{"id":236897,"date":"2022-05-09T06:27:03","date_gmt":"2022-05-08T22:27:03","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=236897"},"modified":"2022-05-09T17:37:14","modified_gmt":"2022-05-09T09:37:14","slug":"%e6%bd%98%e9%94%8b%ef%bc%9a%e5%9f%ba%e4%ba%8e%e5%9b%be%e8%ae%ba%e3%80%81%e5%a4%a7%e6%95%b0%e6%8d%ae%e5%92%8c%e4%ba%ba%e5%b7%a5%e6%99%ba%e8%83%bd%e7%9a%84%e6%96%b0%e8%83%bd%e6%ba%90%e6%9d%90%e6%96%99","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=236897","title":{"rendered":"\u6f58\u950b\uff1a\u57fa\u4e8e\u56fe\u8bba\u3001\u5927\u6570\u636e\u548c\u4eba\u5de5\u667a\u80fd\u7684\u65b0\u80fd\u6e90\u6750\u6599\u57fa\u56e0\u63a2\u7d22"},"content":{"rendered":"<p>\u8c22\u8c22\u6750\u6599\u4eba\u7684\u9080\u8bf7\uff0c\u4e5f\u611f\u8c22\u5927\u5bb6\u5728\u5468\u672b\u65f6\u95f4\u6765\u542c\u6211\u4eec\u5317\u4eac\u5927\u5b66\u6df1\u5733\u7814\u7a76\u751f\u9662\u65b0\u6750\u6599\u5b66\u9662\u56e2\u961f\u5728\u65b0\u80fd\u6e90\u6750\u6599\u7684\u7814\u7a76\u65b0\u8303\u5f0f\u65b9\u9762\u7684\u63a2\u7d22\u601d\u8003\u548c\u8fdb\u5c55\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0 \u6750\u6599\u57fa\u56e0\u5de5\u7a0b<\/strong><\/p>\n<p>\u5bf9\u4f20\u7edf\u7684\u6750\u6599\u7814\u7a76\u6765\u8bf4\uff0c\u5927\u5bb6\u90fd\u662f\u4ece\u8bd5\u9519\u5f00\u59cb\uff0c\u4e00\u822c\u662f\u5408\u6210-\u68c0\u6d4b-\u5206\u6790-\u518d\u5408\u6210\u3002\u73b0\u5728\u5927\u5bb6\u90fd\u77e5\u9053\u4eba\u5de5\u667a\u80fd\u548c\u5927\u6570\u636e\u6210\u4e3a\u4e00\u4e2a\u65b0\u7684\u79d1\u5b66\u7814\u7a76\u7684\u65b0\u5de5\u5177\u3002\u4f46\u600e\u4e48\u66f4\u6709\u6548\u7684\u8fd0\u7528\u5927\u6570\u636e\u548c\u4eba\u5de5\u667a\u80fd\uff1f\u8fd9\u91cc\u9762\u6211\u4eec\u9700\u8981\u4e00\u4e9b\u65b0\u7684\u6570\u5b66\u65b9\u6cd5\u6709\u6548\u5730\u63cf\u8ff0\u6750\u6599\u9886\u57df\u7684\u7ed3\u6784\u4e0e\u6027\u80fd\u7684\u5173\u7cfb\u3002\u8fd9\u4e9b\u65b9\u6cd5\u5bf9\u6211\u4eec\u6750\u6599\u9886\u57df\u6765\u8bf4\u662f\u65b0\u7684\uff0c\u4f46\u662f\u8fd9\u4e9b\u6570\u5b66\u65b9\u6cd5\u4e0d\u4e00\u5b9a\u662f\u65b0\u7684\uff0c\u53ef\u80fd\u5df2\u7ecf\u5728\u7269\u7406\u3001\u8ba1\u7b97\u673a\u548c\u5176\u5b83\u7684\u5f88\u591a\u7684\u9886\u57df\u5df2\u7ecf\u4f7f\u7528\u8fc7\u5f88\u6709\u6548\uff0c\u5177\u6709\u5f3a\u5927\u7684\u529f\u80fd\u3002<\/p>\n<p>\u4eca\u5929\u6211\u5411\u5927\u5bb6\u6c47\u62a5\u7684\u9898\u76ee\u5c31\u662f\u56fe\u8bba\u4f5c\u4e3a\u4e00\u79cd\u6570\u5b66\u5de5\u5177\uff0c\u53ef\u4ee5\u7528\u6765\u6784\u5efa\u9ad8\u8d28\u91cf\u7684\u6750\u6599\u5927\u6570\u636e\uff0c\u6709\u6548\u5730\u7814\u7a76\u6750\u6599\u7684\u6784\u6548\u5173\u7cfb\u3002\u6709\u4e86\u5927\u6570\u636e\u4ee5\u540e\uff0c\u6211\u4eec\u53ef\u4ee5\u5728\u6570\u636e\u91cc\u9762\u5e94\u7528\u4eba\u5de5\u667a\u80fd\u53bb\u6316\u6398\u4e00\u4e9b\u76f8\u5173\u6027\uff0c\u5728\u65b0\u6750\u6599\uff0c\u7279\u522b\u662f\u65b0\u80fd\u6e90\u6750\u6599\u7684\u7814\u53d1\u4e2d\uff0c\u63a2\u7d22\u51fa\u201c\u6750\u6599\u57fa\u56e0\u201d\uff0c\u6216\u8005\u56de\u7b54\u6709\u6ca1\u6709\u6750\u6599\u57fa\u56e0\uff0c\u7528\u6765\u9884\u6d4b\u548c\u51b3\u5b9a\u6750\u6599\u7684\u6027\u80fd\u3002\u8fd9\u5c31\u662f\u6211\u4eca\u5929\u62a5\u544a\u7684\u4e3b\u8981\u5185\u5bb9\u3002\u5177\u4f53\u5185\u5bb9\u5206\u51e0\u4e2a\u65b9\u9762\uff0c\u9996\u5148\u8ddf\u5927\u5bb6\u63a2\u8ba8\u4e00\u4e0b\u201c\u4ec0\u4e48\u662f\u6750\u6599\u57fa\u56e0\uff1f\u201d \uff0c\u7136\u540e\u201c\u5982\u4f55\u5f00\u5c55\u6750\u6599\u57fa\u56e0\u7684\u7814\u7a76?\u201d\u7b49\u3002<\/p>\n<p>\u8bf4\u5230\u6750\u6599\u57fa\u56e0\uff0c\u5176\u540d\u5b57\u6cbf\u7528\u4e86\u662f\u751f\u547d\u79d1\u5b66\u4e2d\u201c\u57fa\u56e0\u201d\uff0c\u6211\u4eec\u77e5\u9053\u751f\u547d\u6709\u57fa\u56e0\uff0c\u5176\u51b3\u5b9a\u4e86\u751f\u547d\u7684\u4e0a\u4e00\u4ee3\u8ddf\u4e0b\u4e00\u4ee3\u4e4b\u95f4\u7684\u9057\u4f20\u3002\u6240\u4ee5\u5f53\u6211\u4eec\u5728\u7814\u7a76\u6750\u6599\u65f6\uff0c\u53ef\u4ee5\u53cd\u590d\u95ee\u6750\u6599\u6709\u6ca1\u6709\u201c\u57fa\u56e0\u201d\uff1f\u6750\u6599\u57fa\u56e0\u7684\u7279\u70b9\u662f\u4ec0\u4e48\uff1f\u600e\u4e48\u7814\u7a76\uff1f\u6211\u4eec\u5728\u505a\u9502\u7535\u6c60\u7814\u7a76\uff0c\u53ef\u4ee5\u901a\u8fc7\u63a2\u7d22\u9502\u7535\u6c60\u6750\u6599\u7684\u57fa\u56e0\uff0c\u6765\u53d1\u73b0\u6750\u6599\u57fa\u56e0\u7684\u5171\u540c\u7279\u70b9\uff0c\u5e76\u8fd0\u7528\u4e8e\u9502\u7535\u6c60\u53ca\u5176\u6750\u6599\u7684\u7814\u7a76\u3002<\/p>\n<p>\u5148\u8bb2\u8bb2\u6750\u6599\u57fa\u56e0\uff0c\u6750\u6599\u57fa\u56e0\u8fd9\u4e2a\u6982\u5ff5\u7531\u6765\u662f\u6e90\u4e8e\u7f8e\u56fd\u4e00\u4e9b\u667a\u5e93\u4e8e2011\u5e74\u5411\u5965\u5df4\u9a6c\u603b\u7edf\u63d0\u51fa\uff0c\u7f8e\u56fd\u672a\u6765\u7684\u56fd\u5bb6\u6218\u7565\u8981\u5f15\u9886\u79d1\u6280\uff0c\u9996\u5148\u8981\u5728\u6750\u6599\u4e0a\u5f15\u9886\uff0c\u65b0\u6750\u6599\u7814\u53d1\u4e0e\u5e94\u7528\u662f\u57fa\u7840\u3002\u4f20\u7edf\u6765\u8bf4\u4e00\u79cd\u9ad8\u6027\u80fd\u65b0\u6750\u6599\u4ece\u53d1\u73b0\u5f00\u59cb\u5230\u4ea7\u4e1a\u5e94\u7528\u9700\u898120\u591a\u5e74\uff0c\u56e0\u6b64\u6025\u9700\u63a2\u7d22\u7f29\u77ed\u8fd9\u4e2a\u65f6\u95f4\uff0c\u9700\u8981\u7814\u7a76\u7684\u65b0\u8303\u5f0f\uff0c\u76ee\u524d\u5df2\u5f62\u6210\u5171\u8bc6\u5e76\u6210\u4e3a\u5404\u56fd\u79d1\u6280\u7ade\u4e89\u7684\u53d1\u5c55\u6218\u7565\u3002\u8fd9\u91cc\u9762\u6211\u7279\u522b\u8ddf\u5927\u5bb6\u5206\u4eab\u4e00\u4e0b\uff0c\u4ec0\u4e48\u662f\u7269\u8d28\uff1f\u4ec0\u4e48\u662f\u6750\u6599\uff1f\u5982\u4f55\u4ece\u7269\u8d28\u7814\u7a76\u5230\u6750\u6599\u5f00\u53d1\u4e0e\u5e94\u7528\uff1f\u7269\u8d28\u662f\u7531\u5176\u7ed3\u6784\u6765\u5b9a\u4e49\u7684\uff0c\u7269\u8d28\u7ed3\u6784\uff08\u7ed3\u6784\u5316\u5b66\uff09\u662f\u7531\u76f8\u540c\u6216\u4e0d\u540c\u539f\u5b50\u4e4b\u95f4\u4ee5\u7279\u5b9a\u7684\u5316\u5b66\u952e\u8fde\u63a5\uff08\u539f\u5b50\u95f4\u5206\u4eab\u7535\u5b50\uff09\u53ca\u5176\u6392\u5e8f\u6784\u6210\u3002\u7269\u8d28\u662f\u6750\u6599\u7684\u57fa\u7840\uff0c\u6750\u6599\u8981\u9488\u5bf9\u4e0d\u540c\u9700\u6c42\u5bf9\u76f8\u5e94\u7684\u7269\u8d28\u8fdb\u884c\u8c03\u63a7\u3002\u4e00\u4e2a\u5178\u578b\u7684\u4f8b\u5b50\u662f\u5355\u6676\u7845\uff0c\u4f5c\u4e3a\u534a\u5bfc\u4f53\u82af\u7247\u5e94\u7528\u548c\u592a\u9633\u80fd\u7535\u6c60\u5e94\u7528\u7684\u5355\u6676\u7845\u6742\u8d28\u542b\u91cf\u7684\u8981\u6c42\u662f\u6709\u5de8\u5927\u5dee\u522b\u7684\u3002<\/p>\n<p>\u7f8e\u56fd2011\u5e74\u63d0\u51fa\u7684\u6750\u6599\u57fa\u56e0\u7ec4\u8ba1\u5212\uff0c\u8bd5\u56fe\u6539\u53d8\u6211\u4eec\u521a\u624d\u8bb2\u7684\u4f20\u7edf\u6750\u6599\u7814\u7a76\u7684\u8303\u5f0f\u3002\u6211\u4eec\u56fd\u5bb6\u4e5f\u610f\u8bc6\u5230\u901a\u8fc7\u6750\u6599\u7814\u7a76\u8303\u5f0f\u7684\u53d8\u9769\u5bf9\u52a0\u901f\u65b0\u6750\u6599\u7814\u53d1\u7684\u91cd\u8981\u6027\uff0c\u79d1\u5b66\u9662\u548c\u5de5\u7a0b\u9662\u8054\u5408\u5f00\u4e86\u597d\u591a\u6b21\u7814\u8ba8\u4f1a\uff0c\u4e8e2016\u5e74\uff0c\u6211\u4eec\u56fd\u5bb6\u8bbe\u7acb\u4e86\u201c\u6750\u6599\u57fa\u56e0\u5de5\u7a0b\u56fd\u5bb6\u91cd\u70b9\u7814\u53d1\u8ba1\u5212\u201d\uff0c\u6750\u6599\u57fa\u56e0\u5de5\u7a0b\u5c31\u662f\u8bf4\u628a\u751f\u547d\u57fa\u56e0\u5de5\u7a0b\u7684\u601d\u60f3\u7528\u5230\u6211\u4eec\u6750\u6599\u7684\u7814\u53d1\u4e2d\u6765\uff0c\u6240\u4ee5\u5728\u7b2c\u4e00\u671f\u7acb\u4e8610\u6765\u4e2a\u9879\u76ee\uff0c\u5176\u4e2d\u6709\u4e00\u4e2a\u9879\u76ee\u5c31\u662f\u5173\u4e8e\u6750\u6599\u57fa\u56e0\u5de5\u7a0b\u6765\u7814\u53d1\u4e0b\u4e00\u4ee3\u5168\u56fa\u6001\u7535\u6c60\u53ca\u5176\u5173\u952e\u6750\u6599\uff0c\u6211\u4eec\u8054\u5408\u9ad8\u6821\u548c\u4f01\u4e1a\u76f8\u5173\u56e2\u961f\u8054\u5408\u627f\u62c5\u5e76\u5b8c\u6210\u4e86\u8be5\u9879\u76ee\u3002\u00a0<\/p>\n<p><strong>\u4ec0\u4e48\u662f\u6750\u6599<\/strong><strong>\u57fa\u56e0\uff1f<\/strong><\/p>\n<p>\u5728\u627f\u62c5\u9879\u76ee\u8fc7\u7a0b\u4e2d\uff0c\u6211\u4eec\u4e0d\u65ad\u95ee\u5230\u5e95\u4ec0\u4e48\u662f\u201c\u6750\u6599\u57fa\u56e0\u5de5\u7a0b\u201d\uff0c\u5b83\u7684\u5185\u6db5\u53ca\u5176\u5916\u5ef6\u662f\u4ec0\u4e48\uff1f\u8fd9\u4e2a\u547d\u9898\u867d\u7136\u8fde\u5728\u4e00\u8d77\uff0c\u5b9e\u9645\u4e0a\u662f\u4e24\u5c42\u542b\u4e49\uff1a\u201c\u6750\u6599\u57fa\u56e0\u201d\u548c\u201c\u57fa\u56e0\u7ec4\u5de5\u7a0b\u201d\uff0c\u524d\u8005\u662f\u4e00\u4e2a\u5173\u4e8e\u79d1\u5b66\u95ee\u9898\u7684\u5b9a\u4e49\uff0c\u540e\u8005\u662f\u5173\u4e8e\u5982\u4f55\u5f00\u5c55\u7684\u5de5\u7a0b\u95ee\u9898\uff0c\u5de5\u7a0b\u5c31\u662f\u65b9\u6cd5\u548c\u6280\u672f\u3002\u53ef\u4ee5\u53c2\u7167\u751f\u547d\u57fa\u56e0\u5de5\u7a0b\u6210\u529f\u7684\u4e00\u4e9b\u65b9\u6cd5\u8bba\u3002\u4ec0\u4e48\u662f\u6750\u6599\u57fa\u56e0\u5462\uff1f\u5176\u5173\u952e\u662f\u6709\u6ca1\u6709\u201c\u6750\u6599\u57fa\u56e0\u201d\uff0c\u5982\u679c\u6709\u5b83\u5e94\u8be5\u53c8\u662f\u5982\u4f55\u8868\u8fbe\uff1f\u6211\u4eec\u53ef\u4ee5\u5148\u7c7b\u6bd4\u4e00\u4e0b\u751f\u547d\u57fa\u56e0\uff0c\u7136\u540e\u518d\u6316\u6398\u6750\u6599\u57fa\u56e0\u7684\u5173\u952e\u8981\u7d20\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u7c7b\u6bd4\uff1a\u751f\u547d\u57fa\u56e0<\/strong><strong>\u00a0vs.\u00a0<\/strong><strong>\u6750\u6599\u57fa\u56e0<\/strong><\/p>\n<p>\u5f88\u4e45\u4ee5\u6765\u751f\u7269\u73b0\u8c61\u89c2\u5bdf\u53d1\u73b0\u4e0a\u4e00\u4ee3\u548c\u4e0b\u4e00\u4ee3\u67d0\u79cd\u7279\u6027\u76f8\u4f3c\uff0c\u53eb\u751f\u547d\u9057\u4f20\u73b0\u8c61\uff0c\u968f\u7740\u7269\u7406\u5b66\u548c\u5316\u5b66\u7406\u8bba\u548c\u6d4b\u91cf\u6280\u672f\u7684\u53d1\u5c55\uff0c\u624d\u53d1\u73b0\u6709\u4e00\u4e2a\u51b3\u5b9a\u751f\u547d\u9057\u4f20\u7684\u201c\u57fa\u56e0\u201d\uff0c\u5b83\u6709\u6700\u57fa\u672c\u7684\u5206\u5b50\u7ed3\u6784\u57fa\uff0c\u5305\u62ec4\u79cd\u78b1\u57fa\u7684\u529f\u80fd\u7ed3\u6784\u57fa\u5143\uff0c\u78b1\u57fa\u4e4b\u95f4\u4ee5\u5171\u4ef7\u5316\u5b66\u952e\u4ee5\u7279\u5b9a\u7684\u6392\u5e8f\u8fde\u63a5\u5728\u4e00\u6761\u94fe\u4e0a\uff0c\u8fd9\u4e24\u6761\u94fe\u4e4b\u95f4\u4ee5\u6c22\u952e\u6784\u6210\u53cc\u87ba\u65cb\u7ed3\u6784\uff0c\u5de6\u8fb9\u94fe\u548c\u53f3\u8fb9\u94fe\u4e4b\u95f4\u8c61\u94a5\u5319\u548c\u9501\u4e00\u6837\u4ee5\u6c22\u952e\u4e3a\u76f8\u4e92\u4f5c\u7528\u529b\u4ee5\u53ca\u7279\u5b9a\u7a7a\u95f4\u8026\u5408\u7ed3\u6784\uff0c\u662f\u4e00\u4e00\u5bf9\u5e94\u7684\uff0c\u4e00\u65e6\u77e5\u9053\u4e86\u5de6\u8fb9\u7ed3\u6784\u4e5f\u5c31\u77e5\u9053\u4e86\u53f3\u8fb9\u7ed3\u6784\uff0c\u4fdd\u8bc1\u5f88\u7cbe\u786e\u7684\u53bb\u590d\u5236\u3002\u51b3\u5b9a\u9057\u4f20\u6027\u72b6\u5c31\u662f\u4e00\u6bb5\u8fd9\u4e9b\u529f\u80fd\u7ed3\u6784\u57fa\u5143\u7684\u6392\u5e8f\u3002\u56e0\u6b64\u751f\u547d\u57fa\u56e0\u91cc\u5305\u542b\u4e86\u4e09\u5927\u8981\u7d20\uff0c\uff081\uff09\u57fa\u672c\u7684\u7ed3\u6784\u57fa\u5143\uff0c\u5305\u62ec\u78b1\u57fa4\u79cd\uff0c\u76f8\u770b\u8d77\u6765\u6bd4\u8f83\u7b80\u5355\u4f46\u53ef\u4ee5\u7ec4\u5408\u6210\u975e\u5e38\u590d\u6742\u7684\u6392\u5e8f\uff0c\u751f\u547d\u4e3a\u4ec0\u4e48\u9009\u8fd9\u79cd4\u79cd\u78b1\u57fa\uff0c\u8bf4\u5b9e\u5728\u6211\u4eec\u73b0\u5728\u4e5f\u4e0d\u5f97\u5176\u89e3\uff1b\uff082\uff094\u79cd\u78b1\u57fa\u7684\u6392\u5e8f\uff1b\uff083\uff09\u78b1\u57fa\u4e4b\u95f4\u7684\u76f8\u4e92\u4f5c\u7528\uff0c\u5305\u62ec\u94fe\u5185\u662f\u5f3a\u76f8\u4e92\u4f5c\u7528\u7684\u5171\u4ef7\u952e\uff08\u79f0\u4e4b\u4e3a\u5316\u5b66\u952e\uff09\uff0c\u94fe\u95f4\u662f\u5f31\u76f8\u4e92\u4f5c\u7528\u7684\u6c22\u952e\u3002<\/p>\n<p>\u6211\u4eec\u518d\u770b\u770b\u6211\u4eec\u7684\u6750\u6599\u4e16\u754c\uff0c\u4ec0\u4e48\u53eb\u6750\u6599\uff1f\u5c31\u662f\u539f\u5b50\u4eec\u5728\u4e00\u8d77\u4ee5\u4e0d\u540c\u7684\u65b9\u5f0f\u7ed3\u5408\u4e0e\u76f8\u4e92\u4f5c\u7528\u3002\u539f\u5b50\u7684\u7279\u70b9\u662f\u57fa\u4e8e\u539f\u5b50\u7684\u8d28\u5b50\u6570\u4ee5\u53ca\u7535\u5b50\u6570\uff0c\u6027\u8d28\u4e3b\u8981\u4e0e\u5916\u5c42\u7535\u5b50\u6570\u76f8\u5173\u3002\u95e8\u6377\u5217\u592b\u4ece\u5143\u7d20\u4e4b\u95f4\u7684\u6027\u80fd\u76f8\u4f3c\u6027\u5f97\u5230\u7684\u5468\u671f\u8868\uff0c\u53ef\u4ee5\u8bf4\u662f\u7b2c\u4e00\u5f20\u7269\u8d28\/\u6750\u6599\u57fa\u56e0\u89c4\u5f8b\u7684\u56fe\u8868\u3002\u91cf\u5b50\u529b\u5b66\u7684\u4e00\u5927\u6210\u7ee9\u80fd\u591f\u53d1\u73b0\u548c\u89e3\u91ca\u5176\u539f\u56e0\uff0c\u4e0d\u540c\u5143\u7d20\u6709\u4e0d\u540c\u7684\u5916\u5c42\u7535\u5b50\u4ece\u800c\u6709\u4e0d\u540c\u7684\u5f97\/\u5931\u7535\u5b50\u7684\u80fd\u529b\uff0c\u8fd9\u51b3\u5b9a\u4e86\u5b83\u5728\u6784\u6210\u6750\u6599\u65f6\u5728\u7ed3\u6784\u57fa\u5143\u4e2d\u7684\u89d2\u8272\u4e0e\u5468\u56f4\u7684\u6392\u5e8f\u4e0e\u76f8\u4e92\u4f5c\u7528\u529b\u3002<\/p>\n<p>\u6240\u4ee5\uff0c\u6750\u6599\u57fa\u56e0\u548c\u751f\u547d\u57fa\u56e0\u6709\u7740\u76f8\u4f3c\u7684\u5730\u65b9\uff0c\u4ece\u539f\u5b50\u7684\u5c3a\u5ea6\u6765\u7406\u89e3\u751f\u547d\u57fa\u56e0\u548c\u6750\u6599\u57fa\u56e0\uff0c\u4e8c\u8005\u5173\u952e\u5171\u540c\u8981\u7d20\u90fd\u662f\u529f\u80fd\u7ed3\u6784\u57fa\u5143\u53ca\u5176\u5b83\u4eec\u4e4b\u95f4\u76f8\u4e92\u4f5c\u7528\u548c\u6392\u5e8f\u3002\u4e00\u822c\u8ba4\u4e3a\u4e00\u4e2a\u6750\u6599\u7279\u5f81\u548c\u6027\u80fd\u7531\u5176\u7ec4\u6210\u4e0e\u7ed3\u6784\u51b3\u5b9a\uff0c\u66f4\u6df1\u5c42\u6b21\u201c\u6750\u6599\u57fa\u56e0\u201d\u63a2\u7d22\u662f\u7531\u5176\u529f\u80fd\u7ed3\u6784\u57fa\u56e2\u4ee5\u53ca\u76f8\u5173\u7684\u6392\u5e8f\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u751f\u547d\u3001\u6750\u6599<\/strong><strong>\u00a0vs\u00a0<\/strong><strong>\u57fa\u56e0<\/strong><\/p>\n<p>\u6211\u4eec\u4ece\u5b8f\u89c2\u5c3a\u5ea6\u6765\u6bd4\u8f83\u6750\u6599\u548c\u751f\u547d\uff0c\u5b83\u4eec\u90fd\u5e94\u8be5\u9075\u5faa\u70ed\u529b\u5b66\u5b9a\u7406\uff0c\u5176\u6f14\u5316\u90fd\u5e94\u8be5\u7b26\u5408\u70ed\u529b\u5b66\u7b2c\u4e8c\u5b9a\u7406\uff0cG=H-ST\uff0cG\u662f\u5409\u5e03\u65af\u81ea\u7531\u80fd\uff0c\u7531\u80fd\u91cf\u9879\uff08H\uff0c\u7113\uff0c\u5bf9\u5e94\u5185\u80fd\uff09\u4e0e\u6709\u5e8f\u5ea6\u9879\uff08S\u662f\u71b5\uff0cT\u662f\u6e29\u5ea6\uff09\u6765\u51b3\u5b9a\uff0c\u7cfb\u7edf\u662f\u81ea\u7531\u80fd\u662f\u8d1f\u7684\u65b9\u5411\u81ea\u53d1\u8fc7\u7a0b\uff0c\u5f53\u80fd\u91cf\u76f8\u5728\u53d1\u751f\u524d\u540e\u53d8\u5316\u4e0d\u5927\u65f6\uff0c\u71b5\u589e\u52a0\uff08\u65e0\u5e8f\u5ea6\u589e\u52a0\uff09\u4f1a\u6210\u4e3a\u81ea\u53d1\u7684\u8fc7\u7a0b\u3002\u4fe1\u606f\uff08\u9700\u8981\u8f93\u5165\u80fd\u91cf\uff09\u7684\u672c\u8d28\u662f\u6d88\u9664\u4e0d\u786e\u5b9a\u6027\u7684\u91cf\u5ea6\uff0c\u71b5\u548c\u4fe1\u606f\u5bf9\u7cfb\u7edf\u63cf\u8ff0\u5728\u672c\u8d28\u4e0a\u662f\u4e00\u81f4\u7684\uff0c\u662f\u5bf9\u7269\u8d28\u4e16\u754c\u548c\u751f\u547d\u7684\u4fe1\u606f\u8868\u8fbe\u3002\u751f\u547d\u662f\u4e00\u4e2a\u6709\u5e8f\u7684\u7ed3\u6784\u7cfb\u7edf\uff0c\u5728\u5f00\u653e\u7684\u4f53\u7cfb\u91cc\uff0c\u80fd\u91cf\u7684\u8f93\u5165\u53ef\u4ee5\u7ef4\u6301\u5176\u6709\u5e8f\u8fd0\u884c\u548c\u4fdd\u6301\u5176\u6709\u5e8f\u5ea6\uff0c\u907f\u514d\u4e0d\u786e\u5b9a\u6027\u56e0\u7d20\u7684\u5e72\u6270\u5176\u6709\u6709\u5e8f\u8fd0\u884c\u3002\u6750\u6599\u7684\u5408\u6210\u6216\u8005\u6750\u6599\u7684\u4f7f\u7528\uff0c\u5b9e\u9645\u4e0a\u662f\u5728\u4e00\u4e2a\u5f00\u653e\u7684\u4f53\u7cfb\u91cc\u9762\u8fdb\u884c\uff0c\u6709\u4e00\u4e2a\u80fd\u91cf\u6d41\u7684\u8f93\u5165\u53ef\u4ee5\u9a71\u52a8\u7ed3\u6784\u7684\u5e8f\u6392\uff0c\u589e\u52a0\u6709\u5e8f\u5ea6\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u751f\u547d\u4e0e\u6750\u6599\u57fa\u56e0\uff1a\u4e09\u8981\u7d20\uff08\u7ed3\u6784\u57fa\u5143\u3001\u76f8\u4e92\u4f5c\u7528\u3001\u6392\u5e8f\uff09<\/strong><\/p>\n<p>\u57fa\u4e8e\u4ece\u5fae\u89c2\u548c\u5b8f\u89c2\u5c3a\u5ea6\u5bf9\u6bd4\uff0c\u7528\u70ed\u529b\u5b66\u5206\u6790\u6750\u6599\u548c\u751f\u547d\u90fd\u6709\u4e24\u5927\u8981\u7d20\uff0c\u4e00\u4e2a\u662f\u80fd\u91cf\u90e8\u5206\u3001\u4e00\u4e2a\u662f\u4fe1\u606f\u90e8\u5206\u3002\u80fd\u91cf\u90e8\u5206\uff0c\u662f\u7269\u8d28\u4e4b\u95f4\u7684\u76f8\u4e92\u4f5c\u7528\u7684\u5f3a\u5ea6\uff0c\u76f8\u4e92\u4f5c\u7528\u7684\u5f3a\u5ea6\u7531\u8c01\u51b3\u5b9a\uff1f\u80af\u5b9a\u662f\u7531\u7ec4\u6210\u7269\u8d28\u7684\u5143\u7d20\uff0c\u4ee5\u53ca\u8fd9\u4e9b\u5143\u7d20\u4e4b\u95f4\u7684\u5f97\u5931\u7535\u5b50\u80fd\u529b\u7684\u5dee\u5f02\uff0c\u53eb\u7535\u8d1f\u6027\uff0c\u5f62\u6210\u4e0d\u540c\u4e92\u76f8\u4f5c\u7528\u7c7b\u578b\uff0c\u5373\u4e0d\u540c\u5316\u5b66\u952e\u3002\u5f53\u539f\u5b50\u95f4\u7684\u7535\u8d1f\u6027\u5dee\u522b\u5f88\u5927\uff0c\u5931\u53bb\u7535\u5b50\u7684\u5f62\u6210\u6b63\u79bb\u5b50\u6216\u8005\u5f97\u5230\u7535\u5b50\u7684\u5f62\u6210\u8d1f\u79bb\u5b50\uff0c\u6b63\u8d1f\u79bb\u5b50\u4e4b\u95f4\u5f62\u6210\u79bb\u5b50\u952e\u3002\u5f53\u7535\u8d1f\u6027\u5dee\u522b\u4e0d\u5927\uff0c\u672c\u8eab\u53c8\u4e0d\u662f\u90a3\u4e48\u5bb9\u6613\u5931\u53bb\u548c\u5f97\u5230\u7535\u5b50\u65f6\u4e00\u822c\u662f\u91c7\u7528\u5171\u4eab\u7535\u5b50\u5f62\u6210\u5171\u4ef7\u952e\u3002\u91d1\u5c5e\u6676\u4f53\u4e2d\u7684\u91d1\u5c5e\u5171\u4eab\u6e38\u79bb\u7684\u7535\u5b50\u5f62\u6210\u91d1\u5c5e\u952e\u3002\u6839\u636e\u7ed3\u6784\u57fa\u5143\u5728\u6750\u6599\u4e2d\u53d1\u6325\u7684\u4f5c\u7528\u53ef\u4ee5\u5206\u7c7b\u6210\u4e3a\u4e0d\u540c\u7684\u529f\u80fd\u7ed3\u6784\u57fa\u56e2\u3002\u5728\u9502\u7535\u6c60\u4e2d\u6bd4\u8f83\u7279\u6b8a\u7684\u6b63\u6781\u6750\u6599\u6709\u8fc7\u6e21\u91d1\u5c5e\u5143\u7d20\u53d8\u4ef7\u5b9e\u73b0\u50a8\u80fd\uff0c\u8fc7\u6e21\u91d1\u5c5e\u5143\u7d20\u6700\u5927\u7684\u7279\u70b9\u662f\u5176\u5916\u56f4d-\u8f68\u9053\u81ea\u65cb\u7535\u5b50\uff0c\u5176\u6c27\u5316\u7269\u7684\u8fc7\u6e21\u91d1\u5c5e\u914d\u4f4d\u591a\u9762\u4f53\u4e4b\u95f4\u901a\u8fc7\u6c27\u4f5c\u4e3a\u8fde\u63a5\u70b9\u5f62\u6210d-\u81ea\u65cb\u7535\u5b50\u4e4b\u95f4\u8d85\u4ea4\u6362\u76f8\u4e92\u4f5c\u7528\u3002\u56e0\u6b64\uff0c\u6750\u6599\u57fa\u56e0\u7684\u80fd\u91cf\u90e8\u5206\u5c31\u662f\u529f\u80fd\u57fa\u56e2\u53ca\u5176\u76f8\u4e92\u4f5c\u7528\uff0c\u6709\u5e8f\u5ea6\uff08\u4fe1\u606f\u90e8\u5206\uff09\u662f\u5b83\u4eec\u7684\u6392\u5e8f\u90e8\u5206\u548c\u5bf9\u79f0\u6027\u3002<\/p>\n<p>\u7269\u7406\u4e16\u754c\u6700\u6709\u8da3\u662f\u5b83\u5b58\u5728\u5bf9\u79f0\u6027\uff0c\u5b83\u8d2f\u7a7f\u5728\u7269\u7406\u5b9a\u7406\u548c\u6750\u6599\u7684\u7ed3\u6784\u4e0e\u6027\u80fd\uff0c\u8fd9\u53ef\u662f\u6210\u4e3a\u6211\u4eec\u7814\u7a76\u6750\u6599\u57fa\u56e0\u7684\u4e00\u4e2a\u5207\u5165\u70b9\u3002\u6211\u4eec\u518d\u770b\u90a3\u4e2a\u5143\u7d20\u5468\u671f\u8868\uff0c\u6bcf\u4e2a\u5143\u7d20\u5b83\u5728\u4e0d\u540c\u72b6\u6001\u4e0b\uff0c\u6709\u5176\u534a\u5f84\u3001\u4ef7\u6001\u4ee5\u53ca\u4e0e\u8fd1\u90bb\u7684\u76f8\u4e92\u4f5c\u7528\u80fd\u529b\uff0c\u5f00\u5c55\u6750\u6599\u57fa\u56e0\u7814\u7a76\uff0c\u6700\u597d\u7684\u529e\u6cd5\u662f\u501f\u9274\u4e2d\u56fd\u4f20\u7edf\u54f2\u5b66\u2018\u9053\u6cd5\u81ea\u7136\u2019\u3002\u81ea\u7136\u754c\u5df2\u7ecf\u6709\u5f88\u591a\u81ea\u7136\u5b58\u5728\u7684\u6216\u5df2\u7ecf\u4eba\u5de5\u5408\u6210\u6676\u4f53\u6750\u6599\uff0c\u53ef\u4ee5\u5411\u5df2\u77e5\u6750\u6599\u7ed3\u6784\u5b66\u4e60\uff0c\u56e0\u6b64\u9700\u8981\u628a\u6240\u6709\u6750\u6599\u7684\u7269\u8d28\u7ed3\u6784\u6536\u96c6\u8d77\u6765\u5f62\u6210\u6750\u6599\u5927\u6570\u636e\uff0c\u7136\u540e\u6316\u6398\u6750\u6599\u57fa\u56e0\u7684\u4fe1\u606f\uff0c\u5f00\u5c55\u57fa\u4e8e\u6570\u636e\u9a71\u52a8\u6750\u6599\u79d1\u5b66\u7814\u7a76\u3002<\/p>\n<p><strong>\u5982\u4f55\u5f00\u5c55\u6750\u6599\u57fa\u56e0\u7684\u7814\u7a76\uff1f<\/strong><\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u6750\u6599\u7814\u7a76\u65b0\u8303\u5f0f(\u6570\u636e\u9a71\u52a8)<\/strong><\/p>\n<p>\u6700\u8fd1\u6709\u4e00\u672c\u4e66\u53eb\u7b2c\u56db\u4e2a\u8303\u5f0f\uff0c\u5b83\u628a\u79d1\u5b66\u7814\u7a76\u8303\u5f0f\u8fdb\u884c\u5206\u7c7b\uff0c\u7b2c\u4e00\u4e2a\u8303\u5f0f\uff0c\u662f\u6211\u4eec\u6700\u65e9\u7684\u4eba\u7c7b\u8fdb\u884c\u4e86\u79d1\u5b66\u6d3b\u52a8\uff0c\u5f00\u59cb\u5236\u5907\u79d1\u5b66\u4eea\u5668\u5bf9\u81ea\u7136\u73b0\u8c61\u8fdb\u884c\u89c2\u5bdf\uff0c\u5bf9\u89c2\u5bdf\u7684\u6570\u636e\u8fdb\u884c\u6536\u96c6\u3002\u4f8b\u5982\u5f00\u666e\u52d2\u7b49\u7528\u79d1\u5b66\u4eea\u5668\u89c2\u5bdf\u5929\u4f53\uff0c\u79ef\u7d2f\u4e86\u89c2\u5bdf\u6570\u636e\uff0c\u5f97\u5230\u5730\u7403\u7ed5\u592a\u9633\u8fd0\u52a8\u7684\u6570\u636e\u3002\u7b2c\u4e8c\u4e2a\u8303\u5f0f\u662f\u4ece\u8fd9\u4e9b\u6570\u636e\u627e\u51fa\u79d1\u5b66\u89c4\u5f8b\uff0c\u6bd4\u5982\u8bf4\u5730\u7403\u56f4\u7ed5\u7740\u592a\u9633\u7684\u8fd0\u52a8\u662f\u692d\u5706\u8fd8\u662f\u5706\uff0c\u8fd8\u662f\u5706\u5f88\u591a\u7684\u5706\u7684\u53e0\u52a0\u7b49\u7b49\uff0c\u6700\u540e\u725b\u987f\u603b\u7ed3\u51fa\u4e07\u6709\u5f15\u529b\u5b9a\u5f8b\uff0c\u81ea\u7136\u754c\u7684\u8fd0\u52a8\u89c4\u5f8b\u4ee5\u7b80\u5355\u65b9\u7a0b\u6765\u63cf\u8ff0\uff0c\u5f97\u5230\u7269\u8d28\u76f8\u4e92\u4f5c\u7528\u529b\uff08\u5f15\u529b\uff09\u90fd\u662f\u8ddf\u8ddd\u79bb\u5e73\u65b9\u6210\u53cd\u6bd4\uff0c\u5929\u4e0a\u7684\u89c4\u5f8b\u4e0e\u5730\u4e0a\u7684\u76f8\u4e92\u4f5c\u7528\u4e0e\u76f8\u5173\u8fd0\u52a8\u7684\u89c4\u5f8b\u7684\u4e00\u6837\u7684\uff0c\u7531\u6b64\u5efa\u7acb\u4e86\u7ecf\u5178\u529b\u5b66\u3002\u5728\u7814\u7a76\u5fae\u89c2\u7c92\u5b50\u76f8\u4e92\u4f5c\u7528\u7684\u65f6\u5019\uff0c\u53d1\u73b0\u4e86\u5fae\u89c2\u4e16\u754c\u52a8\u91cf\u4e0e\u4f4d\u7f6e\u4e0d\u80fd\u540c\u65f6\u7cbe\u786e\u6d4b\u91cf\u7684\u4e0d\u786e\u5b9a\u6027\u539f\u7406\uff0c\u5f62\u6210\u4e86\u91cf\u5b50\u529b\u5b66\u4f53\u7cfb\u3002\u7231\u56e0\u65af\u5766\u53c8\u53d1\u73b0\u4e86\u6211\u4eec\u751f\u6d3b\u7684\u7269\u8d28\u4e0e\u80fd\u91cf\u3001\u7a7a\u95f4\u4e0e\u65f6\u95f4\u4e0d\u80fd\u5206\u5272\uff0c\u53ef\u4ee5\u7edf\u4e00\u6765\u8868\u8fbe\u4e00\u4e2a\u65f6\u7a7a\u4e0e\u7269\u8d28\u80fd\u91cf\u7684\u65b9\u7a0b\u8868\u8fbe\u5f0f\uff0c\u56e0\u6b64\u6574\u4e2a\u4e16\u754c\u6709\u4e86\u57fa\u7840\u7684\u76f8\u4e92\u4f5c\u7528\u7684\u7269\u7406\u8868\u8fbe\u5f0f\u3002\u503c\u5f97\u5f3a\u8c03\u7684\u662f\u6211\u4eec\u5b9e\u9645\u751f\u6d3b\u5728\u7684\u4e16\u754c\u662f\u590d\u6742\u7684\uff0c\u5982\u6d77\u4e0a\u7684\u6ce2\u6d6a\u4ee5\u53ca\u9e1f\u7684\u98de\u884c\uff0c\u90fd\u4e0d\u80fd\u7528\u7b80\u5355\u7684\u65b9\u7a0b\u6765\u63cf\u8ff0\uff0c\u5728\u505a\u4e00\u67b6\u98de\u673a\u7b49\u5927\u5de5\u7a0b\u65f6\u8981\u7528\u6570\u636e\u4eff\u771f\u548c\u6a21\u62df\uff0c\u79f0\u4e4b\u4e3a\u7b2c\u4e09\u4e2a\u8303\u5f0f\u3002\u73b0\u5728\u6211\u4eec\u5df2\u7ecf\u6709\u5927\u91cf\u7684\u79d1\u5b66\u548c\u5de5\u7a0b\u6570\u636e\uff0c\u590d\u6742\u7cfb\u7edf\u80cc\u540e\u90fd\u6709\u5b58\u5728\u4e0d\u540c\u5c42\u6b21\u7684\u76f8\u4e92\u4f5c\u7528\uff0c\u6709\u4e00\u5bf9\u4e00\u7684\u76f8\u4e92\u4f5c\u7528\uff0c\u4e5f\u6709\u591a\u4f53\u590d\u6742\u7684\u76f8\u4e92\u4f5c\u7528\uff0c\u8fd9\u4e9b\u76f8\u4e92\u4f5c\u7528\u80cc\u540e\u662f\u6709\u5e95\u5c42\u7684\u7269\u7406\u539f\u56e0\u3001\u903b\u8f91\u5173\u7cfb\uff0c\u57fa\u4e8e\u5927\u6570\u636e\u548c\u4eba\u5de5\u667a\u80fd\u7684\u79d1\u5b66\u4e0e\u5de5\u7a0b\u7814\u53d1\u79f0\u4e4b\u4e3a\u7b2c\u56db\u4e2a\u8303\u5f0f\u3002<\/p>\n<p>\u901a\u8fc7\u6536\u96c6\u7ed3\u6784\u4e0e\u6027\u80fd\u6570\u636e\uff0c\u7528\u6570\u5b66\u8868\u8fbe\u548c\u4eba\u5de5\u667a\u80fd\u7b97\u6cd5\u53bb\u6316\u6398\u6784\u6548\u5173\u7cfb\uff0c\u5728\u6750\u6599\u79d1\u5b66\u4e0e\u5de5\u7a0b\u9886\u57df\uff0c\u5f00\u5c55\u57fa\u4e8e\u6750\u6599\u5927\u6570\u636e\u7684\u7ed3\u6784\u548c\u6027\u80fd\u7684\u76f8\u5173\u6027\u65b0\u8303\u5f0f\u7814\u7a76\u3002\u6750\u6599\u662f\u4e2a\u590d\u6742\u7cfb\u7edf\uff0c\u5f88\u96be\u51c6\u786e\u7684\u8ba1\u7b97\uff0c\u6240\u4ee5\u9700\u8981\u53d1\u73b0\u6709\u6548\u7684\u6570\u5b66\u8868\u8fbe\u548c\u8ba1\u7b97\u65b9\u6cd5\u8282\u7701\u8fd0\u7b97\u7684\u65f6\u95f4\uff0c\u80fd\u591f\u76f4\u63d2\u95ee\u9898\u7684\u672c\u8d28\uff0c\u8fd9\u662f\u8fd9\u4e2a\u62a5\u544a\u8981\u6c47\u62a5\u7684\u4e00\u4e9b\u601d\u8def\u548c\u53d6\u5f97\u7684\u8fdb\u5c55\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u6750\u6599\u5927\u6570\u636e vs \u4ece\u6570\u636e\u5230\u77e5\u8bc6\uff1f<\/strong><\/p>\n<p>\u56fd\u5916\u51e0\u4e2a\u56e2\u961f\u5df2\u7ecf\u5f00\u5c55\u4e86\u6750\u6599\u7684\u5927\u6570\u636e\u5efa\u8bbe\uff0c\u5728\u9502\u7535\u6c60\u9886\u57df\u4f2f\u514b\u5229Ceder\u6559\u6388\u5efa\u7acb\u4e86\u201cMaterial-project\u201d\uff0c \u901a\u8fc7\u5b9e\u9a8c\u5f97\u5230\u6676\u4f53\u7ed3\u6784\u6570\u636e\u8ba1\u7b97\u51fa\u7684\u80fd\u5e26\u548c\u70ed\u529b\u5b66\u53c2\u6570\u4ee5\u53ca\u9502\u7535\u6c60\u7684\u6027\u80fd\uff0c\u5f88\u591a\u4eba\u90fd\u5728\u7528\u3002\u6b64\u5916\u8fd8\u6709\u7f8e\u56fd\u675c\u514b\u5927\u5b66\u548c\u897f\u5317\u5927\u5b66\u5efa\u8bbe\u6750\u6599\u6570\u636e\u5e93\uff0c\u5176\u5305\u62ec\u4e86\u8bb8\u591a\u5b9e\u9a8c\u4e0e\u8ba1\u7b97\u9884\u6d4b\u7684\u65b0\u6750\u6599\u6570\u636e\u3002ICSD\u662f\u4f20\u7edf\u7684\u65e0\u673a\u6676\u4f53\u7ed3\u6784\u6570\u636e\u5e93\uff0c\u5b83\u7684\u6765\u6e90\u662f\u5404\u56fd\u5b9e\u9a8c\u5ba4\u53d1\u8868\u6587\u7ae0\u7684\u6676\u4f53\u7ed3\u6784\u6570\u636e\u3002\u5404\u56fd\u4e0d\u540c\u7684\u6750\u6599\u534f\u4f1a\uff0c\u50cf\u7f8e\u56fd\u9676\u74f7\u534f\u4f1a\u6709\u81ea\u5df1\u7684\u6570\u636e\u5e93\uff0c\u6709\u673a\u5316\u5408\u7269\u6709\u5251\u6865\u6570\u636e\u5e93\u7b49\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u4f20\u7edf\u6676\u4f53\u7ed3\u6784\u5316\u5b66\uff1a\u8bc6\u522b\u540c\u6784\u6027\u6311\u6218<\/strong><\/p>\n<p>ICSD\u5b9e\u9a8c\u6570\u636e\u5927\u6982\u5df2\u7ecf\u670918\u4e07\u4e2a\uff0c\u6bcf\u5e74\u90fd\u589e\u52a0\u4e00\u4e24\u4e07\u4e2a\u65b0\u7684\u65e0\u673a\u6676\u4f53\u7ed3\u6784\u6570\u636e\uff0c\u4ee5\u6c2f\u5316\u94a0\u7ed3\u6784\u6570\u636e\u4e3a\u4f8b\u5df2\u7ecf\u670934\u6761\uff0c\u6765\u81ea\u4e8e\u4e0d\u540c\u5e74\u4ee3\u548c\u4e0d\u540c\u7684\u5b9e\u9a8c\u5ba4\u6d4b\u91cf\u7684\u6570\u636e\uff0c\u6309\u7167\u4f20\u7edf\u7ed3\u6676\u5b66\u6216\u7ed3\u6784\u5316\u5b66\u7684\u65b9\u6cd5\u662f\u7528x-\u5c04\u7ebf\u884d\u5c04\u6765\u6d4b\u5f97\u884d\u5c04\u70b9\u83b7\u5f97\u7279\u5b9a\u5bf9\u79f0\u6027\u4ee5\u53ca\u5bf9\u5e94\u7684\u5e73\u884c\u516d\u8fb9\u5f62\u6676\u80de\u683c\u5b50\u7c7b\u578b(\u6b63\u65b9\u3001\u957f\u65b9\u3001\u659c\u65b9\u3001\u4e09\u89d2\u6216\u516d\u89d2\u7b49)\u3001\u5927\u5c0f\uff08\u6676\u683c\u5e38\u6570,a\u3001b\u3001c\uff0c\u659c\u65b9\u6709\u9762\u5939\u89d2\u03b1\u3001\u03b2\u3001\u03b3\u7b49\uff09\u3001\u5404\u539f\u5b50\u5728\u6676\u80de\u4e2d\u6709\u4e0d\u540c\u7684\u4f4d\u7f6e\uff0c\u6839\u636e\u5bf9\u79f0\u6027\u53ef\u4ee5\u5f97\u5230\u591a\u5c11\u4e2a\u72ec\u7acb\u7684\u539f\u5b50\u4f4d\u7f6e\uff0c\u5177\u6709\u5bf9\u79f0\u5173\u7cfb\u7684\u539f\u5b50\u53ef\u4ee5\u7528\u5bf9\u79f0\u6027\u6362\u7b97\u51fa\u6765\u3002\u5bf9\u79f0\u5173\u7cfb\u7531\u70b9\u7fa4\u4e2d\u7684\u5bf9\u79f0\u64cd\u4f5c\uff08\u65cb\u8f6c\u3001\u6676\u9762\u3001\u53cd\u6f14\uff09\u63cf\u8ff0\uff0c\u70b9\u7fa4\u52a0\u4e0a\u5e73\u79fb\u64cd\u4f5c\u6784\u6210\u7a7a\u95f4\u7fa4\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u4f20\u7edf\u7ed3\u6784\u5316\u5b66\u6311\u6218: \u6676\u4f53\u7ed3\u6784\u7684\u201c\u6d4b\u4e0d\u51c6\u201d\u539f\u7406<\/strong><\/p>\n<p>\u7528\u4f20\u7edf\u7684\u7ed3\u6784\u5316\u5b66\u6765\u770bICSD\u4e2d\u7684\u6c2f\u5316\u94a0\u7acb\u65b9\u6676\u683c\u7684\u6676\u80de\u53c2\u6570\uff0c\u6700\u5c0f\u548c\u6700\u5927\u5dee\u5f97\u975e\u5e38\u5927\uff0c\u7ea6\u5dee0.04nm\uff0c\u6bd4x-\u5c04\u7ebf\u884d\u5c04\u7cbe\u5ea6(0.0001nm)\u5927\u7ea6\u591a\u51fa\u4e24\u4e2a\u6570\u91cf\u7ea7\u3002\u4e0d\u540c\u5b9e\u9a8c\u5ba4\u7684\u5236\u5907\u6761\u4ef6\u7684\u5dee\u5f02\u4f1a\u5bfc\u81f4\u6750\u6599\u5b58\u5728\u7f3a\u9677\u4e0d\u540c\u4ee5\u53ca\u6d4b\u91cf\u672c\u8eab\u6709\u8bef\u5dee\u90fd\u4f1a\u5bfc\u81f4\u6240\u6d4b\u91cf\u7684\u6676\u80de\u7684\u539f\u5b50\u5750\u6807\u4e0e\u95f4\u8ddd\u5b58\u5728\u5dee\u5f02\u3002\u5982\u679c\u7528\u6d4b\u91cf\u5355\u80de\u53c2\u6570\u4e0e\u4f4d\u7f6e\u6765\u5b9a\u4e49\u4e8c\u4e2a\u7ed3\u6784\u662f\u5426\u76f8\u540c\u5fc5\u7136\u9762\u4e34\u201c\u540c\u6784\u6027\u201d\u5224\u65ad\u7684\u9608\u503c\u8bbe\u5b9a\u7684\u95ee\u9898\uff0c\u5373\u5dee\u5f02\u591a\u5927\u8303\u56f4\u5185\u624d\u7b97\u540c\u6784\u7684\uff1f\u4f1a\u5f62\u6210\u4ee5\u4e0b2\u79cd\u60c5\u51b5\u201c\u4e0d\u786e\u5b9a\u6027\u201d\uff1a\u6d4b\u91cf\u8bef\u5dee\u9608\u503c\u5185\u8ba4\u4e3a\u662f\u76f8\u540c\u7684\u7ed3\u6784\u4e5f\u53ef\u80fd\u662f\u4e0d\u76f8\u540c\u7ed3\u6784\uff0c\u4ee5\u53ca\u6d4b\u91cf\u8bef\u5dee\u9608\u503c\u5916\u8ba4\u4e3a\u662f\u4e0d\u540c\u7ed3\u6784\u4e5f\u53ef\u80fd\u662f\u76f8\u540c\u7684\u7ed3\u6784\u3002\u4f20\u7edf\u7ed3\u6784\u5316\u5b66\u5c31\u6709\u8fd9\u4e48\u4e00\u4e2a\u201c\u540c\u6784\u6027\u8bc6\u522b\u201d\u7684\u6311\u6218\uff0c\u4f8b\u5982\u6676\u4f53\u7ed3\u6784\u4e2d\u7684\u6676\u80de\u53c2\u6570a\u548cb\u5206\u522b\u662f\u00a00.415\u7eb3\u7c73\u548c0.414\uff0c\u5982\u679c\u8bef\u5dee\u7684\u9608\u503c\u8bbe\u5b9a\u57280.002\uff0ca\u548cb\u4e24\u4e2a\u4e4b\u95f4\u6ca1\u6709\u5dee\u522b\uff0c\u5373a\u548cb\u76f8\u540c\uff0c\u5982\u679c\u9608\u503c\u8bbe\u5b9a\u57280.0005\uff0ca\u548cb\u662f\u4e0d\u540c\u7684\u3002\u770b\u6c2f\u5316\u94a0\u7684ICSD\u6570\u636e\uff0c\u6211\u4eec\u8bbe\u5b9a\u591a\u5927\u7684\u9608\u503c\u8ba4\u4e3a\u4e8c\u4e2aNaCl\u7ed3\u6784\u662f\u76f8\u7b49\u7684\uff1fSiC\u6709250\u591a\u79cd\u76f8\u7ed3\u6784\uff0c\u5373\u4f7f\u8bbe\u5b9a\u9608\u503c\u5f88\u5c0f\uff0c\u5b83\u4e5f\u53ef\u80fd\u662f\u4e0d\u540c\u7684\u76f8\u7ed3\u6784\u3002\u56e0\u6b64\uff0c\u5bf9\u5728\u8bbe\u5b9a\u8bef\u5dee\u9608\u503c\u5185\u8ba4\u4e3a\u76f8\u540c\u7684\u7ed3\u6784\uff0c\u4f1a\u627e\u5230\u4e00\u4e2a\u201c\u9ed1\u5929\u9e45\u201d\uff0c\u662f\u65b0\u7684\u4e0d\u540c\u7684\u7ed3\u6784\u3002<\/p>\n<p>\u6211\u4eec\u5728\u5efa\u7acb\u81ea\u5df1\u6750\u6599\u5927\u6570\u636e\u7684\u8fc7\u7a0b\u5f53\u4e2d\uff0c\u9762\u4e34\u7684\u4e00\u4e2a\u6311\u6218\u5c31\u662f\u7528\u4ec0\u4e48\u65b9\u6cd5\u6765\u8868\u8fbe\u6216\u5224\u65ad\u4e8c\u4e2a\u7ed3\u6784\u662f\u76f8\u540c\uff08\u540c\u6784\u6027\uff09\uff1f\u6d4b\u91cf\u603b\u662f\u6709\u8bef\u5dee\uff0c\u8981\u907f\u514d\u521a\u624d\u8bb2\u7684\u7ed3\u6784\u6d4b\u91cf\u5e26\u6765\u7684\u201c\u6d4b\u4e0d\u51c6\u201d\u7684\u95ee\u9898\uff0c\u6211\u4eec\u5c31\u60f3\u5230\u53e6\u5916\u4e00\u79cd\u601d\u60f3\uff0c\u4e0d\u53bb\u6bd4\u8f83\u6d4b\u91cf\u539f\u5b50\u4f4d\u7f6e\u7684\u7edd\u5bf9\u5927\u5c0f\uff0c\u800c\u662f\u5927\u6570\u636e\u7684\u601d\u60f3\u7814\u7a76\u4e8b\u7269\u4e4b\u95f4\u7684\u201c\u5173\u7cfb\u201d\uff0c\u5373\u7814\u7a76\u539f\u5b50\u548c\u539f\u5b50\u4e4b\u95f4\u7684\u76f8\u4e92\u8fde\u63a5\u5173\u7cfb\uff0c\u628a\u540c\u6784\u6027\u5224\u65ad\u8f6c\u6362\u6210\u6bd4\u8f83\u539f\u5b50\u4e4b\u95f4\u7684\u8fde\u63a5\u5173\u7cfb\uff0c\u7528\u8fde\u63a5\u5173\u7cfb\u7684\u7f51\u7edc\u56fe\u6765\u8868\u8fbe\u662f\u5426\u76f8\u540c\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u6570\u5b66\u65b9\u6cd5\uff1a\u00a0\u56fe\u8bba \u00a0<\/strong><\/p>\n<p>\u6570\u5b66\u56fe\u8bba\u662f\u6b27\u62c9\u5148\u521b\u5efa\uff0c\u4ee5\u6b64\u89e3\u51b3\u4e86\u8457\u540d\u4e03\u6865\u95ee\u9898\uff0c\u628a\u80fd\u5426\u4e00\u6b21\u8d70\u8fc77\u4e2a\u6865\uff08\u4e0d\u91cd\u590d\u8d70\uff09\u7684\u95ee\u9898\u62bd\u8c61\u4e3a\u70b9\u4e0e\u8fb9\uff08\u4e24\u70b9\u4e4b\u95f4\u7684\u8fde\u901a\u7684\u8868\u8fbe\u6210\u8fb9\uff0c\u4e24\u70b9\u4e4b\u95f4\u4e0d\u8fde\u901a\u5c31\u6ca1\u6709\u8fb9\uff09\u6784\u6210\u7684\u56fe\u3002\u70b9\u4e0e\u70b9\u4e4b\u95f4\u6709\u8fde\u901a\u4e0e\u65ad\u5f00\uff0c\u4f8b\u5982\u4e24\u4e2a\u70b9\u9694\u7740\u6cb3\u6ca1\u6709\u6865\u5c31\u4e0d\u80fd\u8fde\u901a\u3002\u56fe\u8bba\u7684\u57fa\u672c\u601d\u60f3\u5c31\u662f\u8bf4\u628a\u662f\u81ea\u7136\u754c\u7684\u7269\u53ef\u4ee5\u62bd\u8c61\u6210\u201c\u70b9\u201d\uff0c\u70b9\u4e4b\u95f4\u662f\u8fde\u901a\u53ef\u4ee5\u7528\u201c\u7ebf\u201d\u8868\u8fbe\uff0c\u4e0d\u8fde\u901a\u5c31\u662f\u65ad\u5f00\u7684\uff0c\u8fd9\u201c\u70b9\u201d\u4e0e\u201c\u7ebf\u201d\u5c31\u6784\u6210\u4e86\u4e00\u5f20\u56fe\uff0c\u6211\u4eec\u628a\u8fd9\u4e2a\u601d\u60f3\u5c31\u7528\u5230\u6676\u4f53\u548c\u6750\u6599\u4e2d\u6765\u8868\u8fbe\u7ed3\u6784\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u7ed3\u6784\u5316\u5b66\u65b0\u8868\u8fbe\uff1a\u56fe\u8bba<\/strong><\/p>\n<p>\u6211\u4eec\u53ef\u4ee5\u628a\u6676\u4f53\u7ed3\u6784\u91cc\u9762\u539f\u5b50\u62bd\u8c61\u6210\u56fe\u8bba\u7684\u70b9\uff0c\u5982\u679c\u8fd9\u4e24\u4e2a\u70b9\u6709\u5316\u5b66\u952e\u53ef\u4ee5\u8ba4\u4e3a\u7535\u5b50\u5728\u4e24\u4e2a\u539f\u5b50\u95f4\u662f\u8fde\u901a\uff0c\u8868\u8fbe\u6210\u56fe\u8bba\u7684\u7ebf\u3002\u4ec0\u4e48\u53eb\u5316\u5b66\u952e\uff1f\u5c31\u662f\u4e24\u4e2a\u539f\u5b50\u4e4b\u95f4\u6709\u7535\u5b50\u4e4b\u95f4\u7684\u4ea4\u6362\uff0c\u8fd9\u5c31\u662f\u5316\u5b66\u952e\u3002\u5982\u679c\u4e00\u4e2a\u539f\u5b50\u628a\u7535\u5b50\u5168\u90e8\u51fa\uff0c\u53e6\u4e00\u4e2a\u539f\u5b50\u628a\u7535\u5b50\u5168\u90e8\u62ff\u8d70\uff0c\u8fd9\u4e24\u4e2a\u539f\u5b50\u5f62\u6210\u79bb\u5b50\u952e\u3002\u5982\u679c\u4e24\u4e2a\u539f\u5b50\u7684\u7535\u5b50\u5171\u4eab\uff0c\u90a3\u5c31\u662f\u5171\u4ef7\u952e\uff0c\u5f88\u591a\u539f\u5b50\u4e4b\u95f4\u7684\u7ed3\u5408\u90fd\u57fa\u4e8e\u79bb\u5b50\u952e\u548c\u5171\u4ef7\u952e\uff0c\u8fd8\u6709\u4e00\u79cd\u91d1\u5c5e\u952e\u662f\u5728\u5168\u57df\u8303\u56f4\u5f7b\u5e95\u5171\u4eab\u7535\u5b50\uff0c\u5927\u591a\u6570\u539f\u5b50\u4e4b\u95f4\u5316\u5b66\u952e\u662f\u542b\u6709\u4e0d\u540c\u6bd4\u4f8b\u79bb\u5b50\u952e\u3001\u5171\u4ef7\u952e\u4e0e\u91d1\u5c5e\u952e\u7684\u7ec4\u5408\u3002\u56e0\u6b64\u539f\u5b50\u95f4\u6709\u5316\u5b66\u952e\uff0c\u5c31\u662f\u8054\u901a\u7684\uff0c\u6ca1\u6709\u5316\u5b66\u952e\u5c31\u4e0d\u8fde\u901a\uff0c\u4ece\u800c\u6784\u5efa\u5316\u5b66\u548c\u6676\u4f53\u7684\u56fe\u8bba\u3002<\/p>\n<p>\u56fe\u8bba\u7684\u70b9\u53ef\u4ee5\u5c31\u7814\u7a76\u5bf9\u8c61\u6765\u62bd\u8c61\u3002\u6bd4\u5982\u8bf4\u6211\u4eec\u5728\u7814\u7a76\u4e00\u4e2a\u57ce\u5e02\u7684\u7279\u70b9\u7684\u65f6\u5019\uff0c\u6211\u4eec\u53ef\u4ee5\u628a\u4e00\u4e2a\u5c0f\u533a\u4f5c\u4e3a\u4e00\u4e2a\u70b9\uff0c\u7136\u540e\u770b\u770b\u6709\u591a\u5c11\u6761\u8def\u8ddf\u8fd9\u4e2a\u5c0f\u533a\u548c\u53e6\u5916\u4e00\u4e2a\u5c0f\u533a\u8fde\u63a5\uff0c\u6211\u4eec\u4e5f\u53ef\u4ee5\u628a\u5c0f\u533a\u628a\u6bcf\u680b\u697c\u4f5c\u4e3a\u4e00\u4e2a\u70b9\uff0c\u7136\u540e\u518d\u770b\u5230\u8fd9\u697c\u548c\u697c\u4e4b\u95f4\uff0c\u697c\u5230\u53e6\u5916\u4e00\u4e2a\u5c0f\u533a\u7684\u697c\u4e4b\u95f4\uff0c\u56e0\u6b64\u53ef\u4ee5\u6839\u636e\u5bf9\u8c61\u4e0d\u540c\u6784\u5efa\u4e0d\u540c\u7684\u56fe\u3002\u540c\u6837\u5728\u6676\u4f53\u91cc\u9762\u4e0d\u4ec5\u53ef\u4ee5\u628a\u539f\u5b50\u5f53\u4f5c\u70b9\uff0c\u4e5f\u53ef\u4ee5\u628a\u539f\u5b50\u7ec4\u5408\u6784\u6210\u529f\u80fd\u7ed3\u6784\u57fa\u5143\u5f53\u4f5c\u70b9\uff0c\u7814\u7a76\u5176\u8fde\u63a5\u65b9\u5f0f\uff0c\u5f62\u6210\u4e0d\u540c\u5c42\u6b21\u7684\u56fe\u8868\u8fbe\u3002\u56fe\u7684\u65b9\u5f0f\u6765\u8868\u8fbe\u6700\u5927\u7684\u597d\u5904\u662f\u53ef\u4ee5\u7528\u8ba1\u7b97\u673a\u91cc\u9762\u7684\u77e9\u9635\u65b9\u7a0b\u6765\u8fdb\u884c\u8fd0\u7b97\uff0c\u539f\u5b50\u7684\u5b9e\u4f53\u7a7a\u95f4\u4f4d\u7f6e\u8f6c\u53d8\u6210\u8ba1\u7b97\u673a\u865a\u62df\u7684\u77e9\u9635\u7a7a\u95f4\u7684\u6570\u5b57\u8fdb\u884c\u6570\u5b66\u8fd0\u7b97\u7684\u95ee\u9898\u3002<\/p>\n<blockquote>\n<p><strong>&gt;&gt;\u00a0\u4f8b\u5982\uff1a\u56fe\u8bba vs \u540c\u6784\u8bc6\u522b<\/strong><\/p>\n<\/blockquote>\n<p>\u6211\u4eec\u73b0\u5728\u4e3e\u4e00\u4e9b\u4f8b\u5b50\u7ed9\u5927\u5bb6\u770b\u770b\uff0c\u8fd9\u662f\u6211\u4eec\u53d1\u8868\u7684\u7b2c\u4e00\u7bc7\u57fa\u4e8e\u56fe\u8bba\u7684\u7ed3\u6784\u5316\u5b66\u7684\u6587\u7ae0\uff0c\u7528\u4e8e\u89e3\u51b3\u521a\u624d\u8bb2\u7684\u6676\u4f53\u7ed3\u6784\u7684\u540c\u6784\u6027\u95ee\u9898\u3002\u4ee5\u6211\u4eec\u624b\u673a\u5728\u7528\u7684\u9502\u7535\u6c60\u6b63\u6781\u6750\u6599\u94b4\u9178\u9502\u7684\u57fa\u7840\u539f\u6599\u56db\u6c27\u5316\u4e09\u94b4\u4e3a\u4f8b\uff0c\u56db\u6c27\u5316\u4e09\u94b4\u5728\u77ff\u7269\u5b66\u4e0a\u53eb\u5c16\u7ed3\u6676\u77f3\u76f8\uff0c\u4e00\u79cd\u6c27\u5bc6\u5806\u65b9\u5f0f\uff0c\u7acb\u65b9\u6676\u7cfb\uff0c\u6676\u80de\u957f\u5ea6\u90fd\u76f8\u540c\u89d2\u5ea6\u662f90<sup>\u00b0<\/sup>\uff0c\u4ee5\u4e00\u4e2a\u6676\u80de\u4e3a\u57fa\u7840\u770b\u6709\u72ec\u7acb\u7684\u51e0\u4e2a\u6c27\u51e0\u4e2a\u94b4\uff0c\u628a\u6bcf\u4e2a\u94b4\u4e0e\u6700\u8fd1\u90bb\u7684\u5316\u5b66\u952e\u8fde\u63a5\uff0c\u518d\u4e0e\u6b21\u8fd1\u90bb\u7684\u8fde\u63a5\uff0c\u518d\u4e0e\u7b2c\u4e09\u5c42\u7b49\u4e0d\u65ad\u5730\u8fde\u63a5\u6784\u6210\u4e00\u5f20\u8fde\u63a5\u56fe\u3002\u7528\u8fd9\u79cd\u65b9\u5f0f\u53ef\u4ee5\u53d1\u73b0\u5b9e\u9645\u4e0a\u6709\u4e09\u79cd\u72ec\u7acb\u7684\u56fe\uff0c\u7b2c\u4e00\u79cd\u4ee5\u67d01\u4e2a\u94b4\u4e3a\u4e2d\u5fc3\u8ddf6\u4e2a\u6c27\u8fde\u63a5\uff0c\u8fd8\u67091\u79cd\u662f\u94b4\u8ddf4\u4e2a\u6c27\u8fde\u63a5\uff0c\u8fd8\u67091\u79cd\u4ee5\u6c27\u4e3a\u4e2d\u5fc3\u4e0e4\u4e2a\u94b4\u8fde\u63a5\uff0c\u8fd9\u6837\u5c31\u53ef\u4ee5\u53d1\u73b0\u5355\u80de\u91cc\u9762\u6709\u51e0\u4e2a\u72ec\u7acb\u7684\u539f\u5b50\u6784\u6210\u72ec\u7acb\u7684\u5c0f\u56fe\uff0c\u8fd9\u4e9b\u72ec\u7acb\u7684\u5c0f\u56fe\u7684\u7ec4\u5408\u6784\u6210\u5c16\u6676\u77f3\u76f8\u7684\u5b8c\u6574\u8868\u8fbe\u7684\u5927\u56fe\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u4f8b\u5982\uff1a\u56fe\u8bba vs \u540c\u6784\u8bc6\u522b \uff1a<\/strong><strong>Li<\/strong><strong><sub>11<\/sub><\/strong><strong>Ti<\/strong><strong><sub>4<\/sub><\/strong><strong>Fe<\/strong><strong><sub>9<\/sub><\/strong><strong>O<\/strong><strong><sub>32 \u00a0\u00a0<\/sub><\/strong><strong>\u662f\u5426\u662f\u5c16\u6676\u77f3\u76f8\uff1f<\/strong><\/p>\n<p><strong>Li<\/strong><strong><sub>11<\/sub><\/strong><strong>Ti<\/strong><strong><sub>4<\/sub><\/strong><strong>Fe<\/strong><strong><sub>9<\/sub><\/strong><strong>O<\/strong><strong><sub>32<\/sub><\/strong>\u50cf\u4e00\u4e2a\u9502\u7535\u6c60\u6750\u6599\uff0c\u5b83\u4e0e\u5c16\u6676\u77f3\u76f8Co<sub>3<\/sub>O<sub>4<\/sub>\u00a0\u7684\u6676\u80de\u7279\u5f81\u4e0d\u540c\uff08\u6676\u80de\u957f\u5ea6\u548c\u89d2\u5ea6\u90fd\u4e0d\u76f8\u540c\uff09\uff0c\u662f\u6700\u4f4e\u5bf9\u79f0\u6027\u7684\u5355\u659c\u76f8\uff0c\u5b83\u662f\u5426\u662f\u5c16\u6676\u77f3\u76f8?\u7528\u4f20\u7edf\u7684\u7ed3\u6784\u5316\u5b66\u65b9\u6cd5\u5f88\u96be\u8bc6\u522b\u3002\u6211\u4eec\u7528\u4ee5\u4e0a\u56fe\u8bba\u7684\u65b9\u6cd5\u628a\u5355\u80de\u4e2d\u7684\u6bcf\u4e2a\u539f\u5b50\u4e0e\u6700\u8fd1\u90bb\u3001\u6b21\u8fd1\u90bb\u7b494-5\u5c42\u6784\u6210\u8fde\u63a5\u56fe\uff0c\u53d1\u73b0\u5b9e\u9645\u4e0a\u4e5f\u53ea\u6709\u4e09\u79cd\u72ec\u7acb\uff0c\u4e00\u79cd\u662f\u91d1\u5c5e\u4e0e4\u4e2a\u6c27\u8fde\u63a5\uff0c\u53e61\u79cd\u662f\u91d1\u5c5e\u4e0e6\u4e2a\u6c27\u8fde\u63a5\uff0c\u8fd8\u67091\u4e2a\u662f\u6c27\u8ddf4\u4e2a\u91d1\u5c5e\u5143\u7d20\u8fde\u63a5\u7b49\u3002\u4ece\u56fe\u8bba\u7684\u5b9a\u4e49\u6765\u770b\uff0c\u8fd9\u4e2a\u6750\u6599\u9502\u3001\u949b\u3001\u94c1\u3001\u6c27\u5c31\u662f\u8ddf\u4e0a\u9762\u7684\u56db\u6c27\u5316\u4e09\u94b4\u662f\u540c\u4e00\u79cd\u5927\u56fe\u7c7b\u578b\uff0c\u56e0\u6b64\u53ef\u4ee5\u786e\u8ba4\u5b83\u662f\u5c16\u6676\u77f3\u76f8\u3002\u6211\u4eec\u73b0\u5728\u53ef\u4ee5\u628a\u4f20\u7edf\u7684\u77ff\u7269\u5b66\u7684\u6bcf\u79cd\u6676\u4f53\u7ed3\u6784\u53d8\u6210\u4e00\u79cd\u7279\u5b9a\u56fe\u7684\u5b9a\u4e49\u548c\u8868\u8fbe\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u56fe\u8bba vs \u7ed3\u6784\u5316\u5b66\u5927\u6570\u636e\uff08\u5317\u5927\uff09<\/strong><\/p>\n<p>\u57fa\u4e8e\u4ee5\u4e0a\u6240\u8ff0\u57fa\u4e8e\u56fe\u8bba\u7684\u7ed3\u6784\u5316\u5b66\u65b9\u6cd5\uff0c\u53d1\u73b0\u521a\u624d\u8bb2\u7684\u6c2f\u5316\u94a0\u4e0d\u540c\u6676\u80de\u53c2\u6570\u7684\u8fde\u63a5\u65b9\u5f0f\u662f\u76f8\u540c\uff0c\u4ece\u56fe\u8bba\u7ed3\u6784\u5316\u5b66\u6765\u8bf4\u662f\u76f8\u540c\u7684\u7ed3\u6784\u3002\u7528\u56fe\u8bba\u65b9\u6cd5\u6211\u4eec\u5c31\u53ef\u4ee5\u628a\u5df2\u53d1\u8868\u6240\u6709\u7684\u6676\u4f53\u7ed3\u6784\u62ff\u6765\u505a\u6570\u636e\u6e05\u6d17\uff0c\u4e5f\u5c31\u662f\u8bf4\u7528\u56fe\u8bba\u7684\u529e\u6cd5\u6765\u5b9a\u4e49\u548c\u8bc6\u522b\u6676\u4f53\u7ed3\u6784\u662f\u5426\u540c\u6784\uff0c\u5f97\u5230\u4e86\u5927\u6982\u72ec\u7acb\u7684\u7ea665\u4e07\u4e2a\u72ec\u7acb\u7684\u6676\u4f53\u7ed3\u6784\uff0c\u7ecf\u8fc7\u91cf\u5b50\u5316\u5b66\u7684\u7ed3\u6784\u4f18\u5316\u8ba1\u7b97\uff0c\u4f5c\u4e3a\u6211\u4eec\u6676\u4f53\u7ed3\u6784\u5927\u6570\u636e\u3002<\/p>\n<p>\u662f\u5426\u6709\u5316\u5b66\u952e\u8fde\u63a5\u600e\u4e48\u5224\u65ad\u5462\uff1f\u5f90\u5149\u5baa\u5148\u751f\u5199\u7684\u300a\u7269\u8d28\u7ed3\u6784\u300b\u7684\u4e66\u540e\u9762\u6709\u4e00\u4e2a\u79bb\u5b50\u534a\u5f84\u8868\uff08\u9c8d\u6797\u534a\u5f84\uff09\uff0c\u6839\u636e\u7ed3\u5408\u539f\u5b50\u4e24\u8005\u7535\u8d1f\u6027\u53ea\u5dee\uff0c\u53ef\u4ee5\u521d\u6b65\u5224\u65ad\u662f\u5171\u4ef7\u952e\u8fd8\u662f\u79bb\u5b50\u952e\uff08\u662f\u9009\u7528\u5171\u4ef7\u534a\u5f84\u8fd8\u662f\u79bb\u5b50\u534a\u5f84\uff09\uff0c\u5982\u679c\u662f\u79bb\u5b50\u952e\uff0c\u6839\u636e\u7535\u4ef7\u5e73\u8861\u8ba1\u7b97\u662f\u51e0\u4ef7\uff08\u5bf9\u4e8e\u53ef\u53d8\u4ef7\u7684\u539f\u5b50\uff09\u3002\u5b83\u7684\u539f\u5b50\u534a\u5f84\uff0c\u79bb\u5b50\u534a\u5f84\u3001\u91d1\u5c5e\u534a\u5f84\u6765\u4f30\u7b97\u4e24\u4e2a\u4e4b\u95f4\u7684\u8ddd\u79bb\uff0c\u4e0e\u5b9e\u9645\u539f\u5b50\u95f4\u8ddd\u79bb\u6bd4\u8f83\u786e\u5b9a\u662f\u5426\u6709\u5316\u5b66\u952e\u8fde\u63a5\u3002\u56e0\u4e3a\u5982\u679c\u539f\u5b50\u95f4\u6ca1\u6709\u5316\u5b66\u952e\uff0c\u662f\u8303\u5fb7\u74e6\u8033\u65af\u529b\uff0c\u539f\u5b50\u95f4\u7684\u8ddd\u79bb\u8981\u5927\u5f97\u591a\u3002\u7528\u56fe\u8bba\u5728\u8bc6\u522b\u7684\u540c\u6784\u7ed3\u6784\u53ef\u4ee5\u5bb9\u5fcd\u6709\u952e\u89d2\u5fae\u5c0f\u7684\u5dee\u522b\uff0c\u5bb9\u8bb8\u7ed3\u6784\u7684\u4e00\u4e9b\u7578\u53d8\uff0c\u8fd9\u8981\u8fde\u63a5\u5173\u7cfb\u4e00\u6837\u53ef\u4ee5\u4f5c\u4e3a\u540c\u4e00\u7c7b\u7684\u56fe\u7ed3\u6784\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u56fe\u8bba-&gt;\u4ee3\u6570\u56fe\u8bba<\/strong><\/p>\n<p>\u4ee3\u6570\u56fe\u8bba\u7684\u6301\u7eed\u540c\u8c03\u662f\u6bd4\u8f83\u5b9a\u91cf\u7684\u56fe\u8bba\u65b9\u6cd5\uff0c\u5b83\u80fd\u6709\u6548\u5f97\u5230\u539f\u5b50\u4e4b\u95f4\u76f8\u4e92\u8fde\u63a5\u66f4\u7ec6\u5316\u7684\u56fe\u4fe1\u606f\u3002\u8fd9\u4e2a\u65b9\u6cd5\u5b83\u9009\u7528\u4e86\u4e09\u79cd\u8d1d\u5854\u53c2\u6570\u63cf\u8ff02\u70b9\u4e4b\u95f4\u4ec0\u4e48\u65f6\u5019\u8fde\u63a5\u30013\u4e2a\u70b9\u80fd\u5426\/\u4ec0\u4e48\u65f6\u5019\u8fde\u63a5\u5728\u4e00\u8d77\u5f62\u6210\u4e00\u4e2a\u5b54\u4ee5\u53ca4\u4e2a\u70b9\u80fd\u5426\/\u4ec0\u4e48\u65f6\u5019\u8fde\u63a5\u5728\u4e00\u8d77\u5f62\u6210\u4e00\u4e2a\u6d1e\u3002\u6301\u7eed\u540c\u8c03\u62ff\u8fc7\u7a0b\u662f\u4e24\u4e2a\u76f8\u90bb\u539f\u5b50\uff0c\u4ee5\u6bcf\u4e2a\u539f\u5b50\u4e3a\u4e2d\u5fc3\uff0c\u50cf\u6ce2\u4e00\u6837\u4e0d\u65ad\u7684\u5f84\u5411\u6269\u5927\uff0c\u5230\u4e00\u5b9a\u7a0b\u5ea6\u80af\u5b9a\u4f1a\u78b0\u5728\u4e00\u8d77\uff0c\u78b0\u5728\u4e00\u8d77\u5c31\u8bb0\u5f55\u4e0b\u78b0\u5728\u4e00\u8d77\u7684\u7a7a\u95f4\u8ddd\u79bb\uff0c\u662f\u4e24\u4e2a\u539f\u5b50\u4e4b\u95f4\u7684\u8ddd\u79bb\uff0c\u7528\u8d1d\u58540\u8868\u793a\u3002\u6309\u7167\u8fd9\u4e2a\u65b9\u5f0f\u5bf9\u4e09\u4e2a\u539f\u5b50\u8fdb\u884c\u5173\u7cfb\u8fdb\u884c\u63cf\u8ff0\uff0c\u8fd93\u4e2a\u539f\u5b50\u6cbf\u7740\u5f84\u5411\u6269\u5927\u78b0\u5728\u4e00\u8d77\u5f62\u6210\u4e2d\u95f4\u6709\u5b54\uff0c\u7528\u8d1d\u58541\u8868\u793a\u3002\u6309\u7167\u8fd9\u4e2a\u65b9\u5f0f\u5bf94\u4e2a\u539f\u5b50\u8fdb\u884c\u5173\u7cfb\u8fdb\u884c\u63cf\u8ff0\uff0c\u6709\u4e00\u79cd\u53ef\u80fd\u5c31\u5f62\u6210\u4e00\u4e2a\u6d1e\uff0c\u7528\u8d1d\u58542\u8868\u793a\u3002\u4ee3\u6570\u56fe\u8bba\u7684\u6301\u7eed\u540c\u8c03\u65b9\u6cd5\u5df2\u7ecf\u6210\u529f\u5e94\u7528\u4e8e\u751f\u7269\u533b\u5b66\u9886\u57df\uff0c\u6210\u529f\u5730\u5f00\u5c55\u4e86\u836f\u7269\u8bbe\u8ba1\u3002\u6211\u4eec\u628a\u5b83\u7528\u4e8e\u6750\u6599\u7814\u7a76\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u7528\u6750\u6599\u5927\u6570\u636e\u7814\u7a76\uff1a\u539f\u5b50\u6709\u6548\u5927\u5c0f \u9c8d\u6797\u79bb\u5b50\u534a\u5f84\u7684\u4fee\u6b63<\/strong><\/p>\n<p>\u5efa\u7acb\u4e86\u5927\u6570\u636e\uff0c\u6211\u4eec\u53ef\u4ee5\u68c0\u9a8c\u4e00\u4e0b\u300a\u7269\u8d28\u7ed3\u6784\u300b\u4e66\u4e2d\u9c8d\u6797\u534a\u5f84\u8868\u4e0a\u7684\u6570\u636e\u4e0e\u4e0d\u540c\u5b9e\u9645\u6676\u4f53\u662f\u5426\u7b26\u5408\uff0c\u4ee5Fe\u4e3a\u4f8b\uff0c\u67e5\u5230\u5176\u9c8d\u6797\u534a\u5f84\u4e0e\u4ef7\u6001\uff08Fe<sup>2+<\/sup>\uff0cFe<sup>3+<\/sup>\uff09\u548c\u914d\u4f4d\u591a\u9762\u4f53\uff08\u56db\u9762\u4f53\uff0c\u516b\u9762\u4f53\uff09\u76f4\u63a5\u76f8\u5173\uff0c\u901a\u8fc7\u8fd9\u4e24\u9879\u53ef\u4ee5\u4ece\u79bb\u5b50\u534a\u5f84\u7684\u8868\u683c\u67e5\u5230\u76f8\u5e94\u7684\u534a\u5f84\u503c\u3002\u5982\u679c\u6211\u4eec\u628a\u8fd9\u4e9b\u79bb\u5b50\u534a\u5f84\u4ee3\u5165\u5b9e\u9645\u7684\u6676\u4f53\u7ed3\u6784\u5927\u6570\u636e\u4e2d\u53d1\u73b0\u8bef\u5dee\u5f88\u5927\uff0c\u539f\u56e0\u662f\u4ec0\u4e48\uff1f\u6211\u4eec\u53d1\u73b0\u5728\u9c8d\u6797\u534a\u5f84\u8868\u683c\u91cc\u9762\u867d\u7136\u8003\u8651\u4e86\u4ef7\u6001\u548c\u914d\u4f4d\u6570\uff0c\u4f46\u6ca1\u6709\u8003\u8651\u4e0e\u8c01\u914d\u4f4d\uff0c\u5176\u4f7f\u7528\u7684\u662f\u201c\u786c\u7403\u6a21\u578b\u201d\uff0c\u4f46\u5b9e\u9645\u7684\u4e2d\u5fc3\u79bb\u5b50\u548c\u914d\u4f4d\u79bb\u5b50\u7684\u6781\u5316\u6027\uff08\u8ba9\u4eba\u5bb6\u53d8\u5f62\u80fd\u529b\uff09\u548c\u53ef\u6781\u5316\u6027\uff08\u81ea\u5df1\u53d8\u5f62\u7684\u80fd\u529b\uff09\u662f\u4e0d\u540c\u7684\uff0c\u4ece\u800c\u5bfc\u81f4\u4e2d\u5fc3\u79bb\u5b50\u548c\u914d\u4f4d\u79bb\u5b50\uff08\u4f8b\u5982\u786b\u4e0e\u6c1f\u7684\u6781\u5316\u6027\u548c\u53ef\u6781\u5316\u6027\u5dee\u522b\u5f88\u5927\uff09\u4f1a\u6709\u4e0d\u540c\u7a0b\u5ea6\u7684\u91cd\u53e0\uff0c\u56e0\u4e3a\u9c8d\u6797\u534a\u5f84\u8868\u6ca1\u6709\u8003\u8651\uff0c\u6240\u4ee5\u5c31\u6709\u5f88\u5927\u7684\u8bef\u5dee\u3002\u5982\u679c\u6211\u4eec\u628a\u5b83\u8003\u8651\u8fdb\u53bb\uff0c\u7528\u201c\u8f6f\u7403\u6a21\u578b\u201d\u6570\u5b66\u65b9\u6cd5\uff0c\u4ece\u800c\u52a0\u4e0a\u914d\u4f4d\u79cd\u7c7b\u5bf9\u9c8d\u6797\u534a\u5f84\u8fdb\u884c\u4fee\u6b63\uff0c\u53ef\u4ee5\u66f4\u52a0\u51c6\u786e\u7684\u9884\u6d4b\u4e24\u4e2a\u539f\u5b50\u4e4b\u95f4\u7684\u8ddd\u79bb\u3002\u8fd9\u662f\u6211\u4eec\u5e94\u7528\u6750\u6599\u5927\u6570\u636e\u4ee5\u540e\u7684\u7b2c\u4e00\u4e2a\u5de5\u4f5c\uff0c\u8fdb\u4e00\u6b65\u63a2\u7d22\u4e86\u79bb\u5b50\u534a\u5f84\u7684\u771f\u5b9e\u7684\u610f\u4e49\u548c\u5728\u5b9e\u9645\u73af\u5883\u91cc\u9762\u7684\u5927\u5c0f\u7684\u4e00\u79cd\u4fee\u6b63\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u91cf\u5b50\u5316\u5b66\u8ba1\u7b97<\/strong>\uff1a<strong>\u6676\u4f53\u7ed3\u6784\u4e0e\u7535\u5b50\u7ed3\u6784\u7684\u76f8\u5173\u6027\u7814\u7a76\uff08\u9ad8\u901a\u91cf\u548c\u7cbe\u786e\u7684\u7535\u5b50\u7ed3\u6784\u8ba1\u7b97 \uff1aHSE WKM\uff09<\/strong><\/p>\n<p>\u6709\u4e86\u6676\u4f53\u7ed3\u6784\u5927\u6570\u636e\u4ee5\u540e\uff0c\u8fd0\u7528\u4eba\u5de5\u667a\u80fd\u7684\u673a\u5668\u5b66\u4e60\uff0c\u5e0c\u671b\u628a\u5df2\u6709\u7684\u4e00\u4e2a\u6676\u4f53\u7ed3\u6784\u4e0e\u7535\u5b50\u7ed3\u6784\u5173\u7cfb\u5b66\u4e60\u5230\uff0c\u7136\u540e\u6709\u4e86\u65b0\u7684\u6676\u4f53\u7ed3\u6784\u5c31\u53ef\u4ee5\u9884\u6d4b\u7535\u5b50\u7ed3\u6784\u3002\u673a\u5668\u5b66\u4e60\u7c7b\u4f3c\u4e8e\u4eba\u7684\u5b66\u4e60\uff0c\u5728\u8bc6\u522b\u4e00\u7fa4\u52a8\u7269\u662f\u9e21\u8fd8\u662f\u9e2d\uff0c\u5148\u8981\u901a\u8fc7\u4e86\u4e00\u4e9b\u6837\u672c\u7684\u8bad\u7ec3\uff0c\u518d\u653e\u8fdb\u4e00\u4e2a\u9e21\u8fd8\u662f\u9e2d\uff0c\u5b83\u9a6c\u4e0a\u5c31\u53ef\u4ee5\u8bc6\u522b\u51fa\u6765\u3002\u7c7b\u4f3c\u6709\u4e86\u4e00\u4e2a\u6676\u4f53\u7ed3\u6784\uff0c\u7528\u91cf\u5b50\u5316\u5b66\u7b2c\u4e00\u6027\u539f\u7406\u8ba1\u7b97\uff0c\u6211\u4eec\u7528\u4e86\u66f4\u7cbe\u786e\u7684HSE\u65b9\u6cd5\uff0c\u8ba1\u7b97\u80fd\u5e26\u7684\u5e26\u9699\uff0c\u518d\u7528\u673a\u5668\u5b66\u4e60\u6765\u5b66\u4e60\u7ed3\u6784\u4e0e\u5e26\u9699\u7684\u76f8\u5173\u6027\uff0c\u7136\u540e\u518d\u8fdb\u884c\u65b0\u7ed3\u6784\u7684HSE\u5e26\u9699\u7684\u7cbe\u786e\u8ba1\u7b97\u7528\u6765\u4fee\u6b63\u673a\u5668\u5b66\u4e60\uff0c\u8fd9\u6837\u591a\u6b21\u7684\u8fed\u4ee3\uff0c\u5f97\u523090%\u4ee5\u4e0a\u7684\u7ed3\u6784\u4e0e\u5e26\u9699\u76f8\u5173\u6027\uff08\u5373\u4e00\u4e2a\u7ed3\u6784\u5c31\u53ef\u4ee5\u9884\u6d4b\u5176\u5e26\u9699\uff09\u7684\u9884\u6d4b\u7cbe\u5ea6\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u91cf\u5b50\u5316\u5b66+\u4eba\u5de5\u667a\u80fd\uff1a\u00a0\u673a\u5668\u5b66\u4e60\u5efa\u7acb\u529b\u573a<\/strong><\/p>\n<p>\u7528\u91cf\u5b50\u5316\u5b66\u548c\u4eba\u5de5\u667a\u80fd\u6765\u7814\u7a76\u539f\u5b50\u95f4\u76f8\u4e92\u4f5c\u7528\u529b\uff0c\u4efb\u4f55\u4e00\u4e2a\u539f\u5b50\/\u79bb\u5b50\u653e\u5728\u6676\u4f53\u4e2d\uff0c\u8981\u611f\u53d7\u5230\u5468\u56f4\u73af\u5883\u5f62\u6210\u7684\u529b\u573a\u3002\u6211\u4eec\u5728\u56fa\u6001\u7269\u7406\u4e2d\u5b66\u4e60\u5230\u7b80\u5355\u7684\u79bb\u5b50\u6676\u4f53\u76f8\u4e92\u4f5c\u7528\uff0c\u5229\u7528\u5176\u5468\u671f\u6027\u89c4\u5f8b\u5f97\u5230\u9a6c\u5fb7\u9686\u5e38\u6570\uff0c\u8fd0\u7528\u8be5\u5e38\u6570\u53ef\u4ee5\u8ba1\u7b97\u6676\u683c\u80fd\uff0c\u5176\u7ed3\u679c\u4e0e\u5b9e\u9a8c\u6d4b\u91cf\u5f88\u63a5\u8fd1\u3002\u5bf9\u590d\u6742\u7cfb\u7edf\u7684\u539f\u5b50\u6216\u79bb\u5b50\u8fc1\u79fb\u7684\u52a8\u529b\u5b66\u8ba1\u7b97\u9700\u8981\u5f97\u5230\u539f\u5b50\/\u5206\u5b50\u76f8\u4e92\u4f5c\u7528\u7684\u529b\u573a\uff0c\u6709\u4e86\u7cbe\u786e\u7684\u529b\u573a\u53c2\u6570\u5c31\u53ef\u4ee5\u5feb\u901f\u7684\u6765\u9884\u6d4b\u7269\u8d28\u7684\u7194\u70b9\u3001\u786c\u5ea6\u548c\u539f\u5b50\/\u79bb\u5b50\u7684\u8fd0\u52a8\u3002<\/p>\n<p>\u6280\u672f\u7ec6\u8282\uff1a\u7528\u673a\u5668\u5b66\u4e60\u5f00\u53d1\u529b\u573a\u662f\u57fa\u4e8e\u52bf\u80fd\u9762\u65b9\u6cd5\uff0c\u9009\u53d6Rcut\u8303\u56f4\u5185\u7684\u539f\u5b50\u4f5c\u4e3a\u8fd1\u90bb\u539f\u5b50\uff0c\u8fd1\u4f3c\u8ba4\u4e3a\u4e2d\u5fc3\u539f\u5b50\u53ea\u53d7\u8fd1\u90bb\u539f\u5b50\u7684\u5f71\u54cd\u3002SANNP\u6a21\u578b\u7684\u7279\u70b9\u662f\u5c06DFT\u8ba1\u7b97\u83b7\u5f97\u7684total energy\u62c6\u5206\u5230\u6bcf\u4e2a\u539f\u5b50\u4e0a\uff0c\u76f4\u63a5\u83b7\u5f97\u4e86\u6bcf\u4e2a\u539f\u5b50\u7684\u80fd\u91cf\uff0c\u4f20\u7edf\u7684\u529b\u573a\u6a21\u578b\u901a\u5e38\u5047\u8bbeEtot\u7b49\u4e8e\u4f53\u7cfb\u4e2d\u6240\u6709\u539f\u5b50\u7684\u539f\u5b50\u80fd\u4e4b\u548c\uff0c\u62e5\u6709\u4e86\u539f\u5b50\u80fd\u6570\u636e\u4e00\u65b9\u9762\u63d0\u5347\u4e86\u8bad\u7ec3\u4e2d\u5305\u542b\u7684\u6570\u636e\u91cf\uff0c\u53e6\u4e00\u65b9\u9762\u4f7f\u5f97\u6a21\u578b\u80fd\u66f4\u597d\u7684\u6355\u6349\u5230\u8868\u9762\u7b49\u4e0d\u540c\u5c40\u90e8\u7279\u5f81\u4f1a\u5e26\u6765\u7684\u80fd\u91cf\u53d8\u5316\u3002\u529b\u573a\u65b9\u6cd5\u7684\u6574\u4e2a\u8bad\u7ec3\u6d41\u7a0b\u5982\u4e0b\uff1a1\u3001\u63d0\u53d6\u8fd1\u90bb\u539f\u5b50\u7684\u5c40\u90e8\u73af\u5883\u7279\u5f81\u3002\u672c\u6587\u4e2d\u4f7f\u7528\u4e24\u4f53\u52bf\u4e0e\u4e09\u4f53\u52bf\u6765\u63d0\u53d6\u539f\u5b50\u95f4\u7684\u76f8\u5bf9\u4f4d\u7f6e\u5173\u7cfb\u4f5c\u4e3a\u5c40\u90e8\u73af\u5883\u7279\u5f81\u30022\u3001\u5c06\u4e2d\u5fc3\u539f\u5b50\u7684\u5c40\u90e8\u73af\u5883\u7279\u5f81\u8f93\u5165\u795e\u7ecf\u7f51\u7edc\u4e2d\uff0c\u9884\u6d4b\u4e2d\u5fc3\u539f\u5b50\u7684\u539f\u5b50\u80fd\u3002\u53f3\u4e0b\u56fe\u5c55\u793a\u4e86\u6211\u4eec\u7684SANNP\u6a21\u578b\u4e0eDFT\u6a21\u578b\u53ca\u7ecf\u9a8c\u5d4c\u5165\u539f\u5b50\u52bf\u95f4\u7684\u6bd4\u8f83\uff0c\u53ef\u4ee5\u770b\u5230SANNP\u4e0eEAM\u76f8\u6bd4\u8f83DFT\u7684\u7ed3\u679c\u66f4\u4e3a\u76f8\u4f3c\u3002\u6211\u4eec\u7528\u8fd9\u65b9\u6cd5\u8fdb\u884c\u4e86\u9502\u91d1\u5c5e\u8d1f\u6781\u6750\u6599\u679d\u6676\u7684\u751f\u957f\u6a21\u62df\u548c\u9884\u6d4b\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u5927\u6570\u636e+\u4eba\u5de5\u667a\u80fd\uff1a\u00a0\u9884\u6d4b\u7ed3\u6784\u4e0e\u6027\u8d28<\/strong><\/p>\n<p>\u56de\u5230\u521a\u624d\u5c06\u91cf\u5b50\u5316\u5b66\u8ba1\u7b97\u4e0e\u673a\u5668\u5b66\u4e60\u76f8\u7ed3\u5408\u6765\u4ece\u6676\u4f53\u7ed3\u6784\u9884\u6d4b\u7535\u5b50\u7ed3\u6784\uff0c\u6211\u4eec\u62ff\u4e8615,000\u4e2a\u6676\u4f53\uff0c\u8fdb\u884c\u91cf\u5b50\u5316\u5b66\u8ba1\u7b97\u4e0e\u673a\u5668\u5b66\u4e60\u7279\u5f81\u63d0\u53d6\u4e0e\u8bad\u7ec3\u76f8\u7ed3\u5408\uff0c\u8fdb\u884c\u53cd\u590d\u7684\u8fed\u4ee3\u6539\u8fdb\u8bad\u7ec3\u6a21\u578b\uff0c\u4e0d\u65ad\u63d0\u9ad8\u9884\u6d4b\u7684\u7cbe\u5ea6\u3002\u673a\u5668\u5b66\u4e60\u5f00\u5c55\u6750\u6599\u7814\u7a76\u7684\u5de5\u4f5c\u73b0\u5728\u8d8a\u6765\u8d8a\u591a\uff0c\u5927\u5bb6\u53ef\u80fd\u5df2\u7ecf\u77e5\u9053\u4e0d\u5c11\u4e86\uff0c\u5927\u5bb6\u611f\u5174\u8da3\u7684\u7f51\u4e0a\u6709\u8bb8\u591a\u8d44\u6599\u3002<\/p>\n<p>\u6211\u8fd9\u91cc\u60f3\u8bb2\u7684\u662f\u4eba\u5de5\u667a\u80fd\u548c\u5927\u6570\u636e\u8fd8\u80fd\u5e72\u4ec0\u4e48\uff1f\u5728\u8d77\u521d\u7814\u7a76\u751f\u547d\u73b0\u8c61\u65f6\u53d1\u73b0\u690d\u7269\u7684\u6709\u4e9b\u6027\u72b6\u51e0\u4ee3\u4e4b\u95f4\u90fd\u6709\u76f8\u4f3c\u6027\uff0c\u79f0\u4e4b\u4e3a\u9057\u4f20\uff0c\u5206\u5b50\u751f\u7269\u5b66\u53d1\u73b0\u4e86\u9057\u4f20\u7684\u672c\u8d28\u662f\u57fa\u56e0\u7684\u590d\u5236\u3002\u53ef\u7531\u4e8e\u9057\u4f20\u9884\u6d4b\u5176\u76f8\u4f3c\u7684\u6027\u72b6\uff0c\u4f46\u4e5f\u53d1\u73b0\u6709\u4e9b\u65f6\u5019\u504f\u79bb\u4e86\u9884\u6d4b\u79f0\u4e4b\u4e3a\u53d8\u5f02\u3002\u6211\u4eec\u5728\u4eba\u5de5\u667a\u80fd\u673a\u5668\u5b66\u4e60\u9884\u6d4b\u6027\u80fd\u65f6\u603b\u4f1a\u53d1\u73b0\u4e00\u79cd\u73b0\u8c61\uff0c\u4e0d\u7ba1\u600e\u4e48\u6539\u8fdb\u7684\u6a21\u578b\u8bad\u7ec3\u63d0\u9ad8\u9884\u6d4b\u7cbe\u5ea6\uff0c\u5373\u4f7f\u9884\u6d4b\u5df2\u7ecf\u505a\u5230\u767e\u5206\u4e4b\u4e5d\u5341\u51e0\u4e86\uff0c\u603b\u6709\u90a3\u4e9b\u4e0d\u80fd\u88ab\u9884\u6d4b\u7684\u90e8\u5206\uff0c\u6211\u4eec\u80fd\u5426\u95ee\u8fd9\u4e9b\u662f\u5426\u662f\u7279\u6b8a\u53d8\u5f02\u7684\u7ed3\u6784\uff1f\u6211\u4eec\u628a\u8fd9\u504f\u79bb\u9884\u6d4b\u7684\uff08\u56fe\u4e2d\u7684\u201c\u5f02\u5e38\u70b9\u201d\uff09\u6750\u6599\u7ed3\u6784\u62ff\u51fa\u6765\u770b\u770b\u662f\u4ec0\u4e48\u539f\u56e0\u4e5f\u53ef\u4ee5\u770b\u5230\u53d8\u5f02\u7684\u65b0\u7269\u79cd\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u5927\u6570\u636e\u4e0e\u4eba\u5de5\u667a\u80fd\u00a0<\/strong>\uff1a<strong>\u53d1\u73b0\u65b0\u578b\u7ed3\u6784\u57fa\u5143\u4e0e\u7535\u5b50\u7ed3\u6784<\/strong><\/p>\n<p>\u8fd9\u91cc\u4e3e\u4e86\u4e00\u4e2a\u5f02\u5e38\u70b9\u7ed3\u6784\u7684\u4f8b\u5b50AgO<sub>2<\/sub>F\uff0c\u673a\u5668\u5b66\u4e60\u5f97\u5230\u7684\u5e26\u9699\u662f3eV\u4f5c\u7528\uff0c\u91cf\u5b50\u5316\u5b66\u8ba1\u7b97\u7684\u5e26\u9699\u53ea\u67090.6eV\u3002\u8fdb\u4e00\u6b65\u7684\u7ed3\u6784\u5206\u6790\u53d1\u73b0\u94f6\u4f5c\u4e3a\u4e2d\u5fc3\u79bb\u5b50\u4e0e\u4e24\u4e2a\u6c1f\u548c\u4e24\u4e2a\u8d85\u6c27\u79bb\u5b50\u914d\u4f4d\uff0c\u5927\u5bb6\u77e5\u9053\u6c27\u5316\u6027\u8d8a\u5927\u628a\u7535\u5b50\u62c9\u8fc7\u6765\u7684\u80fd\u529b\u5c31\u8d8a\u5f3a\uff0c\u8d85\u6c27\u79bb\u5b50\u548cF\u90fd\u662f\u5f3a\u6c27\u5316\u6027\u7684\u3002\u6211\u4eec\u77e5\u9053\u53cc\u6c27\u6c34\u662f\u6c27\u5316\u6027\u5f88\u5f3a\u7684\uff0c\u6700\u559c\u6b22\u5f97\u5230\u7535\u5b50\u81ea\u5df1\u53d8\u6210-2\u4ef7\uff0c\u6c1f\u4e5f\u6709\u6700\u5f3a\u62c9\u7535\u5b50\u80fd\u529b\u3002\u94f6\u5728\u8fd9\u79cd\u73af\u5883\u4e0b\u4e0d\u662f\u6211\u4eec\u5e73\u5e38\u7684+1\u4ef7\uff0c\u800c\u662f+3\u4ef7\uff0c\u8d85\u6c27\u79bb\u5b50\u7684\u80fd\u5e26\u5728\u539f\u6765\u4ef7\u5e26\u548c\u5bfc\u5e26\u4e4b\u95f4\uff0c\u6240\u4ee5\u5e26\u9699\u5c31\u662f\u4e0d\u662f\u5e73\u5e38\u9884\u6d4b\u76843eV\uff0c\u800c\u662f\u4e2d\u95f4\u6709\u8d85\u6c27\u79bb\u5b50\u4f7f\u5f97\u5e26\u9699\u53ea\u67090.6eV\u3002<\/p>\n<p>\u56e0\u6b64\uff0c\u8fd0\u7528\u5927\u6570\u636e\u548c\u4eba\u5de5\u667a\u80fd\u65e2\u53ef\u4ee5\u9884\u6d4b\u6784\u6548\u5173\u7cfb\u7684\u89c4\u5f8b\u540c\u65f6\u4e5f\u80fd\u53d1\u73b0\u4e0d\u80fd\u88ab\u9884\u6d4b\u7684\u5f02\u5e38\u70b9\uff0c\u4ece\u5f02\u5e38\u70b9\u4e2d\u53ef\u4ee5\u53d1\u73b0\u53d8\u5f02\u7684\u65b0\u7684\u529f\u80fd\u7ed3\u6784\u57fa\u5143\u2014-\u65b0\u201c\u7269\u79cd\u201d\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u57fa\u4e8e\u56fe\u8bba\u548c\u6750\u6599\u5927\u6570\u636e \u53d1\u73b0\u65b0\u76842\u7ef4\u30011\u7ef4\u30010\u7ef4\u6750\u6599<\/strong><\/p>\n<p>\u6709\u4e86\u57fa\u4e8e\u56fe\u8bba\u7684\u7ed3\u6784\u5316\u5b66\u548c\u6676\u4f53\u7ed3\u6784\u5927\u6570\u636e\uff0c\u53ef\u4ee5\u91cd\u65b0\u6765\u63cf\u8ff0\u548c\u5b9a\u4e49\u4ec0\u4e48\u662f\u771f\u6b63\u7684\u4f4e\u7ef4\u6750\u6599\uff0c\u59822\u7ef4,1\u7ef4\u548c0\u7ef4\u6750\u6599\uff1a<\/p>\n<p>\u4e8c\u7ef4\u6750\u6599\u5c31\u50cf\u77f3\u58a8\u70ef\u4e00\u6837\uff0c\u53ef\u4ee5\u7528\u4e00\u4e2a\u80f6\u5e26\u7eb8\u4e0d\u65ad\u5730\u6495\u6700\u540e\u5f97\u5230\u4e8c\u7ef4\u7247\uff0c\u5176\u5728\u67d0\u4e00\u65b9\u5411\u4e0a\u6ca1\u6709\u5316\u5b66\u952e\uff0c\u539f\u56e0\u662f\u5c42\u4e4b\u95f4\u7684\u76f8\u4e92\u4f5c\u7528\u529b\u662f\u5f88\u5f31\u7684\u5206\u5b50\u95f4\u8303\u5fb7\u534e\u5c14\u529b\u3002\u6839\u636e\u521a\u624d\u56fe\u8bba\u7ed3\u6784\u5316\u5b66\uff0c\u628a\u5728\u4e8c\u7ef4\u65b9\u5411\u4e0a\u6709\u5316\u5b66\u952e\u8fde\u63a5\u6210\u4e00\u4e2a\u7f51\u7edc\uff0c\u4f46\u5728\u4e0e\u5b83\u5782\u76f4\u7684\u65b9\u5411\u4e0a\u6ca1\u6709\u5316\u5b66\u952e\uff0c\u53ea\u6709\u5206\u5b50\u95f4\u5f31\u7684\u76f8\u4e92\u4f5c\u7528\u7684\u6750\u6599\u5b9a\u4e49\u4e3a\u4e8c\u7ef4\u6750\u6599\u3002\u4ee5\u6b64\u7c7b\u63a8\uff0c\u5982\u679c\u53ea\u6709\u5728\u4e00\u7ef4\u65b9\u5411\u4e0a\u6709\u5316\u5b66\u952e\u8fde\u63a5\uff0c\u53e6\u5916\u4e24\u4e2a\u7ef4\u5ea6\u90fd\u662f\u6ca1\u6709\u5316\u5b66\u952e\u8fde\u63a5\uff0c\u53ea\u6709\u8303\u5fb7\u534e\u5c14\u529b\uff0c\u5b9a\u4e49\u4e3a\u4e00\u7ef4\u6750\u6599\u3002\u53ef\u4ee5\u7528\u80f6\u5e26\u7eb8\u53ef\u4ee5\u4e0d\u65ad\u7684\u6495\uff0c\u6700\u540e\u5f97\u5230\u4e00\u7ef4\u6750\u6599\u3002\u540c\u6837\u5982\u679c\u4ed6\u5728\u6240\u6709\u7ef4\u5ea6\u4e0a\u9762\u90fd\u6ca1\u6709\u5316\u5b66\u952e\u8fde\u63a5\uff0c\u90a3\u5c31\u53ef\u4ee5\u5b9a\u4e49\u4e3a\u96f6\u7ef4\u6750\u6599\u3002<\/p>\n<p>\u8fd0\u7528\u56fe\u8bba\u4f4e\u7ef4\u6750\u6599\u7684\u5b9a\u4e49\u548c\u7ed3\u6784\u5927\u6570\u636e\u53ef\u4ee5\u91cd\u65b0\u53d1\u73b0\u65b0\u578b\u7684\u4e8c\u7ef4\u3001\u4e00\u7ef4\u3001\u96f6\u7ef4\u6750\u6599\uff0c\u6211\u4eec\u6700\u8fd1\u5728\u56fd\u5bb6\u79d1\u5b66\u8bc4\u8bba\u4e0a\u9762\u53d1\u8868\u4e86\u7814\u7a76\u6587\u7ae0\uff0c\u6280\u672f\u7ec6\u8282\uff1a\u5728\u6750\u6599\u7684\u5316\u5b66\u56fe\u8bba\u7814\u7a76\u65b9\u6cd5\u4e2d\uff0c\u539f\u5b50\u88ab\u5b9a\u4e49\u4e3a\u70b9\uff0c\u76f8\u90bb\u539f\u5b50\u95f4\u5b58\u5728\u7684\u5316\u5b66\u952e\u88ab\u62bd\u8c61\u4e3a\u8fb9\u3002\u6211\u4eec\u57fa\u4e8e88159\u79cd\u65e0\u5206\u6570\u5360\u636e\u60c5\u51b5\u7684\u6676\u4f53\u6750\u6599\uff0c\u6839\u636e\u5143\u7d20\u7684\u7535\u8d1f\u6027\u9009\u62e9\u76f8\u5e94\u539f\u5b50\u7684\u5171\u4ef7\u3001\u79bb\u5b50\u6216\u91d1\u5c5e\u534a\u5f84\u4ece\u800c\u786e\u5b9a\u539f\u5b50\u95f4\u7684\u8fd1\u90bb\u5173\u7cfb\u3002\u901a\u8fc7\u8be5\u65b9\u6cd5\u53ef\u4ee5\u6784\u9020\u6bcf\u79cd\u6750\u6599\u7684\u7ed3\u6784\u56fe\uff0c\u5e76\u8868\u8fbe\u4e3a\u90bb\u63a5\u77e9\u9635\u3002\u901a\u8fc7\u56fe\u8bba\u65b9\u6cd5\uff0c\u627e\u5230\u7ed3\u6784\u56fe\u4e2d\u7684\u72ec\u7acb\u8054\u901a\u5355\u5143\uff0c\u5bf9\u5176\u8fdb\u884c\u5206\u6790\u53ef\u83b7\u5f97\u8be5\u8fde\u901a\u5355\u5143\u7684\u7ef4\u5ea6\uff0c\u7531\u6b64\u7b5b\u9009\u51fa\u4e00\u7cfb\u5217\u4e8c\u7ef4\u3001\u4e00\u7ef4\u548c\u96f6\u7ef4\uff082D\u30011D\u548c0D\uff09\u6750\u6599\u3002\u57fa\u4e8e\u56fe\u540c\u6784\u6bd4\u5bf9\u65b9\u6cd5\uff0c\u53ef\u4ee5\u8fdb\u4e00\u6b65\u5c06\u4f4e\u7ef4\u7ed3\u6784\u5206\u6210\u4e0d\u540c\u79cd\u7c7b\u7684\u62d3\u6251\u7ed3\u6784\u7c7b\u578b\u3002\u91c7\u7528\u4ece\u7b2c\u4e00\u6027\u539f\u7406\u5206\u5b50\u52a8\u529b\u5b66\u65b9\u6cd5\u8bc4\u4f30\u4e00\u7ef4\u5316\u5408\u7269\u7684\u52a8\u529b\u5b66\u7a33\u5b9a\u6027\uff0c\u4ece\u800c\u6392\u9664\u4e0d\u7a33\u5b9a\u7684\u5316\u5408\u7269\u3002\u7ecf\u8fc7\u4e0a\u8ff0\u6b65\u9aa4\u540e\uff0c\u603b\u5171\u5f97\u5230\u4e86244\u79cd\u7a33\u5b9a\u7684\u4e00\u7ef4\u6750\u6599\uff0c\u8fd9\u4e9b\u5316\u5408\u7269\u53ef\u88ab\u5f52\u7c7b\u4e3a138\u4e2a\u62d3\u6251\u7ed3\u6784\u7c7b\u578b\u3002\u53f3\u4e0a\u89d2\u56fe\uff1a\u4e3a\u4e86\u8fdb\u4e00\u6b65\u5206\u6790\u6750\u6599\u7684\u5316\u5b66\u4fe1\u606f\uff0c\u7814\u7a76\u56e2\u961f\u4ece\u6210\u952e\u7279\u6027\u4e0e\u539f\u5b50\u5c3a\u5bf8\u6548\u5e94\u4e24\u4e2a\u65b9\u9762\u8fdb\u884c\u7814\u7a76\u3002\u5176\u4e2d\u6210\u952e\u7279\u6027\u7531\u6676\u4f53\u8f68\u9053\u54c8\u5bc6\u987f\u5e03\u5c45\uff08COHP\uff09\u7684\u79ef\u5206\u9879\u6765\u4ee3\u8868\uff0c\u539f\u5b50\u5c3a\u5bf8\u6548\u5e94\u7531\u9633\u79bb\u5b50\u4e2d\u5fc3\u914d\u4f4d\u591a\u9762\u4f53\u4e2d\u6b63\u79bb\u5b50\u548c\u8d1f\u79bb\u5b50\u7684\u534a\u5f84\u6bd4\u4f5c\u4e3a\u91cf\u5316\u6307\u6807\u3002\u4e00\u7ef4\u6750\u6599\u5728\u5316\u5b66\u7a7a\u95f4\u7684\u5206\u5e03\u60c5\u51b5\u53cd\u6620\u51fa\u76f8\u540c\u7ed3\u6784\u7c7b\u578b\u7684\u6750\u6599\u62e5\u6709\u76f8\u4f3c\u7684\u6027\u8d28\uff0c\u8bf4\u660e\u4e86\u56fe\u8bba\u5206\u7c7b\u65b9\u6cd5\u6f5c\u85cf\u7740\u5bf9\u6750\u6599\u6027\u8d28\u7684\u5206\u7c7b\u3002\u53f3\u4e0b\u89d2\u56fe\uff1a(a) 2D\u30011D\u548c0D\u5316\u5408\u7269\u7684\u5265\u79bb\u80fd\u5206\u5e03\u7684\u7c7b\u4f3c\u5c0f\u63d0\u7434\u5f62\u72b6\u56fe\u3002\u7070\u8272\u7ebf\u8868\u793a\u7531\u77f3\u58a8\u70ef\u7684\u5265\u79bb\u80fd\u5b9a\u4e49\u7684\u9608\u503c\u3002\u63a5\u8fd1\u534a\u6570\u7684\u4e00\u7ef4\u6750\u6599\u62e5\u6709\u8f83\u4f4e\u7684\u7406\u8bba\u5265\u79bb\u80fd\uff08\u80f6\u5e26\u53ef\u4ee5\u6495\u5f00\uff09\uff0c\u610f\u5473\u7740\u8fd9\u4e9b\u6750\u6599\u5747\u6709\u53ef\u80fd\u5728\u5b9e\u9a8c\u4e2d\u88ab\u6210\u529f\u5236\u5907 (b)\u4e00\u7ef4\u6750\u6599\u4e2d\u5143\u7d20\u7ec4\u5206\u7684\u6570\u76ee\u7edf\u8ba1\u56fe\uff0c\u5176\u4e2d\u7070\u8272\u7684\u5143\u7d20\u4ee3\u8868\u5176\u4e0d\u5b58\u5728\u4e8e\u4efb\u4f55\u4e00\u7ef4\u5316\u5408\u7269\u4e2d\u3002<\/p>\n<p>\u7531\u6b64\u6211\u4eec\u53d1\u73b0\u4e86200\u591a\u79cd\u65b0\u578b\u7684\u4e00\u7ef4\u6750\u6599\u3002\u4e00\u7ef4\u6750\u6599\u6709\u4ec0\u4e48\u7528\uff1f\u56fd\u9645\u534a\u5bfc\u4f53\u7ec4\u7ec7\u89c4\u5212\u7684\u4e0b\u4e00\u4ee3\u534a\u5bfc\u4f53\u5c06\u628a\u4e00\u7ef4\u6750\u6599\u4f5c\u4e3a\u5668\u4ef6\u57fa\u7840\u6750\u6599\u3002\u76ee\u524d\u7528\u7684\u7845\u57fa\u534a\u5bfc\u4f53\uff0c\u6240\u6709\u7684\u7845\u5355\u6676\u5b83\u90fd\u662f\u7845\u7684\u56db\u9762\u4f53\u5171\u4ef7\u8fde\u63a5\u6210\u7684\u6676\u4f53\u7f51\u7edc\uff0c\u5f53\u5668\u4ef6\u7684\u6c9f\u9053\u53d8\u5f97\u8d8a\u6765\u8d8a\u5c0f\uff0c\u52301nm\u53ea\u6709\u5341\u51e0\u4e2a\u539f\u5b50\u6392\u5217\uff0c\u8fb9\u754c\u5c06\u670910%\u5de6\u53f3\u65ad\u952e\uff0c\u5b83\u8fd8\u662f\u7845\u5417\uff1f\u8fd9\u4e9b\u65ad\u952e\u8981\u754c\u9762\u91cd\u6784\u5f62\u6210\u949d\u5316\u5c42\uff0c\u672c\u5f81\u7845\u7684\u6027\u8d28\u5c06\u88ab\u8c03\u63a7\uff0c\u4f1a\u56e0\u4e3a\u7845\u7684\u65ad\u952e\u6570\u4e0d\u540c\u53ca\u91cd\u6784\u4e0d\u5747\u5300\u4f7f\u5f97\u5668\u4ef6\u5728\u539f\u5b50\u5c3a\u5ea6\u4e0a\u7684\u4e0d\u4e00\u81f4\u800c\u4e0d\u7a33\u5b9a\u3002\u6240\u4ee5\u771f\u6b63\u7684\u4e00\u7ef4\u6750\u6599\u5728\u81ea\u8eab\u65b9\u5411\u662f\u4e00\u7ef4\u5316\u5b66\u952e\u8fde\u63a5\uff0c\u6ca1\u6709\u5176\u5b83\u7ef4\u7684\u5316\u5b66\u952e\u8981\u88ab\u5207\u65ad\u548c\u91cd\u6784\uff0c\u4ece\u800c\u5728\u539f\u5b50\u5c3a\u5ea6\u4fdd\u6301\u7a33\u5b9a1\u7ef4\u672c\u5f81\u7684\u6027\u8d28\u3002<\/p>\n<p>\u8fd9\u7bc7\u6587\u7ae0\u5927\u5bb6\u611f\u5174\u8da3\uff0c\u8fd8\u53ef\u4ee5\u770b\u5230\u4e00\u7ef4\u548c\u4e8c\u7ef4\u662f\u600e\u4e48\u6f14\u5316\u7684\uff0c\u4e8c\u7ef4\u548c\u4e00\u7ef4\u4e4b\u95f4\u76f8\u4e92\u8f6c\u5316\u7684\u89c4\u5f8b\u3002\u8fd8\u6709\u4e00\u4e2a\u6709\u8da3\u6676\u4f53\u5316\u5b66\u95ee\u9898\uff0c\u6309\u7167\u9c8d\u6797\u89c4\u5219\uff0c\u4e24\u4e2a\u91d1\u5c5e\u914d\u4f4d\u591a\u9762\u4f53\u8fde\u63a5\u65f6\u4ee5\u4e24\u4e2a\u91d1\u5c5e\u4e2d\u5fc3\u539f\u5b50\u4e4b\u95f4\u8ddd\u79bb\u8fdc\uff08\u6392\u65a5\u529b\u5c0f\uff09\u4f1a\u6bd4\u8f83\u7a33\u5b9a\uff0c\u4e24\u4e2a\u591a\u9762\u4f53\u4ee5\u5171\u9876\u70b9\u8fde\u63a5\u6700\u8fdc\uff0c\u5176\u6b21\u662f\u5171\u8fb9\u8fde\u63a5\uff0c\u6700\u8fd1\u7684\u662f\u5171\u9762\u8fde\u63a5\uff0c\u5927\u5bb6\u60f3\u60f3\u5982\u679c\u4e24\u4e2a\u91d1\u5c5e\u5143\u7d20\u8d8a\u9760\u8d8a\u8fd1\u8fd9\u4e24\u4e2a\u539f\u5b50\u7684\u7535\u5b50\u5c31\u4f1a\u53d1\u751f\u4ea4\u4e92\u4f5c\u7528\u5f62\u6210\u5171\u4eab\uff08Interaction\uff09\uff0c\u7535\u5b50\u5728\u591a\u9762\u4f53\u7f51\u7edc\u4f1a\u5f62\u6210\u6e17\u6d41\u6548\u5e94\uff0c\u8fd9\u79cd\u7535\u5b50\u6e17\u6d41\u5c31\u4f7f\u5f97\u6750\u6599\u5177\u6709\u534a\u5bfc\u4f53\u6216\u5bfc\u4f53\u7684\u6027\u8d28\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u56fe\u8bba+\u673a\u5668\u5b66\u4e60\uff1a\u9884\u6d4b\u7ed3\u6784\u4e0e\u6027\u8d28<\/strong><\/p>\n<p>\u4e00\u4e2a\u6beb\u7c73\u5927\u5c0f\u7684\u6676\u4f53\u670910<sup>20<\/sup>\u591a\u4e2a\u539f\u5b50\u6784\u6210\uff0c10\u4e2a\u7eb3\u7c73\u5927\u5c0f\u7684\u6676\u4f53\u4e5f\u6709\u4e0a\u4e07\u4e2a\u539f\u5b50\uff0c\u6709\u8da3\u7684\u662f\u8fd9\u4e9b\u6676\u4f53\u53ea\u67091\u79cd\u6216\u5c11\u6570\u51e0\u79cd\u786e\u5b9a\u5468\u671f\u6027\u6392\u5217\u7ed3\u6784\u3002\u4f8b\u5982\u78b3\u539f\u5b50\u6784\u6210\u7684\u6676\u4f53\u5e38\u89c1\u53ea\u6709\u77f3\u58a8\u548c\u91d1\u521a\u77f3\u3002\u5982\u679c\u539f\u5b50\u6570\u5c11\u5230\u53ea\u6709\u51e0\u4e2a\u6216\u51e0\u5341\u4e2a\u65f6\uff0c\u539f\u5b50\u5806\u79ef\u4e0e\u6392\u5e8f\u7684\u53ef\u80fd\u6027\u4f1a\u968f\u539f\u5b50\u6570\u5448\u73b0\u6307\u6570\u7ea7\u589e\u52a0\u3002\u8fd9\u91cc\u9762\u5f88\u6709\u8da3\u7684\u95ee\u9898\u662f\u8fd9\u79cd\u968f\u7740\u539f\u5b50\u6570\u76ee\u589e\u52a0\u65e0\u9650\u591a\u7684\u6392\u5e8f\u53ef\u80fd\u6027\u662f\u5982\u4f55\u6700\u540e\u53d8\u6210\u6709\u9650\u51e0\u79cd\u6676\u4f53\uff1f\u662f\u5982\u4f55\u8fc7\u6e21\u6216\u6f14\u5316\u7684\uff1f\u6211\u4eec\u5982\u4f55\u53bb\u9884\u6d4b\u548c\u53d1\u73b0\uff1f\u8fd8\u6709\u50ac\u5316\u9886\u57df\u4ece\u7eb3\u7c73\u50ac\u5316\u5230\u76ee\u524d\u5f88\u70ed\u7684\u5355\u539f\u5b50\u6216\u56e2\u7c07\uff08\u51e0\u4e2a\u5230\u51e0\u5341\u4e2a\u539f\u5b50\uff09\u50ac\u5316\u90fd\u5b58\u5728\u201c\u539f\u5b50\u6570\u4e0e\u5176\u51e0\u4f55\u6784\u578b\/\u7535\u5b50\u7ed3\u6784\u53ca\u5176\u6027\u80fd\u7684\u76f8\u5173\u6027\u201d\u79d1\u5b66\u95ee\u9898\u3002<\/p>\n<p>\u6211\u4eec\u628a\u91cf\u5b50\u5316\u5b66\u8ba1\u7b97\u3001\u4ee3\u6570\u56fe\u8bba\u6301\u7eed\u540c\u8c03\u65b9\u6cd5\u548c\u673a\u5668\u5b66\u4e60\u76f8\u7ed3\u5408\u9884\u6d4b\u591a\u539f\u5b50\u5806\u79ef\u80fd\u91cf\u6700\u4f4e\u7684\u53ef\u80fd\u7ed3\u6784\uff0c\u8003\u8651\u6676\u80de\u4e2d\u6bcf\u4e2a\u539f\u5b50\u5468\u56f4\u4e0d\u540c\u73af\u5883\u6784\u6210\u7684\u6301\u7eed\u540c\u8c03\uff0c\u4ece\u800c\u5728\u62d3\u6251\u4e0d\u53d8\u91cf\u4e2d\u5f15\u5165\u539f\u5b50\u4fe1\u606f\u3002\u57fa\u4e8e\u8be5\u7279\u5f81\u6240\u6784\u5efa\u7684\u6676\u4f53\u5316\u5408\u7269\u673a\u5668\u5b66\u4e60\u6a21\u578b\uff0c\u53ef\u4ee5\u51c6\u786e\u9884\u6d4b\u6750\u6599\u7684\u5f62\u6210\u80fd\uff0c\u8bef\u5dee\u4ec5\u4e3a61 meV\/atom\u3002\u8fd0\u7528\u8fd9\u539f\u5b50\u95f4\u7684\u77ed\u7a0b\u4f5c\u7528\u548c\u957f\u7a0b\u4f5c\u7528\u7b49\u6570\u636e\u4fe1\u606f\uff0c\u57fa\u4e8e\u63d0\u53d6\u7684\u62d3\u6251\u7279\u5f81\uff0c\u6784\u5efa\u56e2\u7c07\u80fd\u91cf\u9884\u6d4b\u673a\u5668\u5b66\u4e60\u6a21\u578b\u3002\u5229\u7528\u5c11\u91cf\u539f\u5b50\u6570\u56e2\u7c07\u7ed3\u6784\u6784\u6210\u7684\u6570\u636e\u96c6\u6765\u8bad\u7ec3\u6240\u5f97\u7684\u6a21\u578b\u5373\u53ef\u5bf9\u4e2d\u578b\u548c\u5927\u578b\u56e2\u7c07\u5f62\u6210\u975e\u5e38\u9ad8\u7684\u9884\u6d4b\u7cbe\u5ea6\u3002\u8be5\u6a21\u578b\u53ef\u7528\u4e8e\u56e2\u7c07\u7ed3\u6784\u7684\u5feb\u901f\u7b5b\u9009\uff0c\u52a0\u5feb\u6700\u7a33\u5b9a\u56e2\u7c07\u7ed3\u6784\u641c\u7d22\u7684\u901f\u5ea6\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u56fe\u8bba+\u673a\u5668\u5b66\u4e60\uff1a\u9884\u6d4b\u7ed3\u6784\u4e0e\u6027\u8d28<\/strong>\u00a0<strong>\u81ea\u76d1\u7763\u5b66\u4e60<\/strong><strong>-&gt;<\/strong><strong>\u5173\u952e\u7ed3\u6784\u8868\u793a<\/strong><\/p>\n<p>\u4e2d\u56fd\u6709\u4e00\u4e2a\u5173\u4e8e\u77db\u548c\u76fe\u7684\u6545\u4e8b\uff0c\u5356\u77db\u5c31\u662f\u4ed6\u7684\u77db\u975e\u5e38\u5c16\u5229\uff0c\u53ef\u4ee5\u523a\u7a7f\u6240\u6709\u7684\u4e1c\u897f\uff0c\u5356\u76fe\u7684\u8bf4\u4ed6\u7684\u76fe\u53ef\u4ee5\u6321\u4f4f\u4e16\u754c\u6240\u6709\u7684\u4e1c\u897f\uff0c\u90a3\u4eba\u4eec\u4f1a\u95ee\u628a\u80fd\u523a\u7a7f\u6240\u6709\u4e1c\u897f\u7684\u77db\u53bb\u523a\u80fd\u6321\u4f4f\u6240\u6709\u4e1c\u897f\u7684\u76fe\u7684\u7ed3\u679c\u5982\u4f55\uff1f\u81ea\u76d1\u7763\u5b66\u4e60\u5c31\u662f\u81ea\u5df1\u628a\u81ea\u5df1\u7684\u77db\u53d8\u5f97\u66f4\u5c16\u5229\u6765\u523a\u7a7f\u81ea\u5df1\u7684\u76fe\uff0c\u76fe\u8981\u628a\u81ea\u5df1\u53d8\u5f97\u66f4\u5f3a\u786c\u4e0d\u88ab\u81ea\u5df1\u77db\u523a\u7a7f\uff0c\u8fd9\u6837\u53cd\u590d\u7684\u6539\u8fdb\u548c\u63d0\u5347\uff0c\u81ea\u76d1\u7763\u8fed\u4ee3\u5b66\u4e60\u3002\u4e3a\u4e86\u5bf9\u6750\u6599\u7684\u6027\u8d28\u9884\u6d4b\u66f4\u52a0\u51c6\u786e\uff0c\u6211\u4eec\u8fd0\u7528\u81ea\u76d1\u7763\u673a\u5668\u5b66\u4e60\u65b9\u6cd5\u6765\u9884\u6d4b\u7ed3\u6784\u548c\u6027\u8d28\u3002<\/p>\n<p>\u6280\u672f\u7ec6\u8282\uff1a\u5de6\u56fe\u5229\u7528\u201c\u6b63\u786e\u201d\u7684\u5c0f\u5206\u5b50\u5b57\u7b26\u4e32\uff0c\u5373smiles\u8fdb\u884c\u6784\u9020\uff0c\u8ba4\u4e3a\u6784\u9020\u51fa\u201c\u4e0d\u5b8c\u6574\u201c\u7684\u5b57\u7b26\u4e32\u4e0e\u76f8\u5e94\u7684\u7b54\u6848\uff1b\u7136\u540e\u5728\u8bad\u7ec3\u8fc7\u7a0b\u4e2d\uff0c\u8f93\u5165&#8221;\u4e0d\u5b8c\u6574\u201d\u7684\u5b57\u7b26\u4e32\uff0c\u8ba9\u6a21\u578b\u63a8\u6d4b\u51fa\u6b63\u786e\u7684\u90e8\u5206\u3002\u53f3\u56fe\u63cf\u8ff0\u4e86\u6587\u7ae0\u7684\u6574\u4f53\u903b\u8f91\uff1a\u57fa\u4e8e\u81ea\u76d1\u7763\u5b66\u4e60\u7684\u7b56\u7565\uff0c\u6211\u4eec\u57fa\u4e8eChembl\uff0cZINC,\u548cPubChem\u4e09\u4e2a\u5927\u578b\u6570\u636e\u96c6\uff0c\u8bad\u7ec3\u51fa\u4e86\u4e09\u79cd\u9884\u8bad\u7ec3\u6a21\u578b\u3002\u5e76\u4e14\u57fa\u4e8e\u8fd9\u4e09\u4e2a\u5927\u6a21\u578b\uff0c\u8fdb\u884c\u4e86\u4e00\u7cfb\u5217\u7684\u4e0b\u6e38\u673a\u5668\u5b66\u4e60\u4efb\u52a1\uff08\u5305\u542b\u4e86\u56de\u5f52\u4efb\u52a1\uff0c\u5206\u7c7b\u4efb\u52a1\uff0c\u4ee5\u53cavirtual screening\u7684\u4efb\u52a1\uff09\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u56fe\u8bba+\u673a\u5668\u5b66\u4e60\uff1a\u52a0\u5165\u9884\u5b66\u4e60\u7528\u5c0f\u6837\u672c\u6570\u636e\u5b9e\u73b0\u51c6\u786e\u9884\u6d4b\u7ed3\u6784\u4e0e\u6027\u8d28<\/strong><\/p>\n<p>\u6709\u4e00\u6b21\u4e0e\u5927\u6570\u636e\u4eba\u5de5\u667a\u80fd\u56e2\u961f\u8ba8\u8bba\uff0c\u5982\u4f55\u9884\u6d4b\u5728\u4e00\u4e2a\u673a\u573a\u91cc\u9762\u5224\u522b\u4e00\u5806\u4eba\u662f\u5728\u4e00\u8d77\u8ba8\u8bba\u95ee\u9898\uff0c\u8fd8\u662f\u5728\u5435\u67b6\u53ca\u8981\u5f15\u53d1\u6253\u67b6\uff1f\u901a\u8fc7\u5f88\u591a\u573a\u666f\u65e2\u5b66\u4e60\u201c\u8ba8\u8bba\u573a\u666f\u201d\u8fd8\u8981\u5b66\u4e60\u201c\u5435\u67b6\u573a\u666f\u201d\uff0c\u4f46\u8fd9\u79cd\u611f\u6027\u7684\u573a\u666f\u90fd\u662f\u6709\u9650\u7684\u3002\u4f46\u4eba\u7c7b\u5173\u4e8e\u201c\u8ba8\u8bba\u201d\u4ee5\u53ca\u201c\u5435\u67b6\u201d\u6709\u7406\u6027\u7684\u6982\u5ff5\u5b9a\u4e49\u4e0e\u60c5\u666f\u63cf\u8ff0\uff0c\u5982\u7535\u5f71\u3001\u5c0f\u8bf4\u3001\u7ed8\u753b\u7b49\u90fd\u6709\u611f\u6027\u60c5\u666f\u63cf\u8ff0\u4fe1\u606f\uff0c\u5bf9\u8fd9\u4e9b\u4fe1\u606f\u8fdb\u884c\u201c\u9884\u201d\u5b66\u4e60\uff0c\u5e94\u8be5\u53ef\u4ee5\u589e\u52a0\u5224\u65ad\u7684\u51c6\u786e\u6027\u3002\u5176\u5b9e\u6211\u4eec\u4eba\u7684\u5b66\u4e60\u4e5f\u662f\u4e0d\u65ad\u4ece\u611f\u6027\u5230\u7406\u6027\uff0c\u53c8\u56de\u5230\u5b9e\u9645\u7684\u611f\u6027\u573a\u666f\u53bb\u5224\u65ad\u4e0e\u4f5c\u51b3\u5b9a\u3002\u8fd0\u7528\u8fd9\u4e2a\u601d\u60f3\u6211\u4eec\u62ff\u6750\u6599\u76f8\u5173\u7684\u77e5\u8bc6\u4f5c\u4e3a\u201c\u9884\u5b66\u4e60\u201d\uff0c\u4f7f\u5f97\u5bf9\u5c0f\u6837\u672c\u6750\u6599\u6570\u636e\u9884\u6d4b\u7684\u51c6\u786e\u6027\u5927\u5927\u63d0\u9ad8\u3002<\/p>\n<p>\u6211\u4eec\u5728 Nat commun.\u8bb2\u4e86\u5982\u4f55\u5728\u6709\u9650\u7684\u5c0f\u6837\u672c\u6570\u636e\u8fdb\u884c\u673a\u5668\u5b66\u4e60\u5b9e\u73b0\u9ad8\u7cbe\u5ea6\u7684\u9884\u6d4b\u6709\u673a\u5316\u5408\u7269\u7684\u6027\u80fd\uff0c\u5305\u62ec\u6bd2\u6027\u7b49\uff0c\u6709\u673a\u7269\u6bd2\u6027\u6837\u672c\u6570\u6bd4\u8f83\u5c11\uff081\u4e07\u5de6\u53f3\uff09\uff0c\u4f46\u6709\u673a\u7269\u591a\u6a21\u6001\/\u7ef4\u5ea6\u7684\u76f8\u5173\u4fe1\u606f\u662f\u5927\u6570\u636e\uff08SMILES \u6709\u673a\u6570\u636e\u5e93\u67097\u4ebf\u4e2a\uff09\uff0c\u57fa\u4e8e\u5927\u6570\u636e\u6837\u672c\u9884\u5b66\u4e60\uff0c\u6709\u6548\u9884\u6d4b\u5c0f\u6837\u672c\u6709\u673a\u5316\u5408\u7269\u7684\u6bd2\u6027\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u6750\u6599\u5927\u6570\u636e&lt;-&gt;\u53cd\u5411\u8bbe\u8ba1<\/strong><\/p>\n<p>\u641e\u6750\u6599\u7684\u4eba\u6709\u4e00\u4e2a\u68a6\u60f3\u77e5\u9053\u9700\u5177\u6709\u7279\u5b9a\u6027\u80fd\u7684\u6750\u6599\u770b\u5982\u4f55\u628a\u5b83\u8bbe\u8ba1\u548c\u5236\u5907\u51fa\u6765\uff1f\u8fd9\u53eb\u505a\u53cd\u5411\u8bbe\u8ba1\uff0c\u6bd4\u5982\u822a\u5929\u9700\u8981\u4e00\u4e2a\u6750\u6599\uff0c\u9700\u8981\u786c\u5ea6\u591a\u5c11\uff0c\u97e7\u6027\u591a\u5c11\uff0c\u4e00\u822c\u5c31\u9676\u74f7\u5f88\u786c\uff0c\u91d1\u5c5e\u6709\u5ef6\u5c55\u6027\u5f88\u97e7\uff0c\u5bb9\u6613\u53d8\u5f62\uff0c\u4f46\u5b83\u4e0d\u5bb9\u6613\u65ad\u88c2\uff0c\u80fd\u4e0d\u80fd\u6709\u4e00\u4e2a\u6750\u6599\u53c8\u786c\u53c8\u97e7\uff0c\u5982\u4f55\u6309\u7167\u8fd9\u4e2a\u9700\u6c42\u8fdb\u884c\u6750\u6599\u7684\u53cd\u5411\u8bbe\u8ba1\uff1f\u00a0\u6211\u4eec\u5bf9\u57fa\u4e8e\u5927\u6570\u636e\u548c\u4eba\u5de5\u667a\u80fd\u5f00\u5c55\u6750\u6599\u53cd\u5411\u8bbe\u8ba1\u7684\u7814\u7a76\u8fdb\u5c55\u4f5c\u4e86\u7efc\u8ff0\uff0c\u8bb2\u4e86\u53cd\u5411\u8bbe\u8ba1\u7684\u4e00\u4e2a\u6982\u5ff5\uff0c\u5373\u5df2\u6709\u6676\u4f53\u7ed3\u6784\u6570\u636e\u5e93\u4e2d\u7684\u7ed3\u6784\u6570\u636e\u4f5c\u4e3a\u6570\u636e\u57fa\u7840\uff0c\u901a\u8fc7\u6750\u6599\u7279\u5f81\u63d0\u53d6\u65b9\u6cd5\u63d0\u53d6\u7ed3\u6784\u7279\u5f81\uff0c\u5e76\u5c06\u7279\u5f81\u9001\u5165\u795e\u7ecf\u7f51\u7edc\u53cd\u5411\u8bbe\u8ba1\u6a21\u578b\u4e2d\u53cd\u5411\u8bbe\u8ba1\u51fa\u65b0\u7684\u6750\u6599\uff0c\u901a\u8fc7DFT\u8ba1\u7b97\u8fdb\u884c\u9a8c\u8bc1\uff0c\u5c06\u9a8c\u8bc1\u540e\u7684\u65b0\u6750\u6599\u4f5c\u4e3a\u6570\u636e\u5e93\u7684\u8865\u5145\uff0c\u5f62\u6210\u4e00\u4e2a\u5b8c\u6574\u7684\u6570\u636e\u8fed\u4ee3\u751f\u6210\u8fc7\u7a0b\u3002<\/p>\n<p>\u7ec6\u8282\uff1a\u5de6\u4e0b\u56fe\u4e2d\u5c55\u73b0\u7684\u53cd\u5411\u8bbe\u8ba1\u6a21\u578b\u4e3aVAE\uff08\u53d8\u5206\u81ea\u7f16\u7801\u5668\uff09\uff0c\u8be5\u6a21\u578b\u7531\u7f16\u7801\u5668\uff0c\u9690\u53d8\u91cf\u548c\u89e3\u7801\u5668\u6784\u6210\u3002\u53d8\u5206\u7684\u6838\u5fc3\u601d\u60f3\u4e3a\u5f3a\u8feb\u7f16\u7801\u5668\u4ece\u9ad8\u7ef4\u6750\u6599\u7f16\u7801\u83b7\u5f97\u4e00\u4e2a\u7b26\u5408\u9ad8\u65af\u5206\u5e03\u7684\u4f4e\u7ef4\u6295\u5f71\u5411\u91cfZ\uff0c\u5373VAE\u5e0c\u671b\u5c06\u8bad\u7ec3\u6570\u636eX\u7684\u6982\u7387\u5206\u5e03\u6620\u5c04\u5230\u9ad8\u65af\u5206\u5e03\uff0c\u4f7f\u5f97\u4eba\u4e3a\u8f93\u5165\u4efb\u610f\u4e00\u4e2a\u9ad8\u65af\u5206\u5e03\u6216\u8005\u4ece\u6750\u6599\u7a7a\u95f4\u6309\u56fa\u5b9a\u89c4\u5219\u641c\u7d22\u5230\u7684\u9690\u53d8\u91cf\uff0c\u5373\u53ef\u901a\u8fc7\u89e3\u7801\u5668\u83b7\u5f97\u4e00\u4e2a\u63a5\u8fd1\u771f\u5b9e\u7684\u6750\u6599\u3002\u540c\u65f6\u5728\u6b64\u8fc7\u7a0b\u4e2d\uff0c\u901a\u8fc7\u5c06\u6750\u6599\u6027\u8d28\u52a0\u5165\u6750\u6599\u7f16\u7801\u6216\u8005\u635f\u5931\u51fd\u6570\uff0c\u8fd8\u53ef\u4ee5\u63a7\u5236\u751f\u6210\u6750\u6599\u7684\u6027\u80fd\u3002\u5176\u5927\u81f4\u7684\u5de5\u4f5c\u6d41\u7a0b\u5982\u4e0b\uff1a1\u3001\u901a\u8fc7\u5377\u79ef\u53ca\u591a\u5c42\u5168\u8fde\u63a5\u7f51\u7edc\uff08\u6f0f\u6597\u72b6\u7f51\u7edc\u7684\u5de6\u8fb9\u90e8\u5206\uff09\u5b9e\u73b0\u9ad8\u7ef4\u6750\u6599\u7a7a\u95f4\u5230\u4f4e\u7ef4\u7a7a\u95f4\uff08\u9690\u53d8\u91cf\uff09\u7684\u6620\u5c04\uff0c\u8be5\u90e8\u5206\u88ab\u79f0\u4e3a\u7f16\u7801\u5668\uff08encoder\uff09\u3002\u5728VAE\u4e2d\uff0c\u4f1a\u5bf9\u7f16\u7801\u5668\u6dfb\u52a0\u7ea6\u675f\uff0c\u5f3a\u8feb\u8be5\u9690\u53d8\u91cf\u670d\u4ece\u6807\u51c6\u6b63\u6001\u5206\u5e03\u30022\u3001\u901a\u8fc7\u53e6\u4e00\u4e2a\u591a\u5c42\u5168\u8fde\u63a5\u7f51\u7edc\u53ca\u53cd\u5377\u79ef\uff08\u6f0f\u6597\u72b6\u7f51\u7edc\u7684\u53f3\u8fb9\u90e8\u5206\uff09\u5c06\u4f4e\u7ef4\u5411\u91cf\u6295\u5f71\u56de\u9ad8\u7ef4\u7a7a\u95f4\uff0c\u5b9e\u73b0\u5bf9\u65b0\u7ed3\u6784\u7684\u751f\u6210\u3002\u8be5\u90e8\u5206\u88ab\u79f0\u4e3a\u89e3\u7801\u5668\uff08decoder\uff09\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u77e5\u8bc6\u56fe\u8c31\u7684\u8bde\u751f<\/strong><\/p>\n<p>\u8bb2\u5927\u6570\u636e\uff0c\u6211\u4eec\u770b\u6709\u4e9b\u4ec0\u4e48\u6570\u636e\u53ef\u4ee5\u6536\u96c6\u3002\u521a\u624d\u8bb2\u7684\u6676\u4f53\u7ed3\u6784\u6570\u636e\uff0c\u8fd9\u8fd8\u662f\u975e\u5e38\u6709\u9650\u7684\uff0c\u65e0\u673a\u6676\u4f53\u7ed3\u6784\u5df2\u7ecf\u5408\u6210\u7684\u6570\u636e\u5927\u698218\u4e07\uff0c\u52a0\u8ba1\u7b97\u9884\u6d4b\u603b\u5171\u4e5f\u5c3165\u4e07\u4e2a\u72ec\u7acb\u3002\u6587\u672c\u6570\u636e\u66f4\u5927\uff0c\u6211\u4eec\u5df2\u7ecf\u6709\u5927\u6982\u5343\u4e07\u7bc7\u7684\u79d1\u5b66\u6587\u7ae0\u53d1\u8868\uff0c\u6bcf\u5e74\u53d1\u8868\u7684\u6587\u7ae0\u7684\u91cf\u4e0d\u65ad\u5728\u589e\u52a0\uff0c\u4eba\u662f\u8bfb\u4e0d\u8fc7\u6765\u7684\u3002\u8fd8\u6709\u975e\u6587\u672c\u7684\u7167\u7247\uff08\u5982\u7535\u955c\u3001x-\u5c04\u7ebf\u7167\u7247\uff09\u548c\u89c6\u9891\u4fe1\u606f\u3002\u6211\u4eec\u6b63\u5728\u6784\u5efa\u7ed3\u6784\u3001\u6587\u672c\u3001\u56fe\u7247\u3001\u89c6\u9891\u7b49\u591a\u6a21\u6001\u4fe1\u606f\u878d\u5408\uff0c\u501f\u9274\u8c37\u6b4c\u57282012\u5e74\u5c31\u63d0\u51fa\u4e86\u4e00\u4e2a\u77e5\u8bc6\u56fe\u8c31\uff0c\u6784\u5efa\u6750\u6599\u77e5\u8bc6\u56fe\u8c31\u6765\u9884\u6d4b\u4e0b\u4e00\u4ee3\u6750\u6599\u3002<\/p>\n<p>\u8bb8\u591a\u4eba\u89c9\u5f97\u8c37\u6b4c\u7684\u641c\u7d22\u6bd4\u5176\u4ed6\u7684\u641c\u7d22\u7cbe\u51c6\u3002\u5927\u5bb6\u77e5\u9053\u8981\u51c6\u786e\u548c\u5feb\u901f\u627e\u5230\u76ee\u7684\u5730\u901a\u5e38\u9700\u8981\u4e00\u79cd\u5f88\u597d\u7684\u5730\u56fe\u30022012\u5e74\uff0cGoogle\u6b63\u5f0f\u63d0\u51fa\u4e86\u201c\u77e5\u8bc6\u56fe\u8c31\uff08Knowledge Graph\uff09\u201d\u7684\u6982\u5ff5\uff0c\u5176\u521d\u8877\u662f\u4e3a\u4e86\u4f18\u5316\u641c\u7d22\u5f15\u64ce\u8fd4\u56de\u7684\u7ed3\u679c\uff0c\u589e\u5f3a\u7528\u6237\u641c\u7d22\u8d28\u91cf\u53ca\u4f53\u9a8c\u3002\u672c\u8d28\u4e0a\uff0c\u77e5\u8bc6\u56fe\u8c31\u662f\u63ed\u793a\u5b9e\u4f53\u4e4b\u95f4\u5173\u7cfb\u7684\u8bed\u4e49\u7f51\u7edc\uff0c\u4ee5\u7b26\u53f7\u5f62\u5f0f\u63cf\u8ff0\u7269\u7406\u4e16\u754c\u4e2d\u7684\u6982\u5ff5\u4ee5\u53ca\u76f8\u4e92\u5173\u7cfb\uff0c\u5b9e\u73b0\u51c6\u786e\u800c\u5feb\u901f\u627e\u5230\u76ee\u6807\u4fe1\u606f\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u6784\u5efa\u6750\u6599\u77e5\u8bc6\u56fe\u8c31<\/strong><\/p>\n<p>\u4eceGoogle \u201c\u77e5\u8bc6\u56fe\u8c31\u201d\u542f\u53d1\uff0c\u6211\u4eec\u6784\u5efa\u6750\u6599\u77e5\u8bc6\u56fe\u8c31\uff0c\u628a\u4e0a\u9762\u63d0\u5230\u7684\u591a\u6a21\u6001\u4fe1\u606f\u8fdb\u884c\u4fe1\u606f\u62bd\u53d6\u51fa\u6765\u3002\u4e3a\u4e86\u4fe1\u606f\u7684\u878d\u5408\uff0c\u6211\u4eec\u8981\u5bf9\u4fe1\u606f\u8fdb\u884c\u7ed3\u6784\u5316\u5904\u7406\uff0c\u4ece\u800c\u7814\u7a76\u8fd9\u4e9b\u4fe1\u606f\u4e4b\u95f4\u7684\u5173\u8054\uff0c\u8fd0\u7528\u548c\u53d1\u5c55\u6570\u5b66\u65b9\u6cd5\u770b\u5982\u4f55\u5f62\u6210\u63a8\u7406\uff0c\u6784\u5efa\u4e00\u4e2a\u6750\u6599\u77e5\u8bc6\u56fe\u8c31\uff0c\u5f62\u6210\u5bf9\u672a\u6765\u6750\u6599\u7684\u63a8\u7406\u548c\u9884\u6d4b\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u6750\u6599\u77e5\u8bc6\u56fe\u8c31\u6574\u4f53\u6784\u5efa\u601d\u8def<\/strong><\/p>\n<p>\u603b\u7684\u601d\u8def\u662f\u6750\u6599\u5b66\u672f\u6587\u732e\u4fe1\u606f\u63d0\u53d6\u9700\u8981\u5bf9<strong>\u6587\u672c\u5f62\u5f0f<\/strong>\u7684\u6750\u6599\u79d1\u5b66\u4fe1\u606f\u8fdb\u884c<strong>\u7ed3\u6784\u5316\u8868\u793a<\/strong>\uff0c\u7ed3\u5408<strong>\u77e5\u8bc6\u5173\u8054\u3001\u878d\u5408\u3001\u63a8\u7406<\/strong>\u7b49\u65b9\u6cd5\u6784\u5efa\u6750\u6599\u77e5\u8bc6\u56fe\u8c31\uff0c\u53ef\u4f7f\u7814\u7a76\u4eba\u5458\u51c6\u786e\u800c\u53c8\u9ad8\u6548\u5730\u83b7\u53d6\u4fe1\u606f\uff0c\u5bf9\u8fc7\u5f80\u7814\u7a76\u8fdb\u884c<strong>\u8109\u7edc\u68b3\u7406<\/strong>\uff0c\u5bf9\u6709\u6f5c\u529b\u7684\u6750\u6599\u8fdb\u884c<strong>\u63a8\u7406\u9884\u6d4b<\/strong>\u3002\u8981\u89e3\u51b3\u7684\u4e00\u4e2a\u5173\u952e\u95ee\u9898\u662f\u8981\u51c6\u786e\u5730\u8bc6\u522b\u6587\u732e\u4e2d\u7684\u201c\u4e3b\u4f53\uff08\u4f5c\u8005\uff09+ \u5ba2\u4f53\uff08\u6750\u6599\uff09\u201d\u3002\u00a0\u6750\u6599\u662f\u7814\u7a76\u5bf9\u8c61\uff0c\u662f\u5ba2\u4f53\u3002\u662f\u8c01\u6765\u7814\u7a76\uff1f\u7814\u7a76\u8005\u662f\u4e3b\u4f53\uff0c\u4e00\u7bc7\u6587\u7ae0\u662f\u5305\u542b\u4e3b\u4f53\u548c\u5ba2\u4f53\uff0c\u53ca\u5176\u76f8\u4e92\u5173\u7cfb\uff0c\u5230\u5e95\u662f\u201c\u8c01\uff08\u4e3b\u4f53\uff09\u201d\u5728\u5f00\u5c55\u7814\u7a76\u8981\u641e\u6b63\u786e\uff0c\u4e3e\u4e2a\u4f8b\u5b50\uff0c\u5317\u5927\u6709\u4e00\u4e2a\u6f58\u950b\uff0c\u6e05\u534e\u6709\u4e00\u4e2a\u6f58\u5cf0\uff0c\u82f1\u6587\u90fd\u662fFeng\u7136\u540e\u540e\u9762\u662fPan\uff0c\u6216\u8005\u662f\u7f29\u5199F.Pan\uff0c\u8fd9\u4e24\u4e2a\u662f\u5426\u662f\u540c\u4e00\u4e2a\u4eba\uff08\u6e05\u534e\u7684F.Pan\u8c03\u5230\u5317\u5927\u6765\u4e86\uff1f\uff09\u8fd8\u662f\u4e8c\u4e2a\u4e0d\u540c\u7684\u4eba\uff1f<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u6750\u6599\u79d1\u5b66\u6587\u732e\u4f5c\u8005\u6d88\u6b67\u2014\u6b67\u4e49\u5316\u73b0\u8c61<\/strong><\/p>\n<p>\u79d1\u5b66\u6587\u732e\u91cc\u9762\u8981\u8bc6\u522b\u6587\u7ae0\u7684\u4f5c\u8005\u662f\u8c01\uff0c\u51e0\u7bc7\u6587\u7ae0\u4f5c\u8005\u662f\u4e0d\u662f\u540c\u4e00\u4e2a\u4eba\uff0c\u8fd9\u4e0e\u4e0a\u9762\u8c08\u7684\u4e24\u4e2a\u6676\u4f53\u7ed3\u6784\u662f\u5426\u540c\u6784\u7c7b\u4f3c\uff0c\u662f\u6784\u5efa\u6750\u6599\u77e5\u8bc6\u56fe\u8c31\u5927\u6570\u636e\u8981\u89e3\u51b3\u7684\u7b2c\u4e00\u4e2a\u95ee\u9898\uff0c\u79f0\u4e4b\u4e3a\u201c\u4f5c\u8005\u6d88\u6b67\u201d\u3002\u673a\u5668\u5b66\u4e60\u4e0e\u4eba\u7684\u5b66\u4e60\u76f8\u4f3c\uff0c\u201c\u5411\u597d\u4eba\u4f1a\u5b66\u597d\u3001\u5411\u574f\u4eba\u4f1a\u5b66\u574f\u201d\u3002\u673a\u5668\u5b66\u4e60\u4e5f\u7c7b\u4f3c\uff0c\u5b66\u201c\u574f\u201d\u7684\u6570\u636e\uff08\u9519\u8bef\u7684\u4fe1\u606f\uff09\u4e0d\u4f1a\u5f97\u51fa\u6b63\u786e\u7684\u5224\u65ad\uff0c\u5b66\u201c\u597d\u201d\u7684\u6570\u636e\uff08\u6b63\u786e\u6570\u636e\u548c\u4fe1\u606f\uff09\u7684\u5c31\u53ef\u80fd\u5f97\u5230\u6b63\u786e\u5224\u65ad\u548c\u7ed3\u8bba\u3002\u5982\u679c\u6570\u636e\u7684\u9519\u8bef\u591a\uff0c\u5f97\u51fa\u9519\u8bef\u7684\u7ed3\u8bba\u53ef\u80fd\u6027\u9ad8\u3002\u907f\u514d\u4f5c\u8005\u4fe1\u606f\u641e\u9519\uff0c\u5148\u8981\u8fdb\u884c\u4f5c\u8005\u6d88\u6b67\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u6750\u6599\u79d1\u5b66\u6587\u732e\u4f5c\u8005\u6d88\u6b67\u2014<\/strong><strong>MatKG<\/strong><strong>\u6846\u67b6<\/strong><\/p>\n<p>\u57fa\u4e8e<strong>\u4f5c\u8005<\/strong>\u4ee5\u53ca<strong>\u6587\u672c<\/strong>\u4fe1\u606f\uff0c\u6211\u4eec\u7ed3\u5408<strong>\u673a\u5668\u5b66\u4e60<\/strong>\u548c<strong>\u5339\u914d\u4f9d\u8d56\u7b97\u6cd5<\/strong>\u5bf9\u6750\u6599\u77e5\u8bc6\u56fe\u8c31\u4e2d\u7684\u4e3b\u4f53\uff08\u4f5c\u8005\uff09\u8fdb\u884c<strong>\u9ad8\u7cbe\u5ea6\u6d88\u6b67<\/strong>\uff0c\u5e76\u5f15\u5165<strong>\u526a\u679d\u7b56\u7565<\/strong>\u4ee5\u89e3\u51b3\u5728\u9762\u5bf9\u5e9e\u5927\u4e14\u590d\u6742\u7684\u6570\u636e\u65f6\u67e5\u627e\u6548\u7387\u8f83\u4f4e\u7684\u95ee\u9898\uff0c\u5b9e\u73b0<strong>\u9ad8\u6548\u4fe1\u606f\u5339\u914d\u548c\u641c\u7d22<\/strong>\uff0c\u4ece\u800c\u6784\u5efa\u4e86<strong>MatKG<\/strong>\u7684\u6846\u67b6\u3002<\/p>\n<p>2019\u5e74\u8bfa\u8d1d\u5c14\u5956\u53d1\u7ed9\u9502\u7535\u6c60\u94b4\u9178\u9502\u548c\u78f7\u9178\u94c1\u9502\u7684\u53d1\u660e\u8005Goodenough\u5148\u751f\u7b49\u3002\u4f5c\u4e3a\u6750\u6599\u77e5\u8bc6\u56fe\u8c31\u7684\u7b2c\u4e00\u4e2a\u5e94\u7528\uff0c\u6211\u4eec\u53bb\u590d\u539f\u78f7\u9178\u94c1\u9502\u8fd9\u4e2a\u6750\u6599\u53d1\u73b0\u7684\u6574\u4e2a\u8fc7\u7a0b\uff0c\u8be0\u91ca\u201c\u524d\u4e16\u201d(\u7b2c\u4e00\u6b21\u88ab\u53d1\u73b0\uff0c\u5e76\u4e0d\u662f\u4f5c\u4e3a\u9502\u7535\u6c60\u6750\u6599\u7528)\u548c\u201c\u4eca\u751f\u201d\uff08\u4f5c\u4e3a\u9502\u7535\u6c60\u6b63\u6781\u6750\u6599\u88ab\u5e7f\u6cdb\u5e94\u7528\uff09\u3002\u5728\u6240\u6709\u7684\u8fc7\u7a0b\u5f53\u4e2d\uff0c\u8c01\u505a\u4e86\u91cd\u8981\u7684Mile-stone\u7684\u8d21\u732e\u3002\u770b\u5230\u4ece\u53d1\u73b0\u4f5c\u4e3a\u9502\u7535\u6c60\u6b63\u6781\u6750\u6599\u5230\u6700\u8fd1\u7684\u5e7f\u6cdb\u88ab\u5e94\u7528\u7ecf\u5386\u4e8615\u5e74\u7684\u65f6\u95f4\u3002\u8fd9\u4e4b\u524d\u4e0d\u662f\u4f5c\u4e3a\u9502\u7535\u6c60\u6750\u6599\u7684\u57fa\u7840\u7814\u7a76\u8fd8\u8981\u518d\u8ffd\u6eaf\u524d10\u5e74\uff0c\u603b\u5171\u7ea625\u5e74\u65f6\u95f4\u3002\u4ece\u4e2d\u6211\u4eec\u7406\u89e3\u5f53\u4e00\u4e2a\u6750\u6599\u4ece\u88ab\u53d1\u73b0\/\u53d1\u660e\u5230\u88ab\u5e94\u7528\u6709\u7740\u6f2b\u957f\u8def\u5f84\uff0c\u6750\u6599\u77e5\u8bc6\u56fe\u8c31\u53ef\u4ee5\u8ba9\u6211\u4eec\u5bf9\u4e8e\u65b0\u6750\u6599\u7684\u6574\u4e2a\u79d1\u5b66\u53d1\u73b0\u8fc7\u7a0b\u8fdb\u884c\u590d\u76d8\uff0c\u4e3a\u4e86\u63a2\u7d22\u65b0\u6750\u6599\u63d0\u4f9b\u501f\u9274\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u6750\u6599\u5173\u8054\u4e0e\u63a8\u7406\u6846\u67b6<\/strong><strong>DATWEM\u2014\u6a21\u578b\u7ed3\u6784\u4e0e\u8868\u73b0<\/strong><\/p>\n<p>\u901a\u8fc7\u6750\u6599\u77e5\u8bc6\u56fe\u8c31\u80fd\u4e0d\u80fd\u8ba9\u673a\u5668\u628a\u6240\u6709\u9502\u7535\u6c60\u6b63\u6781\u6750\u6599\u7684\u6587\u7ae0\u8bfb\u4e00\u904d\uff0c\u544a\u8bc9\u6211\u4eec\u4e0b\u4e00\u4ee3\u6b63\u6781\u9ad8\u6027\u80fd\u7684\u6750\u6599\u662f\u4ec0\u4e48\uff1f\u8fd9\u662f\u6211\u4eec\u7684\u521d\u8877\uff0c\u76f8\u5f53\u4e8e\u5f00\u59cb\u641e\u79d1\u5b66\u7814\u7a76\u8981\u53bb\u505a\u8c03\u7814\uff0c\u5728\u505a\u5b9e\u9a8c\u4e4b\u524d\uff0c\u8981\u95ee\u81ea\u5df1\u4e3a\u4ec0\u4e48\u8981\u8fd9\u6837\u505a\u5b9e\u9a8c\uff0c\u5b9e\u9a8c\u505a\u4e0b\u53bb\u53ef\u80fd\u80fd\u53d1\u73b0\u4ec0\u4e48\u65b0\u6750\u6599\uff0c\u8fd9\u662f\u201c\u79d1\u5b66\u7814\u7a76\u7684\u6ce8\u610f\u529b\u201d\u3002\u8c03\u7814\u5b8c\u4f1a\u5f62\u6210\u6ce8\u610f\u529b\uff0c\u5f62\u6210\u60f3\u6cd5\u548c\u63a8\u7406\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u6750\u6599\u5173\u8054\u4e0e\u63a8\u7406\u6846\u67b6<\/strong><strong>DATWEM\u2014\u2014\u5173\u8054\u6548\u679c\u7684\u663e\u8457\u63d0\u5347<\/strong><\/p>\n<p>\u6211\u4eec\u57fa\u4e8e\u6750\u6599\u77e5\u8bc6\u56fe\u8c31\u53cc\u5c42\u6ce8\u610f\u529b\u673a\u5236\u7684\u591a\u6e90\u6570\u636e\u878d\u5408\uff0c\u878d\u5165\u9886\u57df\u5148\u9a8c\u77e5\u8bc6\uff0c\u663e\u8457\u589e\u5f3a\u53ef\u89e3\u91ca\u6027\uff0c\u6b63\u6781\u6750\u6599\u63a8\u5bfc\u4efb\u52a1\u7684\u6548\u679c\u5168\u9762\u63d0\u5347\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u6750\u6599\u5173\u8054\u4e0e\u63a8\u7406\u6846\u67b6<\/strong><strong>DATWEM<\/strong><strong>\u2014\u2014\u63a8\u7406\u529f\u80fd<\/strong><\/p>\n<p>DATWEM\u6846\u67b6\u53ef\u660e\u663e\u6539\u5584\u6b63\u6781\u6750\u6599\u7684\u5173\u8054\u6548\u679c\uff0c\u7ea0\u6b63\u8fdd\u53cd\u6750\u6599\u79d1\u5b66\u77e5\u8bc6\u7684\u5173\u8054\u6848\u4f8b\u3002\u901a\u8fc7\u81ea\u7136\u8bed\u8a00\u5904\u7406\u6280\u672f\u6784\u5efa\u6570\u636e\u9a71\u52a8\u7684\u6750\u6599\u4fe1\u606f\u63a2\u7d22\u7684\u65b0\u8303\u5f0f\uff0c\u4e3a\u65b0\u6750\u6599\u7684\u53d1\u73b0\u4e0e\u8bbe\u8ba1\u63d0\u4f9b\u65b0\u89c1\u89e3\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u6587\u732e\u5927\u6570\u636e@\u6784\u5efa\u6750\u6599\u77e5\u8bc6\u56fe\u8c31 \u9884\u6d4b<\/strong><strong>\u9ad8\u6027\u80fd<\/strong><strong>\u9502\u7535\u6c60\u6b63\u6781\u6750\u6599<\/strong><\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u57fa\u4e8e\u6750\u6599\u77e5\u8bc6\u56fe\u8c31\u9884\u6d4b<\/strong><strong>Li<sub>2<\/sub>TiMn<sub>3<\/sub>O<sub>8<\/sub><\/strong><strong>\u4f5c\u4e3a\u6f5c\u5728\u7684\u9ad8\u6027\u80fd<\/strong><strong>\u9502\u7535\u6c60\u6b63\u6781\u6750\u6599<\/strong><\/p>\n<p>\u7528\u6750\u6599\u77e5\u8bc6\u56fe\u8c31\u76f8\u4f3c\u7684\u9502\u7535\u6c60\u7535\u6781\u6750\u6599\u78f7\u9178\u94c1\u9502\uff0c\u94b4\u9178\u9502\uff0c\u5bcc\u9502\u9530\u6c27\uff0c\u5c16\u6676\u77f3\u9530\u9178\u9502\u7b49\u6784\u5efa\u4e00\u79cd\u5411\u91cf\u548c\u5b83\u4eec\u4e4b\u95f4\u7684\u76f8\u4f3c\u5ea6\u3002\u6570\u5b66\u5f88\u5947\u5999\uff0c\u76f8\u4f3c\u6027\u7684\u6bd4\u8f83\u53ef\u4ee5\u591a\u7ef4\u5ea6\u3002\u6211\u4eec\u53ef\u4ee5\u4e0d\u7528\u6709\u7ebf\u6027\u7684\u76f8\u4f3c\u6027\u6bd4\u8f83\uff0c\u800c\u662f\u7528\u975e\u7ebf\u6027\u7684\u4f59\u5f26\u76f8\u4f3c\u5ea6\uff0c\u4e0e\u7edf\u8ba1\u6982\u7387\u76f8\u5173\uff0c\u6765\u9884\u6d4b\u4e0b\u4e00\u4ee3\u3002\u53cc\u5c42\u6ce8\u610f\u529b\u591a\u5143\u878d\u5408\uff0c\u53bb\u63a8\u7406\u8ddf\u94b4\u9178\u9502\u76f8\u4f3c\u7684\u662f\u4ec0\u4e48\uff0c\u7136\u540e\u8ddf\u5176\u5b83\u6b63\u6781\u6750\u6599\u4ec0\u4e48\u76f8\u4f3c\uff0c\u628a\u5404\u81ea\u7684\u4f18\u70b9\u770b\u80fd\u4e0d\u80fd\u7ed3\u5408\u8d77\u6765\u3002\u8fd9\u6837\u9884\u6d4b\u5230\u4e86<strong>Li<sub>2<\/sub>TiMn<sub>3<\/sub>O<sub>8<\/sub><\/strong>\u6750\u6599\uff0c\u8fd9\u4e2a\u6750\u6599\u53ef\u80fd\u6709\u6f5c\u5728\u7684\u5e94\u7528\uff0c\u8fd8\u9700\u8981\u7528\u5b9e\u9a8c\u53bb\u9a8c\u8bc1\u3002<\/p>\n<p>\u6280\u672f\u7ec6\u8282\uff1a\u6a21\u578b\u4f7f\u7528\u7684\u673a\u5668\u5b66\u4e60\u6846\u67b6\u4e3aBiLSTM\uff0cLSTM\u5373\u4e3a\u957f\u77ed\u671f\u8bb0\u5fc6\uff08Long short-term memory, LSTM\uff09\u662f\u4e00\u79cd\u7279\u6b8a\u7684RNN\uff0c\u4e3b\u8981\u662f\u4e3a\u4e86\u89e3\u51b3\u957f\u5e8f\u5217\u8bad\u7ec3\u8fc7\u7a0b\u4e2d\u7684\u68af\u5ea6\u6d88\u5931\u548c\u68af\u5ea6\u7206\u70b8\u95ee\u9898\u3002\u7b80\u5355\u6765\u8bf4\uff0c\u5c31\u662f\u76f8\u6bd4\u666e\u901a\u7684RNN\uff0cLSTM\u80fd\u591f\u5728\u66f4\u957f\u7684\u5e8f\u5217\u4e2d\u6709\u66f4\u597d\u7684\u8868\u73b0\u3002\u524d\u5411\u7684LSTM\u4e0e\u540e\u5411\u7684LSTM\u7ed3\u5408\u6210BiLSTM\u3002\u4f20\u7edfLSTM\u65e0\u6cd5\u7f16\u7801\u4ece\u540e\u5230\u524d\u7684\u4fe1\u606f\uff0c\u4e3e\u4e00\u4e2a\u4f8b\u5b50\uff0c\u201c\u8fd9\u4e2a\u9910\u5385\u810f\u5f97\u4e0d\u884c\uff0c\u6ca1\u6709\u9694\u58c1\u597d\u201d\uff0c\u8fd9\u91cc\u7684\u201c\u4e0d\u884c\u201d\u662f\u5bf9\u201c\u810f\u201d\u7684\u7a0b\u5ea6\u7684\u4e00\u79cd\u4fee\u9970\uff0c\u901a\u8fc7BiLSTM\u53ef\u4ee5\u66f4\u597d\u7684\u6355\u6349\u53cc\u5411\u7684\u8bed\u4e49\u4f9d\u8d56\u3002\u5de6\u4e0a\u89d2\u56fe\uff1a\u5728BiLSTM\u6a21\u578b\u4e2d\u878d\u5165\u53cc\u91cd\u6ce8\u610f\u529b\u673a\u5236\uff0c\u878d\u5165\u9886\u57df\u5148\u9a8c\u77e5\u8bc6\uff08\u6b63\u6781\u6750\u6599\u5173\u952e\u8bcd\uff09\uff0c\u663e\u8457\u589e\u5f3a\u53ef\u89e3\u91ca\u6027\u3002\u5de6\u4e0b\u89d2\u56fe\uff1aDATWEM\u6846\u67b6\u53ef\u660e\u663e\u6539\u5584\u6b63\u6781\u6750\u6599\u7684\u5173\u8054\u6548\u679c\uff0c\u7ea0\u6b63\u8fdd\u53cd\u6750\u6599\u79d1\u5b66\u77e5\u8bc6\u7684\u5173\u8054\u6848\u4f8b\u3002\u53f3\u4e0b\u89d2\u56fe\uff1a\u57fa\u4e8e\u8bcd\u5411\u91cf\u964d\u7ef4\u540e\u7684\u65e0\u76d1\u7763\u5b66\u4e60\u805a\u7c7b\u6b63\u6781\u6750\u6599\u56fe\u8c31\u3002\u8f93\u5165\u5d4c\u5165\u91cf\u4e3a62\u4e07\u4e2a\uff0c\u4fdd\u7559\u4e86\u56db\u79cd\u5178\u578b\u6b63\u6781\u6750\u6599\u7684\u5927\u7c07\uff0c\u4ee5\u53ef\u89c6\u5316\u4e0d\u540c\u6750\u6599\u4e4b\u95f4\u7684\u8bed\u4e49\u76f8\u4f3c\u5ea6\u3002\u53f3\u4e0a\u89d2\u56fe\uff1aLi<sub>2<\/sub>TiMn<sub>3<\/sub>O<sub>8<\/sub>\u4e0eLiCoO<sub>2<\/sub>\u76f8\u4f3c\u7279\u5f81\u7684\u81ea\u52a8\u8bc6\u522b\u3002\u901a\u8fc7\u6316\u6398\u4e0d\u540c\u6750\u6599\u5bf9\u5e94\u8282\u70b9\u4e4b\u95f4\u7684\u76f4\u63a5\u6216\u95f4\u63a5\u8def\u5f84\uff0c\u53ef\u4ee5\u4ece\u79d1\u5b66\u6587\u732e\u8bed\u6599\u5e93\u4e2d\u81ea\u52a8\u8bc6\u522b\u51fa\u4e0e\u5178\u578b\u9634\u6781\u76f8\u4f3c\u5ea6\u9ad8\u7684\u6f5c\u5728\u6b63\u6781\u6750\u6599\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u5982\u4f55\u7cfb\u7edf\u63d0\u5347<\/strong><strong>\u65b0\u80fd\u6e90\uff08\u9502\u7535\u6c60\uff09\u6750\u6599<\/strong><strong>\u6027\u80fd\uff1f<\/strong><\/p>\n<p>\u4e0b\u9762\u4ecb\u7ecd\u5982\u4f55\u628a\u6750\u6599\u57fa\u56e0\u4e0e\u65b0\u80fd\u6e90\/\u9502\u7535\u6c60\u6750\u6599\u8981\u89e3\u51b3\u7684\u79d1\u5b66\u95ee\u9898\u5173\u8054\u8d77\u6765\u7814\u7a76\u3002\u9502\u7535\u6c60\u6784\u67b6\u5305\u542b\u4e24\u4e2a\u7535\u6781\uff0c\u5b9e\u73b0\u5916\u7535\u8def\u7684\u7535\u5b50\u6d41\u52a8\u548c\u7535\u6c60\u5185\u90e8\u7684\u9502\u79bb\u5b50\u7a7f\u68ad\uff0c\u6b63\u6781\u4e0e\u8d1f\u6781\u5b83\u4eec\u4e4b\u95f4\u6709\u7535\u52bf\u5dee\uff0c\u5145\u7535\u65f6\u5916\u7535\u8def\u63a8\u52a8\u7535\u5b50\u505a\u529f\u5e76\u628a\u9502\u79bb\u5b50\u4ece\u6b63\u6781\u63a8\u5230\u8d1f\u6781\uff0c\u653e\u7535\u65f6\u7535\u6c60\u5bf9\u5916\u7535\u8def\u505a\u529f\uff0c\u9502\u79bb\u5b50\u4ece\u8d1f\u6781\u88ab\u63a8\u5230\u6b63\u6781\u3002\u7535\u6c60\u6027\u80fd\u6700\u91cd\u8981\u5305\u62ec\u4e09\u4e2a\u65b9\u9762\u3002\u7b2c\u4e00\u4e2a\u65b9\u9762\u662f\u50a8\u80fd\u5bc6\u5ea6\uff0c\u5bf9\u5e94\u7684\u662f\u65e5\u5e38\u7684\u624b\u673a\u80fd\u7528\u591a\u4e45\uff0c\u50a8\u80fd\u5bc6\u5ea6\u662f\u9502\u7535\u6c60\u6750\u6599\u5b58\u50a8\u9502\u79bb\u5b50\u7684\u5bb9\u91cf\uff08\u80fd\u5b58\u591a\u5c11\u4e2a\u9502\u79bb\u5b50\uff09\u548c\u5bf9\u5e94\u7684\u7535\u52bf\u5dee\u76f8\u4e58\u7684\u7ed3\u679c\u3002\u9502\u79bb\u5b50\u5b58\u591a\u4e86\u4f1a\u4e92\u76f8\u9759\u7535\u6392\u65a5\u5f15\u53d1\u7ed3\u6784\u7684\u7a33\u5b9a\u6027\u4e0b\u964d\u548c\u4ea7\u751f\u76f8\u53d8\u3002\u7b2c\u4e8c\u65b9\u9762\u662f\u529f\u7387\u5bc6\u5ea6\uff0c\u5bf9\u5e94\u7684\u662f\u5145\u653e\u7535\u901f\u5ea6\uff0c\u7ecf\u5e38\u542c\u5230\u9502\u7535\u6c60\u5145\u7535\u65f6\u95f4\u592a\u957f\u592a\u6162\u4e86\uff0c\u73b0\u5728\u5f88\u591a\u65b0\u7684\u7535\u6c60\u8bf4\u53ef\u4ee5\u5feb\u5145\uff0c\u7535\u52a8\u8f66\u548c\u65e0\u4eba\u673a\u52a0\u901f\u8981\u6c42\u5feb\u901f\u653e\u7535\uff0c\u5bf9\u5e94\u7684\u662f\u9502\u79bb\u5b50\u5728\u7535\u6781\u6750\u6599\u4f53\u76f8\u4e2d\u3001\u7535\u6781\u754c\u9762\u5904\u548c\u5728\u7535\u89e3\u6db2\u4e2d\u4ece\u6b63\u6781\u5230\u8d1f\u6781\u6216\u53cd\u5411\u7684\u8fd0\u52a8\u901f\u5ea6\u6709\u591a\u5feb\u3002\u7b2c\u4e09\u65b9\u9762\u7535\u6781\u6750\u6599\u4e0e\u754c\u9762\u7684\u7ed3\u6784\u7a33\u5b9a\u6027\uff0c\u5bf9\u5e94\u7684\u662f\u4f7f\u7528\u5faa\u73af\u6027\u80fd\u4e0e\u65f6\u95f4\u5bff\u547d\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u7814\u7a76\u601d\u8def\uff1a\u7ed3\u6784\u5316\u5b66\u4e0e\u6750\u6599\u57fa\u56e0\u00a0<\/strong><strong>\u4ece\u539f\u5b50\u5c3a\u5ea6\u63ed\u793a\u65b0\u80fd\u6e90\u6750\u6599\u7ed3\u6784\u4e0e\u6027\u80fd\u7684\u76f8\u5173\u6027<\/strong><\/p>\n<p>\u5173\u952e\u95ee\u9898\uff1b<strong>\u8f6c\u5316\u6548\u7387\u3001\u50a8\u80fd\u5bc6\u5ea6 \u3001\u529f\u7387\u5bc6\u5ea6\u3001\u7a33\u5b9a\u6027\u4e0e\u5b89\u5168\u6027<\/strong><\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u7ed3\u6784\u5316\u5b66\u65b9\u6cd5\uff1a1. \u521b\u5efa\u57fa\u4e8e\u56fe\u8bba\u7ed3\u6784\u5316\u5b66\/\u6750\u6599\u57fa\u56e0\u65b9\u6cd5\u00a0<\/strong><strong>; 2.<\/strong><strong>\u00a0<\/strong><strong>\u9502\u7535\u6c60\u6750\u6599\u57fa\u56e0 \u4e0ed\u7535\u5b50\u7ed3\u6784\u5316\u5b66;<\/strong><strong>\u00a0<\/strong><strong>3. \u6784\u5efa\u754c\u9762\u7ed3\u6784\/\u6750\u6599\u57fa\u56e0\u4e0e\u7535\u5316\u5b66\u7814\u7a76\u4f53\u7cfb<\/strong><\/p>\n<p>\u8ba9\u6211\u4eec\u91cd\u65b0\u601d\u8003\u4e00\u4e0b\u4ec0\u4e48\u53eb\u6750\u6599\uff0c\u6750\u6599\u662f\u4e3a\u4e86\u7528\u7684\uff0c\u7528\u5b83\u7684\u6027\u80fd\u3002\u8981\u8ba9\u6676\u4f53\u6750\u6599\u8868\u73b0\u51fa\u4f18\u5f02\u7684\u6027\u80fd\u7684\u5fc5\u8981\u548c\u5145\u5206\u6761\u4ef6\u5206\u522b\u662f\u5176\u4f53\u76f8\u7ed3\u6784\u548c\u754c\u9762\u7ed3\u6784\u3002\u6211\u4eec\u751f\u547d\u7ec6\u80de\u8981\u8868\u73b0\u51fa\u529f\u80fd\uff0c\u4e00\u5b9a\u8981\u7ecf\u8fc7\u5b83\u7684\u7ec6\u80de\u819c\u6765\u5b9e\u73b0\u3002\u4e00\u4e2a\u6750\u6599\u6027\u80fd\u8981\u8868\u73b0\u51fa\u6765\uff0c\u4e5f\u4e00\u5b9a\u8981\u901a\u8fc7\u5176\u754c\u9762\u6765\u5b9e\u73b0\u3002\u6750\u6599\u754c\u9762\u4e0e\u4f53\u76f8\u662f\u6709\u5de8\u5927\u5dee\u522b\u7684\uff1a\u7b2c\u4e00\uff0c\u4ece\u5bf9\u79f0\u6027\u7ef4\u5ea6\u4e0a\u9762\u5c31\u6709\u5dee\u522b\uff0c\u6676\u4f53\u5177\u6709\u4e09\u7ef4\u5bf9\u79f0\u6027\uff0c\u5230\u4e86\u8fb9\u754c\u8fd9\u79cd\u5bf9\u79f0\u6027\u4e0d\u5b58\u5728\uff0c\u7ed3\u6784\u57fa\u5143\u7684\u914d\u4f4d\u591a\u9762\u4f53\u5bf9\u79f0\u6027\u4e5f\u7834\u7f3a\u4e86\uff0c\u6309\u7167\u73af\u5883\u63d0\u4f9b\u7684\u6761\u4ef6\u8981\u91cd\u65b0\u914d\u4f4d\u548c\u91cd\u6784\u754c\u9762\u3002\u7b2c\u4e8c\u754c\u9762\u91cd\u6784\u8fd8\u6709\u53d7\u5230\u73af\u5883\u548c\u4f7f\u7528\u6761\u4ef6\u7684\u5f71\u54cd\uff0c\u7535\u6c60\u8981\u5f62\u6210\u7a33\u5b9a\u7684\u754c\u9762\u7ed3\u6784\uff0c\u662f\u5f88\u96be\u7684\u4e00\u4e2a\u95ee\u9898\uff0c\u4e5f\u53ef\u80fd\u7531\u754c\u9762\u5f00\u59cb\u7ed3\u6784\u4e0d\u65ad\u5730\u88ab\u7834\u574f\uff0c\u4ece\u800c\u5f71\u54cd\u6750\u6599\u4f53\u76f8\u7684\u7ed3\u6784\u7a33\u5b9a\u6027\u3002\u7b2c\u4e09\u65b9\u9762\u9502\u79bb\u5b50\u501f\u52a9\u7535\u89e3\u8d28\u5f53\u505a\u6865\u6881\u8ba9\u9502\u79bb\u5b50\u80fd\u591f\u5728\u6b63\u6781\u4e0e\u8d1f\u6781\u4e4b\u95f4\u4f20\u8f93\uff0c\u73b0\u5728\u4f7f\u7528\u7684\u9502\u7535\u6c60\u7535\u89e3\u8d28\u90fd\u662f\u6db2\u4f53\uff0c\u6db2\u4f53\u7684\u7279\u70b9\u662f\u6d41\u52a8\u6027\u548c\u201c\u6da6\u6e7f\u6027\u201d\u80fd\u591f\u8ba9\u9502\u79bb\u5b50\u5728\u56fa\u6001\u9897\u7c92\u754c\u9762\u7684\u7a7a\u95f4\u8ddd\u79bb\u6700\u5c0f\uff08\u53ef\u4ee5\u8fbe\u5230\u5316\u5b66\u952e\u7684\u5c3a\u5ea6\uff09\u548c\u4f20\u8f93\u9762\u79ef\u6700\u5927\u5316\uff08\u8986\u76d6\u6574\u4e2a\u9897\u7c92\uff09\u4ece\u800c\u963b\u6297\u53ef\u4ee5\u8fbe\u5230\u6700\u5c0f\u3002\u56fa\u6001\u7535\u6c60\u7684\u7535\u89e3\u8d28\u662f\u56fa\u4f53\uff0c\u4f1a\u6d89\u53ca\u5230\u4e24\u4e2a\u56fa\u4f53\u4e4b\u95f4\u7684\u63a5\u89e6\u95ee\u9898\uff0c\u4e0e\u6db2\u4f53\u4e0d\u540c\u786c\u7684\u56fa\u4f53\u9897\u7c92\u63a5\u89e6\u7684\u7a7a\u95f4\u8ddd\u79bb\u5927\uff08\u8fbe\u4e0d\u5230\u5316\u5b66\u952e\u7684\u8ddd\u79bb\u5c3a\u5ea6\uff09\u548c\u9762\u79ef\u5c0f\uff08\u53ea\u6709\u56fa\u6001\u9897\u7c92\u63a5\u89e6\u7684\u6324\u538b\u5e94\u53d8\u627f\u53d7\u7684\u9762\u79ef\uff0c\u5c5e\u4e8e\u70b9\u63a5\u89e6\uff09\uff0c\u56e0\u6b64\u7535\u963b\u4f1a\u5f88\u5927\uff0c\u5f15\u53d1\u526f\u53cd\u5e94\u3001\u6d88\u8017\u80fd\u91cf\uff0c\u4ee5\u53ca\u56e0\u4e3a\u963b\u6297\u592a\u5927\u4f7f\u5f97\u7535\u6781\u9897\u7c92\u611f\u53d7\u7684\u6709\u6548\u7535\u538b\u4f1a\u4e0b\u964d\u3002\u6240\u4ee5\u56fa\u6001\u7535\u6c60\u8981\u89e3\u51b3\u6700\u5927\u7684\u95ee\u9898\u5c31\u662f\u63a5\u89e6\u963b\u6297\u3002<\/p>\n<p>\u73b0\u5728\u9502\u7535\u6c60\u8d1f\u6781\u662f\u4ee5\u77f3\u58a8\u4e3a\u4e3b\uff0c\u4e3a\u4ec0\u4e48\u4e0d\u7528\u9502\u91d1\u5c5e\uff08\u9502\u91d1\u5c5e\u7684\u5bb9\u91cf\u662f\u77f3\u58a8\u7684\u5341\u591a\u500d\uff09\uff1f\u5982\u679c\u8981\u7528\u7684\u8bdd\u9700\u8981\u89e3\u51b3\u54ea\u4e9b\u5173\u952e\u79d1\u5b66\u95ee\u9898\uff1f\u9502\u7535\u6c60\u9886\u57df\u83b7\u8bfa\u8d1d\u5c14\u5956\u521b\u65b0\u672c\u8d28\u662f\u5f00\u521b\u4e86\u57fa\u4e8e\u8131\u5d4c\u673a\u5236\u9502\u7535\u6c60\u53ca\u7535\u6781\u6750\u6599\uff0c\u6b63\u6781\u76f8\u5f53\u4e8e\u4e00\u4e2a\u201c\u65c5\u9986C\u201d\uff0c\u8d1f\u6781\u662f\u201c\u65c5\u9986A\u201d\uff0c\u6b63\u6781\u548c\u8d1f\u6781\u90fd\u4e3a\u9502\u79bb\u5b50\u63d0\u4f9b\u8fdb\u51fa\u7684\u5b58\u50a8\u201c\u65c5\u9986\u623f\u95f4\u201d\uff0c\u5145\u7535\u65f6\u9502\u79bb\u5b50\u4ece\u6b63\u6781\u201c\u65c5\u9986C\u201d\u81ea\u5df1\u201c\u623f\u95f4\u201d\u51fa\u6765\u5230\u8d1f\u6781\u662f\u201c\u65c5\u9986A\u201d \u81ea\u5df1\u7684\u201c\u623f\u95f4\u201d\uff0c\u653e\u7535\u9502\u79bb\u5b50\u53c8\u4ece\u8d1f\u6781\u56de\u5230\u6b63\u6781\uff0c\u662f\u5b9a\u57df\u7684\u53ef\u9006\u7684\u9502\u79bb\u5b50\u8fd0\u52a8\uff0c\u5f88\u5c11\u4f1a\u4ea7\u751f\u989d\u5916\u4e0d\u53ef\u9006\u548c\u4e0d\u53ef\u63a7\u53cd\u5e94\uff0c\u4f53\u79ef\u53d8\u5316\u5c0f\u3002\u53ef\u9006\u6027\uff08\u8fd1\u4f3c\u53ef\u9006\uff09\u662f\u9502\u7535\u6c60\u957f\u65f6\u95f4\u5faa\u73af\u4f7f\u7528\u7684\u7269\u7406\u57fa\u7840\u3002\u00a0\u9502\u91d1\u5c5e\u4f5c\u4e3a\u8d1f\u6781\u7684\u4f18\u70b9\u662f\u5bb9\u91cf\u9ad8\uff084400mAh\/g\uff09\uff0c\u4f46\u5145\u653e\u7535\u7684\u672c\u8d28\u662f\u4e0d\u540c\u7684\uff0c\u4f34\u968f\u7684\u662f\u9502\u91d1\u5c5e\u81ea\u7531\u751f\u957f(\u975e\u9650\u57df)\u6c89\u79ef\u548c\u6eb6\u89e3\uff0c\u5f15\u53d1\u9502\u679d\u6676\u7684\u751f\u957f\u548c\u4e00\u7cfb\u5217\u7684\u201c\u4e0d\u53ef\u9006\u526f\u53cd\u5e94\u201d\u3002<\/p>\n<p>\u603b\u7ed3\u4e00\u4e0b\uff0c\u9502\u7535\u6c60\u7684\u5173\u952e\u8981\u7d20\uff0c1.\u6b63\u8d1f\u6781\u6750\u6599\u80fd\u5b58\/\u653e\u591a\u5c11\u4e2a\u79bb\u5b50\uff0c\u7535\u538b\u591a\u9ad8\uff0c\u6784\u6210\u50a8\u80fd\u5bc6\u5ea6\uff1b2.\u9502\u79bb\u5b50\u5728\u6b63\u6781\u91cc\u9762\u4f20\u8f93\u51fa\u6765\uff0c\u4f20\u8f93\u5230\u754c\u9762\uff0c\u4ece\u754c\u9762\u53c8\u8981\u4f20\u8f93\u5230\u8d1f\u6781\uff0c\u8fd9\u4e2a\u901f\u5ea6\u6709\u591a\u5feb\uff0c\u79f0\u4e4b\u4e3a\u5145\u7535\u7684\u529f\u7387\u5bc6\u5ea6\uff0c\u53cd\u5411\u662f\u653e\u7535\u7684\u529f\u7387\u5bc6\u5ea6\u30023.\u5145\u653e\u7535\u53ca\u5728\u4e0d\u540c\u529f\u7387\u4e0b\u7684\u5145\u653e\u7535\u7684\u53ef\u9006\u6027\uff0c\u8fd9\u4e2a\u4e0e1\u548c2\u70b9\u5f80\u5f80\u662f\u77db\u76fe\u7684\u3002\u00a0\u7535\u6c60\u548c\u6750\u6599\u5982\u679c\u8bbe\u8ba1\u5f97\u4e0d\u597d\uff0c\u5bb9\u91cf\u592a\u9ad8\u548c\u5145\u653e\u7535\u592a\u5feb\uff08\u8fdc\u79bb\u5e73\u8861\u72b6\u6001\uff09\u4f1a\u5f15\u53d1\u76f8\u7ed3\u6784\u7684\u6f14\uff0c\u7ed3\u6784\u53ef\u80fd\u4ea7\u751f\u4e0d\u53ef\u9006\u7834\u574f\u3002\u6b64\u5916\uff0c\u754c\u9762\u4e0d\u7a33\u5b9a\uff0c\u4f1a\u6ce2\u53ca\u5230\u6676\u4f53\u7ed3\u6784\u7684\u76f8\u53d8\uff0c\u4e25\u91cd\u4f1a\u5f15\u53d1\u5b89\u5168\u6027\uff0c\u5145\u653e\u7535\u65f6\u7ed3\u6784\u7684\u7a33\u5b9a\u6027\u7834\u574f\u5bb9\u6613\u91ca\u653e\u51fa\u81ea\u7531\u57fa\uff0c\u81ea\u7531\u57fa\u4f1a\u70b9\u71c3\u6709\u673a\u7535\u89e3\u6db2\u548c\u76f8\u5173\u7684\u53ef\u71c3\u7269\u8d28\uff0c\u5f15\u53d1\u5b89\u5168\u6027\u95ee\u9898\u3002\u9502\u7535\u6c60\u662f\u7c7b\u4f3c\u751f\u547d\u7684\u590d\u6742\u7684\u5e76\u6709\u7ec4\u7ec7\u7684\u4f53\u7cfb\uff0c\u6709\u4e00\u7cfb\u5217\u4e92\u76f8\u5236\u7ea6\u8981\u7d20\uff0c\u8fd9\u5bfc\u81f4\u9502\u7535\u6c60\u5341\u51e0\u5e74\u6765\u8fdb\u6b65\u867d\u7136\u6709\u4e00\u70b9\uff0c\u4f46\u8fd8\u662f\u5f88\u6162\u7684\u539f\u56e0\uff0c\u6240\u4ee5\u6211\u4eec\u7528\u6750\u6599\u57fa\u56e0\uff0c\u5927\u6570\u636e\u548c\u539f\u4f4d\u5927\u79d1\u5b66\u88c5\u7f6e\u8868\u5f81\u7b49\u65b9\u6cd5\u6765\u53d1\u73b0\u9502\u7535\u6c60\u7684\u76f8\u5173\u76f8\u4e92\u7ed3\u6784\u5236\u7ea6\u7684\u672c\u8d28\u539f\u56e0\u3002\u4ece\u5e95\u5c42\u7269\u8d28\u548c\u673a\u7406\u7684\u51fa\u53d1\uff0c\u5373\u4ece\u539f\u5b50\u5c3a\u5ea6\u6765\u53d1\u73b0\u7ed3\u6784\u548c\u6027\u80fd\u76f8\u5173\u6027\uff0c\u6240\u5bf9\u5e94\u7684\u4e00\u95e8\u5b66\u79d1\u53eb\u505a\u7ed3\u6784\u5316\u5b66\uff08\u4e5f\u6709\u53eb\u7269\u8d28\u7ed3\u6784\uff09\uff0c\u7ed3\u6784\u5316\u5b66\u5c31\u662f\u7814\u7a76\u7269\u8d28\u5728\u539f\u5b50\u5c3a\u5ea6\u6392\u5e8f\u548c\u76f8\u4e92\u4f5c\u7528\u53ca\u5176\u5316\u5b66\u7269\u7406\u4e0a\u6240\u8868\u73b0\u7684\u6027\u80fd\u3002\u6240\u4ee5\u6211\u4eec\u53d1\u5c55\u7684\u56fe\u8bba\u65b9\u6cd5\u8868\u8fbe\u5b83\u7684\u7ed3\u6784\uff0c\u4f1a\u66f4\u6709\u6548\u5730\u63a2\u7d22\u6750\u6599\u7684\u57fa\u56e0\u53ca\u5176\u6784\u6548\u5173\u7cfb\u3002<\/p>\n<p>\u4e0b\u9762\u4f1a\u4e3e\u4e00\u4e2a\u4f8b\u5b50\uff0c\u5728\u7814\u7a76\u6750\u6599\u57fa\u56e0\u4e2d\uff0c\u63a2\u7d22\u7ed3\u6784\u57fa\u5143\u7684\u76f8\u4e92\u4f5c\u7528\u4f1a\u6df1\u5165\u5230 \u66f4\u6df1\u5c42\u6b21\u7684\u8fc7\u6e21\u91d1\u5c5e\u7535\u5b50\u81ea\u65cb\u7535\u5b50\u76f8\u4e92\u4f5c\u7528\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u65b0\u65b9\u6cd5\uff1a\u57fa\u4e8e\u56fe\u8bba\u7684\u7ed3\u6784\u5316\u5b66\u548c\u6750\u6599\u57fa\u56e0<\/strong><\/p>\n<p>\u6211\u4eec\u57282019\u5e74\u5728\u300a\u56fd\u5bb6\u79d1\u5b66\u8bc4\u8bba\u300b<strong>\u5b9a\u4e49\u9502\u7535\u6c60\u6750\u6599\u57fa\u56e0\uff1a<\/strong><strong>\u529f\u80fd\u57fa\u5143\u3001\u4f5c\u7528\u529b-\u952e\u3001\u8fde\u63a5-\u6392\u5e8f\u3002<\/strong><\/p>\n<p>\u78f7\u9178\u94c1\u9502\u4e3a\u4f8b\uff0c\u4e3a\u4ec0\u4e48\u78f7\u9178\u94c1\u9502\u5f88\u5b89\u5168\u5462\uff1f\u5c31\u662f\u56e0\u4e3a\u5b83\u6709\u78f7\u9178\u6839\uff0c\u5927\u5bb6\u77e5\u9053\u6240\u6709\u7684\u963b\u71c3\u7269\u8d28\u4f60\u53bb\u67e5\u4e00\u4e0b\u90fd\u662f\u542b\u78f7\u7684\uff0c\u4e3a\u4ec0\u4e48\u542b\u78f7\uff1f\u56e0\u4e3a\u78f7\u5f88\u5bb9\u6613\u6355\u83b7\u81ea\u7531\u57fa\u3002\u78f7\u6c27\u5316\u5408\u7269\u548c\u78f7\u9178\u6839\u5f88\u5bb9\u6613\u5438\u6c34\uff0c\u8fd9\u4e24\u4e2a\u8981\u7d20\u662f\u5b83\u963b\u71c3\u539f\u56e0\u3002\u78f7\u9178\u94c1\u9502\u6709\u78f7\u6c27\u5171\u4ef7\u952e\u7684\u78f7\u9178\u6839\u56db\u9762\u4f53\u3001\u9502\u6c27\u79bb\u5b50\u952e\u516b\u9762\u4f53\u548c\u8fc7\u6e21\u91d1\u5c5e\u94c1\u6c27\u914d\u4f4d\u952e\uff08\u79bb\u5b50\u4e0e\u5171\u4ef7\u952e\u6df7\u5408\uff09\u516b\u9762\u4f53\u7b49\u4e09\u7c7b\u7ed3\u6784\u57fa\u5143\u3002\u4ece\u7ed3\u6784\u57fa\u5143\u6765\u8bf4\u6709\u78f7\u6c27\u5171\u4ef7\u952e\u7a33\u5b9a\u4f7f\u5f97\u6c27\u7a33\u5b9a\uff0c\u56e0\u6b64\u78f7\u6c27\u56db\u9762\u4f53\u8d77\u5230\u4e86\u7a33\u5b9a\u7ed3\u6784\u6846\u67b6\u7684\u529f\u80fd\u57fa\u5143\u4f5c\u7528\u3002\u9502\u6c27\u516b\u9762\u4f53\u662f\u4f20\u5bfc\u9502\u79bb\u5b50\u7684\u529f\u80fd\u7ed3\u6784\u57fa\u5143\uff0c\u94c1\u6c27\u516b\u9762\u4f53\u7684\u94c1\u4ece\u5145\u7535\uff08\u9502\u62d6\u51fa\u53bb\u65f6\u5019\uff092\u4ef7\u52303\u4ef7\u53ca\u653e\u7535\uff08\u9502\u5d4c\u8fdb\u53bb\u65f6\u5019\uff09\u76843\u4ef7\u52302\u4ef7\uff0c\u662f\u50a8\u80fd\u529f\u80fd\u57fa\u56e2\u3002\u56e0\u6b64\uff0c\u9502\u7535\u6c60\u7535\u6781\u6750\u6599\u4e00\u822c\u53ef\u4ee5\u89e3\u6784\u6210\u4f20\u8f93\u529f\u80fd\u57fa\u5143\uff0c\u50a8\u80fd\u529f\u80fd\u57fa\u5143\u3001\u53ca\u6784\u67b6\u529f\u80fd\u57fa\u56e2\u3002<\/p>\n<p>\u73b0\u5728\u7535\u52a8\u8f66\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u7684\u6b63\u6781\u662f\u4e09\u5143\u9ad8\u954d\u5c42\u72b6\u6750\u6599\uff0c\u636e\u8bf4\u7279\u65af\u62c9\u7535\u52a8\u8f66\u5927\u91cf\u7528\u9ad8\u5bb9\u91cf\u7684\u6750\u6599\uff0c\u5927\u5bb6\u5df2\u7ecf\u53d1\u73b0\u5176\u5b89\u5168\u6027\u4e0d\u5982\u78f7\u9178\u94c1\u9502\uff0c\u56e0\u4e3a\u6c27\u7684\u7ed3\u6784\u57fa\u5143\u662f\u6c27\u4e0e\u8fc7\u6e21\u91d1\u5c5e\u5c423\u4e2a\u8fc7\u6e21\u91d1\u5c5e\u8fde\u63a5\u5e76\u4e0e\u9502\u5c42\u76843\u4e2a\u9502\u7ed3\u5408\uff0c\u4ee5\u6b64\u6c27\u53ea\u6709\u914d\u4f4d\u952e\u548c\u79bb\u5b50\u952e\uff0c\u6ca1\u6709\u7a33\u5b9a\u7684\u5171\u4ef7\u952e\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u9502\u7535\u6c60\u6750\u6599\u7b5b\u9009\uff1a\u6676\u4f53\u7ed3\u6784\u4e0e\u7535\u5b50\u7ed3\u6784<\/strong><\/p>\n<p>\u4ece\u6676\u4f53\u7ed3\u6784\u5927\u6570\u636e\u6211\u4eec\u53ef\u4ee5\u7b5b\u9009\u73b0\u6709\u7684\u9502\u7535\u6c60\u548c\u94a0\u79bb\u5b50\u7535\u6781\u6750\u6599\u548c\u56fa\u6001\u7535\u89e3\u8d28\u6750\u6599\uff0c\u4f5c\u4e3a\u7535\u6781\u6750\u6599\u5b83\u8981\u4e24\u4e2a\u5173\u952e\u8981\u7d20\uff0c\u9502\u6709\u53ef\u4f20\u8f93\u6027\uff0c\u8fc1\u79fb\u80fd\u5792\uff0c\u4f4e\u9502\u79bb\u5b50\u5bb9\u6613\u79fb\u52a8\u3002\u6211\u4eec\u53d1\u5c55\u4e86\u4e00\u79cd\u952e\u4ef7-Ewald\uff08BV-Ewald\uff09\u79bb\u5b50\u8fc1\u79fb\u6a21\u578b\uff0c\u9ad8\u901a\u91cf\u53d1\u73b0\u7ed3\u6784\u5927\u6570\u636e\u4e2d\u54ea\u4e9b\u542b\u9502\u6216\u542b\u94a0\u6676\u4f53\u7684Li\u6216Na\u662f\u201c\u53ef\u8fc1\u79fb\u201d\u7684\u3002\u6b64\u5916\uff0c\u7528\u4e8e\u7535\u6c60\u6750\u6599\u8981\u6c42\u662f\u7535\u5b50\u80fd\u5e26\u7ed3\u6784\u7684\u5e26\u9699\u4e0d\u5bbd\u7684\u534a\u5bfc\u4f53\uff08\u5bfc\u4f53\u66f4\u597d\uff0c\u94b4\u9178\u9502\u8131\u4e86\u4e00\u4e9b\u9502\u6210\u5bfc\u4f53\uff09\u3002\u7528\u4e8e\u56fa\u6001\u7535\u89e3\u8d28\u6750\u6599\u8981\u6c42\u5bf9\u7535\u5b50\u662f\u7edd\u7f18\u7684\uff0c\u7535\u5b50\u80fd\u5e26\u7ed3\u6784\u7684\u5e26\u9699\u8981\u5bbd\u3002\u6211\u4eec\u53ef\u4ee5\u7528\u7ed3\u6784\u5927\u6570\u636e\u6309\u7167\u79bb\u5b50\u53ef\u8fc1\u79fb\u6027\u4e0e\u7535\u5b50\u80fd\u5e26\u7ed3\u6784\u7684\u5e26\u5bbd\u53bb\u7b5b\u9009\u53ef\u80fd\u7684\u7535\u6781\u6750\u6599\u548c\u56fa\u6001\u7535\u89e3\u8d28\u6750\u6599\uff0c\u53d1\u73b0\u65b0\u7684\u7ed3\u6784\u57fa\u5143\u3001\u6392\u5e8f\u4ee5\u53ca\u53ef\u80fd\u4f4e\u6210\u672c\u7684\u5143\u7d20\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u5c42\u72b6\u6750\u6599\uff1a\u7ed3\u6784\u57fa\u5143\u4e0eLi\u6269\u6563\u8def\u5f84<\/strong><\/p>\n<p>\u9502\u79bb\u5b50\u5728\u954d\u94b4\u95303\u5143\u5c42\u72b6\uff08NCM\uff09\u6b63\u6781\u6750\u6599\u662f\u600e\u4e48\u4f20\u8f93\u7684\uff1f\u6211\u4eec\u9ad8\u7aef\u624b\u673a\u7528\u7684\u662f\u5c42\u72b6\u94b4\u9178\u9502\u800c\u7535\u52a8\u8f66\u8bb8\u591a\u7528\u7684\u662f3\u5143\u5c42\u72b6\u6750\u6599\u3002\u7528\u6750\u6599\u57fa\u56e0\u5206\u6790\u65b9\u6cd5\uff0c\u5c42\u72b6\u6750\u6599\u7684\u9502\u5c42\u7531\u9502\u6c27\u516b\u9762\u4f53\uff0c\u9502\u79bb\u5b50\u6ee1\u7684\u65f6\u5019\u9502\u79bb\u5b50\u4f20\u8f93\u4ece\u4e00\u4e2a\u516b\u9762\u4f53\u4f20\u5230\u90bb\u8fd1\u4e00\u4e2a\u516b\u9762\u4f53\uff08\u516b\u9762\u4f53-\u516b\u9762\u4f53\u4f20\u8f93\uff09\uff0c\u53d7\u5230\u4e24\u8fb9\u8fc7\u6e21\u91d1\u5c5e\u7684\u76f8\u4e92\u4f5c\u7528\u3002\u5f53\u9502\u8dd1\u4e8620%\u5de6\u53f3\uff0c\u9502\u79bb\u5b57\u503e\u5411\u4e8e\u4ece\u516b\u9762\u4f53\u5230\u56db\u9762\u4f53\u518d\u5230\u516b\u9762\u4f53\uff08\u516b\u9762\u4f53-\u56db\u9762\u4f53-\u516b\u9762\u4f53\uff09\u7684\u4f20\u8f93\u8def\u5f84\u673a\u5236\uff0c\u5f53\u5c42\u95f4\u8ddd\u5927\u5bf9\u5e94\u516b\u9762\u4f53\u4e5f\u5927\u548c\u9502\u6c27\u952e\u4e5f\u957f\uff0c\u6c27\u5bf9\u9502\u7684\u675f\u7f1a\u5f31\uff0c\u9502\u79bb\u5b50\u4f20\u8f93\u7684\u80fd\u5792\u4f1a\u4f4e\u4ece\u800c\u4f20\u8f93\u4f1a\u5feb\uff0c\u8fd9\u662f\u7ed3\u6784\u57fa\u5143\u4e0e\u9502\u79bb\u5b50\u4f20\u8f93\u76f8\u5173\u6027\u7684\u4e00\u4e2a\u5173\u952e\u8981\u7d20\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u5c42\u72b6\u6750\u6599\uff1a\u4e2d\u5b50\u6d4b\u91cf\u539f\u4f4d\u5168\u7535\u6c60Li\u6269\u6563\u52a8\u529b\u5b66<\/strong><\/p>\n<p>2015\u5e74\u6211\u4eec\u7406\u8bba\u9884\u6d4b\u5c42\u72b63\u5143\u9502\u79bb\u5b50\u7684\u4f20\u8f93\u673a\u7406\u3002\u73b0\u5728\u6211\u4eec\u53ef\u4ee5\u7528\u56fd\u5bb6\uff08\u4e1c\u839e\uff09\u6563\u88c2\u4e2d\u5b50\u6e90\u7684\u884d\u5c04\u8c31\u4eea\u539f\u4f4d\u68c0\u6d4b\u5b9e\u9645\u9502\u7535\u6c60\u539f\u4f4d\u9502\u79bb\u5b50\u5728\u4e0d\u540c\u7684\u7535\u538b\u4e0b\u7684\u4f20\u8f93\u52a8\u529b\u5b66\u8def\u5f84\uff0c\u4e0e\u7406\u8bba\u7684\u9884\u6d4b\u57fa\u672c\u4e00\u81f4\uff0c\u65b0\u7684\u4e2d\u5b50\u8868\u5f81\u89c2\u5bdf\u53d1\u73b0\u662f\u5f53\u9502\u8131\u51fa40%\u4ee5\u4e0a\u65f6\uff0c\u9502\u662f\u516b\u9762\u4f53-\u516b\u9762\u4f53\u4ee5\u53ca\u516b\u9762\u4f53-\u56db\u9762\u4f53-\u516b\u9762\u4f53\u4e8c\u79cd\u4f20\u8f93\u673a\u5236\u540c\u65f6\u5b58\u5728\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u9502\u79bb\u5b50\u9ad8\u7535\u5bfc\uff1a\u7ed3\u6784\u57fa\u5143\u4e0e\u534f\u540c\u4f20\u8f93<\/strong><\/p>\n<p>\u600e\u4e48\u8ba9\u9502\u79bb\u5b50\u5728\u56fa\u4f53\u91cc\u9762\u80fd\u591f\u5feb\u901f\u4f20\u8f93\uff1f\u751a\u81f3\u4f20\u5f97\u6bd4\u7535\u89e3\u6db2\u66f4\u5feb\uff1f\u6700\u8fd1\u5b9e\u9a8c\u53d1\u73b0\u5728Li-P-S\u56fa\u6001\u7535\u89e3\u8d28\u6bd4\u6db2\u4f53\u9502\u4f20\u8f93\u8981\u5feb\uff0c\u7528\u6750\u6599\u7ed3\u6784\u57fa\u5143\u53ca\u5176\u5b83\u7684\u8fde\u63a5\u65b9\u5f0f\u6765\u7814\u7a76\u5176\u9502\u79bb\u5b50\u4f20\u8f93\u673a\u7406\uff0c\u53d1\u73b0\u5176\u5feb\u901f\u4f20\u8f93\u7684\u673a\u7406\u662f\u76f8\u90bb\u7684\u9502\u79bb\u5b50\u7ed3\u6784\u57fa\u5143\u4e4b\u95f4\u6709\u4e92\u52a8\uff0c\u5c31\u76f8\u5f53\u4e8e\u6784\u6210\u4e00\u4e2a\u534f\u540c\u4f20\u8f93\u7684\u8d85\u7ed3\u6784\u57fa\u5143\uff0c\u4e00\u4e2a\u4f4e\u80fd\u5792\u7ed3\u6784\u57fa\u5143\uff08\u79f0A\uff09\u7684\u9502\u79bb\u5b50\u4f20\u8f93\u7684\u8fc7\u7a0b\u4e2d\u4f1a\u5f71\u54cd\u76f8\u90bb\u7ed3\u6784\u57fa\u5143\uff08\u79f0B\uff09\u7684\u6784\u578b\u4ece\u800c\u964d\u4f4e\u4e86\u5176\u4f20\u8f93\u80fd\u5792\u52a0\u901fB\u7684\u9502\u79bb\u5b50\u79fb\u52a8\u548c\u4f20\u8f93\uff0cB\u7684\u9502\u79bb\u5b50\u79fb\u52a8\u53cd\u8fc7\u6765\u53c8\u5f71\u8d77A\u7684\u6784\u578b\u8fdb\u4e00\u6b65\u53d8\u5316\u4f7f\u5f97\u5176\u80fd\u5792\u66f4\u4f4e\u4f20\u8f93\u66f4\u5feb\uff0c\u5f62\u6210\u4e86\u6b63\u53cd\u9988\u4e92\u52a0\u901f\u9502\u79bb\u5b50\u7684\u534f\u540c\u4f20\u8f93\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u4e09\u5143\u5c42\u72b6\u9502\u7535\u6c60\u6b63\u6781(NMC<\/strong><strong>)<\/strong><strong>\u00a0\u70ed\u7a33\u5b9a\u6027vs \u7ed3\u6784\u57fa\u5143<\/strong><\/p>\n<p>\u9502\u7535\u6c60\u600e\u4e48\u505a\u5f97\u5b89\u5168\u548c\u7a33\u5b9a\uff1f\u4ece\u6750\u6599\u57fa\u56e0\u7684\u89d2\u5ea6\u53bb\u6316\u6398\u7ed3\u6784\u7684\u7a33\u5b9a\u6027\uff0c\u5256\u6790\u4e00\u4e0b\u9502\u7535\u6c60\u7684\u5145\u653e\u7535\u8fc7\u7a0b\uff0c\u5bf9\u5c42\u72b6\u7684\u6750\u6599\u6765\u8bf4\uff0c\u6700\u91cd\u8981\u5b89\u5168\u6027\u548c\u7a33\u5b9a\u6027\u662f\u6c27\u7684\u7a33\u5b9a\u6027\u3002\u6c27\u7684\u7ed3\u6784\u57fa\u5143\u662f\u6c27\u4e0e\u8fc7\u6e21\u91d1\u5c5e\u5c423\u4e2a\u8fc7\u8fc7\u6e21\u91d1\u5c5e\u8fde\u63a5\u5e76\u4e0e\u9502\u5c42\u76843\u4e2a\u9502\u7ed3\u5408\uff0c\u4ee5\u6b64\u6c27\u53ea\u6709\u4e0e\u8fc7\u6e21\u91d1\u5c5e\u914d\u4f4d\u952e\u548c\u4e0e\u9502\u7684\u79bb\u5b50\u952e\uff0c\u6ca1\u6709\u7a33\u5b9a\u7684\u5171\u4ef7\u952e\u3002\u5145\u7535\u7684\u65f6\u5019\u628a\u9502\u62d6\u51fa\u53bb\uff0c\u6c27\u4e0a\u7684Li\u4ece\u4e09\u4e2a\u9502\u53d8\u6210\u4e24\u4e2a\u3001\u518d\u53d8\u6210\u4e00\u4e2a\u76f4\u5230\u5168\u90e8\u8131\u5b8c\u3002\u7528\u70ed\u5206\u6790\u53d1\u73b0\u5176\u70ed\u7a33\u5b9a\u6027\u4ece900\u2103\u4e00\u76f4\u4f1a\u964d\u5230150<span style=\"font-size: xx-small;\">\u2103<\/span>\u5de6\u53f3\uff0c\u5c42\u72b6\u6750\u6599\u7684\u7ed3\u6784\u7a33\u5b9a\u6027\u4e0e\u9502\u6709\u6ca1\u6709\u5728\u9502\u5c42\u5bc6\u5207\u76f8\u5173\uff0c\u5373\u9502\u5c42\u662f\u7a7a\u7684\u53caNi4+\u4f1a\u5bfc\u81f4\u6c27\u7684\u7a33\u5b9a\u6027\u4e0b\u964d\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u6784\u6548\u5173\u7cfb\uff1a\u9502\u7535\u6c60\u6750\u6599d\u7535\u5b50\u7ed3\u6784\u5316\u5b66<\/strong><\/p>\n<p>\u600e\u4e48\u80fd\u591f\u4f7f\u5f97\u5c42\u72b6\u7684\u6c27\u7684\u7ed3\u6784\u66f4\u7a33\u5b9a? \u5728NMC\u4e09\u5143\u6750\u6599\u603b\u6709\u9502\u8dd1\u5230\u8fc7\u6e21\u91d1\u5c5e\u5c42\u540c\u65f6\u954d\u8dd1\u5230\u9502\u5c42\u6765\u79f0\u4e4b\u4e3aLi\/Ni\u53cd\u4f4d \uff0c\u8fd8\u6709\u8fc7\u6e21\u91d1\u5c5e\u662f\u53ef\u53d8\u4ef7\uff0c\u4e0d\u540c\u4ef7\u6709\u4e0d\u540c\u7684\u81ea\u65cb\u7535\u5b50\uff0c\u6bd4\u5982\u8bf4\u954d\u4e8c\u4ef7\u5728\u516b\u9762\u4f53\u6709\u4e24\u4e2a\u81ea\u65cb\uff0c\u4e09\u4ef7\u662f\u4e00\u4e2a\u81ea\u65cb\uff0c\u4e0d\u540c\u7684\u81ea\u65cb\u7535\u5b50\u4e92\u76f8\u4f5c\u7528\u4f1a\u5bfc\u81f4\u4ec0\u4e48\u7ed3\u679c\uff1fGoodenough\u6559\u6388\u65e9\u5e74\u4ed6\u8fd8\u6ca1\u6709\u505a\u9502\u7535\u6c60\u7684\u65f6\u5019\uff0c\u53d1\u73b0\u81ea\u65cb\u7535\u5b50\u76f8\u4e92\u4f5c\u7528\u4e00\u4e9b\u89c4\u5f8b\u3002\u4ec0\u4e48\u53eb\u5316\u5b66\u952e\uff1f\u81ea\u65cb\u5411\u4e0a\u7535\u5b50\u4e0e\u81ea\u65cb\u5411\u4e0b\u7684\u7535\u5b50\u914d\u5bf9\uff0c\u53d8\u6210\u4e00\u4e2a\u5355\u952e\u3002\u5982\u679c\u8fc7\u6e21\u91d1\u5c5e\u901a\u8fc7\u4e2d\u95f4\u4e00\u4e2a\u6c27\u8fde\u63a5\uff0cd-\u8fc7\u6e21\u81ea\u65cb\u7535\u5b50\u4e4b\u95f4\u4f1a\u5f62\u6210\u8d85\u4ea4\u6362\u76f8\u4e92\u4f5c\u7528\uff0c\u5982\u679c3\u4e2a\u8fc7\u6e21\u91d1\u5c5e\u901a\u8fc7\u6c27\u4e3a\u6865\u6881\u5f62\u6210\u4e09\u89d2\u7684\u8fde\u63a5\u5173\u7cfb\uff0c3\u4e2a\u8fc7\u6e21\u91d1\u5c5e\u53ea\u67092\u4e2a\u6709\u81ea\u65cb\u8d85\u4ea4\u6362\u4f5c\u7528\u7b2c3\u4e2a\u6ca1\u6709\u81ea\u65cb\u7535\u5b50\uff0c\u8fd9\u4e24\u4e2a\u914d\u5bf9\u662f\u7a33\u5b9a\u3002\u5982\u679c3\u4e2a\u90fd\u6709\u81ea\u65cb\uff0c\u8fd9\u662f\u201c\u4e09\u4f53\u95ee\u9898\u201d\u662f\u4e0d\u7a33\u5b9a\u7684\uff0c\u5b83\u4eec\u4e4b\u95f4\u7684\u81ea\u65cb\u76f8\u4e92\u4f5c\u7528\u5c31\u4f1a\u5e72\u6270\uff0c\u8fd9\u5e72\u6270\u53eb\u78c1\u963b\u6413\uff0c\u4f7f\u5f97\u539f\u5b50\u95f4\u7684\u7ed3\u5408\u529b\u53d8\u5f31\uff0c\u5982\u679c\u7b2c3\u4e2a\u6ca1\u6709\u81ea\u65cb\u7535\u5b50\uff0c\u90a3\u5c31\u6ca1\u6709\u78c1\u963b\u6413\uff0c\u7ed3\u5408\u529b\u5c31\u5f3a\u3002\u75283\u4f53\u81ea\u65cb\u7535\u5b50\u76f8\u4e92\u4f5c\u7528\u4e0e\u78c1\u963b\u6413\u5206\u6790\uff0cLi\/Ni\u53cd\u4f4d\u4f7f\u5f97\u9502\u5230\u8fc7\u6e21\u91d1\u5c5e\u516d\u8fb9\u5f62\u4e2d\u95f4\u66ff\u6362\u6210\u6ca1\u6709\u81ea\u65cb\u7684\u9502\u53ef\u4ee5\u6d88\u9664\u78c1\u963b\u6413\u3002\u94b4\u4e09\u4ef7\u6ca1\u6709d-\u81ea\u65cb\u7535\u5b50\u4e5f\u80fd\u6d88\u9664\u78c1\u963b\u6413\u3002\u53ef\u4ee5\u9884\u89c1Li\/Ni\u53cd\u4f4d\u91cf\u4e0e\u8fc7\u6e21\u91d1\u5c5e\u5c42\u7684\u81ea\u65cb\u7535\u5b50\u6570\u6709\u5173\uff0cCo<sup>3+<\/sup>\u6ca1\u6709\u81ea\u65cb\uff0c\u542b\u91cf\u8d8a\u591aLi\/Ni\u53cd\u4f4d\u8d8a\u5c11\uff0cMn<sup>4+<\/sup>\u67093\u4e2a\u81ea\u65cb\uff0cMn<sup>4+<\/sup>\u8d8a\u591aLi\/Ni\u53cd\u4f4d\u8d8a\u591a\uff0c\u6211\u4eec\u7528\u4e2d\u5b50\u884d\u5c04\u6d4b\u91cf\u4e86\u81ea\u65cb\u7535\u5b50\u6570\u91cf\u4e0e\u53cd\u4f4d\u6570\u91cf\u76f8\u4e92\u5173\u7cfb\uff0c\u5f97\u5230\u76f8\u5173\u7684\u76f8\u56fe\uff0c\u8bc1\u5b9e\u4e86\u6211\u4eec\u7684\u9884\u89c1\u3002<\/p>\n<p>\u603b\u4e4b\uff0c\u6211\u4eec\u7cfb\u7edf\u7814\u7a76\u8fc7\u6e21\u91d1\u5c5e\u81ea\u65cb\u7535\u5b50\u4e92\u76f8\u4f5c\u7528\u5bfc\u81f4\u78c1\u963b\u6413\u3001\u8d85\u4ea4\u6362\u4f5c\u7528\u548cLi\/Ni\u53cd\u4f4d\u7f3a\u9677vs.\u4e09\u5143\u5c42\u72b6NiCoMn\u5143\u7d20\u5404\u81ea\u7684\u4f5c\u7528\uff0c\u63ed\u793aCo\u7684\u4f5c\u7528\u53ca\u66ff\u4ee3\u53ef\u80fd\u6027\u3002\u57fa\u4e8e\u56e2\u961f9\u7bc7\u7cfb\u5217\u7814\u7a76\u8bba\u6587\u6210\u679c\uff0c\u5e94\u9080\u4ee5\u5c01\u9762\u6587\u7ae0\u5728Acc Chem Res\u8fdb\u884c\u603b\u7ed3\u548c\u5c55\u671b\uff0c\u5927\u5bb6\u611f\u5174\u8da3\u53ef\u4ee5\u518d\u770b\u4e00\u4e0b\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u4e09\u5143NMC \u00a0\u70ed\u7a33\u5b9a\u6027vs \u7ed3\u6784\u57fa\u5143<\/strong><\/p>\n<p>Li\/Ni\u53cd\u4f4d\u4f7f\u5f97\u9502\u5c42Ni<sup>2+<\/sup>\u4e0e\u8fc7\u6e21\u91d1\u5c5e\u5c42\u7684\u8fc7\u6e21\u91d1\u5c5e\u4e4b\u95f4\u6709180\u5ea6\u7684\u8f83\u5f3a\u7684\u8d85\u4ea4\u6362\u76f8\u4e92\u4f5c\u7528\uff0c\u6709\u7ea660meV\uff08\u5ba4\u6e29\u662f25meV\uff09\u8fdc\u9ad8\u4e8e\u5ba4\u6e29\u7684\u7a33\u5b9a\u6027\uff0c\u8be5\u53cd\u4f4d\u5728\u9502\u5c42\u7684\u954d\u6c27\u516b\u9762\u4f53\u6210\u4e3a\u4e86\u7a33\u5b9a\u7ed3\u6784\u6846\u67b6\u7684\u529f\u80fd\u7ed3\u6784\u57fa\u5143\uff0c\u540c\u65f6\u6c27\u7684\u7ed3\u6784\u57fa\u5143\u4e5f\u66f4\u52a0\u7a33\u5b9a\u4e86\u3002\u56e0\u6b64\uff0cLi\/Ni\u53cd\u4f4d\u7f3a\u9677\u80fd\u589e\u5f3aNMC\u4e09\u5143\u5c42\u72b6\u7684\u7a33\u5b9a\u6027\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u53d1\u73b0\u9ad8\u7535\u538b\u9ad8\u5bb9\u91cf\u94b4\u9178\u9502\u7684\u673a\u7406<\/strong><\/p>\n<p>\u73b0\u5728\u9ad8\u7aef\u624b\u673a\u7528\u7684\u6b63\u6781\u6750\u6599\u662f\u94b4\u9178\u9502\u3002\u81ea\u4eceGoodenough\u6559\u6388\u53d1\u73b0\u540e\u7528\u5230\u9502\u7535\u6c60\u6b63\u6781\u5927\u6982\u5341\u51e0\u5e74\uff0c\u5bb9\u91cf\u7a33\u5b9a\u5e94\u7528\u53ea\u80fd\u53d1\u6325\u8fd1\u7406\u8bba\u5bb9\u91cf\uff08280mAh\/g\uff09\u7684\u4e00\u534a\uff0c\u5373145 mAh\/g\u7535\u538b\u5728 4.2V\uff0c\u8d85\u8fc7\u8fd9\u4e2a\u5bb9\u91cf\u548c\u7535\u538b\u5c31\u4f1a\u51fa\u73b0\u4e0d\u7a33\u5b9a\uff0c\u5176\u539f\u56e0\u4e00\u76f4\u4e0d\u6e05\u695a\u3002\u8fd1\u51e0\u5e74\u53d1\u5c55\u6210\u529f\u5bb9\u91cf180 mAh\/g\u5176\u7535\u538b\u53ef\u4ee5\u63d0\u9ad8\u52304.5V\uff0c\u6709\u51e0\u7bc7\u6587\u7ae0\u5bf9\u5176\u539f\u56e0\u8bb2\u5f97\u4e5f\u4e0d\u592a\u6e05\u695a\u3002\u5927\u5bb6\u53ef\u4ee5\u53bb\u6bd4\u8f83\u51e0\u7bc7\u53d1\u8868\u6587\u7ae0\u4e2d4.2V\u7a33\u5b9a\u548c\u9ad8\u7535\u538b\u7a33\u5b9a4.5V\u94b4\u9178\u9502\u6750\u6599\u7684\u591a\u6676x-\u5c04\u7ebf\u884d\u5c04\uff08XRD\uff09\u8c31\uff0c\u770b\u4e0d\u51fa\u4ec0\u4e48\u5dee\u522b\u3002\u8ba9\u6211\u4eec\u95ee\u591a\u6676XRD\u6d4b\u91cf\u65b9\u6cd5\u7684\u672c\u8d28\u662f\u4ec0\u4e48\uff1f\u5b83\u662f\u628a\u591a\u6676\u7684\u6bcf\u4e2a\u9897\u7c92\u7684\u6676\u683c\u5468\u671f\u6027\u7684\u884d\u5c04\u4fe1\u53f7\u53e0\u52a0\u5f97\u5e73\u5747\u503c\uff0c\u6d4b\u5f97\u884d\u5c04\u65b9\u5411\uff08hkl\uff09\u7684\u95f4\u8ddd\uff08d-\u503c\uff09\u662f\u5e73\u5747\u503c\uff0c\u5e76\u4e0d\u80fd\u53cd\u6620\u6bcf\u4e2a\u9897\u7c92\u4ee5\u53ca\u4e00\u4e2a\u9897\u7c92\u7684\u4e0d\u540c\u4f4d\u7f6e\u7684\u539f\u5b50\u6392\u5217\u4fe1\u606f\u3002\u56e0\u6b64\uff0c\u8981\u53d1\u73b0\u666e\u901a\u94b4\u9178\u9502\u548c\u9ad8\u7535\u538b\u94b4\u9178\u9502\u7684\u5dee\u522b\u4e00\u5b9a\u662f\u8981\u6d4b\u91cf\u5fae\u89c2\u7ed3\u6784\u5dee\u522b\uff0c\u8fd9\u9700\u8981\u7814\u7a76\u5355\u4e2a\u6676\u4f53\u9897\u7c92\u4ee5\u53ca\u4e00\u4e2a\u5355\u6676\u9897\u7c92\u4e0d\u540c\u4f4d\u7f6e\uff08\u4ece\u754c\u9762\u5230\u6676\u4f53\u4e2d\u5fc3\uff09\u7684\u5fae\u89c2\u7ed3\u6784\u3002\u6211\u4eec\u4e0e\u5317\u5927\u5316\u5b66\u9662\u5b59\u4fca\u826f\u8001\u5e08\u4e00\u8d77\u7528\u81ea\u4e3b\u6539\u8fdb\u76843D\u7535\u5b50\u884d\u5c04\u7684\u6280\u672f\uff0c\u5c06\u900f\u5c04\u7535\u955c\u7684\u7535\u5b50\u675f\u4f5c\u4e3a\u884d\u5c04\u7c92\u5b50\/\u6ce2\u7684\u6e90\uff0c\u900f\u8fc7\u5fae\u7c73\u5927\u5c0f\u7684\u94b4\u9178\u9502\u5355\u6676\uff08\u900f\u5c04\u539a\u5ea6\u8981\u5728\u7ea61-2\u5fae\u7c73\u5de6\u53f3\u6216\u4e4b\u4e0b\uff09\uff0c\u53ef\u4ee5\u9009\u5355\u6676\u7684\u4e0d\u540c\u90e8\u4f4d\u6765\u68c0\u6d4b\u3002\u8fd9\u4e2a\u68c0\u6d4b\u6280\u672f\u53ef\u4ee5\u770b\u5230\u94b4\u9178\u9502\u4e0d\u540c\u7535\u538b\u5145\u653e\u7535\u524d\u540e\u7684\u5fae\u89c2\u7ed3\u6784\u53d8\u5316\u3002\u9502\u7535\u6c60\u6750\u6599\u7ed3\u6784\u68c0\u6d4b\u8981\u5305\u62ec\u672c\u5f81\u7ed3\u6784\u4ee5\u53ca\u4f7f\u7528\u8fc7\u7a0b\u7684\u7ed3\u6784\u53d8\u5316\uff08\u5305\u62ec\u5176\u7ed3\u6784\u7a33\u5b9a\u6027\u548c\u53d8\u5316\u7684\u53ef\u9006\u6027\uff09\uff0c\u7535\u6c60\u6750\u6599\u5728\u7535\u5316\u5b66\u73af\u5883\u4e0b\u5145\u653e\u7535\uff0c\u7535\u5b50\u548c\u79bb\u5b50\u4ece\u754c\u9762\u8fdb\/\u51fa\uff0c\u56e0\u6b64\u7ed3\u6784\u7684\u7834\u574f\u5f80\u5f80\u4f1a\u4ece\u754c\u9762\u5f00\u59cb\u3002\u6211\u4eec\u7528\u8fd9\u6280\u672f\u770b\u5230\u4e86\u666e\u901a\u548c\u9ad8\u7535\u538b\u7a33\u5b9a\u94b4\u9178\u9502\u7684\u5dee\u522b\uff0c\u666e\u901a\u5c42\u72b6\u94b4\u9178\u9502\u7684\u5c42\u6709\u4e0d\u540c\u7a0b\u5ea6\u5f2f\u66f2\uff0c\u5728\u5145\u7535\uff08\u9502\u79bb\u5b50\u8131\u51fa\uff0c\u5c42\u95f4\u8ddd\u6269\u5927\uff09\u8fc7\u7a0b\u5f53\u5f2f\u66f2\u4f1a\u653e\u5927\uff0c\u524d\u9762\u8bb2\u8fc7\u5c42\u95f4\u8ddd\u5927\u9502\u79bb\u5b50\u8fc1\u79fb\u5bb9\u6613\uff0c\u5f2f\u66f2\u5c42\u72b6\u7ed3\u6784\u7684\u5c42\u95f4\u8ddd\u662f\u4e0d\u4e00\u6837\u5927\u7684\uff0c\u5c42\u95f4\u8ddd\u5927\u9502\u79bb\u5b50\u5148\u8131\u51fa\uff0c\u4e00\u65e6\u9502\u79bb\u5b50\u8131\u51fa\u5728\u8be5\u5904\u7684\u5c42\u95f4\u8ddd\u5c31\u4f1a\u8fdb\u4e00\u6b65\u6269\u5927\uff0c\u8fd9\u6837\u5c31\u4f1a\u5f62\u6210\u4e00\u4e2a\u6b63\u53cd\u9988\u5bfc\u81f4\u5c42\u7684\u5f2f\u66f2\u7684\u4e0d\u65ad\u6269\u5927\uff0c\u5f2f\u66f2\u5904\u5f62\u6210\u7684\u5e94\u529b\u8d8a\u6765\u8d8a\u5927\uff0c\u5f53\u5e94\u529b\u79ef\u805a\u5230\u4e00\u5b9a\u7a0b\u5ea6\u5c31\u53ef\u80fd\u5bfc\u81f4\u5c42\u7684\u65ad\u88c2\uff0c\u8fc7\u6e21\u91d1\u5c5e\u4f1a\u53d1\u751f\u8fc1\u79fb\u540c\u65f6\u6c27\u539f\u5b50\u5c31\u6709\u53ef\u80fd\u91ca\u653e\u51fa\u53bb\u3002\u76f8\u5bf9\u6bd4\u7684\u662f\u7528\u8be5\u65b9\u6cd5\u68c0\u6d4b\u53d1\u73b0\u9ad8\u7535\u538b\u94b4\u9178\u9502\u7684\u5c42\u662f\u6bd4\u8f83\u5e73\u6574\u7684\uff0c\u6309\u7167\u4ee5\u4e0a\u8ba8\u8bba\u7c7b\u63a8\u5728\u5145\u7535\u65f6\u5e73\u7684\u5c42\u7684\u5c42\u95f4\u8ddd\u662f\u6bd4\u8f83\u5747\u5300\u7684\u6269\u5927\uff0c\u4ea7\u751f\u5e94\u529b\u7684\u79ef\u805a\u5c31\u5c0f\uff0c\u5c42\u80fd\u4fdd\u6301\u8f83\u9ad8\u7684\u7a33\u5b9a\u6027\uff0c\u56e0\u6b64\u80fd\u627f\u53d7\u9ad8\u7535\u538b\u4e0b\u9ad8\u5bb9\u91cf\u9502\u79bb\u5b50\u7684\u8131\u4e0e\u5d4c\u3002<\/p>\n<p>\u9502\u7535\u6c60\u5c42\u72b6\u6750\u6599\u53ef\u4ee5\u60f3\u8c61\u6210\u4e00\u5757\u5757\u6728\u677f\u5e73\u5806\u8d77\u6765\uff0c\u5806\u79ef\u6728\u677f\u7684\u4e2d\u95f4\u56e0\u7d27\u5bc6\u63a5\u89e6\u662f\u5e73\u6574\u7684\uff0c\u4f46\u5806\u79ef\u6728\u677f\u7684\u8fb9\u5f80\u5f80\u4f1a\u7fd8\u8d77\u6765\u4e0d\u6613\u5e73\u6574\uff0c\u8981\u628a\u5b83\u641e\u5e73\u6574\uff0c\u5728\u5efa\u7b51\u4e0a\u662f\u5728\u8fb9\u4e0a\u9489\u9489\u5b50\u6765\u9632\u6b62\u5b83\u4e0d\u5e73\u6216\u51cf\u5c11\u5f2f\u66f2\uff08\u7fd8\u8d77\u6765\uff09\u3002\u5c42\u72b6\u94b4\u9178\u9502\u7684\u9ad8\u7535\u538b\u7684\u539f\u7406\u4e0e\u6728\u677f\u5806\u79ef\u76f8\u4f3c\uff0c\u8981\u7ecf\u5f97\u8d77\u73af\u5883\u7684\u5e72\u6270\u4f7f\u5f97\u5806\u79ef\u4ece\u4e2d\u5fc3\u5230\u8fb9\u7f18\u59cb\u7ec8\u4fdd\u6301\u4e00\u81f4\uff0c\u56e0\u6b64\uff0c\u5176\u89e3\u51b3\u65b9\u6848\u662f\u5728\u8fb9\u7f18\u201c\u9489\u9489\u5b50\u201d\u3002<\/p>\n<p>\u8fd9\u4e2a\u5de5\u4f5c\u5c31\u7ed9\u5927\u5bb6\u4e00\u4e2a\u542f\u53d1\u548c\u8fdb\u4e00\u6b65\u601d\u8003\u4ec0\u4e48\u662f\u7269\u8d28\uff0c\u4ec0\u4e48\u662f\u6750\u6599\u7684\u57fa\u672c\u95ee\u9898\u3002\u6750\u6599\u7684\u76ee\u6807\u662f\u4f7f\u7528\uff0c\u662f\u4f7f\u7528\u5176\u6027\u80fd\uff0c\u8fd9\u4e0e\u6750\u6599\u4ece\u4e2d\u5fc3\u5230\u754c\u9762\u7684\u7ed3\u6784\u4e00\u81f4\u6027\u5bc6\u5207\u76f8\u5173\uff0c\u7279\u522b\u662f\u4e0e\u754c\u9762\u7684\u6027\u80fd\u6709\u76f4\u63a5\u7684\u5173\u7cfb\u7684\u6750\u6599\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u53d1\u73b0\u9ad8\u6027\u80fd\u9502\u7535\u6c60\u65e0Co\u5c42\u72b6\u6b63\u6781\u6750\u6599<\/strong><\/p>\n<p>\u56de\u5230\u6750\u6599\u57fa\u56e0\uff0c\u7ed3\u6784\u57fa\u5143\u7684\u6700\u5c0f\u7684\u5355\u5143\u662f\u5143\u7d20\u7279\u5f81\uff0c\u5373\u5176\u539f\u5b50\u6216\u79bb\u5b50\u7684\u5916\u5c42\u7535\u5b50\u6570\uff0c\u5728\u9502\u7535\u6c60\u5c42\u72b6\u6b63\u6781\u6750\u6599\u7684\u8fc7\u6e21\u91d1\u5c5e\u7684\u4e0d\u540c\u4ef7\u6001\u6709\u4e0d\u540c\u7684d-\u81ea\u65cb\u7535\u5b50\uff0c\u94b4\u6c27\u516b\u9762\u4f53\u4e2dCo<sup>3+<\/sup>\u200b\u662f\u6ca1\u6709\u81ea\u65cb\u7684\uff0c\u94b4\u662f\u6218\u7565\u7269\u8d44\u5f88\u8d35\uff0c3\u5143\u4e2d\u80fd\u4e0d\u80fd\u4e0d\u8981\u94b4\uff0c\u6750\u6599\u901a\u8fc7Li\/Ni\u53cd\u4f4d\u53c8\u53ef\u4ee5\u66f4\u52a0\u7a33\u5b9a\uff0c\u8fc7\u6e21\u5229\u7528\u91d1\u5c5e\u5c42\u954d\u4e0e\u53cd\u4f4d\u5230\u9502\u5c42\u7684\u954d\u4e4b\u95f4\u5c31\u53ef\u4ee5\u5f62\u6210180\u5ea6\u8d85\u4ea4\u6362\u76f8\u4e92\u4f5c\u7528\u628a\u6750\u6599\u53d8\u5f97\u66f4\u7a33\u5b9a\u3002\u57fa\u4e8e\u8fd9\u4e2a\u601d\u60f3\u6211\u4eec\u8bbe\u8ba1\u591a\u5143\u5c42\u72b6\u6750\u6599\u6ca1\u6709\u94b4\uff0c\u5b9e\u9a8c\u8bc1\u660e\u53ef\u4ee5\u5b9e\u73b0\u65e0\u94b4\u6b63\u6781\u6750\u6599\u5e76\u5728\u9ad8\u7535\u538b\u4e0b\u7ed3\u6784\u66f4\u52a0\u7a33\u5b9a\uff0c\u5f00\u542f\u65e0\u94b4\u5c42\u72b6\u6b63\u6781\u6750\u6599\u65b0\u6750\u6599\u7814\u53d1\u3002\u7279\u65af\u62c9 CEO\u4e5f\u8bb2\uff0c\u5bf9\u5927\u89c4\u6a21\u4f7f\u7528\u7535\u52a8\u8f66\u52a8\u529b\u7535\u6c60\uff0c\u4e0d\u4ec5\u94b4\u5373\u4f7f\u954d\u4e5f\u592a\u8d35\u4e86\uff0c\u56e0\u6b64\u8fde\u954d\u90fd\u8981\u51cf\u5c11\uff0c\u8fd9\u662f\u6211\u4eec\u6b63\u5728\u7814\u7a76\u7684\u4e00\u5927\u65b9\u5411\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u754c\u9762\u6750\u6599\u57fa\u56e0vs.\u7535\u5316\u5b66\u4f53\u7cfb\u63a8\u52a8\u53d1\u73b0\u754c\u9762\u6709\u5e8f\u6c34\u7ed3\u6784<\/strong><\/p>\n<p>\u521a\u624d\u8bb2\u5230\u754c\u9762\u662f\u975e\u5e38\u91cd\u8981\uff0c\u5c24\u5176\u662f\u7535\u5316\u5b66\u4f53\u7cfb\uff0c\u4f8b\u5982\u9502\u79bb\u5b50\u5728\u7535\u6c60\u754c\u9762\u600e\u4e48\u8fdb\u53bb\u53c8\u600e\u4e48\u51fa\u6765\uff1f\u5728\u7535\u6c60\u548c\u7535\u50ac\u5316\u7684\u73af\u5883\u4e0b\uff0c\u6240\u6709\u7684\u79bb\u5b50\u90fd\u662f\u5e26\u7535\u7684\uff0c\u5e26\u7535\u79bb\u5b50\u4f1a\u6eb6\u5242\u5316\uff0c\u5982\u91d1\u5c5e\u9633\u79bb\u5b50\u8981\u4e0e\u6709\u673a\u6eb6\u5242\u548c\u6c34\u5f62\u6210\u6eb6\u5242\u5408\u591a\u9762\u4f53\uff0c\u7535\u6781\u9759\u7535\u7684\u4f5c\u7528\u4e0b\u5728\u5176\u754c\u9762\u9644\u8fd1\u4f1a\u53d8\u6210\u6709\u5e8f\u6392\u5217\u6216\u8131\u5d4c\u3002\u6211\u4eec\u8fd9\u7bc7\u5de5\u4f5c\u4e0e\u53a6\u5927\u674e\u5251\u950b\u8001\u5e08\u5408\u4f5c\uff0c\u5728\u7814\u7a76\u7535\u89e3\u6c34\u5236\u5907\u6c22\u6c14\uff0c\u53d1\u73b0\u6c34\u5728\u754c\u9762\u4e0a\u6709\u4e24\u79cd\u7ed3\u6784\u7684\u6c34\uff0c\u4e00\u79cd\u662f\u6eb6\u5242\u6c34\u5176\u672c\u8eab\u662f\u7531\u6c22\u952e\u6784\u6210\u7684\u7f51\u7edc\u7ed3\u6784\uff0c\u53e6\u4e00\u79cd\u662f4\u4e2a\u6eb6\u5242\u6c34\u4e0e\u9633\u79bb\u5b50\u914d\u4f4d\u7684\u6eb6\u5242\u5316\u6c34\uff0c\u5728\u8d1f\u7535\u4f4d\u4e0b\u7684\u8d1f\u6781\u4e0e\u6c34\u5408\u9633\u79bb\u5b50\u9759\u7535\u76f8\u4e92\u4f5c\u7528\uff0c\u628a\u6eb6\u5242\u5316\u7684\u6c34\u6709\u6548\u5730\u62c9\u5012\u7535\u6781\u754c\u9762\u5f62\u6210\u6709\u5e8f\u7684\u6392\u5217\uff0c\u5e76\u4e14\u4f7f\u5f97\u6c34\u4e0a\u5e26\u6b63\u7535\u8d28\u5b50\u4e0e\u8d1f\u6781\u7684\u6709\u6548\u8ddd\u79bb\u7f29\u77ed\uff0c\u5f62\u6210\u7535\u5b50-\u8d28\u5b50\u6709\u6548\u7684\u7535\u8377\u8f6c\u79fb\uff0c\u5b9e\u73b0\u66f4\u6709\u6548\u5730\u6c34\u5206\u89e3\u4ea7\u751f\u6c22\u6c14\u3002\u603b\u4e4b\uff0c<strong>\u539f\u5b50\u5c3a\u5ea6\u539f\u4f4d\u53d1\u73b0\u7535\u89e3\u8d28<\/strong><strong>\u6eb6\u5242\u5728\u7535\u6781\u754c\u9762\u7684\u6709\u5e8f\u7ed3\u6784\uff0c<\/strong><strong>\u5bf9\u5236\u6c22\/\u71c3\u6599\u7535\u6c60\u548c\u9ad8\u529f\u7387\u9502\u7535\u6c60\u6709\u91cd\u8981\u6307\u5bfc\u610f\u4e49\u3002<\/strong><\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u65b0\u8303\u5f0f@\u65b0\u6750\u6599<\/strong><\/p>\n<p>\u4e0b\u9762\u603b\u7ed3\u4e00\u4e0b\u6750\u6599\u7814\u7a76\u7684\u65b0\u8303\u5f0f\uff0c\u878d\u5408\u5927\u6570\u636e\u3001\u6750\u6599\u57fa\u56e0\u3001\u77e5\u8bc6\u56fe\u8c31\u53ef\u4ee5\u52a0\u901f\u65b0\u6750\u6599\u7684\u7814\u7a76\u4e0e\u5f00\u53d1\uff0c\u901a\u8fc7\u6784\u5efa\u9502\u7535\u6c60\u57fa\u56e0\u5927\u6570\u636e\u662f\u52a0\u901f\u9ad8\u6027\u80fd\u6750\u6599\u7814\u53d1\u7684\u65b0\u8303\u5f0f \u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u57fa\u4e8e\u56fe\u8bba\u548c\u6750\u6599\u5927\u6570\u636e \u00a0\u521b\u5efa\u6676\u4f53\u7ed3\u6784\u89e3\u6790\u7cfb\u7edf<\/strong><\/p>\n<p>\u8fd8\u6709\u4e00\u4e2a\u4e8b\u60c5\u8ddf\u5927\u5bb6\u6c47\u62a5\u4e00\u4e0b\uff0c\u73b0\u5728\u6709\u4e9b\u56fd\u5bb6\u5bf9\u6211\u4eec\u5b9e\u884c\u79d1\u6280\u8f6f\u4ef6\u7684\u7981\u8fd0\uff0c\u5305\u62ec\u4e24\u4e09\u4e2a\u7269\u8d28\u7ed3\u6784\u5206\u6790\u8f6f\u4ef6\uff0c\u8fd9\u4e9b\u5206\u6790\u8f6f\u4ef6\u7684\u529f\u80fd\u662f\u4ece\u6750\u6599\u7684x\u5c04\u7ebf\u884d\u5c04\u6570\u636e\u6a21\u62df\u548c\u5224\u65ad\u51fa\u7269\u76f8\u3001\u89e3\u51fa\u57fa\u672c\u7ed3\u6784\u548c\u7cbe\u4fee\u7ed3\u6784\u5b58\u5728\u7684\u7f3a\u9677\uff0c\u8fd9\u4e9b\u7ed3\u6784\u5206\u6790\u8f6f\u4ef6\u7528\u7684\u662f\u6211\u4eec\u4e0a\u9762\u8bb2\u79d1\u5b66\u8303\u5f0f\u7684\u7b2c\u4e09\u4e2a\u8303\u5f0f\u2014\u57fa\u4e8e\u6a21\u62df\u548c\u8ba1\u7b97\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u6750\u6599\u57fa\u56e0\u5927\u6570\u636e@ \u7ed3\u6784\u89e3\u6790\uff08\u65b0\u8303\u5f0f\u89e3\u51b3\u6676\u4f53\u7ed3\u6784\u8f6f\u4ef6\u5361\u8116\u5b50\u7684\u6311\u6218\uff09<\/strong><\/p>\n<p>\u6211\u4eec\u65e2\u7136\u6709\u4e86\u6750\u6599\u57fa\u56e0\u5927\u6570\u636e\uff0c\u53ef\u4ee5\u7528\u7b2c\u56db\u4e2a\u65b0\u8303\u5f0f\u2014\u57fa\u4e8e\u5927\u6570\u636e\u9a71\u52a8\u7684\u89e3\u51b3\u65b9\u6848\uff0c\u5c06\u5176\u7528\u4e8e\u7684\u6750\u6599\u7ed3\u6784\u89e3\u6790\uff0c\u878d\u5408\u6750\u6599\u5927\u6570\u636e\u3001\u4eba\u5de5\u667a\u80fd\u548c\u6750\u6599\u57fa\u56e0\uff0c\u6211\u4eec\u81ea\u4e3b\u53d1\u5c55\u7269\u8d28\u7ed3\u6784\u7684\u89e3\u6790\u7684\u7cfb\u7edf\uff0c\u73b0\u5728\u653e\u5728\u7f51\u4e0a\uff08www.pkusam.com\uff09\u7ed9\u5927\u5bb6\u516c\u5f00\u514d\u8d39\u8bd5\u7528\uff0c\u4f60\u53ea\u8981\u628ax\u5c04\u7ebf\u884d\u5c04\u6570\u636e\u53ca\u5176\u5316\u5b66\u5143\u7d20\u7ec4\u6210\u8f93\u8fdb\u8be5\u89e3\u6790\u7cfb\u7edf\uff0c\u5c31\u53ef\u4ee5\u81ea\u52a8\u7684\u5f97\u5230\u7269\u76f8\u4fe1\u606f\u548c\u7ed3\u6784\u7684\u539f\u5b50\u4f4d\u7f6e\u3002\u6211\u4eec\u7684\u539f\u7406\u7c7b\u4f3c\u4e8e\u73b0\u5728\u7ecf\u5e38\u7528\u7684\u201c\u4eba\u8138\u8bc6\u522b\u201d\u2014\u8fd0\u7528\u4eba\u5de5\u667a\u80fd\u7b97\u6cd5\u628a\u88ab\u68c0\u6d4b\u7684\u7279\u5f81\u6570\u636e\u63d0\u53d6\u4e0e\u5927\u6570\u636e\u8fdb\u884c\u667a\u80fd\u6bd4\u5bf9\uff0c\u8fdb\u884c\u5feb\u901f\u7684\u8bc6\u522b\uff08\u800c\u4e0d\u662f\u6a21\u62df\uff09\u3002\u00a0\u6211\u4eec\u7528\u65b0\u7684\u8303\u5f0f\u89e3\u51b3\u4e86\u56fd\u5bb6\u79d1\u6280\u8f6f\u4ef6\u4e00\u4e2a\u5361\u8116\u5b50\u95ee\u9898\uff0c\u540c\u65f6\u53ef\u4ee5\u52a0\u901f\u5927\u5bb6\u7684\u6750\u6599\u7814\u7a76\u3002<\/p>\n<p><strong>&gt;&gt;&gt;\u00a0\u5c55\u671b\uff1a\u56fe\u8bba@\u7ed3\u6784\u5316\u5b66 vs \u65b0\u6750\u6599<\/strong><\/p>\n<p>\u52a0\u901f\u6750\u6599\u7814\u7a76\uff0c\u53ef\u4ee5\u540c\u65f6\u8fdb\u884c\u6b63\u5411\uff08\u81ea\u4e0b\u800c\u4e0a\uff09\u65b9\u6cd5\uff0c\u4ece\u5e95\u5c42\u7684\u7269\u8d28\u7ed3\u6784\uff08\u539f\u5b50\u7ed3\u6784\u4e0e\u7535\u5b50\u7ed3\u6784\uff09\u3001\u7ed3\u6784\u5927\u6570\u636e\u7ed3\u5408\u4eba\u5de5\u667a\u80fd\u7b97\u6cd5\u3001\u7531\u7ed3\u6784\u57fa\u5143\u53ca\u5176\u6392\u5e8f\u4e0e\u76f8\u4e92\u4f5c\u7528\u7684\u6750\u6599\u57fa\u56e0\u5230\u65b0\u6750\u6599\u7684\u8bbe\u8ba1\u4e0e\u8ba1\u7b97\u53ca\u5176\u5236\u5907\u4e0e\u8868\u5f81\u3002\u540c\u65f6\u53ef\u4ee5\u8fdb\u884c\u9006\u5411\u8bbe\u8ba1\uff0c\u4ece\u9700\u6c42\u51fa\u53d1\u6765\u8bbe\u8ba1\u6750\u6599\uff0c\u5bfb\u627e\u9002\u5408\u7684\u529f\u80fd\u7ed3\u6784\u57fa\u5143\u4e0e\u76f8\u5173\u7684\u5143\u7d20\u53ca\u5176\u5b83\u4eec\u7684\u6392\u5e8f\u548c\u76f8\u4e92\u4f5c\u7528\u3002\u7136\u540e\u8fdb\u884c\u53ef\u63a7\u5236\u5907\u548c\u6d4b\u91cf\u7ed3\u6784\u4e0e\u6027\u80fd\uff0c\u770b\u662f\u5426\u4e0e\u9884\u60f3\u7684\u4e00\u81f4\uff0c\u7279\u522b\u662f\u8fd0\u7528\u540c\u6b65\u8f90\u5c04x\u5c04\u7ebf\u548c\u4e2d\u5b50\u5927\u79d1\u5b66\u88c5\u7f6e\u8fdb\u884c\u539f\u4f4d\u4e0e\u975e\u539f\u4f4d\u7684\u9ad8\u7cbe\u5ea6\u6d4b\u91cf\u6750\u6599\u5236\u5907\u53ca\u5176\u5e94\u7528\u8fc7\u7a0b\u4e2d\u7684\u7ed3\u6784\u6f14\u5316\u3002\u603b\u4e4b\uff0c\u8fd9\u79cd\u57fa\u4e8e\u56fe\u8bba\u7ed3\u6784\u5316\u5b66\u548c\u6750\u6599\u5927\u6570\u636e\u3001\u5927\u79d1\u5b66\u88c5\u7f6e\u7b49\u5f00\u5c55\u6b63\u5411\u548c\u9006\u5411\u7684\u9884\u6d4b\u4e0e\u5b9e\u9a8c\u7684\u5faa\u73af\u8fed\u4ee3\uff0c\u662f\u52a0\u901f\u65b0\u6750\u6599\u4ece\u57fa\u7840\u7814\u7a76\u548c\u4ea7\u4e1a\u5e94\u7528\u7684\u65b0\u8303\u5f0f\u3002<\/p>\n<section data-role=\"paragraph\"><\/section>\n<section data-role=\"paragraph\"><\/section>\n<section data-role=\"paragraph\"><\/section>\n<section data-role=\"paragraph\"><\/section>\n","protected":false},"excerpt":{"rendered":"<p>\u8c22\u8c22\u6750\u6599\u4eba\u7684\u9080\u8bf7\uff0c\u4e5f\u611f\u8c22\u5927\u5bb6\u5728\u5468\u672b\u65f6\u95f4\u6765\u542c\u6211\u4eec\u5317\u4eac\u5927\u5b66\u6df1\u5733\u7814\u7a76\u751f\u9662\u65b0\u6750\u6599\u5b66\u9662\u56e2\u961f\u5728\u65b0\u80fd\u6e90\u6750\u6599\u7684\u7814\u7a76\u65b0\u8303\u5f0f\u65b9\u9762\u7684\u63a2\u7d22\u601d\u8003\u548c\u8fdb\u5c55\u3002 &gt;&gt;&gt;\u00a0 \u6750\u6599&#8230;<\/p>\n","protected":false},"author":2,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[1187],"tags":[],"class_list":["post-236897","post","type-post","status-publish","format-standard","hentry","category-zhuanlan"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/236897"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/2"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=236897"}],"version-history":[{"count":11,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/236897\/revisions"}],"predecessor-version":[{"id":237036,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/236897\/revisions\/237036"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=236897"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=236897"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=236897"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}