0c\u9897\u7c92\u8d8b\u5411\u65e0\u5b9a\u578b\u5316\uff0c\u4f46\u9897\u7c92\u5c3a\u5bf8\u57fa\u672c\u65e0\u53d8\u5316\uff0c\u65e0\u660e\u663e\u56e2\u805a\u6216\u7834\u788e\uff0c\u663e\u793a\u51fa\u6750\u6599\u826f\u597d\u7684\u7a33\u5b9a\u6027\u3002<\/p>\n<p>*\u672c\u6587\u7531MRL\u7f16\u8f91\u90e8\u9080\u8bf7\uff0c\u4f5c\u8005\u56e2\u961f\u4f9b\u7a3f\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u6587\u732e\u94fe\u63a5 Facile Preparation of MoP\/TiO2 Composite by Electrospinning Method for Sodi&#8230;<\/p>\n","protected":false},"author":11454,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[2],"tags":[],"class_list":["post-225731","post","type-post","status-publish","format-standard","hentry","category-keji"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/225731"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/11454"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=225731"}],"version-history":[{"count":5,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/225731\/revisions"}],"predecessor-version":[{"id":225747,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/225731\/revisions\/225747"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=225731"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=225731"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=225731"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}