{"id":229247,"date":"2021-11-07T06:30:39","date_gmt":"2021-11-06T22:30:39","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=229247"},"modified":"2021-11-06T22:01:13","modified_gmt":"2021-11-06T14:01:13","slug":"%e3%80%90%e5%b7%b2%e6%a0%a1%e7%a8%bf%e3%80%91nat-energy%e5%8f%8c%e5%b1%82%e7%a6%bb%e8%81%9a%e7%89%a9%e4%b8%baco2%e8%bf%98%e5%8e%9f%e5%ae%9a%e5%88%b6%e5%82%ac%e5%8c%96%e5%89%82%e5%be%ae%e7%8e%af","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=229247","title":{"rendered":"Nat. Energy:\u53cc\u5c42\u79bb\u805a\u7269\u4e3aCO2\u8fd8\u539f\u5b9a\u5236\u50ac\u5316\u5242\u5fae\u73af\u5883"},"content":{"rendered":"<p><strong><b>\u3010\u5f15\u8a00\u3011<\/b><\/strong><\/p>\n<p>\u7814\u7a76\u8868\u660e\uff0c\u4f7f\u7528\u6765\u81ea\u53ef\u518d\u751f\u80fd\u6e90\uff08\u4f8b\u5982\u98ce\u80fd\u548c\u592a\u9633\u80fd\uff09\u7684\u7535\u529b\u5bf9H<sub>2<\/sub>O\u548cCO<sub>2<\/sub>\u8fdb\u884c\u7535\u5316\u5b66\u8f6c\u5316\uff0c\u4e3a\u5c06CO<sub>2<\/sub>\u8f6c\u5316\u4e3a\u5177\u6709\u9644\u52a0\u503c\u7684\u5316\u5b66\u54c1\u548c\u71c3\u6599\u63d0\u4f9b\u4e86\u4e00\u6761\u53ef\u6301\u7eed\u7684\u9014\u5f84\u3002\u5176\u4e2d\uff0c\u7535\u5316\u5b66\u4e8c\u6c27\u5316\u78b3\u8fd8\u539f (CO<sub>2<\/sub>R) \u4e3a\u71c3\u6599\u548c\u5316\u5b66\u54c1\u7684\u53ef\u6301\u7eed\u751f\u4ea7\u63d0\u4f9b\u4e86\u53ef\u80fd\u3002\u94dc (Cu) \u50ac\u5316\u5242\u5c06CO<sub>2<\/sub>R\u50ac\u5316\u4e3a\u6709\u4ef7\u503c\u7684\u591a\u78b3 (C<sub>2+<\/sub>\u00a0) \u4ea7\u7269\uff0c\u4f46\u5176\u9009\u62e9\u6027\u53d6\u51b3\u4e8e\u50ac\u5316\u5242\u8868\u9762\u9644\u8fd1\u7684\u5c40\u90e8\u5fae\u73af\u5883\u3002\u6700\u8fd1\u7684\u7814\u7a76\u5df2\u7ecf\u8868\u660e\uff0c\u901a\u8fc7\u5728\u94dc\u8868\u9762\u5f15\u5165\u6709\u673a\u5316\u5408\u7269\uff0c\u80fd\u591f\u8fdb\u4e00\u6b65\u63d0\u9ad8\u94dc\u5bf9CO<sub>2<\/sub>R\u7684\u6d3b\u6027\u548c\u9009\u62e9\u6027\u3002\u8fd9\u4e9b\u7814\u7a76\u5c06\u6539\u8fdb\u7684\u9009\u62e9\u6027\u5f52\u56e0\u4e8e\u6709\u673a\u5c42\u589e\u52a0\u7684\u758f\u6c34\u6027\u548c\/\u6216\u5bf9CO<sub>2<\/sub>\u4eb2\u548c\u529b\uff0c\u4ece\u800c\u63d0\u9ad8\u4e86\u50ac\u5316\u5242\u8868\u9762\u7684CO<sub>2<\/sub>\/H<sub>2<\/sub>O\u6bd4\u3002\u79bb\u5b50\u5bfc\u7535\u805a\u5408\u7269\uff08\u79bb\u805a\u7269\uff09\u53ef\u4ee5\u6539\u53d8\u5176\u5c40\u90e8\u6d53\u5ea6\uff0c\u4ee5\u53ca\u5728\u4fa7\u94fe\u7684\u7aef\u90e8\u90e8\u5206\u8c03\u8282\u79bb\u5b50\u8f93\u9001\u3002\u7136\u800c\uff0c\u4eba\u4eec\u5bf9\u79bb\u805a\u7269\u5bf9CO<sub>2<\/sub>R\u7684\u5f71\u54cd\u77e5\u4e4b\u751a\u5c11\u3002\u5230\u76ee\u524d\u4e3a\u6b62\uff0c\u5927\u591a\u6570\u7814\u7a76\u5df2\u7ecf\u7ecf\u9a8c\u6027\u7684\u548c\u5df2\u7ecf\u7ed9\u51fa\u4e86\u79bb\u805a\u7269\u819c\u662f\u5982\u4f55\u5f71\u54cdCO<sub>2<\/sub>R\u4e0d\u4e00\u81f4\u89e3\u91ca\u3002<\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u7f8e\u56fd\u52a0\u5dde\u5927\u5b66\u4f2f\u514b\u5229\u5206\u6821<\/strong><strong>Alexis T. Bell\u200a<\/strong><strong>\u6559\u6388<\/strong><strong>\uff08<\/strong><strong>\u5171\u540c<\/strong><strong>\u901a\u8baf\u4f5c\u8005\uff09<\/strong>\u4f7f\u7528\u53cc\u5c42\u9633\u79bb\u5b50\u548c\u9634\u79bb\u5b50\u5bfc\u7535\u79bb\u805a\u7269\u6d82\u5c42\u5206\u522b\u63a7\u5236\u5c40\u90e8 pH\u503c\uff08\u901a\u8fc7Donnan\u6392\u65a5\uff09\u548cCO<sub>2<\/sub>\/H<sub>2<\/sub>O\u6bd4\uff08\u901a\u8fc7\u79bb\u805a\u7269\u7279\u6027\uff09\uff0c\u7cfb\u7edf\u5730\u63a2\u7d22\u548c\u4f18\u5316\u8fd9\u79cd\u5fae\u73af\u5883\u3002\u540c\u65f6\uff0c\u8bc1\u660e\u4e86\u79bb\u805a\u7269\u5c42\u53ef\u7528\u4e8e\u4e3aCu\u57fa\u50ac\u5316\u5242\u4e0a\u7684\u9009\u62e9\u6027C<sub>2+<\/sub>\u751f\u6210\u521b\u9020\u6709\u5229\u7684\u5fae\u73af\u5883\u3002\u4e3a\u4e86\u5145\u5206\u9610\u660e\u79bb\u805a\u7269\u5bf9\u5c40\u90e8Cu\u50ac\u5316\u5242\u5fae\u73af\u5883\u7684\u5f71\u54cd\uff0c\u4f5c\u8005\u7ed3\u5408\u4e86\u5bf9\u4e0d\u540c\u79bb\u805a\u7269\u8584\u819c\u8986\u76d6\u7684\u94dc\u7684\u7cfb\u7edf\u7814\u7a76\uff0c\u786e\u5b9a\u4e86\u8fd9\u4e9b\u79bb\u805a\u7269\u8584\u819c\u7684\u7ed3\u6784-\u6027\u8d28\u5173\u7cfb\u3002\u7814\u7a76\u8868\u660e\uff0c\u5f53\u8fd9\u79cd\u5b9a\u5236\u7684\u5fae\u73af\u5883\u4e0e\u8109\u51b2\u7535\u89e3\u76f8\u7ed3\u5408\u65f6\uff0c\u8fdb\u4e00\u6b65\u63d0\u9ad8\u4e86CO<sub>2<\/sub>\/H<sub>2<\/sub>O\u548cpH\u7684\u5c40\u90e8\u6bd4\u4f8b\uff0c\u5bfc\u81f4\u9009\u62e9\u6027C<sub>2+<\/sub>\u00a0\u7684\u4ea7\u751f\uff0c\u4e0e\u9759\u6001\u7535\u89e3\u76f8\u6bd4\uff0cC<sub>2+<\/sub>\u00a0\u589e\u52a0\u4e86250%\uff0c\u5176\u6cd5\u62c9\u7b2c\u6548\u7387\u4e3a90%\uff0c\u800cH<sub>2<\/sub>\u53ea\u67094%\u3002\u8fd9\u4e9b\u7ed3\u679c\u5f3a\u8c03\u4e86\u8c03\u6574\u50ac\u5316\u5242\u5fae\u73af\u5883\u4f5c\u4e3a\u63d0\u9ad8\u7535\u5316\u5b66\u5408\u6210\u6574\u4f53\u6027\u80fd\u7684\u91cd\u8981\u6027\u3002<\/p>\n<p>\u76f8\u5173\u7814\u7a76\u6210\u679c\u4ee5\u201c<strong>Tailored catalyst microenvironments for CO<\/strong><strong><sub>2<\/sub><\/strong><strong>\u00a0electroreduction to multicarbon products on copper using bilayer ionomer coatings<\/strong>\u201d\u4e3a\u9898\u53d1\u8868\u5728<strong><em><i>Nat. <\/i><\/em><\/strong><strong><em><i>Energy<\/i><\/em><\/strong>\u4e0a\u3002<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-229248\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u5c01\u9762.jpg\" alt=\"\" width=\"600\" height=\"242\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u5c01\u9762.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u5c01\u9762-300x121.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/b><\/strong><\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>\u4e00<\/b><\/strong><strong><b>\u3001\u79bb\u805a\u7269\u6d82\u5c42<\/b><\/strong><strong><b>Cu<\/b><\/strong><strong><b>\u7684<\/b><\/strong><strong><b>\u5f62\u8c8c<\/b><\/strong><strong><b>\u548c\u6210\u5206\u5206\u6790<\/b><\/strong><strong><b><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-229249\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u56fe1.jpg\" alt=\"\" width=\"600\" height=\"494\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u56fe1.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u56fe1-300x247.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong>\uff08a-f\uff09Naf1100\/Cu\u548cSus\/Cu\u7684SEM\u56fe\u50cf\u548c\u5143\u7d20\u7ebf\u626b\u63cf\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>\u4e8c\u3001\u79bb\u805a\u7269\u6d82\u5c42Cu\u7684CO<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>R<\/b><\/strong><strong><b><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-229250\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u56fe2.jpg\" alt=\"\" width=\"600\" height=\"364\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u56fe2.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u56fe2-300x182.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\uff08a-d\uff09\u57280.1\u00a0M\u00a0CsHCO<sub>3<\/sub>\u7535\u89e3\u8d28\u5b58\u5728\u4e0b\uff0c\u4f7f\u7528Naf1100\/Cu\u3001\u88f8Cu\u3001Sus\/Cu\u548cNaf850\/Cu\u7684CO2R\u50ac\u5316\u6027\u80fd\uff1b<\/p>\n<p>\uff08e\uff09\u5728100%\u76f8\u5bf9\u6e7f\u5ea6\u4e0b\u6d4b\u91cf\u79bb\u5b50\u5355\u4f53\u6d82\u5c42Cu\u7684\u6c34\u6d53\u5ea6\uff1b<\/p>\n<p>\uff08f\uff09\u6839\u636e\u6d4b\u91cf\u7684\u6c34\u6d53\u5ea6\u4f30\u7b97\u5c40\u90e8CO<sub>2<\/sub>\/H<sub>2<\/sub>O\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>\u4e09<\/b><\/strong><strong><b>\u3001\u79bb\u805a\u7269\u6d82\u8986Cu<\/b><\/strong><strong><b>\u4e2d<\/b><\/strong><strong><b>\u9633\u79bb\u5b50\u5bf9CO<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>R\u7684\u5f71\u54cd<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-229251\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u56fe3.jpg\" alt=\"\" width=\"600\" height=\"378\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u56fe3.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u56fe3-300x189.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a-d\uff09\u57280.1 M LiHCO<sub>3<\/sub>\u7535\u89e3\u8d28\u5b58\u5728\u4e0b\uff0c\u4f7f\u7528Naf1100\/Cu\u3001\u88f8Cu\u3001Sus\/Cu\u548cNaf850\/Cu\u7684CO<sub>2<\/sub>R\u50ac\u5316\u6027\u80fd\uff1b<\/p>\n<p>\uff08e\uff09\u5728100%\u76f8\u5bf9\u6e7f\u5ea6\u4e0b\u6d4b\u91cf\u79bb\u805a\u7269\u6d82\u5c42Cu\u7684\u6c34\u6d53\u5ea6\uff1b<\/p>\n<p>\uff08f\uff09\u6839\u636e\u6d4b\u91cf\u7684\u6c34\u6d53\u5ea6\u4f30\u7b97\u5c40\u90e8CO<sub>2<\/sub>\/H<sub>2<\/sub>O\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>\u56db<\/b><\/strong><strong><b>\u3001\u5806\u53e0\u79bb\u805a\u7269\u5c42\u7684\u6548\u679c<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-229252\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u56fe4.jpg\" alt=\"\" width=\"600\" height=\"537\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u56fe4.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u56fe4-300x269.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u57280.1 M CsHCO<sub>3<\/sub>\u7535\u89e3\u8d28\u7684\u5b58\u5728\u4e0b\uff0c\u5728\u22121.15V\u4f7f\u7528\u5806\u53e0\u79bb\u805a\u7269\u5728Cu\u4e0a\u7684CO<sub>2<\/sub>R\u6027\u80fd\uff1b<\/p>\n<p>\uff08b\uff09\u79bb\u805a\u7269\u6d82\u5c42Cu\u7684H<sub>2<\/sub>\u3001C<sub>1<\/sub>\u548cC<sub>2+<\/sub>\u5f62\u6210\u8d8b\u52bf\uff1b<\/p>\n<p>\uff08c\uff09\u5728\u5c40\u90e8CO<sub>2<\/sub>\/H<sub>2<\/sub>O\u6bd4\uff08\u65e0\u91cf\u7eb2\uff09\u548c\u7a7a\u95f4\u7535\u8377\u914d\u7f6e\u65b9\u9762\u7684Naf850\/Sus\/Cu\uff08\u9876\u90e8\uff09\u548cSus\/Naf850\/Cu\uff08\u5e95\u90e8\uff09\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>\u4e94<\/b><\/strong><strong><b>\u3001\u4f7f\u7528\u79bb\u805a\u7269\u589e\u5f3a<\/b><\/strong><strong>CO<\/strong><strong><sub>2<\/sub><\/strong><strong>R<\/strong><strong><b>\u7684\u793a\u610f\u56fe<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-229253\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u56fe5.jpg\" alt=\"\" width=\"600\" height=\"383\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u56fe5.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u56fe5-300x192.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a-d\uff09\u5728Cu\u50ac\u5316\u5242\u5b58\u5728\u4e0b\u53d1\u751fCO<sub>2<\/sub>R\u7684\u5bf9\u6bd4\uff0c\u968f\u7740AEI\u5c42\u7684\u52a0\u5165\u589e\u52a0\u4e86\u5c40\u90e8CO<sub>2<\/sub>\/H<sub>2<\/sub>O\u6bd4\u503c\uff0c\u5728AEI\u4e0a\u589e\u52a0\u4e86CEI\u5c42\uff0c\u4ece\u800c\u5f62\u6210\u53cc\u5c42\u5c40\u90e8\u73af\u5883\u5e76\u8c03\u8282\u5c40\u90e8\u6c22\u6c27\u5316\u7269\uff0c\u5e76\u4e14\u8109\u51b2\u7535\u89e3\u8fdb\u4e00\u6b65\u589e\u5f3a\u4e86C<sub>2+<\/sub>\u4ea7\u7269\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>\u516d<\/b><\/strong><strong><b>\u3001\u79bb\u805a\u7269\u5c42\u548c\u8109\u51b2CO<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>\u7535\u89e3\u7684\u5fae\u73af\u5883\u4e4b\u95f4\u7684\u534f\u540c\u4f5c\u7528<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-229254\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u56fe6.jpg\" alt=\"\" width=\"600\" height=\"197\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u56fe6.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/\u56fe6-300x99.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a\uff09\u4f7f\u7528\u5404\u79cd\u79bb\u805a\u7269\u6d82\u8986\u7684Cu\u50ac\u5316\u5242\u7684\u8109\u51b2CO<sub>2<\/sub>\u7535\u89e3\u7684\u6cd5\u62c9\u7b2c\u6548\u7387\uff1b<\/p>\n<p>\uff08b\uff09\u5728\u5404\u79cd\u6761\u4ef6\u548c\u914d\u7f6e\u4e0b\u83b7\u5f97\u7684\u5c40\u90e8\u7535\u6d41\u5bc6\u5ea6\u3002<\/p>\n<p><strong><b>\u3010\u5c0f\u7ed3\u3011<\/b><\/strong><\/p>\n<p>\u7efc\u4e0a\u6240\u8ff0\uff0c\u8fd9\u9879\u5de5\u4f5c\u6e05\u695a\u5730\u8868\u660e\uff0c\u53ef\u4ee5\u901a\u8fc7\u4f7f\u7528\u4e0d\u540c\u7684\u9634\u79bb\u5b50\u548c\u9633\u79bb\u5b50\u5bfc\u7535\u79bb\u805a\u7269\u5c42\uff08\u5373\u53cc\u5c42\u8584\u819c\uff09\u8c03\u6574Cu CO<sub>2<\/sub>R\u50ac\u5316\u5242\u8868\u9762\u9644\u8fd1\u7684\u5316\u5b66\u5fae\u73af\u5883\u6765\u8c03\u8282Cu \u5bf9CO<sub>2<\/sub>R\u7684\u6d3b\u6027\u548c\u9009\u62e9\u6027\u3002\u540c\u65f6\uff0c\u53ef\u4ee5\u901a\u8fc7\u8109\u51b2\u7535\u89e3\u8fdb\u4e00\u6b65\u6539\u53d8\u8868\u9762\u5fae\u73af\u5883\uff0c\u4ee5\u5b9e\u73b090% \u7684C<sub>2+<\/sub>\u00a0FE\u548c4% \u7684H<sub>2<\/sub>\u00a0FE\u3002\u6b63\u5982\u6240\u8ba8\u8bba\u7684\uff0c\u8fd9\u4e9b\u53d8\u5316\u662f\u901a\u8fc7\u4f7f\u7528\u79bb\u5b50\u7b5b\u9009\u548c\u56fa\u6709\u79bb\u805a\u7269\u7279\u6027\u5bf9pH\u503c\u548c\u5c40\u90e8H<sub>2<\/sub>O\u548cCO<sub>2<\/sub>\u6d53\u5ea6\u5728Cu\u8868\u9762\u9644\u8fd1\u7684\u7b56\u7565\u63a7\u5236\u6765\u5b9e\u73b0\u7684\uff0c\u9634\u79bb\u5b50\u4ea4\u6362\u79bb\u805a\u7269\u8868\u73b0\u51fa\u589e\u52a0\u7684CO<sub>2<\/sub>\u6eb6\u89e3\u5ea6\uff0c\u9633\u79bb\u5b50\u4ea4\u6362\u79bb\u805a\u7269\u901a\u8fc7OH<sup>&#8211;<\/sup>\u6355\u83b7\u589e\u52a0\u5c40\u90e8pH\u503c\uff0c\u5e76\u4e14\u4e24\u5c42\u90fd\u4f1a\u5f71\u54cd\u6574\u4f53\u6c34\u6d53\u5ea6\u3002\u590d\u5408\u79bb\u805a\u7269\u5c42\u7684\u5408\u7406\u8bbe\u8ba1\u548c\u5b9e\u65bd\u5177\u6709\u5e7f\u6cdb\u7684\u9002\u7528\u6027\uff0c\u5e76\u53ef\u76f4\u63a5\u8f6c\u5316\u4e3a\u5176\u4ed6\u7535\u5316\u5b66\u5408\u6210\uff0c\u5176\u4f4e\u53cd\u5e94\u7269\u6eb6\u89e3\u5ea6\u548c\u590d\u6742\u7684pH\u51b3\u5b9a\u4e86\u4ea7\u54c1\u9009\u62e9\u6027\uff0c\u4ece\u800c\u4f7f\u9009\u62e9\u6027\u5408\u6210\u9014\u5f84\u6210\u4e3a\u53ef\u80fd\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a\u201c<\/strong><a href=\"https:\/\/www.nature.com\/articles\/s41560-021-00920-8\"><strong><u>Tailored catalyst microenvironments for CO<\/u><\/strong><strong><u><sub>2<\/sub><\/u><\/strong><strong><u>\u00a0electroreduction to multicarbon products on copper using bilayer ionomer coatings<\/u><\/strong><\/a><strong>\u201d(<\/strong><strong><em><i>Nat. <\/i><\/em><\/strong><strong><em><i>Energy<\/i><\/em><\/strong><strong><b>\uff0c<\/b><\/strong><strong>202<\/strong><strong>1<\/strong><strong>\uff0c<\/strong><strong>10.1038\/s41560-021-00920-8<\/strong><strong>)<\/strong><\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4ebaCYM\u7f16\u8bd1\u4f9b\u7a3f\u3002\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n<p>\u6750\u6599\u4eba\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaokefu \u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u7814\u7a76\u8868\u660e\uff0c\u4f7f\u7528\u6765\u81ea\u53ef\u518d\u751f\u80fd\u6e90\uff08\u4f8b\u5982\u98ce\u80fd\u548c\u592a\u9633\u80fd\uff09\u7684\u7535\u529b\u5bf9H2O\u548cCO2\u8fdb\u884c\u7535\u5316\u5b66\u8f6c\u5316\uff0c\u4e3a\u5c06CO2\u8f6c\u5316\u4e3a\u5177\u6709\u9644\u52a0\u503c\u7684\u5316\u5b66\u54c1\u548c\u71c3\u6599\u63d0\u4f9b\u4e86\u4e00\u6761\u53ef\u6301\u7eed\u7684\u9014\u5f84\u3002&#8230;<\/p>\n","protected":false},"author":9629,"featured_media":229248,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[116],"class_list":["post-229247","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","tag-catalyst"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/229247"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/9629"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=229247"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/229247\/revisions"}],"predecessor-version":[{"id":229301,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/229247\/revisions\/229301"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/229248"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=229247"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=229247"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=229247"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}