{"id":238389,"date":"2022-06-14T06:29:39","date_gmt":"2022-06-13T22:29:39","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=238389"},"modified":"2022-06-13T17:29:57","modified_gmt":"2022-06-13T09:29:57","slug":"3%e7%af%87nature%ef%bc%8c1%e7%af%87%e5%a4%a7%e5%ad%90%e5%88%8a%ef%bc%8c%e8%bf%9e%e7%bb%ad%e5%86%b2%e5%87%bb%e9%a1%b6%e5%88%8a%e7%9a%84%e6%9c%80%e5%b0%8f%e6%99%b6%e6%a0%bc%e9%94%99%e9%85%8d%e7%bb%93","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=238389","title":{"rendered":"3\u7bc7Nature\uff0c1\u7bc7\u5927\u5b50\u520a\uff0c\u8fde\u7eed\u51b2\u51fb\u9876\u520a\u7684\u6700\u5c0f\u6676\u683c\u9519\u914d\u7ed3\u6784\u8bbe\u8ba1\u601d\u60f3\u7a76\u7adf\u6709\u591a\u5f3a\uff1f"},"content":{"rendered":"<p>\u8fd1\u65e5\uff0c\u5415\u662d\u5e73\u6559\u6388\u8054\u5408\u5317\u5927\u4ed8\u6069\u521a\u6559\u6388\u56e2\u961f\u5728Nature materials\u671f\u520a\u4e0a\u53d1\u8868\u4e86\u5173\u4e8e\u57fa\u4e8e\u6700\u5c0f\u6676\u683c\u9519\u914d\u8d85\u9ad8\u5f3a\u5ea6\u94a2\u65b0\u7684\u6297\u8f90\u7167\u635f\u4f24\u673a\u5236\u7684\u91cd\u91cf\u7ea7\u7814\u7a76\u6210\u679c\u3002\u7acb\u5373\u5f15\u8d77\u5de8\u5927\u7684\u53cd\u54cd\u3002\u8be5\u8bba\u6587\u4e00\u7ecf\u53d1\u8868\uff0c\u5c31\u53d7\u5230\u4e86\u56fd\u9645\u6838\u6750\u6599\u9886\u57df\u8457\u540d\u4e13\u5bb6\u3001\u7f8e\u56fd\u6a61\u6811\u5cad\u56fd\u5bb6\u5b9e\u9a8c\u5ba4Y.W. Zhang\u7814\u7a76\u5458\u7684\u9ad8\u5ea6\u8bc4\u4ef7\u3002\u4ed6\u5728News &amp; Views\u4e13\u680f\u5728\u7ebf\u53d1\u8868\u4e86\u9898\u4e3a \u201cReassembled Nanoprecipitates Resisting Radiation\u201d\u7684\u63a8\u4ecb\u6587\u7ae0\uff0c\u8bc4\u4ef7\u201c\u8fd9\u9879\u5de5\u4f5c\u4e0d\u4ec5\u9f13\u52b1\u7814\u7a76\u4eba\u5458\u91cd\u65b0\u5ba1\u89c6\u4f9d\u8d56\u975e\u5171\u683c\u6216\u534a\u5171\u683c\u754c\u9762\u6765\u6355\u83b7\u8f90\u7167\u5f15\u8d77\u70b9\u7f3a\u9677\u7684\u7b56\u7565\uff0c\u800c\u4e14\u4e3a\u9886\u57df\u57fa\u7840\u7814\u7a76\u53d1\u5c55\uff0c\u4ee5\u53ca\u901a\u8fc7\u754c\u9762\u7a33\u5b9a\u6027\u548c\u6355\u83b7\u5f3a\u5ea6\u534f\u540c\u63a7\u5236\u6297\u8f90\u7167\u6750\u6599\u53d1\u5c55\u63d0\u4f9b\u4e86\u524d\u8fdb\u7684\u9053\u8def\uff0c\u901a\u8fc7\u4f4e\u6210\u672c\u7684\u4f20\u7edf\u65b9\u6cd5\u5c31\u53ef\u4ee5\u5236\u5907\u8fd9\u4e9b\u6750\u6599\uff0c\u610f\u5473\u7740\u5176\u5728\u5de5\u7a0b\u5e94\u7528\u4e2d\u5177\u6709\u5f88\u5f3a\u7684\u5b9e\u7528\u6027\u201d[1]\u3002\u5b9e\u9645\u4e0a\uff0c\u4e4b\u524d\u5173\u4e8e\u8fd9\u4e00\u7ed3\u6784\u8bbe\u8ba1\u6240\u7814\u7a76\u7684\u7ed3\u679c\u5c31\u5df2\u7ecf\u53d1\u88683\u7bc7Nature\uff0c\u56fd\u5185\u5916\u5bf9\u8fd9\u4e00\u7ed3\u6784\u8bbe\u8ba1\u7406\u5ff5\u53ef\u8c13\u662f\u6b23\u559c\u82e5\u72c2\uff0c\u5176\u4e0d\u4ec5\u80fd\u591f\u63d0\u9ad8\u6750\u6599\u7684\u5f3a\u97e7\u6027\u4ee5\u53ca\u6297\u8f90\u7167\u6027\u80fd\uff0c\u5728\u82e5\u5e72\u5176\u5b83\u9886\u57df\u4e5f\u5c55\u793a\u51fa\u4e86\u65fa\u76db\u7684\u751f\u547d\u529b\u3002\u4e0b\u9762\uff0c\u7b14\u8005\u5c06\u4e3a\u5927\u5bb6\u89e3\u8bfb\u8fd9\u4e9b\u91cd\u91cf\u7ea7\u7814\u7a76\u6210\u679c\uff0c\u5e76\u5bf9\u5176\u8fdb\u884c\u5c55\u671b\u3002<\/p>\n<ol>\n<li><strong>\u5b66\u672f\u5e72\u8d27<\/strong><\/li>\n<\/ol>\n<p>(1) \u57fa\u4e8e\u6700\u5c0f\u6676\u683c\u9519\u914d\u548c\u9ad8\u5bc6\u5ea6\u7eb3\u7c73\u6790\u51fa\u7684\u8d85\u5f3a\u94a2<\/p>\n<p>\u65b0\u4e00\u4ee3\u9ad8\u6027\u80fd\u7ed3\u6784\u6750\u6599\u4e3b\u8981\u7684\u53d1\u5c55\u65b9\u5411\u662f\u8f7b\u8d28\uff0c\u9ad8\u5f3a\u4ee5\u53ca\u8282\u80fd\u3002\u9a6c\u6c0f\u4f53\u65f6\u6548\u94a2\u662f\u4e00\u7c7b\u5177\u6709\u9a6c\u6c0f\u4f53\u57fa\u4f53\u548c\u7eb3\u7c73\u6790\u51fa\u9897\u7c92\u7684\u9ad8\u5f3a\u94a2\uff0c\u65b0\u4e00\u4ee3\u9ad8\u6027\u80fd\u7ed3\u6784\u6750\u6599\u7684\u91cd\u8981\u5019\u9009\u6750\u6599\u3002\u5b83\u4eec\u6770\u51fa\u7684\u5f3a\u5ea6\u4e3b\u8981\u6765\u6e90\u4e8e\u534a\u5171\u683c\u6790\u51fa\u7269\u5f15\u8d77\u7684\u9897\u7c92\u5f3a\u5316\uff0c\u8fd9\u4e9b\u5171\u683c\u6790\u51fa\u7269\u4e0d\u53ef\u907f\u514d\u5730\u5728\u4f60\u57fa\u4f53\u4e2d\u975e\u5747\u5300\u5206\u5e03\uff0c\u4ea7\u751f\u8f83\u5927\u7684\u5171\u683c\u5e94\u53d8\uff0c\u8fdb\u800c\u53ef\u80fd\u4fc3\u8fdb\u8f7d\u8377\u4e0b\u7684\u88c2\u7eb9\u840c\u751f\u3002\u672c\u5de5\u4f5c\u8bbe\u8ba1\u4e86\u57fa\u4e8e\u6700\u5c0f\u7684\u6676\u683c\u9519\u914d\u9ad8\u5bc6\u5ea6\u7eb3\u7c73\u6c89\u6dc0\u7684\u8d85\u9ad8\u5f3a\u5ea6\u94a2\u3002\u7814\u7a76\u8868\u660e\uff0c\u8fd9\u4e9b\u9ad8\u5ea6\u5206\u6563\u3001\u5b8c\u5168\u5171\u683c\u7684\u6790\u51fa\u76f8(\u5373\u6790\u51fa\u76f8\u7684\u6676\u683c\u4e0e\u5468\u56f4\u57fa\u4f53\u7684\u6676\u683c\u51e0\u4e4e\u76f8\u540c)\uff0c\u4e0e\u57fa\u4f53\u7684\u6676\u683c\u5931\u914d\u975e\u5e38\u4f4e\uff0c\u53cd\u76f8\u8fb9\u754c\u80fd\u5f88\u9ad8\uff0c\u5728\u4e0d\u727a\u7272\u5ef6\u6027\u7684\u60c5\u51b5\u4e0b\u589e\u5f3a\u4e86\u5408\u91d1\u3002\u8fd9\u79cd\u4f4e\u6676\u683c\u9519\u914d(0.03-0.04 %)\u964d\u4f4e\u4e86\u6790\u51fa\u7269\u7684\u5f62\u6838\u969c\u788d\uff0c\u4ece\u800c\u4f7f\u5177\u6709\u6781\u9ad8\u6570\u91cf\u5bc6\u5ea6(\u6bcf\u7acb\u65b9\u7c73\u8d85\u8fc710<sup>24<\/sup>)\u548c\u5c0f\u5c3a\u5bf8(\u7ea62.7 0.2\u7eb3\u7c73)\u7684\u7eb3\u7c73\u6c89\u6dc0\u7269\u6210\u4e3a\u53ef\u80fd\u5e76\u7a33\u5b9a\u4e0b\u6765\u3002\u7c92\u5b50\u5468\u56f4\u6700\u5c0f\u7684\u5f39\u6027\u5931\u914d\u5e94\u53d8\u5bf9\u4f4d\u9519\u76f8\u4e92\u4f5c\u7528\u6ca1\u6709\u592a\u5927\u7684\u8d21\u732e\uff0c\u4f20\u7edf\u4e0a\u8fd9\u901a\u5e38\u662f\u63d0\u9ad8\u5f3a\u5ea6\u7684\u4e3b\u8981\u7b56\u7565\u3002\u76f8\u53cd\uff0c\u672c\u5de5\u4f5c\u7684\u5f3a\u5316\u673a\u5236\u5229\u7528\u4e86\u5f53\u6790\u51fa\u76f8\u88ab\u4f4d\u9519\u5207\u5272\u65f6\u4ea7\u751f\u80cc\u5e94\u529b(\u53cd\u5bf9\u53d8\u5f62\u7684\u529b)\u7684\u5316\u5b66\u987a\u5e8f\u6548\u5e94\u3002\u4ece\u800c\u521b\u9020\u4e86\u4e00\u7c7b\u7531Ni(Al,Fe)\u6c89\u6dc0\u7269\u5f3a\u5316\u7684\u94a2\uff0c\u5176\u5f3a\u5ea6\u9ad8\u8fbe2.2GPa\uff0c\u5ef6\u5c55\u6027\u826f\u597d(\u7ea68.2%)\u3002\u4e0e\u4f20\u7edf\u7684\u9a6c\u6c0f\u4f53\u65f6\u6548\u94a2\u76f8\u6bd4\uff0c\u6790\u51fa\u76f8\u7684\u5316\u5b66\u6210\u5206\u4f7f\u6210\u672c\u5927\u5e45\u964d\u4f4e\uff0c\u56e0\u4e3a\u5b83\u7528\u5ec9\u4ef7\u800c\u8f7b\u7684\u94dd\u53d6\u4ee3\u4e86\u5fc5\u8981\u7684\u4f46\u6210\u672c\u5f88\u9ad8\u7684\u5408\u91d1\u5143\u7d20\u94b4\u548c\u949b\u3002\u8fd9\u7c7b\u94a2\u5408\u91d1\u7684\u5f3a\u5316\u662f\u57fa\u4e8e\u6700\u5c0f\u7684\u6676\u683c\u9519\u914d\u6765\u5b9e\u73b0\u6700\u5927\u7684\u6790\u51fa\u76f8\u5f25\u6563\u548c\u9ad8\u5207\u5e94\u529b(\u4f4d\u9519\u5207\u5272\u5171\u683c\u6790\u51fa\u76f8\u5e76\u56e0\u6b64\u4ea7\u751f\u5851\u6027\u53d8\u5f62\u6240\u9700\u7684\u5e94\u529b)\uff0c\u8fd9\u79cd\u6676\u683c\u9519\u914d\u8bbe\u8ba1\u6982\u5ff5\u53ef\u4ee5\u5e94\u7528\u4e8e\u8bb8\u591a\u5176\u4ed6\u91d1\u5c5e\u5408\u91d1\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-238390\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/1-5.png\" alt=\"\" width=\"791\" height=\"778\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/1-5.png 791w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/1-5-300x295.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/1-5-768x755.png 768w\" sizes=\"(max-width: 791px) 100vw, 791px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>1 <\/strong><strong>\u9a6c\u6c0f\u4f53\u65f6\u6548\u94a2<\/strong><strong>(Al<\/strong><strong>\u3001<\/strong><strong>Fe)<\/strong><strong>\u56fa\u6eb6\u9000\u706b<\/strong><strong>(950\u00b0C\/15min)<\/strong><strong>\u548c\u65f6\u6548<\/strong><strong>(500\u00b0C\/3h)<\/strong><strong>\u7684\u529b\u5b66\u6027\u80fd\u548c\u5178\u578b\u7684<\/strong><strong>STEM<\/strong><strong>\u56fe\u50cf\uff1b<\/strong><strong>a<\/strong><strong>\u3001\u62c9\u4f38\u66f2\u7ebf\u3001\u5c48\u670d\u5e94\u529b\u589e\u91cf\u548c\u5747\u5300\u4f38\u957f\u7387\u7684\u53d8\u5316\uff1b<\/strong><strong>b<\/strong><strong>\uff0c\u5e38\u89c4\u9a6c\u6c0f\u4f53\u65f6\u6548\u94a2\u65f6\u6548\u540e\u7684\u6297\u62c9\u5f3a\u5ea6\u548c\u5851\u6027\u53d8\u5316\uff1b<\/strong><strong>c, d<\/strong><strong>\uff0c\u5206\u522b\u4e3a\u56fa\u6eb6\u9000\u706b\u548c\u65f6\u6548\u94a2\u7684<\/strong><strong>STEM<\/strong><strong>\u660e\u573a\u50cf\u3002\u63d2\u56fe\u663e\u793a\u4e86\u76f8\u5e94\u5fae\u7ed3\u6784\u7684<\/strong><strong>SAED<\/strong><strong>\u6a21\u5f0f\u3002<\/strong><strong>b<\/strong><strong>\u4e2d\u7ea2\u8272\u6570\u636e\u70b9\u4e0a\u7684\u8bef\u5dee\u6761\u8868\u793a\u4e94\u7ec4\u6d4b\u8bd5\u5747\u503c\u7684\u6807\u51c6\u5dee<\/strong><strong>[2]<\/strong><strong>\u3002<\/strong><\/p>\n<p>(2) \u901a\u8fc7\u6709\u5e8f\u6c27\u590d\u5408\u7269\u63d0\u9ad8\u9ad8\u71b5\u5408\u91d1\u7684\u5f3a\u5851\u6027<\/p>\n<p>\u5728\u5408\u91d1\u7684\u8bbe\u8ba1\u4e2d\uff0cO\u5143\u7d20\u7684\u6dfb\u52a0\u901a\u5e38\u589e\u52a0\u6750\u6599\u7684\u8106\u6027\u3002\u56e0\u6b64\uff0cO\u5143\u7d20\u5e94\u8be5\u5c3d\u91cf\u907f\u514d\u3002\u672c\u5de5\u4f5c\u5219\u53d1\u73b0\uff0cO\u5728\u9ad8\u71b5\u5408\u91d1\u4e2d\u53ef\u4ee5\u4ee5\u6709\u5e8f\u6c27\u590d\u5408\u7269\u7684\u5f62\u5f0f\u5b58\u5728(\u4ecb\u4e8e\u6c27\u5316\u7269\u548c\u968f\u673a\u95f4\u9699\u4e4b\u95f4\u7684\u72b6\u6001)\u3002\u4e0e\u4f20\u7edf\u7684\u95f4\u9699\u5f3a\u5316\u4e0d\u540c\uff0c\u8fd9\u79cd\u6709\u5e8f\u7684\u95f4\u9699\u914d\u5408\u7269\u5728\u6210\u5206\u590d\u6742\u7684\u56fa\u6eb6\u9ad8\u71b5\u5408\u91d1\u4e2d\u5bfc\u81f4\u5f3a\u5ea6\u548c\u5ef6\u5c55\u6027\u7684\u7a7a\u524d\u63d0\u9ad8\u3002\u5f53\u5c06\u6a21\u578bTiZrHfNb HEA\u4e0e2.0%\u542b\u91cf\u7684\u6c27\u63ba\u6742\u65f6\uff0c\u62c9\u4f38\u5f3a\u5ea6\u589e\u5f3a\u4e86(48.5\u00b11.8) %\uff0c\u5ef6\u5c55\u6027\u6539\u5584(95.2\u00b18.1)%\uff0c\u4ece\u800c\u6253\u7834\u4e86\u957f\u671f\u4ee5\u6765\u7684\u5f3a\u5ea6\u5ef6\u5c55\u6027\u63a3\u8098\u3002\u6c27\u590d\u5408\u7269\u662fHEA\u4e2d\u6709\u5e8f\u7684\u7eb3\u7c73\u7ea7\u533a\u57df\uff0c\u5176\u7279\u5f81\u4e3a(O, Zr, Ti)\u5bcc\u539f\u5b50\u590d\u5408\u7269\uff0c\u5b83\u4eec\u662f\u7531\u4e8eHEA\u4e2d\u67d0\u4e9b\u53d6\u4ee3\u57fa\u5143\u7d20\u4e4b\u95f4\u5b58\u5728\u5316\u5b66\u77ed\u7a0b\u6709\u5e8f\u800c\u5f62\u6210\u3002\u636e\u62a5\u9053\uff0c\u78b3\u53ef\u4ee5\u901a\u8fc7\u964d\u4f4e\u5806\u9519\u80fd\u548c\u589e\u52a0\u6676\u683c\u6469\u64e6\u5e94\u529b\uff0c\u540c\u65f6\u63d0\u9ad8\u9762\u5fc3\u7acb\u65b9HEAs\u7684\u5f3a\u5ea6\u548c\u5ef6\u5c55\u6027\u3002\u800c\u6709\u5e8f\u7684\u95f4\u9699\u914d\u5408\u7269\u5219\u901a\u8fc7\u53d8\u5f62\u8fc7\u7a0b\u4e2dFrank-Read\u6e90(\u4e00\u79cd\u89e3\u91ca\u591a\u4e2a\u4f4d\u9519\u4ea7\u751f\u7684\u673a\u5236)\u7684\u5f62\u6210\uff0c\u5c06\u4f4d\u9519\u526a\u5207\u6a21\u5f0f\u7531\u5e73\u9762\u6ed1\u79fb\u8f6c\u53d8\u4e3a\u6ce2\u6d6a\u6ed1\u79fb\uff0c\u5e76\u4fc3\u8fdb\u53cc\u4ea4\u53c9\u6ed1\u79fb\uff0c\u4ece\u800c\u5bfc\u81f4\u4f4d\u9519\u589e\u6b96\u3002\u8fd9\u79cd\u6709\u5e8f\u7684\u95f4\u9699\u7edc\u5408\u7269\u4ecb\u5bfc\u7684\u5e94\u53d8\u786c\u5316\u673a\u5236\u5728\u542bTi\u3001Zr\u548chf\u7684\u5408\u91d1\u4e2d\u7279\u522b\u6709\u7528\uff0c\u5728\u8fd9\u4e9b\u5408\u91d1\u4e2d\uff0c\u7531\u4e8e\u5176\u8106\u5316\u6548\u5e94\uff0c\u95f4\u9699\u5143\u7d20\u662f\u975e\u5e38\u4e0d\u53ef\u53d6\u7684\uff0c\u5728\u5408\u91d1\u4e2d\u8c03\u6574\u5c42\u9519\u80fd\u548c\u5229\u7528\u975e\u70ed\u8f6c\u53d8\u4e0d\u4f1a\u5bfc\u81f4\u6027\u80fd\u589e\u5f3a\u3002\u8fd9\u4e9b\u7ed3\u679c\u4e3a\u7814\u7a76\u91d1\u5c5e\u6750\u6599\u4e2d\u95f4\u9699\u56fa\u6eb6\u4f53\u7684\u4f5c\u7528\u53ca\u5176\u6709\u5e8f\u5f3a\u5316\u673a\u5236\u63d0\u4f9b\u4e86\u65b0\u7684\u601d\u8def\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-238391\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/2-4.png\" alt=\"\" width=\"789\" height=\"783\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/2-4.png 789w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/2-4-150x150.png 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/2-4-300x298.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/2-4-768x762.png 768w\" sizes=\"(max-width: 789px) 100vw, 789px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>2 <\/strong><strong>\u53d8\u5f62\u673a\u7406\uff1b<\/strong><strong>a, TiZrHfNb<\/strong><strong>\u57fa<\/strong><strong>HEA<\/strong><strong>\u5728<\/strong><strong>8%<\/strong><strong>\u62c9\u4f38\u5e94\u53d8\u4e0b\u7684<\/strong><strong>STEM<\/strong><strong>\u56fe\u50cf<\/strong><strong>(<\/strong><strong>\u9ec4\u8272\u7bad\u5934\u8868\u793a\u5171\u9762\u4f4d\u9519\u9635\u5217<\/strong><strong>)<\/strong><strong>\uff1b<\/strong><strong>b, 8%<\/strong><strong>\u62c9\u4f38\u5e94\u53d8\u4e0b<\/strong><strong>O-2 HEA<\/strong><strong>\u7684<\/strong><strong>STEM<\/strong><strong>\u56fe\u50cf<\/strong><strong>(<\/strong><strong>\u7ea2\u8272\u7bad\u5934\u8868\u793a\u5076\u6781\u58c1<\/strong><strong>)<\/strong><strong>\u3002<\/strong><strong>c, 8%<\/strong><strong>\u62c9\u4f38\u5e94\u53d8\u4e0b<\/strong><strong>N-2 HEA<\/strong><strong>\u7684<\/strong><strong>STEM<\/strong><strong>\u56fe\u50cf<\/strong><strong>(<\/strong><strong>\u9ec4\u8272\u7bad\u5934\u8868\u793a\u5e73\u9762\u6ed1\u79fb\u5e26<\/strong><strong>)<\/strong><strong>\u3002\u5728\u57fa\u4f53<\/strong><strong>HEA<\/strong><strong>\u548c\u6c2e\u63ba\u6742<\/strong><strong>N-2 HEA<\/strong><strong>\u4e2d\u89c2\u5bdf\u5230\u5178\u578b\u7684\u5e73\u9762\u6ed1\u79fb\u3002\u800c\u63ba\u6742\u6c27\u7684\u53d8\u4f53<\/strong><strong>O-2 HEA<\/strong><strong>\u7684\u53d8\u5f62\u4ee5\u6ce2\u6ed1\u4e3a\u4e3b\uff0c\u8868\u660e\u6c27\u7684\u52a0\u5165\u5bfc\u81f4\u4e86\u4ee5\u6ce2\u6ed1\u4e3a\u4e3b\u7684\u5851\u6027\u53d8\u5f62\u6a21\u5f0f\u3002<\/strong><strong>a<\/strong><strong>\u548c<\/strong><strong>c<\/strong><strong>\u7684\u6676\u5e26\u8f74\u4e3a<\/strong><strong>[011]<\/strong><strong>\uff0c<\/strong><strong>b<\/strong><strong>\u7684\u6676\u5e26\u8f74\u4e3a\u4e3a<\/strong><strong>[001]<\/strong><strong>\u3002<\/strong><strong>d<\/strong><strong>\uff0c\u539f\u4f4d<\/strong><strong>TEM<\/strong><strong>\u62c9\u4f38\u5b9e\u9a8c\u4e2d<\/strong><strong>TiZrHfNb<\/strong><strong>\u57fa<\/strong><strong>HEA<\/strong><strong>\u548c\u95f4\u9699\u63ba\u6742\u53d8\u4f53<\/strong><strong>O-2<\/strong><strong>\u548c<\/strong><strong>N-2 HEAs<\/strong><strong>\u7684\u4f4d\u9519\u95f4\u8ddd\u3002\u767d\u8272\u7bad\u5934\u8868\u793a\u4f4d\u9519\u95f4\u8ddd\u3002<\/strong><strong>O-2 HEA<\/strong><strong>\u7684\u5e73\u5747\u4f4d\u9519\u95f4\u8ddd<\/strong><strong>(25.06 3.15 nm)<\/strong><strong>\u8fdc\u5c0f\u4e8e\u57fa\u5e95<\/strong><strong>HEA (90.36 14.32 nm)<\/strong><strong>\u548c<\/strong><strong>N-2 HEA (104.06 8.14 nm)<\/strong><strong>\u3002\u8bef\u5dee\u6761\u662f\u5747\u503c\u7684\u6807\u51c6\u5dee<\/strong><strong>[3]<\/strong><strong>\u3002<\/strong><\/p>\n<p>(3) \u4e00\u79cd\u5236\u5907\u5927\u5757\u9ad8\u5f3a\u9ad8\u5851\u7684\u8d85\u7ec6\u6676\u94a2<\/p>\n<p>\u4e9a\u5fae\u7c73\u6676\u7c92\u5c3a\u5bf8\u7684\u94a2\u901a\u5e38\u5177\u6709\u9ad8\u7684\u97e7\u6027\u548c\u5f3a\u5ea6\uff0c\u8fd9\u4f7f\u5b83\u4eec\u5728\u8f7b\u91cf\u5316\u6280\u672f\u548c\u8282\u80fd\u7b56\u7565\u65b9\u9762\u6709\u524d\u666f\u3002\u5230\u76ee\u524d\u4e3a\u6b62\uff0c\u8d85\u7ec6\u6676\u7c92(UFG)\u5408\u91d1\u7684\u5de5\u4e1a\u5236\u9020\uff0c\u901a\u5e38\u4f9d\u8d56\u4e8e\u63a7\u5236\u6269\u6563\u76f8\u53d8\uff0c\u4e00\u76f4\u5c40\u9650\u4e8e\u5965\u6c0f\u4f53-\u94c1\u7d20\u4f53\u76f8\u53d8\u94a2\u3002\u6b64\u5916\uff0cUFG\u94a2\u7684\u52a0\u5de5\u786c\u5316\u6709\u9650\uff0c\u4f38\u957f\u7387\u4e0d\u5747\u5300\uff0c\u963b\u788d\u4e86\u5176\u5e7f\u6cdb\u5e94\u7528\u3002\u672c\u5de5\u4f5c\u5728\u5178\u578b\u7684Fe 22Mn0.6C\u5b6a\u751f\u8bf1\u5bfc\u5851\u6027\u94a2\u4e2d\u6210\u529f\u5730\u6279\u91cf\u751f\u4ea7\u51faUFG\u7ed3\u6784\u94a2\uff0c\u4e3b\u8981\u91c7\u7528\u7684\u7b56\u7565\u662f\u5c11\u91cfCu\u5408\u91d1\u5316+\u64cd\u7eb5\u518d\u7ed3\u6676\u8fc7\u7a0b(\u572830\u79d2\u5185)+\u5229\u7528\u5171\u683c\u65e0\u5e8f\u5bccCu\u76f8\u7684\u6676\u5185\u7eb3\u7c73\u6c89\u6dc0\u3002\u5feb\u901f\u800c\u4e30\u5bcc\u7684\u7eb3\u7c73\u6c89\u6dc0\u4e0d\u4ec5\u963b\u6b62\u4e86\u65b0\u4e9a\u5fae\u7c73\u7ea7\u518d\u7ed3\u6676\u6676\u7c92\u7684\u751f\u957f\uff0c\u800c\u4e14\u901a\u8fc7\u9f50\u7eb3\u9489\u624e\u673a\u5236\u63d0\u9ad8\u4e86\u83b7\u5f97\u7684UFG\u7ed3\u6784\u7684\u70ed\u7a33\u5b9a\u6027\u3002\u6b64\u5916\uff0c\u7531\u4e8e\u5176\u5b8c\u5168\u5171\u683c\u6027\u548c\u65e0\u5e8f\u6027\uff0c\u6790\u51fa\u76f8\u5728\u52a0\u8f7d\u4e0b\u4e0e\u4f4d\u9519\u8868\u73b0\u51fa\u5fae\u5f31\u7684\u76f8\u4e92\u4f5c\u7528\u3002\u8fd9\u79cd\u65b9\u6cd5\u80fd\u591f\u5236\u5907\u6676\u7c92\u5c3a\u5bf8\u4e3a800\u00b1400\u7eb3\u7c73\u7684\u5b8c\u5168\u518d\u7ed3\u6676UFG\u7ed3\u6784\uff0c\u800c\u4e0d\u4f1a\u5f15\u5165\u8106\u6027\u9897\u7c92\u548c\u5206\u79bb\u8fb9\u754c\u7b49\u6709\u5bb3\u6676\u683c\u7f3a\u9677\u3002\u4e0e\u672a\u6dfb\u52a0\u94dc\u7684\u94a2\u76f8\u6bd4\uff0cUFG\u7ed3\u6784\u7684\u5c48\u670d\u5f3a\u5ea6\u63d0\u9ad8\u4e86\u4e00\u500d\uff0c\u7ea6\u4e3a710MPa\uff0c\u5747\u5300\u5ef6\u5c55\u6027\u4e3a45%\uff0c\u6297\u62c9\u5f3a\u5ea6\u7ea6\u4e3a2000MPa\u3002\u8fd9\u79cd\u6676\u7c92\u7ec6\u5316\u7684\u6982\u5ff5\u5e94\u8be5\u53ef\u4ee5\u6269\u5c55\u5230\u5176\u4ed6\u5408\u91d1\u7cfb\u7edf\uff0c\u5236\u9020\u5de5\u827a\u53ef\u4ee5\u5f88\u5bb9\u6613\u5730\u5e94\u7528\u4e8e\u73b0\u6709\u7684\u5de5\u4e1a\u751f\u4ea7\u7ebf\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-238392\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/3-4.png\" alt=\"\" width=\"1058\" height=\"615\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/3-4.png 1058w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/3-4-300x174.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/3-4-768x446.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/3-4-1024x595.png 1024w\" sizes=\"(max-width: 1058px) 100vw, 1058px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>3 4Cu<\/strong><strong>\u5728<\/strong><strong>760<\/strong><strong>\u2103\u9000\u706b<\/strong><strong>5min<\/strong><strong>\u540e\u7684\u663e\u5fae\u7ec4\u7ec7\u8868\u5f81\uff1b<\/strong><strong>a,<\/strong><strong>\u540c\u6b65\u8f90\u5c04\u9ad8\u80fd<\/strong><strong>XRD<\/strong><strong>\u8c31\u56fe\uff1b<\/strong><strong>b<\/strong><strong>\uff0c<\/strong><strong>EBSD<\/strong><strong>\u56fe\u663e\u793a\u4e86\u5177\u6709\u8d85\u7ec6\u7ed3\u6784\u7684\u5355\u4e00<\/strong><strong>fcc<\/strong><strong>\u76f8\u3002<\/strong><strong>a<\/strong><strong>\u4e2d\u7684\u63d2\u56fe\u663e\u793a\u4e86\u7c92\u5ea6\u5206\u5e03\u3002<\/strong><strong>c, ADF-STEM<\/strong><strong>\u56fe\u50cf\u663e\u793a\u9ad8\u5bc6\u5ea6\u7684\u9897\u7c92\u5185\u7eb3\u7c73\u6c89\u6dc0\u7269<\/strong><strong>(<\/strong><strong>\u660e\u4eae\u7684\u9897\u7c92<\/strong><strong>)<\/strong><strong>\u3002\u63d2\u56fe\u662f\u6807\u8bb0\u533a\u57df\u7684<\/strong><strong>STEM EDS-SI<\/strong><strong>\u56fe\u50cf\u3002<\/strong><strong>d<\/strong><strong>\uff0c\u539f\u5b50\u5206\u8fa8\u7387<\/strong><strong>ADF-STEM<\/strong><strong>\u56fe\u50cf\u663e\u793a\u4e86\u5bcc\u94dc\u7eb3\u7c73\u6c89\u6dc0\u7269\u7684\u5b8c\u5168\u5171\u683c\u65e0\u5e8f\u6027\u3002<\/strong><strong>e<\/strong><strong>\uff0c\u900f\u5c04\u7535\u955c<\/strong><strong>(<\/strong><strong>\u5de6<\/strong><strong>)<\/strong><strong>\u548c<\/strong><strong>APT(<\/strong><strong>\u53f3<\/strong><strong>)<\/strong><strong>\u901a\u8fc7\u4e24\u4e2a\u6676\u754c<\/strong><strong>(GB)<\/strong><strong>\u7684\u5206\u6790\u663e\u793a\u5bcc\u94dc\u7eb3\u7c73\u6c89\u6dc0\u7269\u7684\u5927\u5c0f\u3001\u5f62\u6001\u548c\u7a7a\u95f4\u5206\u5e03\u3002<\/strong><strong>f<\/strong><strong>\uff0c\u8ddd\u79bb\u76f4\u65b9\u56fe\uff0c\u663e\u793a\u4e86\u4e00\u4e2a\u7eb3\u7c73\u6c89\u6dc0\u7269\u7684\u6210\u5206\u53d8\u5316<\/strong><strong>(e<\/strong><strong>\u4e2d\u7684\u7eff\u8272\u65b9\u5757\u6807\u8bb0<\/strong><strong>)<\/strong><strong>\u3002<\/strong><strong>g, e<\/strong><strong>\u4e2d\u7684\u5706\u67f1\u5f62\u533a\u57df\u7684\u4e00\u7ef4\u6d53\u5ea6\u5256\u9762\uff0c\u5728\u6676\u754c\u5904\u6ca1\u6709\u660e\u663e\u7684\u5143\u7d20\u504f\u6790<\/strong><strong>[4]<\/strong><strong>\u3002<\/strong><\/p>\n<p>(4) \u8d85\u5f3a\u94a2\u4e2d\u7eb3\u7c73\u5171\u683c\u7c92\u5b50\u4ecb\u5bfc\u7684\u5e94\u53d8\u786c\u5316<\/p>\n<p>\u7531\u4f4d\u9519\u6216\u7eb3\u7c73\u6c89\u6dc0\u7269\u7b49\u5355\u4e00\u6676\u683c\u7f3a\u9677\u5f15\u8d77\u7684\u5f3a\u5316\u901a\u5e38\u4f1a\u5bfc\u81f4\u6240\u8c13\u7684\u5f3a\u5ea6-\u5ef6\u6027\u63a3\u8098\uff0c\u5728\u5f3a\u5ea6\u6c34\u5e73\u9ad8\u4e8e2 GPa\u65f6\u5c24\u4e3a\u660e\u663e\u3002\u5728\u6b64\uff0c\u6211\u4eec\u901a\u8fc7\u64cd\u7eb5\u4e0d\u540c\u6676\u683c\u7f3a\u9677\u4e4b\u95f4\u7684\u76f8\u4e92\u4f5c\u7528\uff0c\u5728\u8d85\u9ad8\u5f3a\u5ea6\u9a6c\u6c0f\u4f53\u94a2\u4e2d\u62a5\u544a\u4e86\u4e00\u79cd\u53ef\u6301\u7eed\u7684\u5e94\u53d8\u786c\u5316\u673a\u5236\u3002\u7ed3\u679c\u8868\u660e\uff0c\u5feb\u901f\u6790\u51fa\u4f4e\u9519\u914d\u4f4d\u7684b2\u6709\u5e8fNi(Al, Fe)\u53ef\u4ee5\u6709\u6548\u5730\u9632\u6b62\u9ad8\u5bc6\u5ea6\u6dec\u706d\u4f4d\u9519\u7684\u6062\u590d\u3002\u5728\u5851\u6027\u53d8\u5f62\u8fc7\u7a0b\u4e2d\uff0c\u6709\u5e8f\u7eb3\u7c73\u6c89\u6dc0\u7269\u6240\u4ea7\u751f\u7684\u9ad8\u5207\u524a\u5e94\u529b\u4e0d\u4ec5\u4f7f\u5927\u91cf\u4fdd\u7559\u7684\u4f4d\u9519\u4ee5\u5e73\u9762\u65b9\u5f0f\u79fb\u52a8\uff0c\u800c\u4e14\u5927\u5927\u6269\u5c55\u4e86\u5305\u542b\u5927\u91cf\u4f4d\u9519\u7684\u4f4d\u9519\u9a6c\u6c0f\u4f53\u4e2d\u4f4d\u9519\u8fd0\u52a8\u7684\u5e73\u5747\u81ea\u7531\u8def\u5f84\u3002\u540c\u65f6\uff0c\u5e73\u9762\u6ed1\u79fb\u4e0e\u539f\u6709\u7684\u4f4d\u9519\u53d1\u751f\u4e25\u91cd\u7684\u4f4d\u9519\u53cd\u5e94\uff0c\u53ca\u65f6\u6062\u590d\u56e0\u5207\u524a\u6790\u51fa\u76f8\u800c\u51cf\u5f31\u7684\u5c40\u90e8\u5207\u524a\u5e94\u529b\u3002\u8fd9\u79cd\u53ca\u65f6\u5efa\u7acb\u7684\u5207\u524a\u5e94\u529b\u540c\u65f6\u964d\u4f4e\u4e86\u5e73\u9762\u6ed1\u79fb\u5e26\u5185\u6ed1\u79fb\u96c6\u4e2d\u7a0b\u5ea6\u548c\u5b58\u50a8\u5171\u9762\u4f4d\u9519\u7684\u5927\u5c0f\uff0c\u4fc3\u8fdb\u4e86\u660e\u663e\u7684\u6ed1\u79fb\u5e26\u7ec6\u5316\u4f5c\u4e3a\u4e3b\u8981\u7684\u5e94\u53d8\u786c\u5316\u673a\u5236\uff0c\u4f7f\u5c48\u670d\u5f3a\u5ea6(2 GPa)\u548c\u5ef6\u4f38\u7387(9%)\u540c\u65f6\u589e\u52a0\u3002\u7814\u7a76\u7ed3\u679c\u63d0\u4f9b\u4e86\u4e00\u79cd\u53ef\u80fd\u7684\u65b9\u6cd5\uff0c\u901a\u8fc7\u8c03\u6574\u4e0d\u540c\u7c7b\u578b\u6676\u683c\u7f3a\u9677\u4e4b\u95f4\u7684\u76f8\u4e92\u4f5c\u7528\uff0c\u540c\u65f6\u63d0\u9ad8\u5f3a\u5ea6\u548c\u5ef6\u6027\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-238393\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/4-4.png\" alt=\"\" width=\"1082\" height=\"654\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/4-4.png 1082w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/4-4-300x181.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/4-4-768x464.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/4-4-1024x619.png 1024w\" sizes=\"(max-width: 1082px) 100vw, 1082px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>4 ECCI<\/strong><strong>\u548c<\/strong><strong>STEM<\/strong><strong>\u5206\u6790\u8868\u660e\uff0c\u65f6\u6548\u540e<\/strong><strong>3Al<\/strong><strong>\u94a2\u7684\u7a7a\u95f4\u5e26\u7ec4\u7ec7\u5e94\u53d8\u4e3a<\/strong><strong>4%<\/strong><strong>\uff1b<\/strong><strong>(a)<\/strong><strong>\u9ad8\u500d<\/strong><strong>ECCI<\/strong><strong>\u56fe\u50cf\uff0c\u68c0\u6d4b\u5230\u591a\u4e2a\u4e0d\u540c\u5e26\u5bbd\u7684\u5e73\u9762\u6ed1\u79fb\u5e26\uff1b<\/strong><strong>(b)<\/strong><strong>\uff0c<\/strong><strong> (c)<\/strong><strong>\u5178\u578b\u7684<\/strong><strong>BF(<\/strong><strong>\u4eae\u573a<\/strong><strong>)<\/strong><strong>\u56fe\u50cf\u548c\u5bf9\u5e94\u7684<\/strong><strong>HAADFSTEM<\/strong><strong>\u56fe\u50cf\uff0c\u5206\u522b\u663e\u793a\u51fa\u9891\u7e41\u7684\u4f4d\u9519\u76f8\u4ea4\u548c\u9ad8\u5bc6\u5ea6\u6790\u51fa\u76f8\u7684\u4fdd\u7559\u3002<\/strong><strong>(d)<\/strong><strong>\u9ad8\u5206\u8fa8\u7387<\/strong><strong>HAADF STEM<\/strong><strong>\u56fe\u50cf\uff0c\u663e\u793a\u6062\u590d\u7684\u4f4d\u9519\u9644\u8fd1\u6790\u51fa\u7269\u7684\u5468\u671f\u6027\u539f\u5b50\u67f1\u7ed3\u6784\uff0c\u7528\u692d\u5706\u7a81\u51fa\u663e\u793a\u3002\u63d2\u56fe\u662f\u4f4e\u500d<\/strong><strong>STEM<\/strong><strong>\u56fe\u50cf\uff0c\u663e\u793a\u4e86\u6790\u51fa\u76f8\u7684\u4f4d\u7f6e\u3002<\/strong><strong>\u00a0(e)<\/strong><strong>\u56fe\u4e2d\u7bad\u5934\u6240\u793a\u533a\u57df\u7684<\/strong><strong>IFFT<\/strong><strong>\u6a21\u5f0f\uff0c\u663e\u793a\u4e86\u4e0d\u540c\u7c7b\u578b\u7684\u4f4d\u9519<\/strong><strong>[5]<\/strong><strong>\u3002<\/strong><\/p>\n<p>(5) \u53d1\u660e\u6297\u8f90\u7167\u65b0\u673a\u5236\uff0c\u5177\u6709\u6781\u5f3a\u7684\u5de5\u7a0b\u5e94\u7528<\/p>\n<p>\u5728\u6838\u53cd\u5e94\u5806\u670d\u5f79\u7684\u6750\u6599\u8981\u7ecf\u53d7\u975e\u5e38\u4e25\u82db\u7684\u73af\u5883\uff0c\u8fd9\u4e0d\u53ef\u907f\u514d\u7684\u4f1a\u5bfc\u81f4\u6750\u6599\u7ed3\u6784\u5b8c\u6574\u6027\u548c\u529b\u5b66\u6027\u80fd\u7684\u9000\u5316\uff0c\u4f8b\u5982\u5b8f\u89c2\u5b54\u6d1e\u81a8\u80c0\u3001\u8f90\u5c04\u786c\u5316\u548c\u8106\u5316\u3002\u8bbe\u8ba1\u51fa\u5728\u8fd9\u79cd\u4e25\u82db\u6761\u4ef6\u4e0b\u80fd\u591f\u5e78\u5b58\u7684\u6750\u6599\u5bf9\u4e8e\u5ef6\u957f\u53cd\u5e94\u5806\u5bff\u547d\uff0c\u4fc3\u8fdb\u6838\u805a\u53d8\u548c\u5148\u8fdb\u6838\u88c2\u53d8\u53cd\u5e94\u5806\u7684\u53d1\u5c55\u975e\u5e38\u91cd\u8981\uff0c\u4f46\u5374\u4e00\u76f4\u5145\u6ee1\u6311\u6218\u3002\u80fd\u591f\u5728\u9ad8\u6e29\u4e0b\u7ef4\u6301\u9ad8\u8f90\u5c04\u5242\u91cf\u7684\u6750\u6599\u662f\u4e0b\u4e00\u4ee3\u88c2\u53d8\u548c\u672a\u6765\u805a\u53d8\u80fd\u6240\u5fc5\u9700\u7684\u3002\u8fc4\u4eca\u4e3a\u6b62\uff0c\u5373\u4f7f\u662f\u6700\u6709\u524d\u9014\u7684\u7ed3\u6784\u6750\u6599\u4e5f\u4e0d\u80fd\u627f\u53d7\u8f90\u5c04\u73af\u5883\u8981\u6c42\uff0c\u56e0\u4e3a\u4e0d\u53ef\u9006\u7684\u8f90\u5c04\u5c06\u9a71\u52a8\u5fae\u89c2\u7ed3\u6784\u9000\u5316\u3002\u8f90\u5c04\u5f15\u8d77\u7684\u6750\u6599\u9000\u5316\u901a\u5e38\u662f\u7531\u4e8e\u8fc7\u591a\u7684\u95f4\u9699\u548c\u7a7a\u4f4d\u7684\u4ea7\u751f\u548c\u968f\u540e\u7684\u805a\u96c6\u9020\u6210\u7684\u3002\u5176\u4e2d\uff0c\u7a7a\u7a74\u81a8\u80c0\u662f\u9ad8\u6e29\u4e0b\u9ad8\u5242\u91cf\u8f90\u5c04\u5bf9\u6750\u6599\u7684\u5173\u952e\u8f90\u5c04\u964d\u89e3\u6548\u5e94\u4e4b\u4e00\uff0c\u901a\u5e38\u6d89\u53ca\u7a7a\u4f4d\u7684\u5f62\u6210\u548c\u9010\u6e10\u805a\u96c6\u3002\u6297\u7a7a\u6d1e\u81a8\u80c0\u80fd\u529b\u7684\u589e\u5f3a\u901a\u5e38\u5f52\u56e0\u4e8e\u9ad8\u6bd4\u4f8b\u7684\u5931\u914d\u754c\u9762\uff0c\u5176\u53ef\u4ee5\u902e\u6355\u8f90\u5c04\u5f15\u8d77\u7684\u95f4\u9699\u548c\u7a7a\u4f4d\u3002\u672c\u5de5\u4f5c\u9996\u5148\u5728\u9a6c\u6c0f\u4f53\u65f6\u6548\u94a2\u4e2d\u5f15\u5165\u7684\u8d85\u6676\u683c\u7eb3\u7c73\u6c89\u6dc0\u7269\uff0c\u8fd9\u79cd\u7ed3\u6784\u7684\u6b8a\u80dc\u4e4b\u5904\u662f\u5728\u7eb3\u7c73\u6c89\u6dc0\u7269\u9644\u8fd1\u53ef\u8bf1\u5bfc\u7ed3\u6784\u53ef\u9006\u7684\u5c40\u90e8\u65e0\u5e8f-\u6709\u5e8f\u8f6c\u53d8\u3002\u7814\u7a76\u8868\u660e\uff1a\u5728\u542b\u6709\u9ad8\u5bc6\u5ea6B2\u6709\u5e8f\u8d85\u6676\u683c\u7684\u9a6c\u6c0f\u4f53\u94a2\u4e2d\uff0c\u5373\u4f7f\u5728400-600\u00b0C\u7684\u8d85\u9ad8\u5242\u91cf\u8f90\u5c04\u635f\u4f24\u540e\uff0c\u4e5f\u6ca1\u6709\u68c0\u6d4b\u5230\u7a7a\u6d1e\u81a8\u80c0\u3002\u5728\u9ad8\u5ea6\u9971\u548c\u7684\u57fa\u4f53\u4e2d\uff0c\u4f4e\u9519\u914d\u8d85\u6676\u683c\u7684\u91cd\u65b0\u6709\u5e8f\u8fc7\u7a0b\u53d1\u751f\u5728\u5feb\u901f\u7684\u65e0\u5e8f\u5316\u4e4b\u540e\u3002\u8fd9\u6837\uff0c\u901a\u8fc7\u8f90\u5c04\u8bf1\u53d1\u7684\u70b9\u7f3a\u9677\u548c\u8fc7\u5269\u6eb6\u8d28\u7684\u4f1a\u53d1\u751f\u77ed\u7a0b\u91cd\u65b0\u6709\u5e8f\u3002\u8fd9\u4e00\u52a8\u6001\u8fc7\u7a0b\u7a33\u5b9a\u4e86\u5fae\u89c2\u7ed3\u6784\uff0c\u4e0d\u65ad\u4fc3\u8fdb\u539f\u4f4d\u7f3a\u9677\u590d\u5408\uff0c\u5e76\u6709\u6548\u5730\u963b\u6b62\u4e86\u957f\u7a0b\u6269\u6563\u8fc7\u7a0b\u3002\u4ece\u800c\u5927\u5e45\u5ea6\u63d0\u9ad8\u4e86\u6750\u6599\u7684\u8010\u8f90\u5c04\u6027\u80fd\u3002\u8be5\u7b56\u7565\u53ef\u5e94\u7528\u4e8e\u5176\u4ed6\u6750\u6599\uff0c\u4e3a\u5f00\u53d1\u9ad8\u8010\u8f90\u5c04\u6750\u6599\u94fa\u5e73\u4e86\u9053\u8def\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-238394\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/2-5.png\" alt=\"\" width=\"2101\" height=\"2401\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/2-5.png 2101w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/2-5-263x300.png 263w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/2-5-768x878.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/06\/2-5-896x1024.png 896w\" sizes=\"(max-width: 2101px) 100vw, 2101px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>5 <\/strong><strong>\u79bb\u5b50\u8f90\u7167\u4e0b\u8d85\u6676\u683c\u94a2\u7684\u7ec4\u7ec7\u6f14\u53d8\uff1b<\/strong><strong>a,b<\/strong><strong>\uff0c\u8d85\u6676\u683c\u94a2\u5728<\/strong><strong>500<\/strong><strong>\u2103<\/strong><strong>0 dpa (a)<\/strong><strong>\u548c<\/strong><strong>840 dpa (b)<\/strong><strong>\u4e0b\u7684<\/strong><strong>HAADF-STEM<\/strong><strong>\u56fe\u50cf\uff1b<\/strong><strong>c,d<\/strong><strong>\uff0c\u9ad8\u5206\u8fa8\u7387<\/strong><strong>HAADF-STEM<\/strong><strong>\u56fe\u50cf\u663e\u793a\u4e86<\/strong><strong>NPs<\/strong><strong>\u548c\u5bcc\u6eb6\u8d28\u533a\u57df\u4e4b\u95f4\u7684\u539f\u5b50\u7ed3\u6784\u5dee\u5f02\uff1b<\/strong><strong>e, APT<\/strong><strong>\u8868\u5f81\u7684<\/strong><strong>NPs<\/strong><strong>\u5728\u79bb\u5b50\u8f90\u7167\u8fc7\u7a0b\u4e2d\u7684\u6f14\u5316\uff0c\u4e3b\u8981\u901a\u8fc7<\/strong><strong>50at%Al<\/strong><strong>\u548c<\/strong><strong>Ni<\/strong><strong>\u7b49\u6d53\u5ea6\u8868\u9762\u663e\u793a\u548c\u5f3a\u8c03\uff1b<\/strong><strong>f,g<\/strong><strong>\uff0c\u8ddd\u79bb\u76f4\u65b9\u56fe\u663e\u793a\u4e86\u6240\u9009\u6c89\u6dc0<\/strong><strong>(f)<\/strong><strong>\u548c\u6eb6\u8d28\u5bcc\u96c6\u533a\u57df<\/strong><strong>(g)<\/strong><strong>\u7684\u6210\u5206\u8f6e\u5ed3\uff0c\u5176\u4e2d\u8bef\u5dee\u6761\u662f\u5747\u503c\u7684\u6807\u51c6\u504f\u5dee\uff1b<\/strong><strong>h, HAADF-STEM<\/strong><strong>\u56fe\u50cf\u663e\u793a\u4e86<\/strong><strong>500\u00b0C\/840 dpa<\/strong><strong>\u8f90\u7167\u540e\u4f4d\u9519\u73af\u7684\u5b58\u5728\uff1b<\/strong><strong>i<\/strong><strong>\uff0c\u9ad8\u5206\u8fa8\u7387<\/strong><strong>HAADF-STEM<\/strong><strong>\u56fe\u50cf\uff0c\u663e\u793a\u4f4d\u9519\u73af\u9644\u8fd1\u5b58\u5728<\/strong><strong>NPs<\/strong><strong>\uff0c\u4ee5\u53ca\u76f8\u5e94\u7684<\/strong><strong>FFT<\/strong><strong>\u7ed3\u679c<\/strong><strong>(<\/strong><strong>\u53f3\u84dd\u7ea2\u6846<\/strong><strong>)<\/strong><strong>\uff1b<\/strong><strong>j, HAADF<\/strong><strong>\u56fe\u50cf\u663e\u793a\u4e00\u4e2a<\/strong><strong>\u201c<\/strong><strong>\u6108\u5408<\/strong><strong>\u201d<\/strong><strong>\u7684<\/strong><strong>a\/2&lt;100&gt;<\/strong><strong>\u4f4d\u9519\u73af\u8fdc\u79bb\u6790\u51fa\u7269\uff1b<\/strong><strong>k,l<\/strong><strong>\uff0c\u5bf9\u5e94<\/strong><strong>Ni (k)<\/strong><strong>\u548c<\/strong><strong>Al (l)<\/strong><strong>\u7684<\/strong><strong>EDS<\/strong><strong>\u9762\u626b<\/strong><strong>[6]<\/strong><strong>\u3002<\/strong><\/p>\n<p>&nbsp;<\/p>\n<ol start=\"2\">\n<li><strong>\u6210\u679c\u542f\u8fea<\/strong><\/li>\n<\/ol>\n<p>\u4ee5\u4e0a\u662f\u5415\u662d\u5e73\u6559\u6388\u56e2\u961f\u57fa\u4e8e\u6700\u4f4e\u6676\u683c\u9519\u914d\u5fae\u89c2\u7ed3\u6784\u8bbe\u8ba1\uff0c\u6240\u53d1\u8868\u7684\u9ad8\u6c34\u5e73\u8bba\u6587\uff0c\u4e3b\u8981\u5305\u542b3\u7bc7Nature\u6b63\u520a\uff0c1\u7bc7Nature Materials\uff0c\u7531\u6b64\u53ef\u89c1\u8be5\u7ed3\u6784\u8bbe\u8ba1\u7684\u5f3a\u5927\u9b45\u529b\u3002\u5176\u5b9e\u5728\u5173\u4e8e\u6700\u4f4e\u6676\u683c\u9519\u914d\u601d\u60f3\u8bbe\u8ba1\u7684\u5fae\u89c2\u7ed3\u6784\u5728\u9ad8\u71b5\u5408\u91d1\u3001\u590d\u5408\u6750\u6599\u4e2d\u5df2\u7ecf\u5927\u653e\u5f02\u5f69\uff0c\u5f88\u591a\u4e0e\u6b64\u76f8\u5173\u7684\u6210\u679c\u90fd\u5df2\u7ecf\u53d1\u8868\u5728\u4e86Nature\u6216\u8005Science\u5b50\u520a\u3002\u57fa\u4e8e\u6700\u4f4e\u6676\u683c\u9519\u914d\u7684\u5fae\u89c2\u7ed3\u6784\u8bbe\u8ba1\u53ef\u4ee5\u5927\u5e45\u5ea6\u63d0\u9ad8\u6750\u6599\u7684\u5f3a\u5ea6\uff0c\u540c\u65f6\u53c8\u4e0d\u635f\u5931\u5851\u6027\u3002\u53e6\u5916\uff0c\u8fd9\u4e00\u7ed3\u6784\u5728\u7ec6\u5316\u6676\u7c92\uff0c\u6297\u8f90\u7167\u7b49\u65b9\u9762\u90fd\u5c55\u793a\u51fa\u4e86\u975e\u51e1\u80fd\u529b\u3002\u5728\u8106\u6027\u6750\u6599\uff0c\u4f8b\u5982\u91d1\u5c5e\u95f4\u5316\u5408\u7269\uff0c\u9676\u74f7\u57fa\u590d\u5408\u6750\u6599\u7b49\u90fd\u5177\u6709\u975e\u5e38\u597d\u7684\u542f\u8fea\u610f\u4e49\u3002\u529f\u80fd\u6750\u6599\u7684\u7814\u7a76\u8005\u4e0d\u59a8\u4e5f\u53ef\u4ee5\u5c1d\u8bd5\u3002<\/p>\n<p>\u53c2\u8003\u6587\u732e\uff1a<\/p>\n<p>[1] Yanwen Zhang. Reassembled nanoprecipitates resisting radiation. News &amp; views, Nature Materials.<\/p>\n<p>[2] Suihe Jiang, Hui Wang, Yuan Wu et al. Ultrastrong steel via minimal lattice misfit and high-density nanoprecipitation. Nature.<\/p>\n<p>[3] Zhifeng Lei, Xiongjun Liu, Yuan Wu et al. Enhanced strength and ductility in a high-entropy alloy via ordered oxygen complexes. Nature.<\/p>\n<p>[4] Junheng Gao, Suihe Jiang, Huairuo Zhang et al. Facile route to bulk ultrafine-grain steels for high strength and ductility. Nature.<\/p>\n<p>[5] S.H. Jiang, X.Q. Xu, W. Li et al. Strain hardening mediated by coherent nanoprecipitates in ultrahigh-strength steels. Acta Mater.<\/p>\n<p>[6] Jinlong Du, Suihe Jiang, Peipei Cao et al. Superior radiation tolerance via reversible disordering\u2013ordering transition of coherent superlattices. Nature Mater.<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u8fd1\u65e5\uff0c\u5415\u662d\u5e73\u6559\u6388\u8054\u5408\u5317\u5927\u4ed8\u6069\u521a\u6559\u6388\u56e2\u961f\u5728Nature materials\u671f\u520a\u4e0a\u53d1\u8868\u4e86\u5173\u4e8e\u57fa\u4e8e\u6700\u5c0f\u6676\u683c\u9519\u914d\u8d85\u9ad8\u5f3a\u5ea6\u94a2\u65b0\u7684\u6297\u8f90\u7167\u635f\u4f24\u673a\u5236\u7684\u91cd\u91cf\u7ea7\u7814\u7a76\u6210\u679c\u3002\u7acb\u5373\u5f15\u8d77\u5de8&#8230;<\/p>\n","protected":false},"author":34569,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[1187],"tags":[],"class_list":["post-238389","post","type-post","status-publish","format-standard","hentry","category-zhuanlan"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/238389"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/34569"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=238389"}],"version-history":[{"count":1,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/238389\/revisions"}],"predecessor-version":[{"id":238395,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/238389\/revisions\/238395"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=238389"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=238389"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=238389"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}