{"id":238092,"date":"2022-06-04T07:46:06","date_gmt":"2022-06-03T23:46:06","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=238092"},"modified":"2022-06-03T21:50:47","modified_gmt":"2022-06-03T13:50:47","slug":"%e5%8c%97%e5%a4%a7%e5%92%8c%e5%8c%97%e7%a7%91%e5%a4%a7%e5%bc%ba%e5%bc%ba%e8%81%94%e6%89%8b%ef%bc%8c%e5%9c%a8nature%e5%a4%a7%e5%ad%90%e5%88%8a%e5%8f%91%e8%a1%a8%e9%87%8d%e9%87%8f%e7%ba%a7%e6%88%90","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=238092","title":{"rendered":"\u5317\u5927\u548c\u5317\u79d1\u5927\u5f3a\u5f3a\u8054\u624b\uff0c\u5728Nature\u5927\u5b50\u520a\u53d1\u8868\u91cd\u91cf\u7ea7\u6210\u679c"},"content":{"rendered":"<ol>\n<li><strong>\u5bfc\u8bfb<\/strong><\/li>\n<\/ol>\n<p>\u5728\u6838\u53cd\u5e94\u5806\u670d\u5f79\u7684\u6750\u6599\u8981\u7ecf\u53d7\u975e\u5e38\u4e25\u82db\u7684\u73af\u5883\uff0c\u8fd9\u4e0d\u53ef\u907f\u514d\u7684\u4f1a\u5bfc\u81f4\u6750\u6599\u7ed3\u6784\u5b8c\u6574\u6027\u548c\u529b\u5b66\u6027\u80fd\u7684\u9000\u5316\uff0c\u4f8b\u5982\u5b8f\u89c2\u5b54\u6d1e\u81a8\u80c0\u3001\u8f90\u5c04\u786c\u5316\u548c\u8106\u5316\u3002\u8bbe\u8ba1\u51fa\u5728\u8fd9\u79cd\u4e25\u82db\u6761\u4ef6\u4e0b\u80fd\u591f\u5e78\u5b58\u7684\u6750\u6599\u5bf9\u4e8e\u5ef6\u957f\u53cd\u5e94\u5806\u5bff\u547d\uff0c\u4fc3\u8fdb\u6838\u805a\u53d8\u548c\u5148\u8fdb\u6838\u88c2\u53d8\u53cd\u5e94\u5806\u7684\u53d1\u5c55\u975e\u5e38\u91cd\u8981\uff0c\u4f46\u5374\u4e00\u76f4\u5145\u6ee1\u6311\u6218\u3002\u80fd\u591f\u5728\u9ad8\u6e29\u4e0b\u7ef4\u6301\u9ad8\u8f90\u5c04\u5242\u91cf\u7684\u6750\u6599\u662f\u4e0b\u4e00\u4ee3\u88c2\u53d8\u548c\u672a\u6765\u805a\u53d8\u80fd\u6240\u5fc5\u9700\u7684\u3002\u8fc4\u4eca\u4e3a\u6b62\uff0c\u5373\u4f7f\u662f\u6700\u6709\u524d\u9014\u7684\u7ed3\u6784\u6750\u6599\u4e5f\u4e0d\u80fd\u627f\u53d7\u8f90\u5c04\u73af\u5883\u8981\u6c42\uff0c\u56e0\u4e3a\u4e0d\u53ef\u9006\u7684\u8f90\u5c04\u5c06\u9a71\u52a8\u5fae\u89c2\u7ed3\u6784\u9000\u5316\u3002<\/p>\n<p>\u8f90\u5c04\u5f15\u8d77\u7684\u6750\u6599\u9000\u5316\u901a\u5e38\u662f\u7531\u4e8e\u8fc7\u591a\u7684\u95f4\u9699\u548c\u7a7a\u4f4d\u7684\u4ea7\u751f\u548c\u968f\u540e\u7684\u805a\u96c6\u9020\u6210\u7684\u3002\u5176\u4e2d\uff0c\u7a7a\u7a74\u81a8\u80c0\u662f\u9ad8\u6e29\u4e0b\u9ad8\u5242\u91cf\u8f90\u5c04\u5bf9\u6750\u6599\u7684\u5173\u952e\u8f90\u5c04\u964d\u89e3\u6548\u5e94\u4e4b\u4e00\uff0c\u901a\u5e38\u6d89\u53ca\u7a7a\u4f4d\u7684\u5f62\u6210\u548c\u9010\u6e10\u805a\u96c6\u3002\u6297\u7a7a\u6d1e\u81a8\u80c0\u80fd\u529b\u7684\u589e\u5f3a\u901a\u5e38\u5f52\u56e0\u4e8e\u9ad8\u6bd4\u4f8b\u7684\u5931\u914d\u754c\u9762\uff0c\u5176\u53ef\u4ee5\u902e\u6355\u8f90\u5c04\u5f15\u8d77\u7684\u95f4\u9699\u548c\u7a7a\u4f4d\u3002\u672c\u6587\u63d0\u51fa\u7684\u7b56\u7565\u4f9d\u8d56\u4e8e\u4e0d\u5339\u914d\u7684\u754c\u9762\u6765\u6355\u83b7\u7f3a\u9677\uff0c\u800c\u662f\u5229\u7528\u5b8c\u5168\u5171\u683c\u7684\u91d1\u5c5e\u95f4\u5316\u5408\u7269\u7eb3\u7c73\u6c89\u6dc0\u7269(NPs)\u7684\u5feb\u901f\u8dc3\u8fc1\u52a8\u529b\u5b66\u6765\u589e\u5f3a\u8f90\u5c04\u8010\u53d7\u6027\uff0cNPs\u7684\u5faa\u73af\u65e0\u5e8f-\u6709\u5e8f\u8fc7\u7a0b\u6709\u6548\u5730\u6e6e\u706d\u4e86\u7f3a\u9677\uff0c\u5927\u5927\u63d0\u9ad8\u4e86\u8010\u8f90\u5c04\u6027\u3002<\/p>\n<ol start=\"2\">\n<li><strong>\u6210\u679c\u63a0\u5f71<\/strong><\/li>\n<\/ol>\n<p>\u8fd1\u65e5\uff0c\u5317\u4eac\u79d1\u6280\u5927\u5b66\u5415\u662d\u5e73\u6559\u6388\u56e2\u961f\uff0c\u5317\u4eac\u5927\u5b66\u4ed8\u6069\u521a\u6559\u6388\u56e2\u961f\u5f3a\u5f3a\u5408\u4f5c\uff0c\u62a5\u9053\u4e86\u4e00\u79cd\u4e0e\u5e38\u7406\u76f8\u53cd\u7684\u7b56\u7565\uff0c\u5229\u7528\u7eb3\u7c73\u4f4e\u9519\u914d\u5171\u683c\u6c89\u6dc0\u9a6c\u6c0f\u4f53\u65f6\u6548\u94a2\uff0c\u53d1\u660e\u4e86\u4e00\u79cd\u65b0\u7684\u8010\u8f90\u5c04\u673a\u5236\uff0c\u5927\u5e45\u5ea6\u63d0\u9ad8\u4e86\u5408\u91d1\u7684\u6297\u8f90\u5c04\u80fd\u529b\u3002\u672c\u5de5\u4f5c\u53d7\u9650\u5728\u9a6c\u6c0f\u4f53\u65f6\u6548\u94a2\u4e2d\u5f15\u5165\u7684\u8d85\u6676\u683c\u7eb3\u7c73\u6c89\u6dc0\u7269\uff0c\u8fd9\u79cd\u7ed3\u6784\u7684\u6b8a\u80dc\u4e4b\u5904\u662f\u5728\u7eb3\u7c73\u6c89\u6dc0\u7269\u9644\u8fd1\u53ef\u8bf1\u5bfc\u7ed3\u6784\u53ef\u9006\u7684\u5c40\u90e8\u65e0\u5e8f-\u6709\u5e8f\u8f6c\u53d8\u3002\u7814\u7a76\u8868\u660e\uff1a\u5728\u542b\u6709\u9ad8\u5bc6\u5ea6B2\u6709\u5e8f\u8d85\u6676\u683c\u7684\u9a6c\u6c0f\u4f53\u94a2\u4e2d\uff0c\u5373\u4f7f\u5728400-600\u00b0C\u7684\u8d85\u9ad8\u5242\u91cf\u8f90\u5c04\u635f\u4f24\u540e\uff0c\u4e5f\u6ca1\u6709\u68c0\u6d4b\u5230\u7a7a\u6d1e\u81a8\u80c0\u3002\u5728\u9ad8\u5ea6\u9971\u548c\u7684\u57fa\u4f53\u4e2d\uff0c\u4f4e\u9519\u914d\u8d85\u6676\u683c\u7684\u91cd\u65b0\u6709\u5e8f\u8fc7\u7a0b\u53d1\u751f\u5728\u5feb\u901f\u7684\u65e0\u5e8f\u5316\u4e4b\u540e\u3002\u8fd9\u6837\uff0c\u901a\u8fc7\u8f90\u5c04\u8bf1\u53d1\u7684\u70b9\u7f3a\u9677\u548c\u8fc7\u5269\u6eb6\u8d28\u7684\u4f1a\u53d1\u751f\u77ed\u7a0b\u91cd\u65b0\u6709\u5e8f\u3002\u8fd9\u4e00\u52a8\u6001\u8fc7\u7a0b\u7a33\u5b9a\u4e86\u5fae\u89c2\u7ed3\u6784\uff0c\u4e0d\u65ad\u4fc3\u8fdb\u539f\u4f4d\u7f3a\u9677\u590d\u5408\uff0c\u5e76\u6709\u6548\u5730\u963b\u6b62\u4e86\u957f\u7a0b\u6269\u6563\u8fc7\u7a0b\u3002\u4ece\u800c\u5927\u5e45\u5ea6\u63d0\u9ad8\u4e86\u6750\u6599\u7684\u8010\u8f90\u5c04\u6027\u80fd\u3002\u8be5\u7b56\u7565\u53ef\u5e94\u7528\u4e8e\u5176\u4ed6\u6750\u6599\uff0c\u4e3a\u5f00\u53d1\u9ad8\u8010\u8f90\u5c04\u6750\u6599\u94fa\u5e73\u4e86\u9053\u8def\u3002\u76f8\u5173\u6210\u679c\u4ee5\u201cSuperior radiation tolerance via reversible disordering\u2013ordering transition of coherent superlattices\u201d\u4e3a\u9898\u53d1\u8868\u5728\u6750\u6599\u5b66\u9876\u7ea7\u671f\u520a\u300aNature Materials\u300b\u4e0a.<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-238093\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/\u5c01\u9762.png\" alt=\"\" width=\"1589\" height=\"648\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/\u5c01\u9762.png 1589w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/\u5c01\u9762-300x122.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/\u5c01\u9762-768x313.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/\u5c01\u9762-1024x418.png 1024w\" sizes=\"(max-width: 1589px) 100vw, 1589px\" \/><\/p>\n<p>\u8bba\u6587\u94fe\u63a5\uff1a<a href=\"https:\/\/www.nature.com\/articles\/s41563-022-01260-y.pdf\">https:\/\/www.nature.com\/articles\/s41563-022-01260-y.pdf<\/a><\/p>\n<p><strong>3.\u6838\u5fc3\u521b\u65b0\u70b9<\/strong><\/p>\n<p>(1) \u53d1\u660e\u4e86\u4e00\u79cd\u5927\u5e45\u5ea6\u63d0\u9ad8\u6297\u8f90\u7167\u6027\u80fd\u7684\u65b0\u673a\u5236\u2014\u53ef\u9006\u65e0\u5e8f\u5316-\u6709\u5e8f\u5316\u8f6c\u53d8\uff1b<\/p>\n<p>\uff082\uff09\u63d0\u4f9b\u4e86\u8fd9\u4e00\u79cd\u5408\u6210\u8010\u8f90\u7167\u6750\u6599\u7684\u65b0\u9014\u5f84\uff1b<\/p>\n<p><strong>4. \u6570\u636e\u6d4f\u89c8<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-238094\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/1-2.png\" alt=\"\" width=\"1582\" height=\"688\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/1-2.png 1582w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/1-2-300x130.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/1-2-768x334.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/1-2-1024x445.png 1024w\" sizes=\"(max-width: 1582px) 100vw, 1582px\" \/><\/p>\n<p>\u56fe1 \u542b\u9ad8\u5bc6\u5ea6Ni(Al,Fe) NPs\u7684\u8d85\u6676\u683c\u94a2\u5177\u6709\u4f18\u826f\u7684\u8f90\u5c04\u8010\u53d7\u6027\u3002b\u548cc\u7684\u6bd4\u8f83\u8868\u660e\uff0c\u8d85\u6676\u683c\u94a2\u7684\u6297\u7a7a\u9699\u81a8\u80c0\u6027\u80fd\u6bd49Cr ODS\u94a2\u5f3a\u5f97\u591a\uff1ba. \u4e0e\u4f20\u7edf\u5965\u6c0f\u4f53\u94a2\u3001\u94c1\u7d20\u4f53\u9a6c\u6c0f\u4f53\u94a2\u548cODS\u94a2\u76f8\u6bd4\uff0c\u8d85\u6676\u683c\u94a2\u4e2d\u7684\u7a7a\u9699\u81a8\u80c0\u73b0\u8c61\u66f4\u4e3a\u660e\u663e\uff0c\u63d2\u56fe(\u865a\u7ebf\u77e9\u5f62\u6846\u7684\u653e\u5927\u89c6\u56fe)\u663e\u793a\uff0c\u4e0e\u51e0\u79cd\u5178\u578b\u7684ODS\u94a2\u76f8\u6bd4\uff0c\u8d85\u6676\u683c\u94a2\u5448\u73b0\u96f6\u7a7a\u6d1e\u81a8\u80c0\uff1bb. 500\u2103\u65f6\uff0c\u8d85\u6676\u683c\u94a2\u57282350 dpa\u540e\u6761\u4ef6\u4e0b\u8f90\u5c04\u635f\u4f24\u540e\u7684TEM\u663e\u5fae\u56fe\uff0c\u672a\u89c1\u7a7a\u6d1e\u4ea7\u751f\uff1bc. 500\u2103\u65f6\uff0c9Cr ODS\u94a2\u5728840 dpa\u540e\u6761\u4ef6\u4e0b\u8f90\u5c04\u635f\u4f24\u540e\u7684TEM\u663e\u5fae\u56fe\uff0c\u89c2\u5bdf\u5230\u5927\u91cf\u7a7a\u6d1e\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-238095\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/2-2.png\" alt=\"\" width=\"2101\" height=\"2401\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/2-2.png 2101w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/2-2-263x300.png 263w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/2-2-768x878.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/2-2-896x1024.png 896w\" sizes=\"(max-width: 2101px) 100vw, 2101px\" \/><\/p>\n<p>\u56fe2 \u79bb\u5b50\u8f90\u7167\u4e0b\u8d85\u6676\u683c\u94a2\u7684\u7ec4\u7ec7\u6f14\u53d8\uff1ba,b\uff0c\u8d85\u6676\u683c\u94a2\u5728500\u21030 dpa (a)\u548c840 dpa (b)\u4e0b\u7684HAADF-STEM\u56fe\u50cf\uff1bc,d\uff0c\u9ad8\u5206\u8fa8\u7387HAADF-STEM\u56fe\u50cf\u663e\u793a\u4e86NPs\u548c\u5bcc\u6eb6\u8d28\u533a\u57df\u4e4b\u95f4\u7684\u539f\u5b50\u7ed3\u6784\u5dee\u5f02\uff1be, APT\u8868\u5f81\u7684NPs\u5728\u79bb\u5b50\u8f90\u7167\u8fc7\u7a0b\u4e2d\u7684\u6f14\u5316\uff0c\u4e3b\u8981\u901a\u8fc750at%Al\u548cNi\u7b49\u6d53\u5ea6\u8868\u9762\u663e\u793a\u548c\u5f3a\u8c03\uff1bf,g\uff0c\u8ddd\u79bb\u76f4\u65b9\u56fe\u663e\u793a\u4e86\u6240\u9009\u6c89\u6dc0(f)\u548c\u6eb6\u8d28\u5bcc\u96c6\u533a\u57df(g)\u7684\u6210\u5206\u8f6e\u5ed3\uff0c\u5176\u4e2d\u8bef\u5dee\u6761\u662f\u5747\u503c\u7684\u6807\u51c6\u504f\u5dee\uff1bh, HAADF-STEM\u56fe\u50cf\u663e\u793a\u4e86500\u00b0C\/840 dpa\u8f90\u7167\u540e\u4f4d\u9519\u73af\u7684\u5b58\u5728\uff1bi\uff0c\u9ad8\u5206\u8fa8\u7387HAADF-STEM\u56fe\u50cf\uff0c\u663e\u793a\u4f4d\u9519\u73af\u9644\u8fd1\u5b58\u5728NPs\uff0c\u4ee5\u53ca\u76f8\u5e94\u7684FFT\u7ed3\u679c(\u53f3\u84dd\u7ea2\u6846)\uff1bj, HAADF\u56fe\u50cf\u663e\u793a\u4e00\u4e2a\u201c\u6108\u5408\u201d\u7684a\/2&lt;100&gt;\u4f4d\u9519\u73af\u8fdc\u79bb\u6790\u51fa\u7269\uff1bk,l\uff0c\u5bf9\u5e94Ni (k)\u548cAl (l)\u7684EDS\u9762\u626b\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-238096\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/3-2.png\" alt=\"\" width=\"1826\" height=\"1403\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/3-2.png 1826w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/3-2-300x231.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/3-2-768x590.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/3-2-1024x787.png 1024w\" sizes=\"(max-width: 1826px) 100vw, 1826px\" \/><\/p>\n<p>\u56fe3 \u8d85\u6676\u683c\u94a2\u4e2dNPs\u7684\u8f90\u5c04\u8bf1\u5bfc\u6eb6\u89e3\u673a\u7406\uff1ba-c\uff0c\u6765\u81eaAPT\u6570\u636e\u96c6\u7684\u4e9a\u4f53\u79ef(7 nm \u00d7 7 nm \u00d7 1 nm)\uff0c\u663e\u793a\u4e86\u5ba4\u6e29\u4e0b\u79bb\u5b50\u8f90\u7167\u524d\u540eNPs\u7684\u6210\u5206\u6f14\u53d8\u3002d,e\uff0c\u8fd1\u8ddd\u79bb\u76f4\u65b9\u56fe\u663e\u793a\u4e86\u79bb\u5b50\u8f90\u7167\u524d\u540eNPs\u4e2dNi (d)\u548cAl (e)\u7684\u6210\u5206\u5206\u5e03\u3002\u8bef\u5dee\u6761\u662f\u5747\u503c\u7684\u6807\u51c6\u504f\u5dee\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-238097\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/4-2.png\" alt=\"\" width=\"1270\" height=\"791\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/4-2.png 1270w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/4-2-300x187.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/4-2-768x478.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/4-2-1024x638.png 1024w\" sizes=\"(max-width: 1270px) 100vw, 1270px\" \/><\/p>\n<p>\u56fe4 \u65f6\u6548\u8fc7\u7a0b\u4e2dNPs\u7684\u5feb\u901f\u5f62\u6210\u52a8\u529b\u5b66\uff1ba\uff0c\u540c\u6b65XRD\u7ed3\u679c\u663e\u793a\uff0c\u5728500\u00b0C\u65f6\u6548\u8fc7\u7a0b\u4e2d\uff0c\u968f\u7740\u65f6\u95f4\u7684\u63a8\u79fb\u5f62\u6210\u4e86NPs\u3002b, x\u5c04\u7ebf\u884d\u5c04\u8c31\u653e\u5927\u56fe\u663e\u793a\u5728500\u00b0C\u65f6\u6548\u8fc7\u7a0b\u4e2dB2\u7684\u5cf0\u53d8\u5bbd\uff1bc\uff0c\u5bf9\u5e94\u7684\u5cf0\u5f3a\u6bd4\u8868\u660eNPs\u7684\u6790\u51fa\u901f\u5ea6\u975e\u5e38\u5feb\u3002\u5176\u4e2dI<sup>t<\/sup> 100\u3001I<sup>f<\/sup> 100\u3001I<sup>t <\/sup>200\u548cI<sup>f <\/sup>200\u5206\u522b\u8868\u793at\u65f6\u523b(100)\u548c\u672b\u6001(200)\u7684\u5cf0\u503c\u5f3a\u5ea6\u3002d\u3001\u5bf9\u8be5\u94a2\u5728500\u2103\u65f6\u65483 h(\u5373\u8d85\u6676\u683c\u94a2\u7684\u5e73\u8861\u6001\u5904\u7406)\u3001500\u2103\u65f6\u654810 min\u548c500\u2103840 dpa\u8f90\u5c04\u4e09\u79cd\u4e0d\u540c\u6761\u4ef6\u4e0b\u7684APT\u5206\u6790\u5f97\u5230\u7684B2\u76f8\u7ec4\u6210\u3002e\uff0c\u5728500\u2103\u4e0b\u65f6\u654810\u5206\u949f\u7684\u94a2\u6eb6\u8d28\u7684APT\u8868\u5f81\uff0c\u663e\u793a\u4ee5\u5361\u5176\u8272\u6807\u8bb0\u7684\u9009\u5b9aNPs\u7684\u6210\u5206\u5206\u5e03\u56fe\u7684\u90bb\u8fd1\u76f4\u65b9\u56fe(\u53f3)\u3002\u8bef\u5dee\u6761\u662f\u5747\u503c\u7684\u6807\u51c6\u504f\u5dee\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-238098\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/5-1.jpg\" alt=\"\" width=\"1270\" height=\"474\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/5-1.jpg 1270w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/5-1-300x112.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/5-1-768x287.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/5-1-1024x382.jpg 1024w\" sizes=\"(max-width: 1270px) 100vw, 1270px\" \/><\/p>\n<p>\u56fe5 \u8d85\u6676\u683c\u94a2\u4e2dNPs\u7684\u65e0\u5e8f\u548c\u91cd\u65b0\u6709\u5e8f\u8fc7\u7a0b\u968f\u65f6\u95f4\u7684\u51fd\u6570\u793a\u610f\u56fe. a-d\u3001Fe\u3001Ni\u548cAl\u539f\u5b50\u5206\u522b\u7528\u7070\u8272\u3001\u7eff\u8272\u548c\u7ea2\u8272\u7684\u7403\u6807\u8bb0<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-238099\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/6-1.jpg\" alt=\"\" width=\"1269\" height=\"995\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/6-1.jpg 1269w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/6-1-300x235.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/6-1-768x602.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/6-1-1024x803.jpg 1024w\" sizes=\"(max-width: 1269px) 100vw, 1269px\" \/><\/p>\n<p>\u56fe6 \u5f53\u524d\u7b56\u7565\u5728fcc Fe35.8Ni37.6Cr22.9Ti1.7Al2 (wt.%) MEA\u4e2d\u7684\u5e94\u7528\uff1ba, TEM\u56fe\u50cf\u663e\u793a\u4e86\u6240\u8bbe\u8ba1\u7684fcc\u5408\u91d1\u7684NPs\u3002\u63d2\u56fe\u4e3a\u76f8\u5e94\u7684SAED\uff0c\u663e\u793a\u4e86NPs\u7684\u6709\u5e8f\u7ed3\u6784\uff1bb &#8211; d\uff0c\u6cbf{110}\u533a\u62cd\u6444\u7684TEM\u56fe\u50cf\u663e\u793a\u4e86\u8bbe\u8ba1\u7684fcc\u5408\u91d1\u5728400\u00b0C (b)\u3001500\u00b0C (C)\u548c600\u00b0C (d)\u7684100 dpa\u8f90\u5c04\u540e\u7684NPs\u3002e\uff0c\u9ad8\u5206\u8fa8\u7387\u7684STEM\u56fe\u50cf\uff0c\u663e\u793a\u4e86\u8bbe\u8ba1\u7684fcc\u5408\u91d1\u5728600\u2103\u4e0b\u7ecf\u8fc7100 dpa\u8f90\u5c04\u540e\u7684NP\u7ec4\u7ec7\uff0c\u5176\u4e2d\u4e00\u4e2a\u5178\u578b\u7684NP\u7528\u7ea2\u5708\u8868\u793a\uff1bf\uff0c\u91cd\u5efa\u4e09\u7ef4APT\u6570\u636e\u96c6\uff0c\u5e76\u5206\u6790\u5728600\u2103\u4e0b\u7ecf\u5386\u4e0d\u540c\u5242\u91cf\u8f90\u5c04\u635f\u4f24\u7684NPs\u7684\u6210\u5206\u3002NPs\u7684\u91cd\u70b9\u662f\u5305\u542b\u8d85\u8fc780%\u7684Ni\u3001Al\u548cTi\u7684\u533a\u57df\uff1bg\uff0c\u5bf9\u5e94\u7684\u63a5\u8fd1\u76f4\u65b9\u56fe\u663e\u793a\u4e86\u901a\u8fc7\u5361\u5176\u8272\u6307\u793a\u7684\u9009\u5b9aNPs\u7684\u7ec4\u6210\u6982\u51b5.<\/p>\n<p><strong>5.\u6210\u679c\u542f\u8fea<\/strong><\/p>\n<p>\u672c\u6587\u63d0\u51fa\u7684\u6709\u5e8f-\u65e0\u5e8f\u5316\u673a\u5236\u662f\u63d0\u9ad8\u6838\u6750\u6599\u6297\u8f90\u7167\u6027\u80fd\u7684\u65b0\u673a\u5236\uff0c\u5177\u6709\u975e\u5e38\u91cd\u8981\u7684\u79d1\u5b66\u610f\u4e49\u548c\u5de5\u7a0b\u4ef7\u503c\u3002\u4e3a\u6297\u8f90\u7167\u6750\u6599\u7684\u5fae\u89c2\u7ed3\u6784\u8bbe\u8ba1\u63d0\u4f9b\u4e86\u4e00\u6761\u65b0\u601d\u8def\u3002<\/p>\n<p>\u672c\u6587\u7531\u865a\u8c37\u7eb3\u7269\u4f9b\u7a3f\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u5bfc\u8bfb \u5728\u6838\u53cd\u5e94\u5806\u670d\u5f79\u7684\u6750\u6599\u8981\u7ecf\u53d7\u975e\u5e38\u4e25\u82db\u7684\u73af\u5883\uff0c\u8fd9\u4e0d\u53ef\u907f\u514d\u7684\u4f1a\u5bfc\u81f4\u6750\u6599\u7ed3\u6784\u5b8c\u6574\u6027\u548c\u529b\u5b66\u6027\u80fd\u7684\u9000\u5316\uff0c\u4f8b\u5982\u5b8f\u89c2\u5b54\u6d1e\u81a8\u80c0\u3001\u8f90\u5c04\u786c\u5316\u548c\u8106\u5316\u3002\u8bbe\u8ba1\u51fa\u5728\u8fd9\u79cd\u4e25\u82db\u6761\u4ef6\u4e0b\u80fd\u591f\u5e78&#8230;<\/p>\n","protected":false},"author":34569,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-238092","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/238092"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/34569"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=238092"}],"version-history":[{"count":3,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/238092\/revisions"}],"predecessor-version":[{"id":238109,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/238092\/revisions\/238109"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=238092"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=238092"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=238092"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}