{"id":227498,"date":"2021-09-20T06:35:52","date_gmt":"2021-09-19T22:35:52","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=227498"},"modified":"2021-09-19T20:36:04","modified_gmt":"2021-09-19T12:36:04","slug":"science%e5%b0%81%e9%9d%a2%ef%bc%9a%e4%bd%8e%e6%b8%a9%e9%94%bb%e9%80%a0%e7%ba%b3%e7%b1%b3%e5%ad%aa%e6%99%b6%e9%92%9b%e4%bb%a5%e5%ae%9e%e7%8e%b0%e8%b6%85%e9%ab%98%e5%bc%ba%e5%ba%a6%e5%92%8c%e5%bb%b6","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=227498","title":{"rendered":"Science\u5c01\u9762\uff1a\u4f4e\u6e29\u953b\u9020\u7eb3\u7c73\u5b6a\u6676\u949b\u4ee5\u5b9e\u73b0\u8d85\u9ad8\u5f3a\u5ea6\u548c\u5ef6\u5c55\u6027"},"content":{"rendered":"<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-227499\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-132-1.png\" alt=\"\" width=\"600\" height=\"277\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-132-1.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-132-1-300x139.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u80cc\u666f\u4ecb\u7ecd<\/strong><\/p>\n<p>\u949b(Ti)\u5728\u6240\u6709\u91d1\u5c5e\u5143\u7d20\u4e2d\u5177\u6709\u6700\u9ad8\u7684\u5f3a\u91cd\u6bd4\uff0c\u5b83\u9664\u4e86\u5177\u6709\u4f18\u5f02\u7684\u8010\u8150\u8680\u6027\u5916\uff0c\u8fd8\u9002\u5408\u4e8e\u5404\u79cd\u5bf9\u91cd\u91cf\u548c\u73af\u5883\u654f\u611f\u7684\u5e94\u7528\u73af\u5883\u3002\u800c\u7eafTi\u7684\u5f3a\u5ea6\u5219\u6bd4\u8f83\u4e00\u822c\u3002Ti\u7684\u4e00\u79cd\u786c\u5316\u65b9\u6cd5\u662f\u5c06\u5176\u4e0e\u5176\u4ed6\u5143\u7d20\u5982\u6c27(O)\u3001\u94dd(Al)\u548c\u9492(V)\u5408\u91d1\u5316\uff0c\u5f62\u6210\u56fa\u6eb6\u4f53\u6216\u7b2c\u4e8c\u76f8\u3002\u8fd9\u4e9b\u5408\u91d1\u7684\u5f3a\u5ea6\u6709\u6240\u63d0\u9ad8\uff0c\u4f46\u51e0\u4e4e\u603b\u662f\u4ee5\u727a\u7272\u5ef6\u5c55\u6027\u4e3a\u4ee3\u4ef7\u3002<\/p>\n<p>\u5f3a\u5316\u7ed3\u6784\u91d1\u5c5e\u7684\u53e6\u4e00\u79cd\u9014\u5f84\u662f\u901a\u8fc7\u70ed-\u673a\u68b0\u52a0\u5de5\u6765\u8c03\u8282\u6676\u7c92\u5c3a\u5bf8\u3002\u5177\u4f53\u6765\u8bf4\uff0c\u5c06\u6676\u7c92\u5c3a\u5bf8\u51cf\u5c0f\u5230\u4e9a\u5fae\u7c73\u548c\u7eb3\u7c73\u7ea7\uff0c\u53ef\u4f7f\u5c48\u670d\u5f3a\u5ea6\u5927\u5e45\u5ea6\u63d0\u9ad8\uff0c\u800c\u5f15\u5165\u67d0\u4e9b\u7c7b\u578b\u7684\u754c\u9762\uff0c\u5219\u53ef\u4fdd\u6301\u5ef6\u6027\u3002<strong><b>\u5bf9\u9762\u5fc3\u7acb\u65b9(fcc)\u91d1\u5c5e\u7684\u5927\u91cf\u7814\u7a76\u8868\u660e\uff0c\u5b6a\u6676\u53ef\u4ee5\u5728\u4e0d\u727a\u7272\u6297\u65ad\u88c2\u6027\u80fd\u7684\u524d\u63d0\u4e0b\uff0c\u5927\u5e45\u5ea6\u63d0\u9ad8\u5f3a\u5ea6\u3002\u8fd9\u79cd\u6027\u80fd\u7684\u63d0\u5347\u5f52\u56e0\u4e8e\u5b6a\u6676\u754c\u7684\u76f8\u5e72\u6027\uff0c\u5b83\u53ef\u4ee5\u6839\u636e\u4f4d\u9519\u7279\u6027\u6765\u9009\u62e9\u6027\u7684\u963b\u65ad\u6216\u4f20\u8f93\u5165\u5c04\u4f4d\u9519\uff0c\u4ece\u800c\u5206\u522b\u63d0\u4f9b\u5f3a\u5ea6\u548c\u5ef6\u5c55\u6027\u3002<\/b><\/strong>\u901a\u8fc7\u8c03\u8282\u5b6a\u6676\u7247\u5c42\u95f4\u8ddd\u548c\u53d6\u5411\uff0c\u53ef\u4ee5\u8fdb\u4e00\u6b65\u4f18\u5316\u529b\u5b66\u6027\u80fd\u3002\u5177\u6709\u68af\u5ea6\u7ec4\u7ec7\u7684\u7eb3\u7c73\u5b6a\u6676\u94dc\u7531\u4e8e\u989d\u5916\u7684\u52a0\u5de5\u786c\u5316\u80fd\u529b\u800c\u8868\u73b0\u51fa\u66f4\u5f3a\u7684\u5f3a\u5ea6\uff0c\u800c\u9ad8\u5ea6\u53d6\u5411\u7684\u7eb3\u7c73\u5b6a\u6676\u94dc\u7531\u4e8e\u4f4d\u9519\u8def\u5f84\u7684\u4e0d\u540c\u800c\u8868\u73b0\u51fa\u66f4\u5f3a\u7684\u6297\u75b2\u52b3\u6027\u80fd\u3002\u53cc\u8fb9\u754c\u4e5f\u4ee3\u8868\u4e86\u4f4e\u80fd\u8fb9\u754c\uff0c\u5728\u9ad8\u6e29\u4e0b\u7684\u8fc1\u79fb\u7387\u5927\u5927\u964d\u4f4e\u3002\u8fd9\u79cd\u6027\u8d28\u4f7f\u5b83\u4eec\u6bd4\u968f\u673a\u7684\u9ad8\u89d2\u5ea6\u6676\u754c\u66f4\u7a33\u5b9a\u3002\u56e0\u6b64\uff0c\u7eb3\u7c73\u5b6a\u6676\u662f\u7ed3\u6784\u91d1\u5c5e\u7684\u6700\u4f73\u7279\u5f81\uff0c\u7136\u800c\u901a\u8fc7\u70ed-\u673a\u68b0\u52a0\u5de5\u5f97\u5230\u7684\u7eb3\u7c73\u5b6a\u6676\u6210\u672c\u8f83\u9ad8\u3002\u540c\u65f6\uff0c\u51e0\u4e4e\u6240\u6709\u7684fcc\u91d1\u5c5e\uff0c\u4e3b\u8981\u662f\u5728\u94dc\u548c\u94a2\uff0c\u90fd\u53ef\u4ee5\u901a\u8fc7\u70ed-\u673a\u68b0\u52a0\u5de5\u65b9\u5f0f\u63d0\u9ad8\u5f3a\u5ea6\u548c\u5ef6\u5c55\u6027\uff0c\u800c\u63a8\u5e7f\u5230\u5bc6\u6392\u516d\u65b9(hcp)\u91d1\u5c5e\u5219\u5f88\u96be\u5b9e\u73b0\u3002<\/p>\n<p><strong><b>\u6210\u679c\u7b80\u4ecb<\/b><\/strong><\/p>\n<p><strong><b>\u8fd1<\/b><\/strong><strong><b>\u65e5\uff0c\u52a0\u5dde\u5927\u5b66\u4f2f\u514b\u5229\u5206\u6821<\/b><\/strong><strong><b>\u3001\u5317\u4eac\u822a\u7a7a\u822a\u5929\u5927\u5b66\u8d75\u58eb\u817e<\/b><\/strong><strong><b>\u56e2\u961f<\/b><\/strong>\u62a5\u9053\u4e86\u4e00\u79cd\u4f4e\u6e29\u953b\u9020\u52a0\u5de5\u6280\u672f\uff0c\u53ef\u4ee5\u5728\u7eafTi (\u8d28\u91cf\u5206\u6570\u4e3a99.95% Ti\u548c0.05% O)\u4e2d\u751f\u6210\u6709\u5c42\u6b21\u7ed3\u6784\u7684\u7eb3\u7c73\u5b6a\u6676\u3002\u7531\u4e8eO\u4f1a\u6291\u5236Ti\u4e2d\u7684\u5b6a\u6676\uff0c\u56e0\u6b64\u4f5c\u8005\u9009\u62e9\u8d85\u4f4eO\u542b\u91cf(\u4f4e\u4e8e\u5546\u7528\u7eafTi )\u6765\u4fc3\u8fdb\u5b6a\u751f\u503e\u5411\uff0c\u4ece\u800c\u5b9e\u73b0\u4e86\u8d85\u9ad8\u7684\u5f3a\u5ea6\u548c\u5ef6\u5c55\u6027\u3002\u591a\u5c3a\u5ea6\u7eb3\u7c73\u5b6a\u6676Ti\u7684\u70ed\u7a33\u5b9a\u6027\u9ad8\u8fbe873\u5f00\u5c14\u6587\uff08\u8fdc\u9ad8\u4e8e\u7eafTi\u768477\u5f00\u5c14\u6587\uff09\uff0c\u56e0\u6b64\u53ef\u5e94\u7528\u4e8e\u7edd\u5927\u591a\u6570\u7684\u6781\u7aef\u73af\u5883\u4e2d\u3002\u4f5c\u8005\u53d1\u73b0\uff0c\u6db2\u6c2e\u6e29\u5ea6\u4e0b\u5927\u91cf\u5b6a\u6676\u5f3a\u5316\u4e86\u52a0\u5de5\u786c\u5316\u80fd\u529b\uff0c\u8bf4\u660e\u7eb3\u7c73\u5b6a\u6676Ti\u5728\u8f83\u9ad8\u5e94\u53d8\u901f\u7387\u4e0b\u4f1a\u8868\u73b0\u51fa\u8f83\u9ad8\u7684\u6297\u51b2\u51fb\u6027\u80fd\u3002\u7531\u4e8e\u4e30\u5bcc\u7684\u7eb3\u7c73\u5b6a\u6676\u8fb9\u754c\u4e3a\u6c9f\u9053\u70b9\u7f3a\u9677\u63d0\u4f9b\u4e86\u9ad8\u5bc6\u5ea6\u7684\u754c\u9762\uff0c\u4ece\u800c\u963b\u6b62\u4e86\u7a7a\u6d1e\u7684\u5f62\u6210\u7eb3\u7c73\u5b6a\u6676Ti\uff0c\u56e0\u6b64\u8fd8\u5177\u6709\u826f\u597d\u7684\u6297\u8f90\u5c04\u635f\u4f24\u80fd\u529b\u3002<strong><b>\u672c\u5de5\u4f5c<\/b><\/strong><strong><b>\u4f7f\u7528\u7ecf\u6d4e\u6548\u76ca\u66f4\u9ad8\u7684\u65b9\u6cd5\u5728\u7eafTi\u4e2d\u8bf1\u5bfc\u5408\u6210\u4e86\u7eb3\u7c73\u5b6a\u6676\uff0c\u5b9e\u73b0\u4e86\u8d85\u9ad8\u7684\u5f3a\u5ea6\u3001\u70ed\u7a33\u5b9a\u6027\u548c\u5ef6\u5c55\u6027\u3002<\/b><\/strong>\u76f8\u5173\u6210\u679c\u4ee5\u9898\u4e3a\u201cCryoforged nanotwinned titanium with ultrahigh strength and ductility\u201d\u53d1\u8868\u5728\u4e86Science\u4e0a\uff0c<strong><b>\u5e76\u88ab\u9009\u4e3aScience\u5c01\u9762<\/b><\/strong><strong><b>\u3002<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-227511\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/11-3.png\" alt=\"\" width=\"600\" height=\"763\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/11-3.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/11-3-236x300.png 236w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u56fe\u6587\u89e3\u6790<\/b><\/strong><\/p>\n<p><strong style=\"line-height: 1.5;\"><b>\u4e00\u3001\u4f4e\u6e29\u673a\u68b0\u5236\u5907\u7eb3\u7c73\u5b6a\u6676Ti\u7684\u5fae\u89c2\u7ed3\u6784\u3002<\/b><\/strong><\/p>\n<p>\u672c\u5de5\u4f5c\u5728\u7eafTi(\u8d28\u91cf\u5206\u6570\u4e3a99.95% Ti\u548c0.05% O)\u4e2d\uff0c\u901a\u8fc7\u4f4e\u6e29\u529b\u5b66\u8fc7\u7a0b\u8bf1\u5bfc\u7684\u5927\u91cf\u529b\u5b66\u5b6a\u751f\uff0c\u53ef\u4ee5\u6784\u5efa\u5c42\u6b21\u7eb3\u7c73\u5b6a\u6676\u7ed3\u6784\u3002\u7535\u5b50\u80cc\u6563\u5c04\u884d\u5c04(EBSD)\u56fe\u8c31\uff08\u56fe1B\uff09\u663e\u793a\u4e86\u591a\u8f74\u953b\u9020Ti\u4e2d\u590d\u6742\u7684\u591a\u5c3a\u5bf8\u5b6a\u6676\u7ed3\u6784\u3002\u4ece\u56fe\u4e2d\u4ecd\u53ef\u4ee5\u770b\u51fa\u521d\u59cb\u7b49\u8f74\u6676\u7ec4\u7ec7\uff0c\u4f46\u7ecf\u4f4e\u6e29\u673a\u68b0\u5904\u7406\u540e\uff0c\u6bcf\u4e2a\u6676\u7c92\u90fd\u542b\u6709\u5927\u91cf\u7684\u835a\u72b6\u5b6a\u6676\u3002\u8fd9\u4e9b\u53d8\u5f62\u7279\u5f81\uff0c\u901a\u8fc7\u4e00\u4e2a\u51b7\u51bb\u673a\u68b0\u8fc7\u7a0b\u5f15\u5165\uff0c\u5728\u968f\u540e\u7684\u70ed\u5904\u7406\u8fc7\u7a0b\u4e2d\u5f97\u4ee5\u4fdd\u7559\u3002\u5728\u900f\u5c04\u7535\u5b50\u663e\u5fae\u955c(TEM)\u663e\u5fae\u7167\u7247\u4e2d\u53ef\u4ee5\u89c2\u5bdf\u5230\u4e00\u7ec4\u7279\u5f81\u7eb3\u7c73\u5b6a\u6676\uff0c\u5176\u4e2d\u5728\u9ad8\u5206\u8fa8\u7387\u539f\u5b50\u6676\u683c\u56fe\u50cf\u4e2d\u7a81\u51fa\u4e86\u5b6a\u6676\u754c\u3002\u7eb3\u7c73\u5b6a\u6676\u5f80\u5f80\u53ef\u4ee5\u76f8\u4e92\u4ea4\u53c9\uff0c\u5f62\u6210\u4e00\u4e2a\u590d\u6742\u7684\u5b6a\u6676\u7f51\u7edc\u3002TEM\u56fe\u50cf\u663e\u793a\u4e86673K\u56de\u706b\u6b65\u9aa4\u524d\u540e\u76f8\u540c\u7684\u7eb3\u7c73\u5b6a\u6676\u7ed3\u6784\u3002\u6837\u54c1\u5728673K\u4fdd\u6e291h\u540e\uff0c\u7eb3\u7c73\u5b6a\u6676\u7ed3\u6784\u88ab\u4fdd\u7559\uff0c\u4f46\u7531\u4e8e\u6b8b\u4f59\u5e94\u529b\u5e94\u53d8\u677e\u5f1b\uff0c\u5b6a\u6676\u5185\u90e8\u7684\u5e94\u53d8\u5bf9\u6bd4\u5ea6\u51cf\u5f31\u3002\u672c\u5de5\u4f5c\u8fdb\u4e00\u6b65\u7528TEM\u539f\u4f4d\u9000\u706b\u524d\u540e\u8ba1\u7b97\u7684\u7eb3\u7c73\u675f\u884d\u5c04\u5e94\u53d8\u56fe\u7684\u5b9a\u91cf\u5206\u6790\u6765\u8bf4\u660e\u8fd9\u79cd\u5e94\u53d8\u5f1b\u8c6b\uff0c\u8fd9\u4e9b\u591a\u5c3a\u5ea6\u7ed3\u6784\u7684\u7edf\u8ba1\u5c3a\u5bf8\u5206\u5e03(\u56fe1G)\u663e\u793a\u4e86\u4e00\u4e2a\u5b8f\u89c2\u5c3a\u5ea6\u7684\u968f\u673a\u5206\u5e03\u7684\u7b49\u8f74\u5728\u51e0\u5341\u5230\u51e0\u767e\u5fae\u7c73\uff0c\u5fae\u89c2\u5c3a\u5ea6\u7684\u5b6a\u6676\u9aa8\u67b6\u5728\u51e0\u5fae\u7c73\uff0c\u7eb3\u7c73\u5c3a\u5ea6\u7684\u5b6a\u6676\u7f51\u7edc\u5728\u51e0\u5341\u5230\u51e0\u767e\u7eb3\u7c73\u3002<br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-227500\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-133.png\" alt=\"\" width=\"600\" height=\"706\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-133.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-133-255x300.png 255w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u56fe1. \u4f4e\u6e29\u529b\u5b66\u5236\u5907\u7eb3\u7c73\u5b6a\u6676Ti\u7684\u5c42\u6b21\u5316\u5fae\u89c2\u7ed3\u6784<\/p>\n<p><b><\/b><strong><b>\u4e8c\u3001\u7eb3\u7c73\u5b6a\u6676Ti\u7684\u529b\u5b66<\/b><\/strong><strong><b>\u6027\u80fd<\/b><\/strong><strong><b>\u3002<\/b><\/strong><\/p>\n<p><strong><b>\u00a0<\/b><\/strong>\u672c\u5de5\u4f5c\u5728\u5ba4\u6e29(RT)\u548c\u4f4e\u6e29(77 K)\u6e29\u5ea6\u4e0b\uff0c\u4f7f\u7528\u5355\u8f74\u62c9\u4f38\u8bd5\u9a8c\u6765\u8868\u5f81\u591a\u5c3a\u5ea6\u5b6a\u6676\u7ed3\u6784\u5e26\u6765\u7684\u529b\u5b66\u6027\u80fd\u63d0\u5347\u3002\u4f5c\u8005\u9a8c\u8bc1\u4e86\u7eb3\u7c73\u5b6a\u6676Ti\u7684\u5e94\u529b-\u5e94\u53d8\u54cd\u5e94\uff0c\u5e76\u4e0e\u5e38\u89c4\u7c97\u6676Ti(\u6676\u7c92\u5c3a\u5bf8\u4e3a~100 mm )\u8fdb\u884c\u4e86\u6bd4\u8f83\u3002RT\u65f6\uff0c\u7eb3\u7c73\u5b6a\u6676Ti\u7684\u6297\u62c9\u5f3a\u5ea6\u4e3a500 MPa\uff0c\u62c9\u4f38\u5ef6\u6027(\u5e94\u53d8\u81f3\u5931\u6548)\u4e3a~70%\uff0c\u4e0e\u7c97\u6676Ti\u76f8\u6bd4\u5206\u522b\u63d0\u9ad8\u4e86~50MPa\u548c~ 17%\u3002\u8be5\u6750\u6599\u7684\u5c48\u670d\u5f3a\u5ea6\u65e2\u53d7\u5c40\u90e8\u7eb3\u7c73\u5b6a\u6676\u533a\u4f4d\u9519\u5e73\u5747\u81ea\u7531\u7a0b\u7684\u51cf\u5c0f\u6240\u63a7\u5236\uff0c\u4e5f\u53d7\u6676\u7c92\u76f8\u5bf9\u7c97\u5927\u7684\u57fa\u4f53\u6240\u63a7\u5236\uff0c\u56e0\u6b64\u5176\u970d\u5c14-\u4f69\u5947\u5f3a\u5316\u4e0d\u5982\u7eb3\u7c73\u6676Ti\uff0c\u4f46\u5176\u52a0\u5de5\u786c\u5316\u80fd\u529b\u8981\u9ad8\u5f97\u591a\u3002\u572877 K\u65f6\uff0c\u7eb3\u7c73\u5b6a\u6676Ti\u7684\u529b\u5b66\u6027\u80fd\u8fdb\u4e00\u6b65\u63d0\u9ad8\uff0c\u62c9\u4f38\u5f3a\u5ea6\u4e3a~2 GPa\uff0c\u62c9\u4f38\u5851\u6027\u63a5\u8fd1100%\u3002<strong><b>\u7eb3\u7c73\u5b6a\u6676Ti\u7684\u8d85\u9ad8\u5f3a\u5ea6\u548c\u5ef6\u5c55\u6027\u4f7f\u5176\u4f18\u4e8e\u8bb8\u591aTi\u5408\u91d1\u751a\u81f3\u67d0\u4e9b\u4f4e\u6e29\u94a2\u3002<\/b><\/strong>\u4ece\u5178\u578b\u7684\u7eb3\u7c73\u5b6a\u6676\u7f51\u7edc\u53ef\u4ee5\u770b\u51fa\uff0c\u4f4d\u9519\u5bc6\u5ea6\u7684\u589e\u52a0\u548c\u7eb3\u7c73\u5b6a\u6676\u7f51\u7edc\u7684\u7ec6\u5316\u95f4\u8ddd\u5bf9\u540e\u7eed\u5b6a\u6676\u4ea7\u751f\u4e86\u66f4\u9ad8\u7684\u6fc0\u6d3b\u5e94\u529b\uff0c\u4ece\u800c\u589e\u52a0\u4e86\u6d41\u52a8\u5e94\u529b\u3002\u4ece\u5b8f\u89c2\u4e0a\u770b\uff0c\u8fd9\u8868\u73b0\u4e3a\u5e94\u53d8\u786c\u5316\u901f\u7387\u4e0a\u5347\u540e\u7684\u5e73\u53f0\u5ef6\u957f\u3002\u5728\u5851\u6027\u53d8\u5f62\u7684\u6700\u540e\u9636\u6bb5\uff0c\u5e94\u53d8\u786c\u5316\u901f\u7387\u8fc5\u901f\u4e0b\u964d\uff0c\u8fd9\u4e00\u9636\u6bb5\u7684\u5fae\u89c2\u7ec4\u7ec7\u4e0e\u4e25\u91cd\u7684\u6676\u7c92\u7ec6\u5316\u6709\u5173\uff0c\u7279\u522b\u662f\u5728\u53d8\u5f62\u5c40\u90e8\u5316\u9636\u6bb5\u3002\u5728\u9888\u7f29\u533a\u9644\u8fd1\u62cd\u6444\u7684TEM\u663e\u5fae\u7167\u7247(\u56fe2F)\u663e\u793a\u4e86\u9ad8\u5bc6\u5ea6\u7684\u7b49\u8f74\u6676\u7c92\uff0c\u6676\u7c92\u5c3a\u5bf8\u4e3a~300 nm\u3002\u5c3d\u7ba1\u4ea7\u751f\u4e86\u8f83\u9ad8\u7684\u6d41\u52a8\u5e94\u529b\uff0c\u4f46\u8fd9\u4e9b\u8d85\u7ec6\u6676\u7c92\u4f7f\u4f4d\u9519\u6d3b\u52a8\u548c\u5b6a\u6676\u96be\u4ee5\u64cd\u4f5c\uff0c\u4ece\u800c\u5371\u53ca\u5e94\u53d8\u786c\u5316\u80fd\u529b\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-227501\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-134.png\" alt=\"\" width=\"600\" height=\"737\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-134.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-134-244x300.png 244w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u56fe2. \u7eb3\u7c73\u5b6a\u6676Ti\u7684\u529b\u5b66\u6027\u80fd\u8868\u5f81<\/p>\n<p><b><\/b><strong><b>\u4e09\u3001\u7eb3\u7c73\u5b6a\u6676Ti\u7684\u5fae\u89c2\u7ed3\u6784\u6f14\u5316\u3002<\/b><\/strong><\/p>\n<p>\u672c\u5de5\u4f5c\u5229\u7528\u51c6\u539f\u4f4dEBSD\u8868\u5f81\uff0c\u6355\u6349\u5230\u4e86\u7eb3\u7c73\u5b6a\u6676Ti\u7684\u5b6a\u751f\u3001\u53bb\u5b6a\u751f\u3001\u518d\u5b6a\u751f\u7684\u6f14\u5316\u8fc7\u7a0b\uff0c\u6765\u8868\u5f81\u7eb3\u7c73\u5b6a\u6676Ti\u8bf1\u5bfc\u5851\u6027\u7684\u673a\u7406\u3002\u672c\u5de5\u4f5c\u603b\u7ed3\u4e86\u5404\u7c7b\u578b\u5b6a\u6676\u7684\u957f\u5ea6\u5206\u6570\u548c\u603b\u5b6a\u6676\u8fb9\u754c\u3002\u5728\u603b\u5b6a\u6676\u6570\u91cf\u5feb\u901f\u589e\u957f\u540e\uff0c\u8fde\u7eed\u5b6a\u6676\u548c\u8131\u5b6a\u6676\u7684\u7ed3\u5408\u548c\u7ade\u4e89\u4f7f\u5b6a\u6676\u5206\u6570\u5728\u5fae\u5c3a\u5ea6\u4e0a\u7684\u589e\u957f\u901f\u5ea6\u5927\u5927\u964d\u4f4e\u3002\u7136\u800c\uff0c\u5373\u4f7f\u5728\u5fae\u5c3a\u5ea6\u5b6a\u6676\u7ec4\u5206\u9971\u548c(~70%)\u65f6\uff0c\u7eb3\u7c73\u5b6a\u6676\u5bc6\u5ea6\u4f3c\u4e4e\u4ecd\u5728\u4e0d\u65ad\u589e\u52a0\uff0c\u76f4\u5230\u5851\u6027\u53d8\u5f62\u7ed3\u675f\u65f6\u4e25\u91cd\u7684\u5b6a\u6676\u4ea4\u53c9\u548c\u5b6a\u6676\u754c\u65cb\u8f6c\u5f00\u59cb\u53d1\u6325\u4f5c\u7528\uff0c\u8fd9\u53ef\u4ee5\u4eceTEM\u4e2d\u5f88\u660e\u663e\u89c2\u5bdf\u5230\u3002\u51fa\u73b0\u8be5\u60c5\u51b5\u7684\u539f\u56e0\u53ef\u5f52\u7ed3\u4e3a\u4e24\u70b9\uff1a<strong><b>\u9996\u5148\uff0c<\/b><\/strong><strong><b>\u7eb3\u7c73\u5b6a\u6676\u7684\u6bd4\u4f8b\u4ecd\u5728\u589e\u52a0\uff0c\u8d85\u51fa\u4e86\u51c6\u539f\u4f4dEBSD\u5206\u6790\u6240\u80fd\u89e3\u51b3\u7684\u8303\u56f4\uff1b<\/b><\/strong><strong><b>\u5176\u6b21\uff0c<\/b><\/strong><strong><b>\u6676\u7c92\u5185\u7684\u53cc\u5b6a\u7ed3\u8fdb\u4e00\u6b65\u7ec6\u5316\u6676\u7c92\u5c3a\u5bf8\uff0c\u4ece\u800c\u4ea7\u751f\u66f4\u591a\u7684\u754c\u9762\uff0c\u963b\u788d\u4f4d\u9519\u8fd0\u52a8\u3002\u5c3d\u7ba1\u5982\u6b64\uff0c\u8fd9\u4e24\u79cd\u673a\u5236\u90fd\u5bfc\u81f4\u4e86\u52a8\u6001\u7684\u970d\u5c14-\u4f69\u5947\u6548\u5e94<\/b><\/strong><strong><b>\uff0c\u4f7f\u5f97<\/b><\/strong><strong><b>\u79fb\u52a8\u4f4d\u9519\u53d7\u5230\u76f8\u5bf9\u521a\u6027\u754c\u9762\u7684\u7ea6\u675f\uff0c\u4f7f\u5176\u5177\u6709\u66f4\u9ad8\u7684\u6297\u5851\u6027\u53d8\u5f62\u80fd\u529b\u3002<\/b><\/strong><\/p>\n<p><strong><b><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-227502\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-135.png\" alt=\"\" width=\"600\" height=\"483\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-135.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-135-300x242.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\u56fe3. \u7eb3\u7c73\u5b6a\u6676Ti\u7684\u5fae\u89c2\u7ed3\u6784\u6f14\u5316<\/p>\n<p><strong style=\"line-height: 1.5;\"><b>\u56db\u3001\u7eb3\u7c73\u5b6a\u6676Ti\u7684\u70ed\u7a33\u5b9a\u6027\u3002<\/b><\/strong><\/p>\n<p>\u4e3a\u4e86\u8fdb\u4e00\u6b65\u4e86\u89e3\u7eb3\u7c73\u5b6a\u6676Ti\u7684\u70ed\u7a33\u5b9a\u6027\uff0c\u672c\u5de5\u4f5c\u8fdb\u884c\u4e86\u539f\u4f4d\u900f\u5c04\u7535\u955c\u52a0\u70ed\u5b9e\u9a8c\u3002\u4e00\u822c\u6765\u8bf4\uff0c\u7eb3\u7c73\u6676\u4f53\u91d1\u5c5e\u5728\u9ad8\u6e29\u4e0b\u7a33\u5b9a\u6027\u4f1a\u9010\u6e10\u4e0b\u964d\uff0c\u56e0\u4e3a\u5728\u5965\u65af\u7279\u74e6\u5c14\u5fb7\u6210\u719f\u8fc7\u7a0b\u4e2d\uff0c\u6676\u7c92\u751f\u957f\u4f1a\u6d88\u8017\u5927\u91cf\u7684\u754c\u9762\u3002\u56e0\u6b64\uff0c\u901a\u5e38\u4e0e\u6750\u6599\u7194\u70b9\u6210\u6b63\u6bd4\u7684\u6807\u5fd7\u6676\u7c92\u7c97\u5316\u5f00\u59cb\u7684\u6e29\u5ea6\uff0c\u4f1a\u6700\u7ec8\u9650\u5236\u8fd9\u7c7b\u7eb3\u7c73\u6676\u4f53\u91d1\u5c5e\u7684\u6709\u7528\u670d\u5f79\u6e29\u5ea6\u3002\u7531\u4e8eTi\u5728\u7ed3\u6784\u91d1\u5c5e\u95f4\u5177\u6709\u76f8\u5f53\u9ad8\u7684\u7194\u5316\u6e29\u5ea6(1941K)\uff0c\u56e0\u6b64\u4f5c\u8005\u63a8\u65ad\u7eb3\u7c73\u5b6a\u6676\u7ed3\u6784\u7684\u6709\u7528\u6027\u4f9d\u8d56\u4e8eTi\u7684\u70ed\u7a33\u5b9a\u6027\u3002\u539f\u4f4dTEM\u52a0\u70ed\u5b9e\u9a8c\u8868\u660e\uff0c\u7eb3\u7c73\u5b6a\u6676\u7ed3\u6784\u70ed\u7a33\u5b9a\u9ad8\u8fbe873 K\u3002\u7136\u800c\uff0c\u7531\u4e8e\u6837\u54c1\u4e3a\u8584\u7684\u7535\u5b50\u900f\u660e\u7b94\uff0c\u8fdb\u4e00\u6b65\u52a0\u70ed\u4f1a\u5bfc\u81f4\u6c27\u5316\u3002\u57281123K\u5de6\u53f3\uff0c\u4e25\u91cd\u7684\u6c27\u5316\u5f00\u59cb\u8513\u5ef6\uff0c\u4f46\u7eb3\u7c73\u5b6a\u6676\u7f51\u7edc\u4ecd\u7136\u4fdd\u6301\u5176\u76f8\u5bf9\u5b8c\u6574\u6027\u3002\u901a\u8fc7\u539f\u4f4d\u9000\u706b\u548cEBSD\u5206\u6790\u53ef\u8fdb\u4e00\u6b65\u8bc1\u5b9eTEM\u52a0\u70ed\u5b9e\u9a8c\u7ed3\u679c\u3002<strong><b>\u4f5c\u8005<\/b><\/strong><strong><b>\u53d1\u73b0\uff0c\u7eb3\u7c73\u5b6a\u6676Ti\u5728673 K\u4e0b\u52a0\u70ed48\u5c0f\u65f6\uff0c\u65e2\u6ca1\u6709\u660e\u663e\u7684\u6676\u7c92\u751f\u957f\uff0c\u4e5f\u6ca1\u6709\u660e\u663e\u7684\u5b6a\u6676\u754c\u6570\u51cf\u5c11<\/b><\/strong><strong><b>\u3002<\/b><\/strong>\u5c40\u57df\u6838\u5e73\u5747\u53d6\u5411\u5931\u914d\u56fe\u8868\u660e\uff0c\u9000\u706b\u6837\u54c1(\u56fe4I)\u6676\u7c92\u5185\u7684\u53d6\u5411\u504f\u5dee\u76f8\u5bf9\u8f83\u4f4e\uff0c\u8fd9\u8bf4\u660e\u51e0\u4f55\u5fc5\u9700\u4f4d\u9519\u5bc6\u5ea6\u964d\u4f4e\u3002<strong><b>\u7eb3\u7c73\u5b6a\u6676Ti\u5177\u6709\u826f\u597d\u7684\u70ed\u7a33\u5b9a\u6027\uff0c\u80fd\u591f\u5728\u9ad8\u6e29\u4e0b\u4fdd\u5b58\u5c42\u6b21\u5316\u7684\u5fae\u89c2\u7ed3\u6784\uff0c\u8868\u660e\u8be5\u6750\u6599\u5177\u6709\u5728\u8f83\u5bbd\u6e29\u5ea6\u8303\u56f4\u5185\u5de5\u4f5c\u7684\u80fd\u529b\uff0c\u5728\u5927\u90e8\u5206\u4f20\u7edf\u7684Ti\u57fa\u5408\u91d1\u9002\u7528\u8303\u56f4\u5185\uff0c\u7eb3\u7c73\u5b6a\u6676Ti\u5747<\/b><\/strong><strong><b>\u9002\u7528<\/b><\/strong><strong><b>\u3002<\/b><\/strong><\/p>\n<p><strong><b><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-227503\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-136.png\" alt=\"\" width=\"600\" height=\"526\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-136.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-136-300x263.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\u56fe4. \u7eb3\u7c73\u5b6a\u6676Ti\u7684\u70ed\u7a33\u5b9a\u6027\u8868\u5f81<\/p>\n<p>\u7b2c\u4e00\u4f5c\u8005\uff1a\u8d75\u58eb\u817e<\/p>\n<p>\u901a\u8baf\u4f5c\u8005\uff1a\u8d75\u58eb\u817e\u3001Andrew M. Minor<\/p>\n<p>\u901a\u8baf\u5355\u4f4d\uff1a\u52a0\u5dde\u5927\u5b66\u4f2f\u514b\u5229\u5206\u6821<\/p>\n<p>\u8bba\u6587doi\uff1a<\/p>\n<p><a href=\"https:\/\/doi.org\/10.1038\/s41586-021-03810-x\"><u>https:\/\/doi.org\/10.1126\/science.abe7252<\/u><\/a><\/p>\n<p>\u672c\u6587\u7531\u6e29\u534e\u4f9b\u7a3f\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u80cc\u666f\u4ecb\u7ecd \u949b(Ti)\u5728\u6240\u6709\u91d1\u5c5e\u5143\u7d20\u4e2d\u5177\u6709\u6700\u9ad8\u7684\u5f3a\u91cd\u6bd4\uff0c\u5b83\u9664\u4e86\u5177\u6709\u4f18\u5f02\u7684\u8010\u8150\u8680\u6027\u5916\uff0c\u8fd8\u9002\u5408\u4e8e\u5404\u79cd\u5bf9\u91cd\u91cf\u548c\u73af\u5883\u654f\u611f\u7684\u5e94\u7528\u73af\u5883\u3002\u800c\u7eafTi\u7684\u5f3a\u5ea6\u5219\u6bd4\u8f83\u4e00\u822c\u3002Ti\u7684\u4e00\u79cd\u786c&#8230;<\/p>\n","protected":false},"author":11454,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-227498","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/227498"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/11454"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=227498"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/227498\/revisions"}],"predecessor-version":[{"id":227513,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/227498\/revisions\/227513"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=227498"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=227498"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=227498"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}