{"id":227673,"date":"2021-09-24T06:30:24","date_gmt":"2021-09-23T22:30:24","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=227673"},"modified":"2021-09-23T15:38:43","modified_gmt":"2021-09-23T07:38:43","slug":"%e6%b2%b3%e5%8c%97%e5%b7%a5%e4%b8%9a%e5%a4%a7%e5%ad%a6ensm%ef%bc%9a%e5%8f%8c%e6%b4%bb%e6%80%a7-%e5%8a%a8%e5%8a%9b%e5%ad%a6%e4%ba%92%e4%bf%83%e7%9a%84li3vo4-%e7%9f%b3%e5%a2%a8%e7%83%af%e5%ae%9e","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=227673","title":{"rendered":"\u6cb3\u5317\u5de5\u4e1a\u5927\u5b66EnSM\uff1a\u53cc\u6d3b\u6027\/\u52a8\u529b\u5b66\u4e92\u4fc3\u7684Li3VO4\/\u77f3\u58a8\u70ef\u5b9e\u73b0\u53ef\u55b7\u6d82\u9ad8\u6bd4\u80fd\u9502\u79bb\u5b50\u5fae\u578b\u7535\u5bb9\u5668"},"content":{"rendered":"<p><strong><b>\u4e00\u3001\u7814\u7a76\u80cc\u666f<\/b><\/strong><\/p>\n<p>\u968f\u77405G\u3001\u7269\u8054\u7f51\u3001\u4eba\u5de5\u667a\u80fd\u3001\u533b\u7597\u4fdd\u5065\u8bbe\u5907\u7684\u98de\u901f\u53d1\u5c55\uff0c\u53ef\u7a7f\u6234\u5fae\u578b\u7535\u5b50\u8bbe\u5907\u7684\u5e02\u573a\u9700\u6c42\u4e0d\u65ad\u589e\u957f\uff0c\u8fd9\u4e5f\u8981\u6c42\u5176\u5185\u7f6e\u7535\u6e90\u9700\u8981\u5411\u5fae\u578b\u5316\u53d1\u5c55\u3002\u5fae\u578b\u7535\u5bb9\u5668\uff08MSCs\uff09\u548c\u5fae\u578b\u9502\u79bb\u5b50\u7535\u6c60\uff08MBs\uff09\u5e94\u8fd0\u800c\u751f\u3002\u7136\u800c\uff0c\u7531\u4e8e\u9502\u79bb\u5b50\u5728\u8d1f\u6781\u6750\u6599\u4e2d\u7684\u63d2\u5165\/\u8131\u51fa\u53cd\u5e94\u52a8\u529b\u5b66\u6ede\u540e\uff0c\u5bfc\u81f4MBs\u529f\u7387\u5bc6\u5ea6\u8f83\u4f4e\uff08&lt;\u00a05 mW cm<sup>\u2212<\/sup><sup>2<\/sup>\uff09\uff0c\u5bff\u547d\u8f83\u77ed\uff08&lt;\u00a01000\u4e2a\u5faa\u73af\uff09\uff1bMSCs\u56e0\u4e3a\u5176\u53cc\u7535\u5c42\u5b58\u50a8\u673a\u5236\u8868\u73b0\u51fa\u56fa\u6709\u7684\u9ad8\u529f\u7387\u5bc6\u5ea6\u548c\u957f\u5faa\u73af\u5bff\u547d\u7279\u5f81\uff0c\u7136\u800c\u5176\u4f4e\u80fd\u91cf\u5bc6\u5ea6\u7684\u95ee\u9898\u65e0\u6cd5\u6ee1\u8db3\u4e0d\u65ad\u589e\u957f\u7684\u9ad8\u6bd4\u80fd\u9700\u6c42\u3002\u56e0\u6b64\uff0c\u5f15\u5165\u4e0d\u540c\u7684\u7535\u6781\u80fd\u91cf\u5b58\u50a8\u673a\u5236\u4ee5\u53ca\u6269\u5c55MSCs\u7684\u5de5\u4f5c\u7535\u538b\u5f15\u8d77\u4e86\u5927\u91cf\u7814\u7a76\u5174\u8da3\u3002<\/p>\n<p>\u91d1\u5c5e\u79bb\u5b50\u6df7\u5408\u7535\u5bb9\u5668\uff08MICs\uff0c\u5982Li<sup>+<\/sup>\u3001Na<sup>+<\/sup>\u3001K<sup>+<\/sup>\u3001Zn<sup>2+<\/sup>\u7b49\uff09\u5df2\u5728\u5b66\u672f\u754c\u5f15\u8d77\u4e86\u6781\u5927\u7684\u5173\u6ce8\u3002\u5176\u7535\u6c60\u578b\u8d1f\u6781\u548c\u7535\u5bb9\u578b\u6b63\u6781\u8d4b\u4e88\u4e86MICs\u6bd4\u8d5d\u7535\u5bb9\/\u6c34\u7cfb\u975e\u5bf9\u79f0\u7535\u5bb9\u5668\u66f4\u9ad8\u7684\u80fd\u91cf\u5bc6\u5ea6\uff0c\u540c\u65f6\u53ef\u4fdd\u6301\u4f18\u5f02\u7684\u529f\u7387\u5bc6\u5ea6\u548c\u957f\u5faa\u73af\u5bff\u547d\uff0c\u4ece\u800c\u663e\u793a\u51fa\u4f5c\u4e3a\u9ad8\u6bd4\u80fd\/\u9ad8\u529f\u7387\u50a8\u80fd\u8bbe\u5907\u7684\u7edd\u4f73\u524d\u666f\u3002\u800cMICs\u6027\u80fd\u53d7\u9650\u7684\u4e3b\u8981\u539f\u56e0\u662f\u6b63\u8d1f\u6781\u4e4b\u95f4\u7535\u5316\u5b66\u53cd\u5e94\u52a8\u529b\u5b66\u4e0d\u5339\u914d\uff0c\u9700\u5f00\u53d1\u7535\u538b\u5e73\u53f0\u5b89\u5168\u3001\u6bd4\u5bb9\u91cf\u5927\u3001\u500d\u7387\u6027\u80fd\u597d\u3001\u7a33\u5b9a\u6027\u597d\u7684\u8d1f\u6781\u6750\u6599\uff1b\u53e6\u5916\u5fae\u578bMICs\u5668\u4ef6\u7684\u5236\u5907\u548c\u7ec4\u88c5\u6280\u672f\u76f8\u5bf9\u590d\u6742\uff0c\u9700\u8981\u66f4\u4e3a\u7b80\u4fbf\u7684\u6280\u672f\u8def\u7ebf\u6765\u6ee1\u8db3\u5b9e\u9645\u9700\u6c42\u3002<\/p>\n<p><strong><b>\u4e8c\u3001\u5185\u5bb9\u7b80\u4ecb<\/b><\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c\u6cb3\u5317\u5de5\u4e1a\u5927\u5b66\u6750\u6599\u5b66\u9662\u6bb7\u798f\u661f\u6559\u6388\u56e2\u961f<strong><b>\u738b\u606d\u51ef<\/b><\/strong>\u526f\u7814\u7a76\u5458\u4e3a\u9502\u79bb\u5b50\u5fae\u7535\u5bb9\u5668\uff08LIMCs\uff09\u8bbe\u8ba1\u4e86\u4e00\u79cd\u53cc\u6d3b\u6027\u3001\u52a8\u529b\u5b66\u4e92\u4fc3\u7684Li<sub>3<\/sub>VO<sub>4<\/sub>\u00a0(LVO)\/\u77f3\u58a8\u70ef\u8d1f\u6781\u6750\u6599\u3002\u5176\u4e2d\u9492\u6e90\u524d\u9a71\u4f53\u901a\u8fc7\u539f\u5b50\u5c42\u6c89\u79ef\uff08ALD\uff09\u6280\u672f\u9884\u5148\u6c89\u79ef\u5728\u77f3\u58a8\u70ef\u7eb3\u7c73\u7247\u4e0a\uff0c\u518d\u501f\u52a9\u56fa\u76f8\u53cd\u5e94\u5c06\u9492\u6e90\u524d\u9a71\u4f53\u8f6c\u5316\u6210\u5747\u5300\u5206\u6563\u7684LVO\u7eb3\u7c73\u9897\u7c92\u3002LVO\/\u77f3\u58a8\u70ef\u590d\u5408\u6750\u6599\u4f5c\u4e3a\u53cc\u6d3b\u6027\u7ec4\u5206\u8d1f\u6781\uff0cLVO\u7eb3\u7c73\u9897\u7c92\u548c\u77f3\u58a8\u70ef\u7eb3\u7c73\u7247\u90fd\u53ef\u4ee5\u6709\u6548\u5730\u5b58\u50a8\u9502\u79bb\u5b50\u5e76\u53ef\u4ee5\u76f8\u4e92\u4f5c\u7528\uff0c\u534f\u540c\u63d0\u9ad8\u9502\u79bb\u5b50\u5b58\u50a8\u6027\u80fd\u3002\u9ad8\u5bfc\u7535\u77f3\u58a8\u70ef\u7eb3\u7c73\u7247\u53ef\u4ee5\u6781\u5927\u5730\u6539\u5584LVO\u7684\u53cd\u5e94\u52a8\u529b\u5b66\uff0c\u540c\u65f6\u5728LIMCs\u7684\u53c9\u6307\u7535\u6781\u4e2d\uff0c\u539f\u672c\u6613\u5806\u53e0\u4e14\u6613\u4e8e\u805a\u96c6\u7684\u77f3\u58a8\u70ef\u7247\u4e4b\u95f4\u5b58\u5728\u7740\u5206\u6563\u7684LVO\u7eb3\u7c73\u9897\u7c92\uff0c\u4f7f\u590d\u5408\u6750\u6599\u95f4\u5177\u5907\u8db3\u591f\u7684\u7a7a\u9699\uff0c\u589e\u52a0\u754c\u9762\u63a5\u89e6\u5e76\u7f29\u77ed\u9502\u79bb\u5b50\u6269\u6563\u8def\u5f84\u3002LVO\/\u77f3\u58a8\u70ef\u8d1f\u6781\u8868\u73b0\u51fa\u975e\u51e1\u7684\u500d\u7387\u6027\u80fd\u548c\u9ad8\u7535\u6d41\u5bc6\u5ea6\u7a33\u5b9a\u6027\uff0c\u572840 A g<sup>\u2212<\/sup><sup>1<\/sup>\u7684\u9ad8\u7535\u6d41\u5bc6\u5ea6\u4e0b\u53ef\u5b9e\u73b098.5 mAh g<sup>\u2212<\/sup><sup>1<\/sup>\u7684\u6bd4\u5bb9\u91cf\u3002LIMCs\u6240\u7528\u7684\u96c6\u6d41\u4f53\u548c\u975e\u5bf9\u79f0\u53c9\u6307\u7535\u6781\u5747\u53ef\u55b7\u6d82\u5236\u5907\uff0c\u8fd9\u4e3a\u5927\u89c4\u6a21\u751f\u4ea7LIMCs\u5f00\u53d1\u4e86\u4e00\u79cd\u7b80\u4fbf\u800c\u7cbe\u5bc6\u7684\u6280\u672f\u8def\u7ebf\u3002\u5355\u4e2aLIMCs\u7684\u5de5\u4f5c\u7535\u538b\u7a97\u53e3\u53ef\u8fbe4 V\uff0c\u4f53\u79ef\u80fd\u91cf\u5bc6\u5ea6\u9ad8\u8fbe51.4 mWh cm<sup>\u2212<\/sup><sup>3<\/sup>\uff0c\u529f\u7387\u5bc6\u5ea6\u9ad8\u8fbe511 mW cm<sup>\u2212<\/sup><sup>3<\/sup>\uff0c\u4e14\u5177\u6709\u4f18\u5f02\u7684\u67d4\u6027\u548c\u5faa\u73af\u7a33\u5b9a\u6027\uff0c\u5728\u7528\u4e8e\u672a\u6765\u5c0f\u578b\u5316\u3001\u67d4\u6027\u548c\u9ad8\u6027\u80fd\u7684\u50a8\u80fd\u8bbe\u5907\u65b9\u9762\u663e\u793a\u51fa\u5de8\u5927\u7684\u6f5c\u529b\u3002\u76f8\u5173\u6210\u679c\u4ee5\u201cDual Active and Kinetically Inter-Promoting Li<sub>3<\/sub>VO<sub>4\/<\/sub>Graphene Anode Enabling Printable High Energy Density Lithium Ion Micro Capacitors\u201d\u53d1\u8868\u5728\u4e86\u5728\u56fd\u9645\u9876\u5c16\u671f\u520a\u300aEnergy Storage Material\u300b\u4e0a\uff0c\u535a\u58eb\u7814\u7a76\u751f\u5f20\u6dfc\u946b\u4e3a\u672c\u6587\u7b2c\u4e00\u4f5c\u8005\u3002\u8be5\u7814\u7a76\u5de5\u4f5c\u5f97\u5230\u4e86\u5929\u6d25\u5e02\u81ea\u7136\u79d1\u5b66\u57fa\u91d1\uff0819JCYBJC17900\uff09\u548c\u6cb3\u5317\u5de5\u4e1a\u5927\u5b66\u5efa\u534e\u79d1\u7814\u57fa\u91d1\uff08No. HB1921\uff09\u7684\u8d44\u52a9\u3002<\/p>\n<p>\u5168\u6587\u94fe\u63a5\uff1ahttps:\/\/www.sciencedirect.com\/science\/article\/pii\/S2405829721004554\u00a0<\/p>\n<p><strong><b>\u4e09\u3001\u56fe\u6587\u5bfc\u8bfb<\/b><\/strong><\/p>\n<p><strong><b>\u2160. <\/b><\/strong><strong><b>LVO\/\u77f3\u58a8\u70ef\u7eb3\u7c73<\/b><\/strong><strong><b>\u590d\u5408\u6750\u6599<\/b><\/strong><strong><b>\u53caL<\/b><\/strong><strong><b>IMC<\/b><\/strong><strong><b>s<\/b><\/strong><strong><b>\u7684\u5236\u5907\u8fc7\u7a0b<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-227674\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-4-10.png\" alt=\"\" width=\"600\" height=\"372\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-4-10.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-4-10-300x186.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u56fe1. LIMCs\u7684\u5236\u5907\u793a\u610f\u56fe\uff1a(a)\u00a0ALD\u7ed3\u5408\u56fa\u6001\u70e7\u7ed3\u5236\u5907\u7684LVO\/\u77f3\u58a8\u70ef\u7eb3\u7c73\u590d\u5408\u6750\u6599\u4f5c\u4e3a\u8d1f\u6781\uff1b(b)\u00a0\u53c9\u6307\u7535\u6781\u7684\u55b7\u6d82\u548c\u57fa\u4e8e\u79bb\u5b50\u51dd\u80f6\u7535\u89e3\u8d28\u7684LIMCs\u7684\u7ec4\u88c5\uff1b(c)\u00a0AC\u4e0eMXene\u6df7\u5408\u4f5c\u4e3a\u6b63\u6781<\/p>\n<p><strong><b>\u2161<\/b><\/strong><strong><b>.<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>LVO\/\u77f3\u58a8\u70ef\u7eb3\u7c73<\/b><\/strong><strong><b>\u590d\u5408\u6750\u6599\u7684\u7ed3\u6784\u8868\u5f81<\/b><\/strong><\/p>\n<p><strong><b><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-227675\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-5-10.png\" alt=\"\" width=\"600\" height=\"473\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-5-10.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-5-10-300x237.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\u56fe2. ALD-VO-1\u548cALD-LVO-1\u6837\u54c1\u7684\u5f62\u8c8c\u7ed3\u6784\u8868\u5f81\uff1a(a)\u00a0XRD\u56fe\uff1b(b) \u62c9\u66fc\u5149\u8c31\uff1b(c) ALD-LVO-1\u7684V2p\u7684XPS\u8c31\uff1b(d) N<sub>2<\/sub>\u5438\u9644\/\u89e3\u6790\u7b49\u6e29\u7ebf\uff1b(e) ALD-VO-1\u7684TEM\u56fe\u50cf\uff0c\u63d2\u56fe\uff1a\u9009\u533a\u7535\u5b50\u884d\u5c04\u7ed3\u679c\uff1b(f) C\u3001O\u3001V \u7684EDS\u56fe\u50cf\uff1b(g, h) ALD-LVO-1\u7684TEM\u56fe\u50cf\uff0c\u63d2\u56fe\uff1a\u9009\u533a\u7535\u5b50\u884d\u5c04\u7ed3\u679c\uff1b(i) C\u3001O\u3001V \u7684\u7684EDS\u56fe\u50cf<\/p>\n<p><strong><b>\u2162.<\/b><\/strong>\u00a0<strong><b>LVO\/\u77f3\u58a8\u70ef\u7eb3\u7c73<\/b><\/strong><strong><b>\u590d\u5408\u6750\u6599\u7684<\/b><\/strong><strong><b>\u50a8\u9502<\/b><\/strong><strong><b>\u6027\u80fd<\/b><\/strong><strong><b>\u8bc4\u4ef7<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-227676\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-6-6.png\" alt=\"\" width=\"600\" height=\"404\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-6-6.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-6-6-300x202.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\u56fe3. \u7ebd\u6263\u5f0f\u534a\u7535\u6c60\u7684\u7535\u5316\u5b66\u6027\u80fd\u548c\u52a8\u529b\u5b66\u5206\u6790\uff1a(a) \u8d28\u91cf\u6bd4\u500d\u7387\u6027\u80fd\uff1b(b) \u5728\u8d28\u91cf\u500d\u7387\u6027\u80fd\u65b9\u9762\u4e0e\u5176\u4ed6\u5df2\u53d1\u8868\u7684\u5de5\u4f5c\u6bd4\u8f83\uff1b(c) \u4f53\u79ef\u6bd4\u500d\u7387\u6027\u80fd\uff1b(d) 0.2 mV s<sup>\u22121<\/sup>\u626b\u63cf\u901f\u7387\u4e0bCV\u66f2\u7ebf\u7684\u7535\u5bb9\u8d21\u732e\uff1b(e) \u5728\u4e0d\u540c\u626b\u63cf\u901f\u7387\u4e0b\u7684\u7535\u5bb9\u8d21\u732e\u7387\uff1b(f) \u5faa\u73af\u6027\u80fd\u548c\u5e93\u4ed1\u6548\u7387\uff1b(g) \u539f\u4f4dXRD\u56fe\uff1b\u00a0(h) \u975e\u539f\u4f4d\u62c9\u66fc\u5149\u8c31\u548c(i)\u76f8\u5e94\u7684\u00a0I<sub>D<\/sub>\/I<sub>G<\/sub>\u6bd4<\/p>\n<p><strong><b>\u2163<\/b><\/strong><strong><b>.<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>\u6263\u5f0f\u9502\u79bb\u5b50<\/b><\/strong><strong><b>\u7535\u5bb9\u5668<\/b><\/strong><strong><b>\u7684<\/b><\/strong><strong><b>\u6027\u80fd<\/b><\/strong><strong><b>\u4f18\u5316<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-227677\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-7-2.png\" alt=\"\" width=\"600\" height=\"673\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-7-2.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-7-2-267x300.png 267w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\u56fe4. \u57fa\u4e8eAC\u6b63\u6781\u548cALD-LVO-1\u8d1f\u6781\u7684LICs\u7684\u7535\u5316\u5b66\u6027\u80fd\u4f18\u5316\uff1a(a) LICs\u7684\u793a\u610f\u56fe\uff1b(b) 0.2 mA g<sup>\u22121<\/sup>\u00a0\u7535\u6d41\u5bc6\u5ea6\u4e0b\u6b63\u6781\u3001\u8d1f\u6781\u548cLICs\u7684GCD\u66f2\u7ebf\u6bd4\u8f83\uff1b(c) LICs\u7684GCD\u66f2\u7ebf\uff1b (e) Ragone\u56fe\uff1b(f) \u7535\u6d41\u5bc6\u5ea6\u4e3a 1 A g<sup>\u22121<\/sup>\u65f6\u7684\u5faa\u73af\u6027\u80fd\u548c\u5e93\u4ed1\u6548\u7387<\/p>\n<p><strong>\u2164. <b>\u9502\u79bb\u5b50\u5fae<\/b><\/strong><strong><b>\u7535\u5bb9\u5668<\/b><\/strong><strong><b>\u7684<\/b><\/strong><strong><b>\u6027\u80fd<\/b><\/strong><strong><b>\u8bc4\u4ef7<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-227678\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-10-1.png\" alt=\"\" width=\"600\" height=\"536\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-10-1.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/09\/\u56fe\u7247-10-1-300x268.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\u56fe5. LIMCs \u7684\u7535\u5316\u5b66\u6027\u80fd\uff1a\uff08a\uff09LIMCs \u7684\u7167\u7247\uff1b(b) \u55b7\u5370\u53c9\u6307\u7535\u6781\u7684SEM\u56fe\u50cf\uff1b(c, d) \u8d1f\u6781\u548c\u6b63\u6781\u4fef\u89c6\u56fe\u7684SEM\u56fe\u50cf\uff1b(e) \u4e0d\u540c\u626b\u63cf\u901f\u7387\u4e0b\u7684CV\u66f2\u7ebf\uff1b(f) 2\u4e2a\u4e32\u8054\u6216\u5e76\u8054\u7684LIMCs\u57285 mV s<sup>\u22121<\/sup>\u626b\u63cf\u901f\u7387\u4e0b\u7684CV\u66f2\u7ebf\uff1b(g) 2\u4e2aLIMCs\u4e32\u8054\u7684GCD\u66f2\u7ebf\uff1b(h)\u00a0\u7535\u6d41\u5bc6\u5ea6\u4e3a0.02 mA cm<sup>\u22122<\/sup>\u00a0\u65f6\u7684\u5faa\u73af\u6027\u80fd\u548c\u5e93\u4ed1\u6548\u7387\uff1b(i) \u5728\u4e0d\u540c\u5f2f\u66f2\u89d2\u5ea6\u4e0b\u6d4b\u91cf\u7684LIMCs\u7684CV\u66f2\u7ebf\uff0c\u63d2\u56fe\uff1a\u5f2f\u66f2LIMCs\u7684\u7167\u7247\uff1b(j) Ragone\u56fe\uff1b(k) \u75312\u4e2aLIMCs\u4e32\u8054\u4e3a\u67d4\u6027\u6570\u5b57\u624b\u8868\u4f9b\u7535\u7684\u7167\u7247\u3002<\/p>\n<p>Miaoxin Zhang, Ruijun Bai, Shane King, Fuxing Yin, Huifen Peng*, Gongkai Wang*, Dual Active and Kinetically Inter-Promoting Li<sub>3<\/sub>VO<sub>4<\/sub>\/Graphene Anode Enabling Printable High Energy Density Lithium Ion Micro Capacitors,<\/p>\n<p>Energy Storage Materials, https:\/\/www.sciencedirect.com\/science\/article\/pii\/S2405829721004554.<\/p>\n<p>\u672c\u6587\u7531\u4f5c\u8005\u6295\u7a3f\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u4e00\u3001\u7814\u7a76\u80cc\u666f \u968f\u77405G\u3001\u7269\u8054\u7f51\u3001\u4eba\u5de5\u667a\u80fd\u3001\u533b\u7597\u4fdd\u5065\u8bbe\u5907\u7684\u98de\u901f\u53d1\u5c55\uff0c\u53ef\u7a7f\u6234\u5fae\u578b\u7535\u5b50\u8bbe\u5907\u7684\u5e02\u573a\u9700\u6c42\u4e0d\u65ad\u589e\u957f\uff0c\u8fd9\u4e5f\u8981\u6c42\u5176\u5185\u7f6e\u7535\u6e90\u9700\u8981\u5411\u5fae\u578b\u5316\u53d1\u5c55\u3002\u5fae\u578b\u7535\u5bb9\u5668\uff08MSCs&#8230;<\/p>\n","protected":false},"author":11454,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-227673","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/227673"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/11454"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=227673"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/227673\/revisions"}],"predecessor-version":[{"id":227680,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/227673\/revisions\/227680"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=227673"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=227673"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=227673"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}