{"id":235203,"date":"2022-03-30T06:24:28","date_gmt":"2022-03-29T22:24:28","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=235203"},"modified":"2022-03-29T15:24:53","modified_gmt":"2022-03-29T07:24:53","slug":"%e5%86%85%e8%92%99%e5%8f%a4%e5%a4%a7%e5%ad%a6%e7%8e%8b%e5%8b%a4%e6%95%99%e6%8e%88nano-letters%ef%bc%9a%e5%85%ab%e9%9d%a2%e4%bd%93%e4%bd%8d%e6%8e%ba%e6%9d%82%e5%92%8c%e7%bc%ba%e9%99%b7%e5%b7%a5","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=235203","title":{"rendered":"\u5185\u8499\u53e4\u5927\u5b66\u738b\u52e4\u6559\u6388Nano Letters\uff1a\u516b\u9762\u4f53\u4f4d\u63ba\u6742\u548c\u7f3a\u9677\u5de5\u7a0b\u63d0\u5347\u5c16\u6676\u77f3\u7535\u50ac\u5316\u6027\u80fd"},"content":{"rendered":"<p><strong><b>\u3010\u7814\u7a76\u80cc\u666f\u3011<\/b><\/strong><\/p>\n<p>\u7535\u89e3\u6c34\u5236\u6c22\u6280\u672f\u662f\u76ee\u524d\u5de5\u4e1a\u5316\u5236\u5907\u9ad8\u7eaf\u6c22\u6c14\u7684\u91cd\u8981\u624b\u6bb5\u4e4b\u4e00\u3002\u7136\u800c\uff0c\u9633\u6781\u6790\u6c27\u53cd\u5e94\u7684\u8fc7\u7535\u4f4d\u8f83\u9ad8\u3001\u52a8\u529b\u5b66\u76f8\u5bf9\u7f13\u6162\uff0c\u9700\u8981\u9ad8\u6548\u7684\u7535\u50ac\u5316\u5242\u52a0\u901f\u8be5\u7c7b\u53cd\u5e94\u7684\u52a8\u529b\u5b66\uff0c\u4ece\u800c\u8fbe\u5230\u5728\u8f83\u5c0f\u7684\u8fc7\u7535\u4f4d\u4e0b\u83b7\u5f97\u5927\u7684\u7535\u6d41\u5bc6\u5ea6\u3002\u76ee\u524d\u5546\u4e1a\u7535\u50ac\u5316\u5242\u4ecd\u4ee5RuO<sub>2<\/sub>\u7b49\u8d35\u91d1\u5c5e\u6c27\u5316\u7269\u4e3a\u4e3b\uff0c\u4f46\u7531\u4e8e\u50a8\u91cf\u4f4e\u3001\u4ef7\u683c\u6602\u8d35\uff0c\u6781\u5927\u5730\u9650\u5236\u4e86\u5176\u5927\u89c4\u6a21\u5546\u4e1a\u5316\u5e94\u7528\u3002\u56e0\u6b64\uff0c\u5f00\u53d1\u4ef7\u683c\u4f4e\u5ec9\u3001\u9ad8\u6548\u4e14\u8010\u7528\u7684\u975e\u8d35\u91d1\u5c5e\u7535\u50ac\u5316\u5242\u52a0\u901f\u50ac\u5316\u53cd\u5e94\u52a8\u529b\u5b66\u53d8\u5f97\u81f3\u5173\u91cd\u8981\u3002\u5c16\u6676\u77f3\u6750\u6599\u5177\u6709\u4e30\u5bcc\u7684\u5143\u7d20\u7ec4\u6210\u548c\u72ec\u7279\u7684\u7535\u5b50\u7ed3\u6784\uff0c\u901a\u8fc7\u63a7\u5236\u53cd\u5e94\u6761\u4ef6\u53ef\u4ee5\u5bf9\u5176\u7269\u76f8\u3001\u7ec4\u6210\u3001\u7ed3\u6784\u3001\u5f62\u8c8c\u548c\u7f3a\u9677\u7b49\u8fdb\u884c\u6709\u6548\u8c03\u63a7\u3002\u8fd9\u79cd\u7ed3\u6784\u53ef\u8c03\u7684\u591a\u91d1\u5c5e\u6c27\u5316\u7269\u5177\u6709\u826f\u597d\u7684\u5bfc\u7535\u6027\uff0c\u5df2\u9010\u6b65\u53d1\u5c55\u6210\u4e3a\u65b0\u4e00\u4ee3\u6c27\u6790\u51fa\u53cd\u5e94\u7535\u50ac\u5316\u5242\u7684\u5019\u9009\u6750\u6599\uff0c\u5176\u7535\u50ac\u5316\u6d3b\u6027\u53ef\u4e0e\u8d35\u91d1\u5c5e\u76f8\u5ab2\u7f8e\u3002<\/p>\n<p><strong><b>\u3010\u6587\u7ae0\u7b80\u4ecb\u3011<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-235206\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-4-27.png\" alt=\"\" width=\"1617\" height=\"576\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-4-27.png 1617w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-4-27-300x107.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-4-27-768x274.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-4-27-1024x365.png 1024w\" sizes=\"(max-width: 1617px) 100vw, 1617px\" \/><\/p>\n<p>\u8fd1\u65e5\uff0c\u5185\u8499\u53e4\u5927\u5b66\u738b\u52e4\u6559\u6388\u8bfe\u9898\u7ec4\u4e0e\u5927\u8fde\u5316\u7269\u6240\u5f20\u6c5f\u5a01\u3001\u4e2d\u56fd\u79d1\u5b66\u6280\u672f\u5927\u5b66\u5b54\u6e90\u5408\u4f5c\uff0c\u5728\u300aNano Letters\u300b\u53d1\u8868\u9898\u4e3a\u201cUnraveling the Synergistic Effect of Heteroatomic Substitution and Vacancy Engineering in CoFe<sub>2<\/sub>O<sub>4<\/sub>\u00a0for Superior Electrocatalysis Performance\u201d\u7684\u7814\u7a76\u8bba\u6587\u3002\u901a\u8fc7\u5728CoFe<sub>2<\/sub>O<sub>4<\/sub>\u7684\u516b\u9762\u4f53B\u4f4d\u5f15\u5165Cr<sup>3+<\/sup>\u79bb\u5b50\uff0c\u8bf1\u5bfc\u91d1\u5c5eCo\u7a7a\u4f4d\u751f\u6210\uff0c\u5e76\u901a\u8fc7S<sup>2-<\/sup>\u79bb\u5b50\u4ea4\u6362\u53cd\u5e94\u751f\u6210Fe-S\u7b49\u65b0\u7684\u50ac\u5316\u6d3b\u6027\u4f4d\u70b9\uff0c\u4f7f\u5f97\u5c16\u6676\u77f3\u56db\u9762\u4f53A\u4f4d\u53d1\u751f\u660e\u663e\u7684\u7ed3\u6784\u7578\u53d8\uff0c\u8fdb\u800c\u63d0\u5347\u5c16\u6676\u77f3\u7684\u6c27\u6790\u51fa\u548c\u6c27\u8fd8\u539f\u53cd\u5e94\u7535\u50ac\u5316\u6027\u80fd\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-235205\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-2-27.png\" alt=\"\" width=\"1267\" height=\"1316\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-2-27.png 1267w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-2-27-289x300.png 289w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-2-27-768x798.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-2-27-986x1024.png 986w\" sizes=\"(max-width: 1267px) 100vw, 1267px\" \/><\/p>\n<p>\u56fe1.\u00a0\u50ac\u5316\u5242\u7684\u5408\u6210\u8fc7\u7a0b\u53ca\u7ed3\u6784\u5f62\u8c8c<\/p>\n<p><strong><b>\u3010\u672c\u6587\u8981\u70b9\u3011<\/b><\/strong><\/p>\n<p><strong><b>\u8981\u70b9\u4e00\uff1a\u516b\u9762\u4f53B\u4f4d\u63ba\u6742\u53d6\u4ee3\uff0c<\/b><\/strong><strong><b>\u8bf1\u5bfc\u91d1\u5c5eCo\u7a7a\u4f4d\u7f3a\u9677\u751f\u6210<\/b><\/strong><\/p>\n<p>\u6839\u636e\u8fc7\u6e21\u91d1\u5c5e\u6676\u4f53\u573a\u7a33\u5b9a\u80fd\u548c\u516b\u9762\u4f53\u62e9\u4f4d\u80fd\u7684\u5dee\u5f02\uff0c\u4f5c\u8005\u5c06\u4e00\u7cfb\u5217\u91d1\u5c5e\u79bb\u5b50\u5206\u522b\u5f15\u5165\u5230CoFe<sub>2<\/sub>O<sub>4<\/sub>\u7684\u56db\u9762\u4f53A\u4f4d\uff08Zn<sup>2+<\/sup>, Mn<sup>2+<\/sup>, Fe<sup>2+<\/sup>, Cd<sup>2+<\/sup>\uff09\u548c\u516b\u9762\u4f53B\u4f4d\uff08Mn<sup>3+<\/sup>, Cr<sup>3+<\/sup>, Sn<sup>4+<\/sup>, Cu<sup>2+<\/sup>\uff09\u3002\u7814\u7a76\u7ed3\u679c\u8868\u660e\uff0c\u5728CoFe<sub>2<\/sub>O<sub>4<\/sub>\u7684\u516b\u9762\u4f53B\u4f4d\u5f15\u5165Cr<sup>3+<\/sup>\u53ef\u4ee5\u660e\u663e\u63d0\u5347\u5176\u6c27\u6790\u51fa\u53cd\u5e94\u7535\u50ac\u5316\u6027\u80fd\u3002X\u5c04\u7ebf\u5438\u6536\u5149\u8c31\u548c\u7406\u8bba\u8ba1\u7b97\u8868\u660e\uff0cCr<sup>3+<\/sup>\u53ef\u4ee5\u7cbe\u786e\u5730\u63ba\u6742\u5230\u516b\u9762\u4f53B\u4f4d\u53d6\u4ee3\u90e8\u5206Fe<sup>3+<\/sup>\uff0c\u540c\u65f6\u8bf1\u5bfc\u90e8\u5206Co\u7a7a\u4f4d\u751f\u6210\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-235204\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-1-34.png\" alt=\"\" width=\"1414\" height=\"1100\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-1-34.png 1414w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-1-34-300x233.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-1-34-768x597.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-1-34-1024x797.png 1024w\" sizes=\"(max-width: 1414px) 100vw, 1414px\" \/><\/p>\n<p>\u56fe2.\u00a0\u8868\u9762\u7f3a\u9677\u3001\u914d\u4f4d\u7ed3\u6784\u4ee5\u53ca\u5316\u5b66\u6210\u952e\u5206\u6790<\/p>\n<p><strong><b>\u8981\u70b9\u4e8c\uff1a<\/b><\/strong><strong><b>\u00a0S<\/b><\/strong><strong><sup><b>2-<\/b><\/sup><\/strong><strong><b>\u79bb\u5b50\u4ea4\u6362\u53cd\u5e94\uff0c\u5f15\u8d77\u56db\u9762\u4f53<\/b><\/strong><strong><b>A<\/b><\/strong><strong><b>\u4f4d\u7ed3\u6784\u53d1\u751f\u7578\u53d8<\/b><\/strong><\/p>\n<p>\u901a\u8fc7S<sup>2-<\/sup>\u7684\u79bb\u5b50\u4ea4\u6362\u53cd\u5e94\u4f1a\u751f\u6210Fe-S\u7b49\u65b0\u7684\u50ac\u5316\u6d3b\u6027\u4f4d\u70b9\uff0c\u4f7f\u5f97\u5c16\u6676\u77f3\u56db\u9762\u4f53A\u4f4d\u53d1\u751f\u660e\u663e\u7684\u7ed3\u6784\u7578\u53d8\u3002\u56db\u9762\u4f53Fe\u7684\u5c40\u57df\u51e0\u4f55\u7ed3\u6784\u548c\u7535\u5b50\u7ed3\u6784\u53d8\u5316\u5bfc\u81f4*OH\u4e2d\u95f4\u4f53\u5b8c\u5168\u504f\u79bby\u8f74\u5e73\u9762\uff0c\u8fd9\u79cd\u5f62\u53d8\u4f1a\u4f7f*OOH\u5438\u9644\u660e\u663e\u589e\u5f3a\uff0c\u8fdb\u800c\u63d0\u5347\u7535\u50ac\u5316\u6027\u80fd\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-235207\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-5-24.png\" alt=\"\" width=\"810\" height=\"614\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-5-24.png 810w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-5-24-300x227.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-5-24-768x582.png 768w\" sizes=\"(max-width: 810px) 100vw, 810px\" \/><\/p>\n<p>\u56fe3.\u00a0\u50ac\u5316\u53cd\u5e94\u52a8\u529b\u5b66\u7814\u7a76<\/p>\n<p><strong><b>\u8981\u70b9\u4e09\uff1a\u91d1\u5c5e\u63ba\u6742\u53d6\u4ee3\u663e\u8457\u63d0\u5347\u94b4\u57fa\u5c16\u6676\u77f3\u7684\u7535\u50ac\u5316\u6027\u80fd<\/b><\/strong><\/p>\n<p>\u4f5c\u8005\u8bbe\u8ba1\u5408\u6210\u7684\u94b4\u57fa\u5c16\u6676\u77f3\u7535\u50ac\u5316\u6750\u6599\u8868\u73b0\u51fa\u4f18\u5f02\u7684\u6c27\u6790\u51fa\u53cd\u5e94\u7535\u50ac\u5316\u6027\u80fd\uff0c\u5176\u8fc7\u7535\u4f4d\u4ec5\u4e3a250 mV\uff0cTafel\u659c\u7387\u4e3a44 mV\u00b7dec<sup>-1<\/sup>\uff0c\u662f\u76ee\u524d\u6027\u80fd\u6700\u4f18\u7684\u5c16\u6676\u77f3\u50ac\u5316\u6750\u6599\u3002\u5728\u4e0d\u5f15\u8d77\u5c16\u6676\u77f3\u6676\u4f53\u7ed3\u6784\u53d1\u751f\u660e\u663e\u53d8\u5316\u7684\u60c5\u51b5\u4e0b\uff0c\u901a\u8fc7Cr<sup>3<\/sup><sup>+<\/sup>\u7684\u9009\u62e9\u6027\u63ba\u6742\u53d6\u4ee3\u548cS<sup>2<\/sup><sup>&#8211;<\/sup>\u7684\u8868\u9762\u4fee\u9970\uff0c\u6709\u6548\u8c03\u8282\u4e86CoFe<sub>2<\/sub>O<sub>4<\/sub>\u50ac\u5316\u5242\u7684\u5c40\u57df\u914d\u4f4d\u73af\u5883\u3001\u51e0\u4f55\u7ed3\u6784\u548c\u7535\u5b50\u7ed3\u6784\uff0c\u63d0\u5347\u4e86\u94b4\u57fa\u5c16\u6676\u77f3\u7684\u672c\u5f81\u7535\u50ac\u5316\u6d3b\u6027\u3002<strong><b><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-235208\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-6-26.png\" alt=\"\" width=\"1065\" height=\"815\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-6-26.png 1065w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-6-26-300x230.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-6-26-768x588.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/03\/\u56fe\u7247-6-26-1024x784.png 1024w\" sizes=\"(max-width: 1065px) 100vw, 1065px\" \/><\/b><\/strong><\/p>\n<p>\u56fe4.\u6c27\u6790\u51fa\u53cd\u5e94\u7535\u50ac\u5316\u6027\u80fd<\/p>\n<p><strong><b>\u3010\u6587\u7ae0\u94fe\u63a5\u3011<\/b><\/strong><\/p>\n<p>Unraveling the Synergistic Effect of Heteroatomic Substitution and Vacancy Engineering in CoFe<sub>2<\/sub>O<sub>4<\/sub>\u00a0for Superior Electrocatalysis Performance\u00a0<\/p>\n<p><a href=\"https:\/\/pubs.acs.org\/doi\/10.1021\/acs.nanolett.1c04425\"><u>https:\/\/pubs.acs.org\/doi\/10.1021\/acs.nanolett.1c04425<\/u><\/a><\/p>\n<p><strong><b>\u3010\u901a\u8baf\u4f5c\u8005\u7b80\u4ecb\u3011<\/b><\/strong><\/p>\n<p>\u738b\u52e4\uff1a\u5185\u8499\u53e4\u5927\u5b66\u5316\u5b66\u5316\u5de5\u5b66\u9662\u6559\u6388\uff0c\u535a\u58eb\u751f\u5bfc\u5e08\uff0c\u62c5\u4efb\u5b66\u6821\u5b66\u79d1\u5efa\u8bbe\u59d4\u5458\u4f1a\u59d4\u5458\u3001\u6821\u5b66\u90e8\u59d4\u5458\u3001\u56fd\u5bb6\u81ea\u7136\u79d1\u5b66\u57fa\u91d1\u901a\u8baf\u8bc4\u8bae\u4e13\u5bb6\u3001\u6559\u80b2\u90e8\u5b66\u4f4d\u4e0e\u7814\u7a76\u751f\u6559\u80b2\u53d1\u5c55\u4e2d\u5fc3\u901a\u8baf\u8bc4\u8bae\u4e13\u5bb6\u4ee5\u53ca\u300aChinese Chemical Letters\u300b\u7b49\u591a\u4e2a\u56fd\u9645\u91cd\u8981\u5b66\u672f\u671f\u520a\u7684\u7f16\u59d4\u30022010\u5e747\u6708\u6bd5\u4e1a\u4e8e\u5409\u6797\u5927\u5b66\u7269\u7406\u5316\u5b66\u4e13\u4e1a\uff0c\u83b7\u7406\u5b66\u535a\u58eb\u5b66\u4f4d\uff0c\u540c\u5e74\u6765\u6821\u4efb\u6559\u81f3\u4eca\u3002\u738b\u52e4\u6559\u6388\u4f5c\u4e3a\u5316\u5b66\u5316\u5de5\u5b66\u9662\u7684\u5b66\u79d1\u5e26\u5934\u4eba\uff0c\u7ed3\u5408\u81ea\u6cbb\u533a\u91cd\u5927\u80fd\u6e90\u9700\u6c42\u548c\u5b66\u79d1\u53d1\u5c55\u65b9\u5411\uff0c\u56f4\u7ed5\u81ea\u6cbb\u533a\u80fd\u6e90\u5316\u5de5\u3001\u7a00\u571f\u53ca\u65b0\u80fd\u6e90\u6750\u6599\u7b49\u5f00\u5c55\u7279\u8272\u7814\u7a76\u5de5\u4f5c\uff0c\u53d6\u5f97\u4e86\u7cfb\u5217\u91cd\u8981\u539f\u521b\u6210\u679c\u3002\u4e3b\u6301\u5404\u7c7b\u79d1\u7814\u9879\u76ee10\u4f59\u9879\uff0c\u5728Nano Letters, Angew. Chem. Int. Ed, Adv. Energy Mater, Appl Catal B-Environ\u7b49\u53d1\u8868\u5b66\u672f\u8bba\u658780\u4f59\u7bc7\uff0c\u5176\u4e2d\u591a\u7bc7\u5165\u9009\u5c01\u9762\u3001\u70ed\u70b9\u548cESI\u9ad8\u88ab\u5f15\u8bba\u6587\u3002\u83b7\u5185\u8499\u53e4\u81ea\u7136\u79d1\u5b66\u4e00\u7b49\u59561\u9879\uff1b\u5165\u9009\u5185\u8499\u53e4\u81ea\u6cbb\u533a\u201c\u8349\u539f\u82f1\u624d\u201d\u5de5\u7a0b\u3001\u201c\u65b0\u4e16\u7eaa321\u4eba\u624d\u5de5\u7a0b\u201d\u3001\u81ea\u6cbb\u533a\u9752\u5e74\u79d1\u6280\u9886\u519b\u4eba\u624d\u3001\u5185\u8499\u53e4\u6770\u51fa\u9752\u5e74\u57f9\u80b2\u57fa\u91d1\uff1b\u83b7\u5185\u8499\u53e4\u5927\u5b66\u6821\u957f\u52b1\u5b66\u5956\u3001\u4e4c\u53ef\u529b\u5956\u3001\u4e09\u80b2\u4eba\u5148\u8fdb\u4e2a\u4eba\u7b49\u79f0\u53f7\u3002<\/p>\n<p>\u90ae\u7bb1\uff1a<a href=\"mailto:qinwang@imu.edu.cn\"><u>qinwang@imu.edu.cn<\/u><\/a><\/p>\n<p>\u8bfe\u9898\u7ec4\u7f51\u7ad9\uff1ahttps:\/\/www.x-mol.com\/groups\/wangqin\/<\/p>\n<p><strong><b>\u3010\u6587\u7ae0\u4fe1\u606f\u3011<\/b><\/strong><\/p>\n<p>\u516b\u9762\u4f53\u4f4d\u63ba\u6742\u548c\u7f3a\u9677\u5de5\u7a0b\u63d0\u5347\u5c16\u6676\u77f3\u7535\u50ac\u5316\u6027\u80fd<\/p>\n<p>\u7b2c\u4e00\u4f5c\u8005\uff1a\u5b59\u9759\uff0c\u859b\u8f89\u00a0<\/p>\n<p>\u901a\u8baf\u4f5c\u8005\uff1a\u5b54\u6e90*\u3001\u5f20\u6c5f\u5a01*\u3001\u738b\u52e4*<\/p>\n<p>\u7b2c\u4e00\u901a\u8baf\u5355\u4f4d\uff1a\u5185\u8499\u53e4\u5927\u5b66<\/p>\n<p>\u672c\u6587\u7531\u4f5c\u8005\u4f9b\u7a3f\u3002<\/p>\n<p>&nbsp;<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u7814\u7a76\u80cc\u666f\u3011 \u7535\u89e3\u6c34\u5236\u6c22\u6280\u672f\u662f\u76ee\u524d\u5de5\u4e1a\u5316\u5236\u5907\u9ad8\u7eaf\u6c22\u6c14\u7684\u91cd\u8981\u624b\u6bb5\u4e4b\u4e00\u3002\u7136\u800c\uff0c\u9633\u6781\u6790\u6c27\u53cd\u5e94\u7684\u8fc7\u7535\u4f4d\u8f83\u9ad8\u3001\u52a8\u529b\u5b66\u76f8\u5bf9\u7f13\u6162\uff0c\u9700\u8981\u9ad8\u6548\u7684\u7535\u50ac\u5316\u5242\u52a0\u901f\u8be5\u7c7b\u53cd\u5e94\u7684\u52a8\u529b\u5b66\uff0c\u4ece\u800c&#8230;<\/p>\n","protected":false},"author":35234,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[2],"tags":[],"class_list":["post-235203","post","type-post","status-publish","format-standard","hentry","category-keji"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/235203"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/35234"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=235203"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/235203\/revisions"}],"predecessor-version":[{"id":235286,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/235203\/revisions\/235286"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=235203"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=235203"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=235203"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}