{"id":236239,"date":"2022-04-29T06:46:09","date_gmt":"2022-04-28T22:46:09","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=236239"},"modified":"2022-04-28T16:46:42","modified_gmt":"2022-04-28T08:46:42","slug":"%e3%80%90%e5%b7%b2%e5%ae%a1%e3%80%91advanced-science%ef%bc%9a%e5%85%b7%e6%9c%89%e8%87%aa%e6%84%88%e5%8a%9f%e8%83%bd%e7%9a%84%e9%ab%98%e6%80%a7%e8%83%bd%e6%9f%94%e6%80%a7%e5%8e%8b%e5%8a%9b%e4%bc%a0","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=236239","title":{"rendered":"Advanced Science\uff1a\u5177\u6709\u81ea\u6108\u529f\u80fd\u7684\u9ad8\u6027\u80fd\u67d4\u6027\u538b\u529b\u4f20\u611f\u5668"},"content":{"rendered":"<p style=\"text-align: center;\"><strong>\u4e00\u3001\u3010\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p>\u751f\u7269\u7535\u5b50\u3001\u667a\u80fd\u5bb6\u5c45\u3001\u667a\u80fd\u673a\u5668\u4eba\u548c\u4eba\u673a\u4ea4\u4e92\u7684\u5feb\u901f\u53d1\u5c55\u6781\u5927\u5730\u4fc3\u8fdb\u4e86\u67d4\u6027\u538b\u529b\u4f20\u611f\u5668\u7684\u5e02\u573a\u53d1\u5c55\u9700\u6c42\u3002\u67d4\u6027\u538b\u529b\u4f20\u611f\u5668\u4e3b\u8981\u57fa\u4e8e\u4ee5\u4e0b\u51e0\u79cd\u5de5\u4f5c\u673a\u5236\uff0c\u5982\u7535\u5bb9\u5f0f\u3001\u538b\u963b\u5f0f\u3001\u538b\u7535\u5f0f\u548c\u6469\u64e6\u5f0f\u3002\u57fa\u4e8e\u538b\u963b\u6548\u5e94\u7684<span style=\"color: #003366;\"><strong>\u538b\u963b\u5f0f\u4f20\u611f\u5668<\/strong><\/span>\u5177\u6709\u7075\u654f\u5ea6\u9ad8\u3001\u4fe1\u53f7\u54cd\u5e94\u5feb\u3001\u5236\u5907\u5de5\u827a\u7b80\u5355\u3001\u4f20\u611f\u6027\u80fd\u7a33\u5b9a\u7b49\u7279\u70b9\u3002\u8fd1\u5e74\u6765\u5173\u4e8e\u67d4\u6027\u538b\u963b\u5f0f\u4f20\u611f\u5668\u7684\u7814\u7a76\u4e3b\u8981\u96c6\u4e2d\u5728\u654f\u611f\u5c42\u7684\u5fae\u7ed3\u6784\u8bbe\u8ba1\u4e0a\u3002\u56e0\u6b64\uff0c\u5236\u5907\u6ee1\u8db3\u5404\u79cd\u573a\u5408\u9700\u6c42\u7684\u9ad8\u6027\u80fd\u538b\u963b\u5f0f\u4f20\u611f\u5668\u6210\u4e3a\u8fd1\u5e74\u6765\u7684\u4e00\u4e2a\u70ed\u95e8\u8bdd\u9898\u3002\u5b9e\u9a8c\u8868\u660e\uff0c\u67d4\u6027\u886c\u5e95\u7684\u5fae\u7ed3\u6784\u8bbe\u8ba1\u53ef\u4ee5\u663e\u8457\u63d0\u9ad8\u4f20\u611f\u5668\u7684\u4f20\u611f\u6027\u80fd\u3002\u867d\u7136\u538b\u963b\u5f0f\u4f20\u611f\u5668\u5728\u5fae\u89c2\u7ed3\u6784\u65b9\u9762\u7684\u7814\u7a76\u5df2\u7ecf\u53d6\u5f97\u4e86\u4e00\u4e9b\u8fdb\u5c55\uff0c\u4f46\u7406\u60f3\u7684\u67d4\u6027\u538b\u963b\u5f0f\u4f20\u611f\u5668\u4ec5\u5177\u6709\u4f18\u5f02\u7684\u4f20\u611f\u6027\u80fd\u662f\u8fdc\u8fdc\u4e0d\u591f\u7684\u3002\u5728\u5b9e\u9645\u5e94\u7528\u4e2d\uff0c\u67d4\u6027\u538b\u963b\u5f0f\u4f20\u611f\u5668\u4e0d\u53ef\u907f\u514d\u5730\u9762\u4e34\u590d\u6742\u7684\u5de5\u4f5c\u73af\u5883\uff0c\u654f\u611f\u5c42\u5bb9\u6613\u53d7\u5230\u5404\u79cd\u5916\u90e8\u673a\u68b0\u635f\u4f24\u3002\u6b64\u5916\uff0c\u5927\u591a\u6570\u67d4\u6027\u4f20\u611f\u5668\u7684\u5236\u5907\u5de5\u827a\u9650\u5236\u4e86\u67d4\u6027\u886c\u5e95\u7684\u9009\u62e9\u3002\u8fd9\u4e9b\u95ee\u9898\u963b\u788d\u4e86\u67d4\u6027\u538b\u963b\u5f0f\u4f20\u611f\u5668\u7684\u5e7f\u6cdb\u5e94\u7528\u3002<\/p>\n<p style=\"text-align: center;\"><strong>\u4e8c\u3001\u3010\u6210\u679c\u63a0\u5f71\u3011<\/strong><\/p>\n<p>\u00a0\u8fd1\u65e5\uff0c<strong>\u6b66\u6c49\u5927\u5b66<\/strong><strong>Wang Ziyu<\/strong><strong>\uff0c\u90d1\u5dde\u5927\u5b66\u5218\u4f1f\u6770\u548c\u90ed\u6d77\u4e2d\uff08\u5171\u540c\u4f5c\u8005\uff09\uff0c\u8054\u5408\u5728<\/strong><strong><em>Advanced Science<\/em><\/strong><strong>\u4e0a\u53d1\u8868\u6587\u7ae0<\/strong>\uff0c\u9898\u4e3a\u201c<strong>High-Performance Flexible Pressure Sensor with a Self-Healing Function for Tactile Feedback<\/strong>\u201d\u3002\u4f5c\u8005\u63d0\u51fa\u4e00\u79cd\u57fa\u4e8eMXene\u7684\u5177\u6709\u81ea\u4fee\u590d\u529f\u80fd\u7684\u9ad8\u6027\u80fd\u67d4\u6027\u538b\u963b\u5f0f\u4f20\u611f\u5668\u6765\u5b9e\u73b0\u89e6\u89c9\u53cd\u9988\uff0c\u8be5\u4f20\u611f\u5668\u91c7\u7528\u7b80\u5355\u7684\u5168\u55b7\u6d82\u65b9\u6cd5\u6765\u5236\u5907\u3002\u4f5c\u8005\u91c7\u7528\u5177\u6709spinosum\u72b6\u7ed3\u6784\u7684\u805a\u6c28\u916f\uff08Polyurethane\uff0cPU\uff09\u4f5c\u4e3a\u654f\u611f\u5c42\u7684\u67d4\u6027\u57fa\u677f\u3002\u5c06MXene\u7eb3\u7c73\u7247\u6c89\u79ef\u5728PU\u7684spinosum\u72b6\u7ed3\u6784\u8868\u9762\uff0c\u5f97\u5230\u5177\u6709\u81ea\u4fee\u590d\u529f\u80fd\u7684MXene\/PU\u654f\u611f\u5c42\u3002\u8fdb\u4e00\u6b65\uff0c\u4f5c\u8005\u91c7\u7528\u4f4e\u6210\u672c\u3001\u901a\u7528\u7684\u6a21\u677f\u55b7\u6d82\u65b9\u6cd5\u5236\u5907\u4e86\u57fa\u4e8eMXene\u7684\u67d4\u6027\u53c9\u6307\u7535\u6781\u3002\u7528\u8fd9\u79cd\u65b9\u6cd5\u5236\u5907\u7684\u53c9\u6307\u7535\u6781\u6240\u9700\u7684\u67d4\u6027\u886c\u5e95\u662f\u4efb\u610f\u7684\u3002\u4e3a\u4e86\u9a8c\u8bc1\u5236\u5907\u53c9\u6307\u7535\u6781\u6240\u9700\u7684\u67d4\u6027\u886c\u5e95\u7684\u4efb\u610f\u6027\uff0c\u4f5c\u8005\u5236\u5907\u4e86\u4ee5PI\u548c\u6ee4\u819c\u4e3a\u886c\u5e95\u7684MXene\u57fa\u538b\u963b\u4f20\u611f\u5668\u3002\u7075\u654f\u5ea6\u5206\u522b\u53ef\u8fbe509.8\u548c408.4 kPa<sup>-1<\/sup>\uff0c\u54cd\u5e94\u65f6\u95f4\u5206\u522b\u4e3a67.3\u548c68.4 ms\uff0c\u6062\u590d\u65f6\u95f4\u5206\u522b\u4e3a44.8\u548c46.5 ms\u3002\u4f20\u611f\u5668\u7684\u7535\u6d41\u572810 000\u6b21\u538b\u529b\u5faa\u73af\u540e\u4ecd\u65e7\u80fd\u591f\u4fdd\u6301\u7a33\u5b9a\u3002\u6b64\u5916\uff0c\u654f\u611f\u5c42\u7ecf\u538618 h\u7684\u201c\u5207\u5272-\u6108\u5408\u201d\u540e\uff0c\u4f20\u611f\u5668(PI\u4f5c\u4e3a\u53c9\u6307\u7535\u6781\u7684\u67d4\u6027\u886c\u5e95)\u7684\u7075\u654f\u5ea6\u4ecd\u53ef\u8fbe\u5230456.9 kPa<sup>-1<\/sup>\u3002\u5728\u5b9e\u9645\u5e94\u7528\u4e2d\uff0c\u4f20\u611f\u5668\u4e0d\u4ec5\u53ef\u4ee5\u68c0\u6d4b\u4eba\u7c7b\u6d3b\u52a8\uff0c\u8fd8\u53ef\u4ee5\u7ed3\u5408\u8f6f\u786c\u4ef6\u8bbe\u8ba1\uff0c\u4f7f\u673a\u68b0\u624b\u5b9e\u73b0\u89e6\u89c9\u53cd\u9988\u529f\u80fd\u3002\u56e0\u6b64\uff0c\u5168\u55b7\u6d82\u7684\u57fa\u4e8eMXene\u7684\u9ad8\u6027\u80fd\u538b\u529b\u4f20\u611f\u5668\u5728\u4eba\u7c7b\u6d3b\u52a8\u68c0\u6d4b\u3001\u7535\u5b50\u76ae\u80a4\u3001\u667a\u80fd\u673a\u5668\u4eba\u7b49\u65b9\u9762\u5177\u6709\u5f88\u5927\u7684\u6f5c\u529b\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-236249\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/1-15.jpg\" alt=\"\" width=\"847\" height=\"262\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/1-15.jpg 847w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/1-15-300x93.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/1-15-768x238.jpg 768w\" sizes=\"(max-width: 847px) 100vw, 847px\" \/><\/p>\n<p style=\"text-align: center;\"><strong>\u4e09\u3001\u3010\u6838\u5fc3\u521b\u65b0\u70b9\u3011<\/strong><\/p>\n<ol>\n<li>\u4f5c\u8005\u63d0\u51fa\u4e00\u79cd\u57fa\u4e8eMXene\u7684\u5177\u6709\u81ea\u4fee\u590d\u529f\u80fd\u7684\u9ad8\u6027\u80fd\u67d4\u6027\u538b\u963b\u5f0f\u4f20\u611f\u5668\u6765\u5b9e\u73b0\u89e6\u89c9\u53cd\u9988\uff0c\u8be5\u4f20\u611f\u5668\u5177\u6709\u9ad8\u7075\u654f\u5ea6\uff0c\u4f4e\u7684\u54cd\u5e94\u65f6\u95f4\u4ee5\u53ca\u9ad8\u7684\u7a33\u5b9a\u6027\u3002<\/li>\n<li>\u4f5c\u8005\u91c7\u7528\u4f4e\u6210\u672c\u3001\u901a\u7528\u7684\u6a21\u677f\u55b7\u6d82\u65b9\u6cd5\u5236\u5907\u4e86\u57fa\u4e8eMXene\u7684\u67d4\u6027\u53c9\u6307\u7535\u6781\u3002\u7528\u8fd9\u79cd\u65b9\u6cd5\u5236\u5907\u7684\u53c9\u6307\u7535\u6781\u6240\u9700\u7684\u67d4\u6027\u886c\u5e95\u662f\u4efb\u610f\u7684\uff0c\u5236\u9020\u6210\u672c\u4f4e\u5ec9\u3002<\/li>\n<\/ol>\n<p style=\"text-align: center;\"><strong>\u56db\u3001\u3010\u6570\u636e\u6982\u89c8\u3011<\/strong><\/p>\n<p style=\"text-align: center;\"><strong>\u56fe1<\/strong>. \u5236\u5907\u8fc7\u7a0b <span style=\"color: #808080;\">\u00a9 2022 The Authors<\/span><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-236250\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/1-0.jpg\" alt=\"\" width=\"1000\" height=\"757\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/1-0.jpg 1000w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/1-0-300x227.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/1-0-768x581.jpg 768w\" sizes=\"(max-width: 1000px) 100vw, 1000px\" \/><\/p>\n<p>a) \u57fa\u4e8eMXene\u7684\u5168\u55b7\u6d82\u9ad8\u6027\u80fd\u538b\u529b\u4f20\u611f\u5668\u5236\u4f5c\u5de5\u827a<\/p>\n<p>b) \u654f\u611f\u5c42\u81ea\u6108\u673a\u7406\u793a\u610f\u56fe<\/p>\n<p style=\"text-align: center;\"><strong>\u56fe2<\/strong>. \u7ed3\u6784\uff0c\u5f62\u8c8c\u8868\u5f81<span style=\"color: #808080;\">\u00a9 2022 The Authors<\/span><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-236251\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/2-14.jpg\" alt=\"\" width=\"1283\" height=\"1634\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/2-14.jpg 1283w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/2-14-236x300.jpg 236w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/2-14-768x978.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/2-14-804x1024.jpg 804w\" sizes=\"(max-width: 1283px) 100vw, 1283px\" \/><\/p>\n<p>a) MXene\u7eb3\u7c73\u7247\u7684TEM\u56fe<\/p>\n<p>b) MXene (Ti<sub>3<\/sub>C<sub>2<\/sub>T<sub>x<\/sub>)\u7684EDS\u56fe<\/p>\n<p>c) MXene\u7eb3\u7c73\u7247\u7684AFM\u56fe<\/p>\n<p>d) MXene\u7eb3\u7c73\u7247\u7684XRD\u56fe<\/p>\n<p>e-j) \u4e0d\u540cspinosum\u7ed3\u6784\u7684\u654f\u611f\u5c42\u7684SEM\u56fe\u50cf(nos.100, 180, 280, 400, 600, and 800)<\/p>\n<p>k) nos. 280\u654f\u611f\u5c42\u7684EDX\u56fe<\/p>\n<p style=\"text-align: center;\"><strong>\u56fe3<\/strong>. \u57fa\u4e8eMXene\u7684\u538b\u529b\u4f20\u611f\u5668\u7684\u4f20\u611f\u7279\u6027\u00a0<span style=\"color: #808080;\">\u00a9 2022 The Authors<\/span><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-236252\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/3-14.jpg\" alt=\"\" width=\"1367\" height=\"1069\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/3-14.jpg 1367w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/3-14-300x235.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/3-14-768x601.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/3-14-1024x801.jpg 1024w\" sizes=\"(max-width: 1367px) 100vw, 1367px\" \/><\/p>\n<p>a) \u4f20\u611f\u5668\u7075\u654f\u5ea6<\/p>\n<p>b) <em>I-T<\/em>\u66f2\u7ebf<\/p>\n<p>c) <em>I-V<\/em>\u66f2\u7ebf<\/p>\n<p>d) \u4f20\u611f\u5668\u7684\u54cd\u5e94\u548c\u6062\u590d\u65f6\u95f4<\/p>\n<p>e) \u4f20\u611f\u5668\u7684\u9891\u7387\u54cd\u5e94\u6027\u80fd<\/p>\n<p>f) \u4f20\u611f\u5668\u7684\u901f\u5ea6\u54cd\u5e94\u6027\u80fd<\/p>\n<p>g) <em>I-T<\/em>\u548c<em>P-T<\/em>\u66f2\u7ebf\u7684\u54cd\u5e94<\/p>\n<p>h) \u7a33\u5b9a\u6027\u6d4b\u8bd5<\/p>\n<p>i) \u654f\u611f\u5c42\u7ecf\u538618 h\u7684\u201c\u5207\u5272-\u6108\u5408\u201d\u540e\uff0c\u4f20\u611f\u5668\u7684\u7075\u654f\u5ea6<\/p>\n<p style=\"text-align: center;\"><strong>\u56fe4.<\/strong> \u5168\u55b7\u6d82\u5f0fMXene\u538b\u529b\u4f20\u611f\u5668\u7684\u5de5\u4f5c\u673a\u7406<span style=\"color: #808080;\">\u00a9 2022 The Authors<\/span><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-236253\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/4-13.jpg\" alt=\"\" width=\"1367\" height=\"641\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/4-13.jpg 1367w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/4-13-300x141.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/4-13-768x360.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/4-13-1024x480.jpg 1024w\" sizes=\"(max-width: 1367px) 100vw, 1367px\" \/><\/p>\n<p>\u5728a) 1.0 Pa\u548cb) 1.0 kPa\u65f6\u654f\u611f\u5c42\u538b\u529b\u5206\u5e03\u7684\u6a21\u62df\u7ed3\u679c<\/p>\n<p>c) 1.0 kPa\u65f6\u53c9\u6307\u7535\u6781\u538b\u529b\u5206\u5e03\u7684\u4eff\u771f\u7ed3\u679c<\/p>\n<p>d)\u521d\u59cb\u72b6\u6001\uff0ce)\u8f7b\u8f7d\u72b6\u6001\uff0cf)\u91cd\u8f7d\u72b6\u6001\u5bf9\u5e94\u7684\u7535\u8def\u6a21\u5177\u793a\u610f\u56fe<\/p>\n<p><strong>\u56fe5.<\/strong> \u5168\u55b7\u6d82\u5f0fMXene\u538b\u529b\u4f20\u611f\u5668\u5728\u6700\u5c0f\u53ef\u6d4b\u538b\u529b\u548c\u5b9e\u65f6\u76d1\u6d4b\u4eba\u7c7b\u6d3b\u52a8\u4e2d\u7684\u5e94\u7528\u00a0<span style=\"color: #808080;\">\u00a9 2022 The Authors<\/span><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-236254\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/5-9.jpg\" alt=\"\" width=\"1367\" height=\"1078\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/5-9.jpg 1367w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/5-9-300x237.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/5-9-768x606.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/5-9-1024x808.jpg 1024w\" sizes=\"(max-width: 1367px) 100vw, 1367px\" \/><\/p>\n<p>\u4ee5\u7535\u6d41\u53d8\u5316\u4e3a\u5f62\u5f0f\u7684\u4fe1\u53f7\u54cd\u5e94\u6765\u81ea\u4e8ea) \u4e00\u7c92\u7eff\u8c46\u63d0\u4f9b\u7684\u5fae\u5c0f\u7269\u4f53\u538b\u529b(7.8 Pa)\uff0c b) \u624b\u8155\u5f2f\u66f2\uff0cc) \u624b\u6307\u5f2f\u66f2\uff0cd) \u624b\u6307\u8f7b\u53e9\uff0ce) \u5fae\u7b11\uff0cf) \u811a\u8e1d\u5f2f\u66f2\uff0cg) \u5589\u5499\u541e\u54bd\uff0ch) \u8098\u90e8\u5f2f\u66f2\u548ci) \u624b\u8155\u8109\u640f<\/p>\n<p style=\"text-align: center;\"><strong>\u56fe6<\/strong>. \u5168\u55b7\u6d82\u5f0fMXene\u538b\u529b\u4f20\u611f\u5668\u5728\u89e6\u89c9\u4f20\u611f\u4e2d\u7684\u5e94\u7528\u00a0<span style=\"color: #808080;\">\u00a9 2022 The Authors<\/span><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-236255\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/6-8.jpg\" alt=\"\" width=\"1367\" height=\"718\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/6-8.jpg 1367w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/6-8-300x158.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/6-8-768x403.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/04\/6-8-1024x538.jpg 1024w\" sizes=\"(max-width: 1367px) 100vw, 1367px\" \/><\/p>\n<p>a) \u901a\u8fc7\u822a\u5929\u5458\u540a\u5760\u5728\u7535\u5b50\u76ae\u80a4\u8868\u9762\u83b7\u5f97\u76f8\u5173\u7684\u538b\u529b\u5206\u5e03<\/p>\n<p>b) \u7535\u5b50\u76ae\u80a4\u8868\u9762\u7684\u5b87\u822a\u5458\u540a\u5760\u548c\u94a5\u5319\u7684\u5149\u5b66\u56fe\u50cf<\/p>\n<p>c) \u901a\u8fc7\u4e00\u628a\u94a5\u5319\u5728\u7535\u5b50\u76ae\u80a4\u8868\u9762\u7684\u83b7\u5f97\u76f8\u5173\u7684\u538b\u529b\u5206\u5e03<\/p>\n<p>d) \u80fd\u4f7f\u673a\u68b0\u624b\u5b9e\u73b0\u7cbe\u786e\u89e6\u89c9\u53cd\u9988\u7684\u538b\u529b\u4f20\u611f\u7cfb\u7edf\u603b\u4f53\u539f\u7406\u56fe<\/p>\n<p>e) \u8be5\u7cfb\u7edf\u7528\u4e8e\u6355\u6349\u8c46\u8150\u548c\u6c14\u7403<\/p>\n<p>f) \u673a\u68b0\u624b\u638c\u6293\u53d6-\u91ca\u653e\u8f6f\u9762\u5305<\/p>\n<p style=\"text-align: center;\"><strong>\u4e94\u3001\u3010\u6210\u679c\u542f\u793a\u3011<\/strong><\/p>\n<p>\u4f5c\u8005\u63d0\u51fa\u4e00\u79cd\u57fa\u4e8eMXene\u7684\u5177\u6709\u81ea\u4fee\u590d\u529f\u80fd\u7684\u9ad8\u6027\u80fd\u67d4\u6027\u538b\u963b\u5f0f\u4f20\u611f\u5668\u6765\u5b9e\u73b0\u89e6\u89c9\u53cd\u9988\uff0c\u8be5\u4f20\u611f\u5668\u91c7\u7528\u7b80\u5355\u7684\u5168\u55b7\u6d82\u65b9\u6cd5\u6765\u5236\u5907\u3002\u8be5\u5668\u4ef6\u7531spinosum MXene\/PU\u548c\u57fa\u4e8eMXene\u7684\u53c9\u6307\u7535\u6781\u7ec4\u6210\uff0c\u8fd9\u4e24\u90e8\u5206\u7684\u76f8\u4e92\u4f5c\u7528\u5b9e\u73b0\u4e86\u5668\u4ef6\u7684\u4f18\u5f02\u6027\u80fd\u3002\u4f5c\u8005\u5236\u5907\u4e86\u4ee5PI\u548c\u819c\u8fc7\u6ee4\u5668\u4e3a\u886c\u5e95\u7684MXene\u57fa\u538b\u963b\u4f20\u611f\u5668\u3002\u7075\u654f\u5ea6\u5206\u522b\u53ef\u8fbe509.8\u548c408.4 kPa<sup>-1<\/sup>\uff0c\u54cd\u5e94\u65f6\u95f4\u5206\u522b\u4e3a67.3\u548c68.4 ms\uff0c\u6062\u590d\u65f6\u95f4\u5206\u522b\u4e3a44.8\u548c46.5 ms\u3002\u4f20\u611f\u5668\u7684\u7535\u6d41\u572810 000\u6b21\u538b\u529b\u5faa\u73af\u540e\u4ecd\u65e7\u80fd\u591f\u4fdd\u6301\u7a33\u5b9a\u3002\u6b64\u5916\uff0c\u654f\u611f\u5c42\u7ecf\u538618 h\u7684\u201c\u5207\u5272-\u6108\u5408\u201d\u540e\uff0c\u4f20\u611f\u5668(PI\u4f5c\u4e3a\u53c9\u6307\u7535\u6781\u7684\u67d4\u6027\u886c\u5e95)\u7684\u7075\u654f\u5ea6\u4ecd\u53ef\u8fbe\u5230456.9 kPa<sup>-1<\/sup>\u3002\u603b\u4e4b\uff0c\u4f5c\u8005\u91c7\u7528\u4f4e\u6210\u672c\u548c\u901a\u7528\u7684\u65b9\u6cd5\u5236\u5907\u4e86\u4e00\u4e2a\u9ad8\u6027\u80fd\u7684\u538b\u529b\u4f20\u611f\u5668\u3002\u8be5\u4f20\u611f\u5668\u5177\u6709\u826f\u597d\u7684\u81ea\u4fee\u590d\u529f\u80fd\uff0c\u53ef\u7528\u4e8e\u89e6\u89c9\u53cd\u9988\uff0c\u5728\u673a\u5668\u4eba\u548c\u7535\u5b50\u76ae\u80a4\u7b49\u9886\u57df\u5177\u6709\u6f5c\u5728\u7684\u5e94\u7528\u524d\u666f\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"https:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/advs.202200507\" target=\"_blank\" rel=\"noopener\">High-Performance Flexible Pressure Sensor with a Self-Healing Function for Tactile Feedback<\/a>. 2022, <em>Advanced Science<\/em>, DOI: 10.1002\/advs.202200507.<\/p>\n<p>\u672c\u6587\u7531\u7eb3\u7c73\u5c0f\u767d\u4f9b\u7a3f<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1\uff1atougao@cailiaoren.com.<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaokefu.<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u4e00\u3001\u3010\u5bfc\u8bfb\u3011 \u751f\u7269\u7535\u5b50\u3001\u667a\u80fd\u5bb6\u5c45\u3001\u667a\u80fd\u673a\u5668\u4eba\u548c\u4eba\u673a\u4ea4\u4e92\u7684\u5feb\u901f\u53d1\u5c55\u6781\u5927\u5730\u4fc3\u8fdb\u4e86\u67d4\u6027\u538b\u529b\u4f20\u611f\u5668\u7684\u5e02\u573a\u53d1\u5c55\u9700\u6c42\u3002\u67d4\u6027\u538b\u529b\u4f20\u611f\u5668\u4e3b\u8981\u57fa\u4e8e\u4ee5\u4e0b\u51e0\u79cd\u5de5\u4f5c\u673a\u5236\uff0c\u5982\u7535\u5bb9\u5f0f\u3001\u538b\u963b&#8230;<\/p>\n","protected":false},"author":31345,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[2],"tags":[],"class_list":["post-236239","post","type-post","status-publish","format-standard","hentry","category-keji"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/236239"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/31345"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=236239"}],"version-history":[{"count":11,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/236239\/revisions"}],"predecessor-version":[{"id":236418,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/236239\/revisions\/236418"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=236239"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=236239"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=236239"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}