{"id":229399,"date":"2021-11-10T12:00:42","date_gmt":"2021-11-10T04:00:42","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=229399"},"modified":"2021-11-10T11:42:58","modified_gmt":"2021-11-10T03:42:58","slug":"%e5%8c%97%e5%8d%a1%e5%a4%a7%e5%ad%a6%e6%95%99%e5%a0%82%e5%b1%b1%e5%88%86%e6%a0%a1%e9%bb%84%e5%8a%b2%e6%9d%be%e5%9b%a2%e9%98%9fsci-adv-%ef%bc%9a%e5%90%b8%e9%93%85%e7%a6%bb%e5%ad%90%e5%87%9d%e8%83%b6","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=229399","title":{"rendered":"\u5317\u5361\u5927\u5b66\u6559\u5802\u5c71\u5206\u6821\u9ec4\u52b2\u677e\u56e2\u961fSci. Adv.\uff1a\u5438\u94c5\u79bb\u5b50\u51dd\u80f6\u7528\u4e8e\u8010\u51b2\u51fb\u3001\u7a33\u5b9a\u548c\u94c5\u5b89\u5168\u7684\u9499\u949b\u77ff\u6a21\u5757"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u91d1\u5c5e\u5364\u5316\u9499\u949b\u77ff\u5728\u4e0b\u4e00\u4ee3\u4f4e\u6210\u672c\u9ad8\u6548\u592a\u9633\u80fd\u7535\u6c60\u4e2d\u663e\u793a\u51fa\u5de8\u5927\u7684\u6f5c\u529b\u3002\u5355\u7ed3\u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60\uff08PSCs\uff09\u7684\u8ba4\u8bc1\u529f\u7387\u8f6c\u6362\u6548\u7387\uff08PCEs\uff09\u5df2\u7ecf\u8d85\u8fc725%\uff0c\u9499\u949b\u77ff\/\u7845\u4e32\u8054\u592a\u9633\u80fd\u7535\u6c60\u7684PCEs\u5df2\u7ecf\u8d85\u8fc729%\u3002\u540c\u65f6\uff0c\u5927\u9762\u79ef\u9499\u949b\u77ff\u6a21\u5757\u7684\u8ba4\u8bc1\u6548\u7387\u8fbe\u523018.6%\uff08\u9762\u79ef\u4e3a30\u81f360 cm<sup>2<\/sup>\uff09\uff0c\u4e0e\u5546\u4e1a\u5316\u7684\u7845\u6a21\u5757\u76f8\u5f53\u3002\u8fd9\u8868\u660ePCE\u4e0d\u518d\u662f\u9499\u949b\u77ff\u5149\u4f0f\u5546\u4e1a\u5316\u7684\u5173\u952e\u95ee\u9898\u3002\u7136\u800c\uff0c\u7531\u4e8e\u9499\u949b\u77ff\u542b\u6c34\u6eb6\u6027\u94c5\u53ef\u80fd\u5bf9\u571f\u58e4\u548c\u5730\u4e0b\u6c34\u8d44\u6e90\u9020\u6210\u5de8\u5927\u7684\u6f5c\u5728\u6c61\u67d3\uff0c\u5176\u5b9e\u9645\u5e94\u7528\u53d7\u5230\u4e86\u5f88\u5927\u7684\u963b\u788d\u3002\u4e00\u79cd\u76f4\u89c2\u7684\u65b9\u6cd5\u662f\u7528\u65e0\u6bd2\u6210\u5206\u66ff\u4ee3\u94c5\u9499\u949b\u77ff\uff0c\u5982\u9521\uff08Sn\uff09\u9499\u949b\u77ff\u6216\u53cc\u9499\u949b\u77ff\u3002\u7136\u800c\uff0c\u9521\u57faPSCs\u7a33\u5b9a\u6027\u8f83\u5dee\uff0c\u56e0\u4e3aSn<sup>2+<\/sup>\u5f88\u5bb9\u6613\u88ab\u6c27\u5316\u4e3aSn<sup>4+<\/sup>\uff0c\u751a\u81f3\u5bb9\u6613\u88ab\u5904\u7406\u9521\u9499\u949b\u77ff\u7684\u6eb6\u5242\u6240\u6c27\u5316\uff0c\u800c\u53cc\u9499\u949b\u77ff\u8bbe\u5907\u7684PCEs\u592a\u5c0f\uff0c\u4e0d\u80fd\u88ab\u8ba4\u4e3a\u662f\u6709\u7528\u7684\u3002\u5c3d\u7ba1\u542b\u94c5\u9499\u949b\u77ff\u5b58\u5728\u7f3a\u9677\uff0c\u4f46\u4ecd\u662f\u5b9e\u73b0\u9ad8\u6548\u7a33\u5b9a\u7684\u9499\u949b\u77ff\u592a\u9633\u80fd\u6a21\u5757\u7684\u9996\u9009\u3002\u6700\u8fd1\u5df2\u7ecf\u63a2\u7d22\u4e86\u66ff\u4ee3\u65b9\u6cd5\uff0c\u4ee5\u51cf\u5c11\u94c5\u57faPSCs\u7684\u94c5\u6cc4\u6f0f\u5230\u73af\u5883\u4e2d\u3002\u4f5c\u4e3a\u9ad8\u6548PSCs\u7684\u7ec4\u6210\u90e8\u5206\uff0c\u7535\u8377\u4f20\u8f93\u5c42\uff0c\u5982\u7a7a\u7a74\u4f20\u8f93\u5c42\u7684\u70f7\u6c27\u57fa\u805a\u56db\u4e59\u4e8c\u9187\uff08PTEG\uff09\u548c\u7535\u5b50\u4f20\u8f93\u5c42\u76842D\u91d1\u5c5e\u6709\u673a\u6846\u67b6\uff0c\u81ea\u7136\u662f\u6355\u83b7\u94c5\u7684\u826f\u597d\u5019\u9009\u6750\u6599\u3002\u7136\u800c\uff0c\u7535\u8377\u4f20\u8f93\u5c42\u901a\u5e38\u53ea\u670920 ~ 50 nm\u7684\u76f8\u5bf9\u8f83\u5c0f\u7684\u539a\u5ea6\uff0c\u4ee5\u5b9e\u73b0\u6709\u6548\u7684\u7535\u8377\u6536\u96c6\uff0c\u5e76\u4e0d\u80fd\u63d0\u4f9b\u8db3\u591f\u7684\u5bb9\u91cf\u6765\u5438\u9644500 ~ 1000 nm\u539a\u7684\u9499\u949b\u77ff\u5c42\u4e2d\u7684\u94c5\u79bb\u5b50\u3002\u53e6\u4e00\u79cd\u65b9\u6cd5\u662f\u7528\u7269\u7406\u5c4f\u969c\u6216\u94c5\u5438\u9644\u6750\u6599\u5305\u88f9PSCs\uff0c\u4ee5\u9632\u6b62\u94c5\u6cc4\u6f0f\u3002\u4f46\u7269\u7406\u5835\u585e\u805a\u5408\u7269\u53ea\u80fd\u51cf\u7f13\u94c5\u7684\u6cc4\u6f0f\u901f\u5ea6\u3002\u5728\u6b63\u9762\u6d82\u8986\u7684\u94c5\u5438\u9644\u5c42\u9700\u8981\u7269\u7406\u5c4f\u853d\uff1b\u5426\u5219\uff0c\u5728\u957f\u671f\u66b4\u9732\u7684\u8fc7\u7a0b\u4e2d\uff0c\u5b83\u53ef\u80fd\u4f1a\u5931\u53bb\u5176\u529f\u80fd\u3002\u5c06\u94c5\u5438\u9644\u5242\u653e\u5165\u9499\u949b\u77ff\u5c42\u5185\uff0c\u5f88\u597d\u5730\u907f\u514d\u4e86\u8fd9\u4e2a\u95ee\u9898\u3002\u53e6\u4e00\u65b9\u9762\uff0c\u5c01\u88c5\u662f\u7b5b\u9009\u73af\u5883\u523a\u6fc0\u7684\u5fc5\u8981\u6761\u4ef6\uff0c\u4ee5\u63d0\u9ad8\u592a\u9633\u80fd\u7535\u6c60\u7684\u8fd0\u884c\u7a33\u5b9a\u6027\uff0c\u8fd9\u9700\u8981\u4e00\u4e2a\u72ec\u7279\u7684\u5c42\u6765\u4fdd\u62a4\u9499\u949b\u77ff\u5668\u4ef6\u3002\u56e0\u6b64\uff0c\u9700\u8981\u4e00\u79cd\u6709\u6548\u7684\u7b56\u7565\u6765\u540c\u65f6\u89e3\u51b3\u9499\u949b\u77ff\u6a21\u5757\u4e2d\u7684\u94c5\u6bd2\u6027\u548c\u4e0d\u7a33\u5b9a\u6027\u8fd9\u4e24\u4e2a\u95ee\u9898\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c\u5728<strong><b>\u5317\u5361\u7f57\u6765\u7eb3\u5927\u5b66\u6559\u5802\u5c71\u5206\u6821\u9ec4\u52b2\u677e<\/b><\/strong><strong><b>\u6559\u6388<\/b><\/strong>\u56e2\u961f\u7b49\u4eba\u5e26\u9886\u4e0b\uff0c\u62a5\u544a\u4e86\u4e00\u79cd\u57fa\u4e8e\u94c5\u5438\u9644\u79bb\u5b50\u51dd\u80f6\u7684\u9499\u949b\u77ff\u6a21\u5757\u5c01\u88c5\u7b56\u7565\uff0c\u53ef\u4ee5\u9632\u6b62\u94c5\u6cc4\u6f0f\uff0c\u5e76\u7ecf\u5f97\u8d77\u957f\u671f\u7684\u7a33\u5b9a\u6027\u6d4b\u8bd5\u3002\u96c6\u6210\u5728\u6a21\u5757\u4e24\u4fa7\u7684\u79bb\u5b50\u51dd\u80f6\u5c42\u589e\u5f3a\u4e86\u6297\u51b2\u51fb\u6027\u3002\u81ea\u4fee\u590d\u79bb\u5b50\u51dd\u80f6\u53ef\u4ee5\u9632\u6b62\u6c34\u6e17\u5165\u9499\u949b\u77ff\u5c42\uff0c\u5438\u9644\u53ef\u80fd\u6cc4\u6f0f\u7684\u94c5\u3002\u5c01\u88c5\u7684\u5668\u4ef6\u901a\u8fc7\u6e7f\u70ed\u548c\u70ed\u5faa\u73af\u52a0\u901f\u7a33\u5b9a\u6027\u6d4b\u8bd5\uff0c\u7b26\u5408\u56fd\u9645\u7535\u5de5\u59d4\u5458\u4f1a61215\u6807\u51c6\u3002\u88ab\u51b0\u96f9\u635f\u574f\u7684\u6a21\u5757\u5728\u6c34\u4e2d\u6d78\u6ce124\u5c0f\u65f6\u540e\uff0c\u79bb\u5b50\u51dd\u80f6\u5c01\u88c5\u53ef\u5c06\u94c5\u6cc4\u6f0f\u964d\u4f4e\u5230\u65e0\u6cd5\u68c0\u6d4b\u7684\u6c34\u5e73\u3002\u5373\u4f7f\u88ab\u6c7d\u8f66\u78be\u538b\u540e\u518d\u7528\u6c34\u6d78\u6ce145\u5929\uff0c\u79bb\u5b50\u51dd\u80f6\u5c01\u88c5\u4e5f\u80fd\u5c06\u94c5\u7684\u6cc4\u6f0f\u51cf\u5c11\u4e09\u4e2a\u6570\u91cf\u7ea7\u3002\u8fd9\u9879\u5de5\u4f5c\u63d0\u4f9b\u4e86\u4e00\u4e2a\u540c\u65f6\u89e3\u51b3\u9499\u949b\u77ff\u6a21\u5757\u7684\u94c5\u6cc4\u6f0f\u548c\u7a33\u5b9a\u6027\u7684\u7b56\u7565\u3002\u8be5\u6210\u679c\u4ee5\u9898\u4e3a<strong><b>\u201cLead-adsorbing ionogel-based encapsulation for impact-resistant, stable, and lead-safe perovskite modules\u201d<\/b><\/strong>\u53d1\u8868\u5728\u4e86<strong><b>Sci. Adv.<\/b><\/strong>\u4e0a\u3002<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-229402\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/0-3.jpg\" alt=\"\" width=\"600\" height=\"198\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/0-3.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/0-3-300x99.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe<\/strong><strong>1 \u5438\u9644\u94c5\u7684\u79bb\u5b50\u51dd\u80f6<\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-229401\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/1-7.jpg\" alt=\"\" width=\"600\" height=\"287\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/1-7.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/1-7-300x144.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(A) \u79bb\u5b50\u51dd\u80f6\u5fae\u89c2\u7ed3\u6784\u548c\u94c5\u5438\u9644\u673a\u7406\u7684\u793a\u610f\u56fe\u3002<\/p>\n<p>(B) \u6709\u548c\u6ca1\u6709\u79bb\u5b50\u51dd\u80f6\uff08\u539a\u5ea6\u4e3a 500 \u03bcm\uff09\u7684\u73bb\u7483\u57fa\u677f\u7684\u900f\u5c04\u7387\u3002\u63d2\u56fe\u662f\u73bb\u7483\u57fa\u677f\uff08\u7531\u84dd\u8272\u865a\u7ebf\u8868\u793a\uff09\u4e0a\u9762\u79ef\u4e3a 15 cm*15 cm\uff08\u7531\u7ea2\u8272\u865a\u7ebf\u8868\u793a\uff09\u7684\u79bb\u5b50\u51dd\u80f6\u56fe\u50cf\u3002<\/p>\n<p>(C) \u79bb\u5b50\u51dd\u80f6\u548cPOE\u7684\u7d2b\u5916\u7a33\u5b9a\u6027\u3002<\/p>\n<p>(D) \u4e0d\u540c\u989c\u8272\u67d3\u8272\u7684\u539f\u59cb\u79bb\u5b50\u51dd\u80f6\u6837\u54c1\uff08\u5de6\u4e0a\uff09\uff1b\u5207\u5272\u6837\u54c1\uff08\u5de6\u4e2d\uff09\u5e76\u572850\u00b0C\u4e0b\u6108\u54082\u5c0f\u65f6\u7684\u56fe\u50cf\uff08\u5de6\u4e0b\uff09\uff1b\u62c9\u4f38\u6108\u5408\u6837\u54c1\u7684\u56fe\u50cf\uff08\u53f3\uff09\u3002<\/p>\n<p>(E)\u79bb\u5b50\u51dd\u80f6\u7684\u94c5\u5438\u9644\u52a8\u529b\u5b66\u3002\u63d2\u56fe\u662f\u6765\u81ea\u62df\u4e8c\u7ea7\u6a21\u578b\u7684\u52a8\u529b\u5b66\u62df\u5408\u66f2\u7ebf\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong>2 \u79bb\u5b50\u51dd\u80f6\u5c01\u88c5\u5fae\u6a21\u5757\u7684\u6027\u80fd<\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-229403\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/2-6.jpg\" alt=\"\" width=\"600\" height=\"672\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/2-6.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/2-6-268x300.jpg 268w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(A)\u5668\u4ef6\u7ed3\u6784\u3002HTL\uff0c\u7a7a\u7a74\u4f20\u8f93\u5c42\uff1b ETL\uff0c\u7535\u5b50\u4f20\u8f93\u5c42\u3002<\/p>\n<p>(B) \u79bb\u5b50\u51dd\u80f6\u5c01\u88c5\u524d\u540e\u9499\u949b\u77ff\u6a21\u5757\uff08\u9762\u79ef\u4e3a 31.5 cm<sup>2<\/sup>\uff09\u79bb\u7684I-V\u66f2\u7ebf\u3002\u63d2\u56fe\u662f\u5c01\u88c5\u6a21\u5757\u7684\u56fe\u50cf\u3002<\/p>\n<p>(C)\u79bb\u5b50\u51dd\u80f6\u5c01\u88c5\u524d\u540e\u5178\u578bPSCs\uff08\u9762\u79ef\u4e3a 0.08 mm<sup>2<\/sup>\uff09\u7684J-V\u66f2\u7ebf\u3002\u63d2\u56fe\u4e3a\u53c2\u6570\u5bf9\u6bd4\u56fe\u3002<\/p>\n<p>(D) \u79bb\u5b50\u51dd\u80f6\u5c01\u88c5\u524d\u540e32\u4e2aPSCs\u7684\u6548\u7387\u5206\u5e03\u7edf\u8ba1\u7ed3\u679c\u3002<\/p>\n<p>(E\uff0cF)\u6839\u636eIEC 61215\u6807\u51c6\uff0cPSCs\u5728DH (E)\u548c\u70ed\u5faa\u73af(F)\u6d4b\u8bd5\u671f\u95f4\u7684\u6548\u7387\u53d8\u5316\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong>3 \u91d1\u5c5e\u7403\u843d\u4e0b\u635f\u574f\u5fae\u578b\u6a21\u5757\u7684\u94c5\u6cc4\u6f0f<\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-229404\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/3-6.jpg\" alt=\"\" width=\"600\" height=\"632\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/3-6.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/3-6-285x300.jpg 285w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(A)\u4e09\u79cd\u5c01\u88c5\u7ed3\u6784\u7684\u65b9\u6848\u3002<\/p>\n<p>(B)\u635f\u574f\u7684\u5fae\u578b\u6a21\u5757\u7684\u6c34\u6d78\u6ce1\u6d4b\u8bd5\u7ed3\u679c\u3002\u63d2\u56fe\u4e3a\u7834\u788e\u6a21\u5757\u6d78\u6ce1\u5728\u53bb\u79bb\u5b50\u6c34\u4e2d\u7684\u56fe\u50cf\u3002<\/p>\n<p>(C~E)\u4e0d\u540c\u5c01\u88c5\u7ed3\u6784\u7684\u53d7\u635f\u9499\u949b\u77ff\u6a21\u5757\u5728\u53bb\u79bb\u5b50\u6c34\u4e2d\u6d78\u6ce1\u7684\u5178\u578b\u53d8\u5316\u56fe\u50cf<\/p>\n<p>\u4e0d\u540c\u5c01\u88c5\u7684\u9499\u949b\u77ff\u6a21\u5757\u5728DI\u6c34\u4e2d\u6d78\u6ce1\u7ed3\u6784A (C)\u3001B (D)\u548cC (E)\u7684\u5178\u578b\u6f14\u5316\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong>4 \u9632\u6b62\u88ab\u6c7d\u8f66\u78be\u538b\u7684\u94c5\u6cc4\u6f0f\u6d4b\u8bd5<\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-229405\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/4-5.jpg\" alt=\"\" width=\"600\" height=\"677\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/4-5.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/11\/4-5-266x300.jpg 266w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(A)\u6c7d\u8f66\u5728\u5c01\u88c5\u7684\u9499\u949b\u77ff\u8584\u819c\u4e0a\u6eda\u52a8\u7684\u56fe\u50cf\u3002<\/p>\n<p>(B)\u7834\u788e\u9499\u949b\u77ff\u8584\u819c\u7684\u6c34\u6d78\u6ce1\u6d4b\u8bd5\u7ed3\u679c\u3002<\/p>\n<p>(C~E) \u7ed3\u6784\u4e3aA (C)\u3001B (D)\u3001C (E)\u7684\u53d7\u635f\u9499\u949b\u77ff\u8584\u819c\u5728\u53bb\u79bb\u5b50\u6c34\u4e2d\u6d78\u6ce1\u540e\u7684\u53d8\u5316\u56fe\u50cf\u3002<\/p>\n<p><strong><b>\u3010\u5c0f\u7ed3\u3011<\/b><\/strong><\/p>\n<p>\u7efc\u4e0a\u6240\u8ff0\uff0c\u56e2\u961f\u62a5\u544a\u4e86\u4e00\u79cd\u8010\u51b2\u51fb\u7684\u3001\u81ea\u4fee\u590d\u7684\u3001\u53ef\u5438\u9644\u94c5\u7684\u79bb\u5b50\u51dd\u80f6\uff0c\u5c06\u88ab\u7eb3\u5165\u9499\u949b\u77ff\u592a\u9633\u80fd\u6a21\u5757\u5c01\u88c5\u4e2d\uff0c\u540c\u65f6\u51cf\u5c11\u94c5\u6cc4\u6f0f\uff0c\u63d0\u9ad8\u5668\u4ef6\u7684\u7a33\u5b9a\u6027\u3002\u79bb\u5b50\u51dd\u80f6\u5c01\u88c5\u7684PSCs\u5177\u6709\u9ad8\u6548\u7684\u517c\u5bb9\u6027\uff08\u5fae\u578b\u6a21\u5757\u7684PCE\u4e3a18.5%\uff0c\u5c0f\u7535\u6c60\u7684PCE\u4e3a22.9%\uff09\uff0c\u5e76\u5177\u6709\u4ee4\u4f18\u5f02\u7684\u957f\u671f\u7a33\u5b9a\u6027\uff08\u5728DH\u548c\u70ed\u5faa\u73af\u6d4b\u8bd5\u540e\uff0c\u76f8\u5bf9\u6548\u7387\u635f\u5931\u5c0f\u4e8e5%\uff09\u3002\u79bb\u5b50\u51dd\u80f6\u7684\u63ba\u5165\u53ef\u4ee5\u660e\u663e\u6291\u5236\u9499\u949b\u77ff\u6a21\u5757\u7684\u94c5\u6cc4\u6f0f\u3002\u5728\u6a21\u62df\u51b0\u96f9\u6d4b\u8bd5\u540e\uff0c\u7ecf\u8fc724\u5c0f\u65f6\u7684\u6c34\u6d78\u6ce1\uff0c\u65e0\u6cd5\u68c0\u6d4b\u5230\u7684\u94c5\uff08&lt;1 ppb\uff09\u53ef\u80fd\u4f1a\u4ece\u635f\u574f\u7684\u9499\u949b\u77ff\u6a21\u5757\u4e2d\u6f0f\u51fa\u3002\u5373\u4f7f\u5728\u6781\u7aef\u6761\u4ef6\u4e0b\uff0c\u5982\u88ab\u6c7d\u8f66\u78be\u538b\uff0c\u8fd9\u79cd\u575a\u56fa\u7684\u79bb\u5b50\u51dd\u80f6\u5c42\u5c01\u88c5\u4ecd\u80fd\u4fdd\u6301\u5b8c\u6574\uff0c\u5e76\u4f5c\u4e3a\u8fc7\u6ee4\u5c42\u6291\u5236\u94c5\u6cc4\u6f0f\uff0c\u6bd4\u6807\u51c6\u73bb\u7483\u76d6\u548cPOE\u5bc6\u5c01\u80f6\u5c01\u88c5\u7684\u8bbe\u5907\u8981\u597d\u8fd13\u4e2a\u6570\u91cf\u7ea7\u3002\u8fd9\u4e9b\u7ed3\u679c\u5c06\u52a0\u901f\u9499\u949b\u77ff\u592a\u9633\u80fd\u6280\u672f\u5728\u73b0\u5b9e\u4e16\u754c\u7684\u5e94\u7528\u3002<\/p>\n<p><strong><b>\u6587\u732e\u94fe\u63a5<\/b><\/strong>\uff1a<a href=\"https:\/\/www.science.org\/doi\/10.1126\/sciadv.abi8249\"><u>Lead-adsorbing ionogel-based encapsulation for impact-resistant, stable, and lead-safe perovskite modules<\/u><\/a>\uff08Sci. Adv.\uff0c2021\uff0cDOI\uff1a10.1126\/sciadv.abi8249\uff09<\/p>\n<p>\u672c\u6587\u7531<strong>\u6728\u6587\u97ec<\/strong>\u7ffb\u8bd1\uff0c\u6750\u6599\u725b\u6574\u7406\u7f16\u8f91\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c<u>\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com<\/u>\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u91d1\u5c5e\u5364\u5316\u9499\u949b\u77ff\u5728\u4e0b\u4e00\u4ee3\u4f4e\u6210\u672c\u9ad8\u6548\u592a\u9633\u80fd\u7535\u6c60\u4e2d\u663e\u793a\u51fa\u5de8\u5927\u7684\u6f5c\u529b\u3002\u5355\u7ed3\u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60\uff08PSCs\uff09\u7684\u8ba4\u8bc1\u529f\u7387\u8f6c\u6362\u6548\u7387\uff08PCEs\uff09\u5df2\u7ecf\u8d85\u8fc725%\uff0c\u9499\u949b\u77ff\/\u7845&#8230;<\/p>\n","protected":false},"author":2109,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[78,4490,244],"class_list":["post-229399","post","type-post","status-publish","format-standard","hentry","category-jiedu","tag-photovoltaic","tag-4490","tag-gaitaikuang"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/229399"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/2109"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=229399"}],"version-history":[{"count":1,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/229399\/revisions"}],"predecessor-version":[{"id":229406,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/229399\/revisions\/229406"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=229399"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=229399"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=229399"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}