{"id":226851,"date":"2021-09-04T06:30:55","date_gmt":"2021-09-03T22:30:55","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=226851"},"modified":"2021-09-03T16:40:25","modified_gmt":"2021-09-03T08:40:25","slug":"%e5%8c%97%e5%b7%a5%e5%a4%a7acta-materialia%ef%bc%9ahcp%e9%87%91%e5%b1%9e11-22%e5%ad%aa%e6%99%b6%e7%9a%84%e5%8d%95%e5%b1%82%e5%ad%aa%e7%94%9f%e4%bd%8d%e9%94%99%e5%8d%8a%e5%89%aa%e5%88%87%e5%8d%8a","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=226851","title":{"rendered":"\u5317\u5de5\u5927Acta Materialia\uff1aHCP\u91d1\u5c5e{11-22}\u5b6a\u6676\u7684\u5355\u5c42\u5b6a\u751f\u4f4d\u9519\u534a\u526a\u5207\u534a\u62d6\u66f3\u673a\u5236"},"content":{"rendered":"<p><strong><b>\u5f15\u8a00<\/b><\/strong><\/p>\n<p>{11-22}&lt;11-2-3&gt;\u5b6a\u6676\u662fHCP\u91d1\u5c5e\u5851\u6027\u53d8\u5f62\u8fc7\u7a0b\u4e2d\u91cd\u8981\u7684\u538b\u7f29\u5b6a\u6676\uff0c\u4f46\u662f\u5176\u5b6a\u751f\u673a\u5236\u76ee\u524d\u4ecd\u7136\u5b58\u5728\u4e89\u8bba\u3002\u7ecf\u5178\u5b6a\u751f\u7406\u8bba\u8ba4\u4e3a\u8be5\u5b6a\u6676\u7684\u7b2c\u4e8c\u4e0d\u53d8\u9762\uff08<em><i>K<\/i><\/em><sub>2<\/sub>\u9762\uff09\u662f{11-2-4}\uff0c\u5b83\u7684\u5b6a\u751f\u526a\u5207\u91cf<em><i>s<\/i><\/em>\u5f88\u5c0f\uff0c\u5bf9\u949b\u800c\u8a00\u53ea\u6709\u5927\u7ea60.22\uff0c\u5176\u5b6a\u751f\u8fc7\u7a0b\u662f\u7531\u5305\u542b\u4e09\u5c42\u539f\u5b50\u9762\u7684\u5e26\u72b6\u5b6a\u751f\u4f4d\u9519\uff08zonal twinning dislocation\uff09\u5b8c\u6210\u3002\u4f46\u662f\u8be5\u673a\u5236\u5b58\u5728\u7684\u95ee\u9898\u662f\uff1a\u539f\u5b50\u62d6\u66f3\uff08shuffle\uff09\u590d\u6742\uff0c\u751a\u81f3\u90e8\u5206\u539f\u5b50\u9700\u8981\u5411\u526a\u5207\u65b9\u5411\u7684\u53cd\u65b9\u5411\u79fb\u52a8\uff1b\u800c\u4e14\u5728\u539f\u5b50\u5c3a\u5ea6\u7684\u5b9e\u9a8c\u53ca\u8ba1\u7b97\u6a21\u62df\u7ed3\u679c\u4e2d\u5e76\u6ca1\u6709\u5f97\u5230\u8bc1\u5b9e\u3002\u5df2\u6709\u7684\u8ba1\u7b97\u6a21\u62df\u7ed3\u679c\u5747\u663e\u793a{11-22}&lt;11-2-3&gt;<span style=\"line-height: 1.5;\">\u5b6a\u751f\u7684<\/span><em style=\"line-height: 1.5;\"><i>K<\/i><\/em><sub>2<\/sub><span style=\"line-height: 1.5;\">\u9762\u4e0d\u662f{11-2-4}\u9762\uff0c\u800c\u662f(0002)\u9762\uff0c\u5bf9\u5e94\u4e8e\u53ea\u5305\u542b\u4e00\u5c42\u5b6a\u751f\u9762\u7684\u5b6a\u751f\u4f4d\u9519\u673a\u5236\u3002\u7136\u800c\uff0c\u8be5\u5355\u5c42\u5b6a\u751f\u4f4d\u9519\u673a\u5236\u88ab\u8ba4\u4e3a\u662f\u5f88\u96be\u5b9e\u73b0\u7684\uff0c\u56e0\u4e3a\u5b83\u9700\u8981\u7684\u5b6a\u751f\u526a\u5207\u91cf\u5f88\u5927\uff0c\u5bf9\u949b\u800c\u8a00\u8fbe\u5230\u4e861.26\uff0c\u9ad8\u4e8e\u5b6a\u751f\u526a\u5207\u91cf\u7684\u7406\u8bba\u9608\u503c1\u3002\u56e0\u6b64\uff0c\u73b0\u6709\u7684\u5b6a\u751f\u673a\u5236\u90fd\u5b58\u5728\u7740\u96be\u4ee5\u89e3\u91ca\u7684\u95ee\u9898\u3002\u5bf9\u4e8e\u949b\u7b49HCP\u91d1\u5c5e\u6765\u8bf4\uff0c{11-22}&lt;11-2-3&gt;\u8fd9\u79cd\u91cd\u8981\u5b6a\u6676\u7684\u5b6a\u751f\u673a\u5236\u7a76\u7adf\u662f\u600e\u6837\u7684\uff0c\u4e9f\u5f85\u7cfb\u7edf\u3001\u7ec6\u81f4\u7684\u7814\u7a76\u3002<\/span><\/p>\n<p><strong><b>\u6210\u679c\u7b80\u4ecb<\/b><\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c\u5317\u4eac\u5de5\u4e1a\u5927\u5b66\u535a\u58eb\u751f\u674e\u7ecf\u7eac\u4e3a\u7b2c\u4e00\u4f5c\u8005\uff0c\u968b\u66fc\u9f84\u6559\u6388\u548c\u7f8e\u56fd\u5185\u534e\u8fbe\u5927\u5b66\uff08University of Nevada\uff09Bin Li\u6559\u6388\u4e3a\u5171\u540c\u901a\u8baf\u4f5c\u8005\u5728\u300aActa Materialia\u300b\u6742\u5fd7\u53d1\u8868\u6587\u7ae0\uff0c\u901a\u8fc7\u5bf9{11-22}\u5b6a\u6676\u754c\u7684\u539f\u5b50\u5c3a\u5ea6STEM\u8868\u5f81\u548c\u5206\u5b50\u52a8\u529b\u5b66\u6a21\u62df\u5206\u6790\uff0c\u63d0\u51fa\u4e86\u4e00\u79cd\u65b0\u7684\u5b6a\u751f\u5f62\u5f0f\u3002\u7814\u7a76\u8005\u5728\u5de5\u4e1a\u7eaf\u949b\u8f67\u5236\u53d8\u5f62\u4e2d\u5f62\u6210\u7684{11-22}\u5f62\u53d8\u5b6a\u6676\u7684\u6676\u754c\u5904\u89c2\u5bdf\u5230\u53ea\u5305\u542b\u4e00\u5c42\u539f\u5b50\u9762\u7684\u5b6a\u751f\u4f4d\u9519\uff0c\u5e76\u53d1\u73b0\u5728\u8be5\u4f4d\u9519\u4e2d\u660e\u663e\u5b58\u5728\u4e00\u4e2a\u8fc7\u6e21\u533a\u57df\uff0c\u4f4d\u9519\u6838\u5904\u4e24\u5c42\u539f\u5b50\u5448\u73b0\u5e76\u6392\u5f0f\u7684\u6392\u5217\uff0c\u8fd9\u5728\u8ba1\u7b97\u6a21\u62df\u7ed3\u679c\u4e2d\u4e5f\u5f97\u5230\u4e86\u5f88\u597d\u7684\u5370\u8bc1\u3002\u7814\u7a76\u7ed3\u679c\u8868\u660e{11-22}&lt;11-2-3&gt;\u5b6a\u751f\u8fc7\u7a0b\u4e2d\u53ea\u5b58\u5728\u5355\u5c42\u5b6a\u751f\u4f4d\u9519\u3002\u7814\u7a76\u8005\u901a\u8fc7\u7efc\u5408\u5206\u6790\u63d0\u51fa\u4e86\u5355\u5c42\u5b6a\u751f\u4f4d\u9519\u534a\u526a\u5207\u534a\u62d6\u66f3\u673a\u5236\uff0c\u5373\uff1a\u5355\u5c42\u5b6a\u751f\u4f4d\u9519\u901a\u8fc7\u5148\u526a\u5207\u4e00\u534a\uff08<em><i>s<\/i><\/em>=0.66\uff09\uff0c\u7136\u540e\u518d\u62d6\u66f3\u4e00\u534a\uff08~0.08 nm\uff09\u7684\u65b9\u5f0f\u5b8c\u6210\u5b6a\u751f\u8fc7\u7a0b\u3002\u8fd9\u4f7f\u5f97\u5b6a\u751f\u526a\u5207\u91cf<em><i>s<\/i><\/em>\u5c0f\u4e8e1\uff0c\u800c\u5269\u4e0b\u7684\u4e00\u534a\u901a\u8fc7\u62d6\u66f3\u8f85\u52a9\u5b8c\u6210\u3002\u6587\u7ae0\u8fd8\u5206\u6790\u4e86\u5176\u4ed6\u51e0\u79cd{11-22}&lt;11-2-3&gt;\u5b6a\u751f\u673a\u5236\uff0c\u89e3\u91ca\u4e86\u4e3a\u4ec0\u4e48\u5176\u4ed6\u673a\u5236\u5f88\u96be\u5b9e\u73b0\u3002\u76f8\u5173\u7ed3\u679c\u8be6\u89c1Acta Materialia 216 (2021), 117150\uff08DOI:10.1016\/j.actamat.2021.117150)\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-226853\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u72471-1.png\" alt=\"\" width=\"600\" height=\"261\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u72471-1.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u72471-1-300x131.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u9009\u56fe\u5bfc\u8bfb<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-226854\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u72472-1.png\" alt=\"\" width=\"600\" height=\"652\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u72472-1.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u72472-1-276x300.png 276w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u56fe1 \u7eaf\u949b\u6837\u54c1\u4e2d{11-22<\/b><\/strong><strong><b>}\u5b6a\u6676\u7684TEM\u8868\u5f81\u3002<\/b><\/strong>\uff08a\uff09 {11-22}\u5b6a\u6676\u7684\u4f4e\u500dTEM\u7167\u7247\u548c\u76f8\u5e94\u884d\u5c04\u7167\u7247; \uff08b-d\uff09\u5b6a\u6676\u754c\u539f\u5b50\u5206\u8fa8\u7387HAADF-STEM\u7167\u7247\u3002\u5b6a\u751f\u4f4d\u9519\u5b58\u5728\u4e00\u4e2a\u8fc7\u6e21\u533a\u57df\uff0c\u4f4d\u9519\u6838\u82af\u5904\u4e24\u5c42\u539f\u5b50\u5448\u73b0\u5e76\u6392\u5f0f\u7684\u6392\u5217\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-226855\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u72473-1.png\" alt=\"\" width=\"598\" height=\"873\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u72473-1.png 598w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u72473-1-205x300.png 205w\" sizes=\"(max-width: 598px) 100vw, 598px\" \/><\/p>\n<p><strong><b>\u56fe2 {11-22<\/b><\/strong><strong><b>}\u5b6a\u6676\u754c\u8fc1\u79fb\u8fc7\u7a0b\u7684\u8ba1\u7b97\u6a21\u62df\u7ed3\u679c\u3002<\/b><\/strong>\uff08a\uff09 {11-22}\u5b6a\u6676\u754c\u8fc1\u79fb\u8fc7\u7a0b\u7684\u8ba1\u7b97\u6a21\u62df\u793a\u610f\u56fe; \uff08b\uff09 \u53ea\u5305\u542b\u4e00\u5c42\u539f\u5b50\u9762\u7684\u5b6a\u751f\u4f4d\u9519\u6838\u82af\u793a\u610f\u56fe\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-226856\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u72474-1.png\" alt=\"\" width=\"600\" height=\"291\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u72474-1.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u72474-1-300x146.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u56fe3 \u5355\u5c42\u539f\u5b50\u9762\u5b6a\u751f\u4f4d\u9519\u534a\u526a\u5207\u534a\u62d6\u66f3\u673a\u5236\u793a\u610f\u56fe\u3002<\/b><\/strong>\u539f\u5b50\u5148\u526a\u5207\u4e00\u534a\uff08<em><i>s<\/i><\/em>=0.66\uff09\u5230\u7d2b\u8272\u865a\u7ebf\u4f4d\u7f6e\uff08\u5982\u7ea2\u8272\u7bad\u5934\u6240\u793a\uff09\uff0c\u7136\u540e\u62d6\u66f3\u4e00\u534a\uff08~0.08nm\uff09\uff08\u5982\u7eff\u8272\u7bad\u5934\u6240\u793a\uff09\u3002\uff080002\uff09\u9762\u4e3a\u7b2c\u4e8c\u4e0d\u53d8\u9762\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-226857\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u72475-1.png\" alt=\"\" width=\"503\" height=\"473\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u72475-1.png 503w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u72475-1-300x282.png 300w\" sizes=\"(max-width: 503px) 100vw, 503px\" \/><\/p>\n<p><strong><b>\u56fe4 \u534a\u526a\u5207\u534a\u62d6\u66f3\u673a\u5236\u4ece\u5b6a\u751f\u9762\u5782\u76f4\u65b9\u5411\u89c2\u5bdf\u7684\u793a\u610f\u56fe\u3002<\/b><\/strong>\u4e0a-\u4e2d-\u4e0b\u4e09\u5c42(11-22)\u539f\u5b50\u9762\u5bf9\u5e94\u4e8e\u7ea2-\u9ec4-\u7eff\u4e09\u79cd\u989c\u8272\u3002\u7ea2\u8272\u539f\u5b50\u5c42\u7ecf\u8fc7\u5148\u526a\u5207\u540e\u62d6\u66f3\u4e4b\u540e\u76f4\u63a5\u5230\u8fbe\u7eff\u8272\u539f\u5b50\u5c42\u6b63\u4e0a\u65b9\uff0c\u5b9e\u73b0\u4ee5\u9ec4\u8272\u539f\u5b50\u5c42\u4e3a\u5b6a\u6676\u9762\u7684\u955c\u9762\u5bf9\u79f0\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-226858\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u72476-1.png\" alt=\"\" width=\"600\" height=\"332\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u72476-1.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u72476-1-300x166.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u56fe5 \u5305\u542b\u4e09\u5c42\u539f\u5b50\u9762\u7684\u7ecf\u5178\u5b6a\u751f\u7406\u8bba\u793a\u610f\u56fe\u3002<\/b><\/strong>\u4ee5\u5f80\u7ecf\u5178\u5b6a\u751f\u4f4d\u9519\u7406\u8bba\u4e2d\uff0c\u4e09\u5c42\u539f\u5b50\u9762\u539f\u5b50\u5206\u522b\u5411\u4e0d\u540c\u65b9\u5411\u62d6\u66f3\uff0c\u8fc7\u4e8e\u590d\u6742\uff0c\u96be\u4ee5\u5b9e\u73b0\u3002<\/p>\n<p><strong><b>\u5c0f\u7ed3<\/b><\/strong><\/p>\n<p>\u7814\u7a76\u8005\u901a\u8fc7\u5bf9HCP\u91d1\u5c5e\u949b\u4e2d{11-22}\u5b6a\u6676\u754c\u539f\u5b50\u5206\u8fa8\u7387HAADF-STEM\u8868\u5f81\u548c\u8ba1\u7b97\u6a21\u62df\u5206\u6790\uff0c\u63ed\u793a\u4e86\u7531\u5355\u5c42\u5b6a\u751f\u4f4d\u9519\u6ed1\u79fb\u4ea7\u751f\u7684\u4e00\u79cd\u72ec\u7279\u7684\u5b6a\u6676\u8fb9\u754c\u7ed3\u6784\uff0c\u63d0\u51fa\u4e86\u4e00\u79cd\u65b0\u7684\u534a\u526a\u5207\u534a\u62d6\u66f3\u5b6a\u751f\u673a\u5236\u3002\u8be5\u673a\u5236\u4e0d\u4ec5\u89e3\u51b3\u4e86\u7ecf\u5178\u5b6a\u6676\u7406\u8bba\u9884\u6d4b\u7ed3\u679c\u4e0e\u6a21\u62df\u7ed3\u679c\u4e4b\u95f4\u7684\u51b2\u7a81\uff0c\u8fd8\u4e3a\u7814\u7a76\u5f62\u53d8\u5b6a\u751f\u7684\u5fae\u89c2\u673a\u5236\u63d0\u51fa\u4e86\u4e00\u79cd\u65b0\u7684\u601d\u8def\u3002<\/p>\n<p>\u8bba\u6587\u94fe\u63a5\uff1aA half-shear-half-shuffle mechanism and the single-layer twinning dislocation for{11-22}&lt;11-2-3&gt; mode in hexagonal close-packed titanium, Acta Materialia 216 (2021) 117150 (https:\/\/doi.org\/10.1016\/j.actamat.2021.117150)<\/p>\n<p>\u672c\u6587\u7531\u4f5c\u8005\u6295\u7a3f\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u5f15\u8a00 {11-22}&lt;11-2-3&gt;\u5b6a\u6676\u662fHCP\u91d1\u5c5e\u5851\u6027\u53d8\u5f62\u8fc7\u7a0b\u4e2d\u91cd\u8981\u7684\u538b\u7f29\u5b6a\u6676\uff0c\u4f46\u662f\u5176\u5b6a\u751f\u673a\u5236\u76ee\u524d\u4ecd\u7136\u5b58\u5728\u4e89\u8bba\u3002\u7ecf\u5178\u5b6a\u751f\u7406\u8bba\u8ba4\u4e3a\u8be5\u5b6a\u6676\u7684\u7b2c\u4e8c\u4e0d\u53d8\u9762&#8230;<\/p>\n","protected":false},"author":11454,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-226851","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/226851"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/11454"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=226851"}],"version-history":[{"count":4,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/226851\/revisions"}],"predecessor-version":[{"id":226861,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/226851\/revisions\/226861"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=226851"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=226851"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=226851"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}