{"id":242805,"date":"2022-10-03T07:50:31","date_gmt":"2022-10-02T23:50:31","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=242805"},"modified":"2022-10-02T18:50:41","modified_gmt":"2022-10-02T10:50:41","slug":"%e5%8d%97%e6%b4%8b%e7%90%86%e5%b7%a5%e5%a4%a7%e5%ad%a6%e9%99%88%e6%99%93%e4%b8%9c%ef%bc%9a%e5%8a%9b%e5%ad%a6%e6%a2%af%e5%ba%a6%e7%94%b5%e6%9e%81%e8%a7%a3%e5%86%b3%e6%9c%ba%e6%a2%b0%e6%9f%94%e6%80%a7","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=242805","title":{"rendered":"\u5357\u6d0b\u7406\u5de5\u5927\u5b66\u9648\u6653\u4e1c\uff1a\u529b\u5b66\u68af\u5ea6\u7535\u6781\u89e3\u51b3\u673a\u68b0\u67d4\u6027-\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u4e0d\u5339\u914d\u96be\u9898"},"content":{"rendered":"<p>\u00a0\u00a0\u00a0\u00a0\u00a0\u4e00.\u3010\u5bfc\u8bfb\u3011<\/p>\n<p>\u8fd1\u5e74\u6765\uff0c\u968f\u7740\u67d4\u6027\u3001\u53ef\u7a7f\u6234\u7535\u5b50\u8bbe\u5907\u7684\u8fc5\u901f\u53d1\u5c55\uff0c\u4eba\u4eec\u5bf9\u4e8e\u67d4\u6027\u50a8\u80fd\u7cfb\u7edf\u7684\u9700\u6c42\u4e5f\u65e5\u76ca\u589e\u52a0\u3002\u53ef\u9760\u7684\u673a\u68b0\u67d4\u6027\u548c\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u662f\u67d4\u6027\u50a8\u80fd\u5668\u4ef6\u7684\u4e24\u4e2a\u5173\u952e\u6307\u6807\uff0c\u4f46\u540c\u65f6\u5b9e\u73b0\u8fd9\u4e24\u79cd\u6027\u80fd\u4ecd\u8f83\u4e3a\u56f0\u96be\u3002\u5bf9\u4e8e\u76ee\u524d\u5546\u4e1a\u5316\u7a0b\u5ea6\u8f83\u9ad8\u7684\u9502\u79bb\u5b50\u7535\u6c60\uff08LIBs\uff09\uff0c\u7ed3\u6784\u8bbe\u8ba1\u548c\u67d4\u6027\u57fa\u5e95\u5f00\u53d1\u662f\u7ec4\u88c5\u67d4\u6027LIBs\u7684\u4e24\u79cd\u4e3b\u8981\u65b9\u6cd5\uff0c\u867d\u7136\u8fd9\u4e9b\u65b9\u6cd5\u53ef\u4ee5\u6781\u5927\u63d0\u9ad8LIBs\u7684\u6297\u5f62\u53d8\u80fd\u529b\uff0c\u4f46\u5f15\u5165\u975e\u6d3b\u6027\u7684\u673a\u68b0\u7ed3\u6784\u6216\u57fa\u4f53\u6750\u6599\u4f1a\u964d\u4f4e\u7535\u6c60\u80fd\u91cf\u5bc6\u5ea6\uff0c\u5e76\u4e14\u5927\u591a\u6570\u67d4\u6027\u529b\u5b66\u7ed3\u6784\u6216\u6750\u6599\u5728\u7535\u538b&gt;3.5 V\u4e0b\u4f1a\u9010\u6e10\u53d1\u751f\u964d\u89e3\u3002\u51cf\u5c11\u7535\u6781\u8d1f\u8f7d\u91cf\u548c\u5236\u5907\u8584\u7535\u6781\u4e5f\u53ef\u4ee5\u63d0\u5347\u673a\u68b0\u67d4\u6027\uff0c\u4f46\u7535\u6c60\u80fd\u91cf\u5bc6\u5ea6\u4e5f\u4f1a\u5927\u5e45\u5ea6\u964d\u4f4e\u3002\u56e0\u6b64\uff0c\u4e9f\u9700\u4e00\u79cd\u7528\u6765\u5236\u5907\u540c\u65f6\u5177\u6709\u4f18\u5f02\u672c\u5f81\u67d4\u6027\u548c\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u7684\u7535\u6781\u7684\u6709\u6548\u7b56\u7565\u3002<\/p>\n<p>\u4e8c.\u3010\u6210\u679c\u63a0\u5f71\u3011<\/p>\n<p>\u7535\u6781\u7684\u672c\u5f81\u67d4\u6027\u53d6\u51b3\u4e8e\u5176\u6700\u5927\u627f\u53d7\u5e94\u53d8\u3002\u5f53\u7535\u6781\u5f2f\u66f2\u65f6\uff0c\u6240\u65bd\u52a0\u7684\u5f2f\u66f2\u5e94\u53d8\u4ece\u7535\u6781\u6d82\u5c42\u5e95\u5c42\uff08\u9760\u8fd1\u96c6\u6d41\u4f53\u4fa7\uff09\u5230\u9876\u5c42\u5448\u68af\u5ea6\u9012\u589e\u5206\u5e03\u3002\u5bf9\u4e8e\u4f20\u7edf\u5747\u5300\u7535\u6781\uff0c\u5176\u6700\u5927\u627f\u53d7\u5e94\u53d8\u4e3a\u5e38\u6570\uff0c\u5f53\u5f2f\u66f2\u5e94\u53d8\u8d85\u8fc7\u6700\u5927\u627f\u53d7\u5e94\u53d8\u65f6\uff0c\u7535\u6781\u5c06\u53d1\u751f\u65ad\u88c2\uff0c\u8fd9\u79cd\u73b0\u8c61\u5728\u539a\u7535\u6781\u4e2d\u5c24\u4e3a\u660e\u663e\u3002\u53d7\u6b64\u542f\u53d1\uff0c<strong>\u65b0\u52a0\u5761\u5357\u6d0b\u7406\u5de5\u5927\u5b66\u9648\u6653\u4e1c\u6559\u6388\u7b49\u4eba<\/strong>\u63d0\u51fa\u529b\u5b66\u68af\u5ea6\u7535\u6781\u7684\u6982\u5ff5\uff0c\u901a\u8fc7\u8c03\u63a7\u7535\u6781\u7684\u6700\u5927\u53ef\u627f\u53d7\u5e94\u53d8\u5206\u5e03\u4f7f\u5176\u4e0e\u5f2f\u66f2\u5e94\u53d8\u5206\u5e03\u76f8\u5339\u914d\uff0c\u8fdb\u800c\u63d0\u9ad8\u4e86\u7535\u6781\u7684\u672c\u5f81\u67d4\u6027\u3002\u8fd9\u4e00\u7b56\u7565\u4e0d\u9700\u7279\u5b9a\u7684\u7ed3\u6784\u8bbe\u8ba1\u6216\u5f15\u5165\u67d4\u6027\u57fa\u5e95\uff0c\u4e5f\u4e0d\u9700\u964d\u4f4e\u6d3b\u6027\u6750\u6599\u8d1f\u8f7d\u91cf\u6216\u7535\u6781\u539a\u5ea6\uff0c\u4ec5\u901a\u8fc7\u6539\u53d8\u7535\u6781\u6d82\u5c42\u4e2d\u7c98\u7ed3\u5242\u5360\u6bd4\u5206\u5e03\u5373\u53ef\u5b9e\u73b0\uff0c\u4ece\u800c\u5728\u4f7f\u529b\u5b66\u68af\u5ea6\u7535\u6781\u83b7\u5f97\u4f18\u5f02\u672c\u5f81\u67d4\u6027\u7684\u540c\u65f6\uff0c\u4ecd\u5177\u6709\u4e0e\u5747\u5300\u7535\u6781\u540c\u6c34\u5e73\u7684\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u3002\u4f5c\u8005\u5206\u522b\u8bbe\u8ba1\u4e86\u5177\u6709\u529b\u5b66\u68af\u5ea6\u9012\u589e\u768470 \u03bcm\u539a\u7684LiNi<sub>1\/3<\/sub>Mn<sub>1\/3<\/sub>Co<sub>1\/3<\/sub>O<sub>2<\/sub>\uff08NMC\uff0c~15 mg cm<sup>\u22122<\/sup>\uff09\u6b63\u6781\u548c105 \u03bcm\u539a\u7684\u77f3\u58a8\uff08~8 mg cm<sup>\u22122<\/sup>\uff09\u8d1f\u6781\uff0c\u5176\u5206\u522b\u53ef\u4ee5\u627f\u53d7400 \u03bcm\u548c600 \u03bcm\u7684\u66f2\u7387\u534a\u5f84\u3002\u6240\u6784\u5efa\u768460 mAh\u8f6f\u5305\u7535\u6c60\u5177\u67092 mAh cm<sup>\u22122<\/sup>\u7684\u9762\u79ef\u6bd4\u5bb9\u91cf\u4ee5\u53ca121.3 mWh cm<sup>\u22123<\/sup>\u7684\u80fd\u91cf\u5bc6\u5ea6\uff08\u76f8\u5bf9\u66f2\u7387\u534a\u5f84\uff09\uff0c\u5728\u91cd\u590d\u7684\u6298\u53e0-\u91ca\u653e\u53d8\u5f62\u4e0b\u53ef\u4ee5\u7a33\u5b9a\u5faa\u73af500\u5708\uff0892.3 %\u5bb9\u91cf\u4fdd\u6301\u7387\uff09\u3002\u5e76\u4e14\uff0c\u8be5\u529b\u5b66\u68af\u5ea6\u7535\u6781\u7684\u5236\u5907\u65b9\u6cd5\u4e0e\u5de5\u4e1a\u8bbe\u5907\u517c\u5bb9\uff0c\u53ef\u4ee5\u5f88\u5bb9\u6613\u5b9e\u73b0\u89c4\u6a21\u5316\u751f\u4ea7\u4e14\u4e0d\u53d7\u6750\u6599\u4f53\u7cfb\u9650\u5236\u3002\u76f8\u5173\u6210\u679c\u4ee5\u9898\u4e3a\u201c<strong>Mechano-Graded Electrodes Mitigate the Mismatch between Mechanical Reliability and Energy Density for Foldable Lithium-Ion Batteries<\/strong>\u201d\u53d1\u8868\u5728\u56fd\u9645\u9876\u7ea7\u671f\u520a\u201cAdvanced Materials\u201d\u4e0a\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-242806\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/09\/1664184959514.png\" alt=\"\" width=\"795\" height=\"383\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/09\/1664184959514.png 795w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/09\/1664184959514-300x145.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/09\/1664184959514-768x370.png 768w\" sizes=\"(max-width: 795px) 100vw, 795px\" \/><\/p>\n<p>\u4e09.\u3010\u6838\u5fc3\u521b\u65b0\u70b9\u3011<\/p>\n<ol>\n<li>\u6839\u636e\u7535\u6781\u5f2f\u66f2\u5931\u6548\u7406\u8bba\uff0c\u63d0\u51fa\u4e86\u529b\u5b66\u68af\u5ea6\u7535\u6781\u7684\u6982\u5ff5\uff08\u6700\u5927\u627f\u53d7\u5e94\u53d8\u5448\u68af\u5ea6\u5206\u5e03\u5e76\u4e0e\u5f2f\u66f2\u5e94\u53d8\u76f8\u5339\u914d\uff09\uff0c\u57fa\u4e8e\u529b\u5b66\u68af\u5ea6\u7535\u6781\u7684\u8f6f\u5305\u9502\u79bb\u5b50\u7535\u6c60\u540c\u65f6\u5177\u5907\u4f18\u5f02\u7684\u673a\u68b0\u67d4\u6027\u548c\u9ad8\u80fd\u91cf\u5bc6\u5ea6\uff1b<\/li>\n<li>\u529b\u5b66\u68af\u5ea6\u7535\u6781\u7684\u5236\u9020\u4e0e\u5de5\u4e1a\u5316\u8bbe\u5907\u76f8\u517c\u5bb9\uff0c\u642d\u914droll-to-roll\u6613\u5b9e\u73b0\u89c4\u6a21\u5316LIBs\u7535\u6781\u5236\u9020\uff0c\u4e14\u4e0d\u53d7\u6750\u6599\u4f53\u7cfb\u9650\u5236\u3002<\/li>\n<\/ol>\n<p>\u56db.\u3010\u6570\u636e\u6982\u89c8\u3011<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-242807\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/09\/\u56fe1-3.jpg\" alt=\"\" width=\"533\" height=\"415\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/09\/\u56fe1-3.jpg 533w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/09\/\u56fe1-3-300x234.jpg 300w\" sizes=\"(max-width: 533px) 100vw, 533px\" \/><\/p>\n<p>\u56fe1. \u529b\u5b66\u68af\u5ea6\u7535\u6781\u7684\u8bbe\u8ba1\u539f\u7406\u3002<\/p>\n<p>\uff08a\uff09\u4f20\u7edf\u5747\u5300\u7535\u6781\u7684\u673a\u68b0\u67d4\u6027\u548c\u80fd\u91cf\u5bc6\u5ea6\u4e4b\u95f4\u7684\u4e0d\u5339\u914d\uff0c\u8fd9\u79cd\u4e0d\u5339\u914d\u914d\u5728\u539a\u7535\u6781\u4e2d\u5c24\u4e3a\u660e\u663e\uff1b\uff08b\uff09\u4e0d\u540c\u66f2\u7387\u534a\u5f84\u4e0b\u7684\u5e94\u53d8\u5206\u5e03\u5206\u6790\uff0c\u5f2f\u66f2\u5e94\u53d8\u6cbf\u7535\u6781\u6d82\u5c42\u5e95\u5c42\u81f3\u9876\u5c42\u5448\u68af\u5ea6\u9012\u589e\u5206\u5e03\uff1b\uff08c\uff09\u5747\u5300\u7535\u6781\u548c\uff08d\uff09\u529b\u5b66\u68af\u5ea6\u9012\u589e\u7535\u6781\u7684\u6700\u5927\u627f\u53d7\u5e94\u53d8\u5206\u5e03\u4ee5\u53ca\u76f8\u5e94\u7684\u5f2f\u66f2\u5e94\u53d8\u5206\u5e03\u3002\u00a9Year The Authors<\/p>\n<p>&nbsp;<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-242808\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/09\/\u56fe2-1.jpg\" alt=\"\" width=\"578\" height=\"487\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/09\/\u56fe2-1.jpg 578w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/09\/\u56fe2-1-300x253.jpg 300w\" sizes=\"(max-width: 578px) 100vw, 578px\" \/><\/p>\n<p>\u56fe2. \u529b\u5b66\u68af\u5ea6\u9012\u589e\/\u9012\u51cf\u548c\u5747\u5300\u7535\u6781\u7684\u793a\u610f\u56fe\u548c\u5149\u5b66\u663e\u5fae\u955c\u56fe\u7247\u3002<\/p>\n<p>\uff08a-c\uff09\u529b\u5b66\u68af\u5ea6\u9012\u589e\uff0c\u5747\u5300\uff0c\u529b\u5b66\u68af\u5ea6\u9012\u51cf\u7535\u6781\u793a\u610f\u56fe\uff1b\uff08d\uff0ce\uff09\u5f2f\u6298\u6761\u4ef6\u4e0b\uff0c\u529b\u5b66\u68af\u5ea6\u548c\u5747\u5300\u7535\u6781\u7684\u5149\u5b66\u663e\u5fae\u955c\u7167\u7247\uff0c\uff08d\uff09\u6b63\u6781\u548c\uff08e\uff09\u8d1f\u6781\u539a\u5ea6\u5206\u522b\u4e3a70\u00b15 \u03bcm\u548c105\u00b110 \u03bcm\uff0c\u6b63\u6781\u548c\u8d1f\u6781\u7684\u66f2\u7387\u534a\u5f84\u5206\u522b\u4e3a400 \u03bcm\u548c600 \u03bcm\u3002\u00a9Year The Authors<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-242809\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/09\/\u56fe3-3.jpg\" alt=\"\" width=\"605\" height=\"551\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/09\/\u56fe3-3.jpg 605w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/09\/\u56fe3-3-300x273.jpg 300w\" sizes=\"(max-width: 605px) 100vw, 605px\" \/><\/p>\n<p>\u56fe3. \u7535\u6781\u7684\u53ef\u5f2f\u6298\u6027\u7684\u91cf\u5316\u53ca\u673a\u68b0\u5931\u6548\u673a\u5236\u3002<\/p>\n<p>\uff08a\uff09\u529b\u5b66\u68af\u5ea6\u548c\uff08b\uff09\u5747\u5300\u7535\u6781\u7684\u53ef\u5f2f\u6298\u6027\u7684\u6bd4\u8f83\u3002\u4e09\u7ef4\u7b49\u9ad8\u7ebf\u56fe\u8868\u793a\u5177\u6709\u4e0d\u540c\u7c98\u7ed3\u5242\u6bd4\u4f8b\u548c\u7535\u6781\u539a\u5ea6\u7684\u5747\u5300\u7535\u6781\u7684\u5f2f\u66f2\u5ea6\uff0c\u901a\u8fc7\u9010\u6e10\u51cf\u5c0f\u5f2f\u66f2\u534a\u5f84\uff0c\u8bb0\u5f55\u4ea7\u751f\u88c2\u7eb9\u65f6\u7684\u5f2f\u66f2\u534a\u5f84\uff0c\u53ef\u5b9e\u73b0\u7535\u6781\u6700\u5927\u66f2\u7387\u7684\u91cf\u5316\uff0c\u68af\u5ea6\u7535\u6781\u8bbe\u8ba1\u8868\u660e\u6b63\u8d1f\u6781\u7684\u5f2f\u66f2\u5ea6\u5747\u5f97\u5230\u63d0\u9ad8\uff1b\uff08c\uff09\u7535\u6781\u5f2f\u66f2\u8fc7\u7a0b\u4e2d\u5e94\u53d8\u5206\u5e03\u7684\u6709\u9650\u5143\u5206\u6790\u7ed3\u679c\uff0c\u5728\u521d\u59cb\u9636\u6bb5\uff0c\u6700\u5927\u5e94\u53d8\u96c6\u4e2d\u5728\u9876\u5c42\uff0c\u88c2\u7eb9\u4ea7\u751f\u540e\uff0c\u5e94\u53d8\u5c06\u96c6\u4e2d\u5728\u88c2\u7eb9\u5c16\u7aef\uff0c\u5e76\u5bfc\u81f4\u88c2\u7eb9\u5feb\u901f\u6269\u6563\uff0c\u5f53\u88c2\u7eb9\u5230\u8fbe\u57fa\u4f53\u65f6\uff0c\u6700\u5927\u5e94\u53d8\u5c06\u6cbf\u7740\u6d3b\u6027\u6750\u6599\u5c42\u4e0e\u57fa\u4f53\u4e4b\u95f4\u7684\u754c\u9762\u4f20\u64ad\uff0c\u5bfc\u81f4\u5265\u79bb\u3002\u00a9Year The Authors<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-242810\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/09\/\u56fe4-1.jpg\" alt=\"\" width=\"605\" height=\"592\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/09\/\u56fe4-1.jpg 605w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/09\/\u56fe4-1-300x294.jpg 300w\" sizes=\"(max-width: 605px) 100vw, 605px\" \/><\/p>\n<p>\u56fe4. \u529b\u5b66\u68af\u5ea6\u9012\u589e\/\u9012\u51cf\u548c\u68af\u5ea6\u5747\u5300\u7535\u6781\u7684\u7efc\u5408\u6027\u80fd\u8bc4\u4f30\u3002<\/p>\n<p>\uff08a\uff0cb\uff09\u4e09\u79cd\u7535\u6781\u6298\u53e0\u540e\u7684\u7535\u5316\u5b66\u7a33\u5b9a\u6027\u3002\uff08a\uff09\u5bf9\u4e8e\u9996\u6b21\u5faa\u73af\u7684\u653e\u7535\u5bb9\u91cf\uff0c\u529b\u5b66\u68af\u5ea6\u9012\u589e\u6b63\u6781\u548c\u8d1f\u6781\u7684\u653e\u7535\u5bb9\u91cf\u90fd\u7565\u9ad8\u4e8e\u529b\u5b66\u9012\u51cf\u7535\u6781\u548c\u5747\u5300\u7535\u6781\uff0c\u7ecf\u8fc7220\u6b21\u5faa\u73af\u540e\uff0c\u529b\u5b66\u68af\u5ea6\u9012\u589e\u6b63\u6781\u7684\u5bb9\u91cf\u4fdd\u6301\u7387\u4e5f\u5747\u9ad8\u4e8e\u529b\u5b66\u9012\u51cf\u7535\u6781\u548c\u5747\u5300\u7535\u6781\uff1b\uff08b\uff09\u57fa\u4e8e\u771f\u5b9e\u80fd\u91cf\u5bc6\u5ea6\uff08Ea\uff09\u4e0e\u5f2f\u66f2\u534a\u5f84\uff08r\uff09\u7684\u54c1\u8d28\u56e0\u7d20Ea\/r\u53ef\u7528\u6765\u6807\u51c6\u5316\u6bd4\u8f83\u67d4\u6027LIBs\u7684\u6027\u80fd\uff0c\u5bf9\u6bd4\u4e0d\u540c\u539a\u5ea6\u7684\u5404\u79cd\u7535\u6c60\u4f53\u7cfb\uff0cFOM\u8d8a\u9ad8\u8868\u793a\u7efc\u5408\u6027\u80fd\u8d8a\u597d\u3002\u00a9Year The Authors<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-242811\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/09\/\u56fe5-1.jpg\" alt=\"\" width=\"605\" height=\"771\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/09\/\u56fe5-1.jpg 605w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/09\/\u56fe5-1-235x300.jpg 235w\" sizes=\"(max-width: 605px) 100vw, 605px\" \/><\/p>\n<p>\u56fe5. \u57fa\u4e8e\u529b\u5b66\u68af\u5ea6\u9012\u589e\u7535\u6781\u7684\u8f6f\u5305\u5168\u7535\u6c60\u6027\u80fd\u3002<\/p>\n<p>\uff08a\uff09\u8f6f\u5305\u5168\u7535\u6c60\uff08~60 mAh\uff09\u5728\u91cd\u590d\u6298\u53e0\u548c\u7535\u5316\u5b66\u5faa\u73af\u4e0b\u7684\u7a33\u5b9a\u6027\uff080.06mA cm<sup>\u22122<\/sup>\uff09\uff1b\uff08b\uff09520\u5708\u5faa\u73af\u8fc7\u7a0b\u7684\u5bb9\u91cf\u53d8\u5316\uff0c\u524d50\u5708\u5faa\u73af\u7684\u6027\u80fd\u5982\u56fe\uff08a\uff09\u6240\u793a\uff0c\u7b2c50\u5708\u540e\uff0c\u4ee5\u91ca\u653e\u72b6\u6001\u548c0.6 mA cm<sup>\u22122<\/sup>\u7684\u7535\u6d41\u5bc6\u5ea6\u5faa\u73af\uff0c\u7ecf\u8fc7\u7b2c500\u5708\u5faa\u73af\u540e\uff0c\u7535\u6d41\u5bc6\u5ea6\u964d\u4f4e\u52300.06 mA cm<sup>\u22122<\/sup>\uff1b\uff08c\uff09\u8f6f\u5305\u7535\u6c60\u5728\u626d\u8f6c\u3001\u6298\u53e0\u548c\u6253\u7ed3\u6761\u4ef6\u4e0b\u4ecd\u53ef\u4e3a\u5e76\u8054led\u63d0\u4f9b\u7a33\u5b9a\u7684\u7535\u80fd\u3002<\/p>\n<p>\u00a9Year The Authors<\/p>\n<p>\u4e94.\u3010\u6210\u679c\u542f\u793a\u3011<\/p>\n<p>\u672c\u6587\u901a\u8fc7\u91c7\u7528\u529b\u5b66\u68af\u5ea6\u7535\u6781\u7684\u7b56\u7565\uff0c\u8c03\u548c\u4e86\u7535\u6781\u672c\u5f81\u67d4\u6027\u4e0e\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u4e4b\u95f4\u7684\u4e0d\u5339\u914d\uff0c\u5de7\u5999\u7684\u83b7\u5f97\u4e86\u517c\u5177\u4f18\u5f02\u672c\u5f81\u673a\u68b0\u67d4\u6027\u548c\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u7684\u7535\u6781\u3002\u529b\u5b66\u68af\u5ea6\u7535\u6781\u7684\u7ec4\u88c5\u6d41\u7a0b\u4e0e\u5de5\u4e1aLIBs\u751f\u4ea7\u8bbe\u5907\u517c\u5bb9\uff0c\u6613\u5b9e\u73b0\u89c4\u6a21\u5316\u751f\u4ea7\u3002\u4e0d\u4ec5\u5982\u6b64\uff0c\u8be5\u7b56\u7565\u5e76\u4e0d\u53d7\u9650\u4e8e\u6750\u6599\u4f53\u7cfb\uff0c\u53ef\u6839\u636e\u4e0d\u540c\u7c7b\u578b\u7684\u67d4\u6027\u7535\u5b50\u8bbe\u5907\u6765\u8bbe\u8ba1\u76f8\u5e94\u7684\u50a8\u80fd\u7cfb\u7edf\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u539f\u6587\u8be6\u60c5\uff1aXiang Ge, Shengkai Cao, Zhisheng Lv, Zhiqiang Zhu, Yuxin Tang, Huarong Xia, Hongwei Zhang, Jiaqi Wei, Wei Zhang, Yanyan Zhang, Yi Zeng, Xiaodong Chen*, Mechano-Graded Electrodes Mitigate the Mismatch between Mechanical Reliability and Energy Density for Foldable Lithium-Ion Batteries, https:\/\/doi.org\/10.1002\/adma.202206797.<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u00a0\u00a0\u00a0\u00a0\u00a0\u4e00.\u3010\u5bfc\u8bfb\u3011 \u8fd1\u5e74\u6765\uff0c\u968f\u7740\u67d4\u6027\u3001\u53ef\u7a7f\u6234\u7535\u5b50\u8bbe\u5907\u7684\u8fc5\u901f\u53d1\u5c55\uff0c\u4eba\u4eec\u5bf9\u4e8e\u67d4\u6027\u50a8\u80fd\u7cfb\u7edf\u7684\u9700\u6c42\u4e5f\u65e5\u76ca\u589e\u52a0\u3002\u53ef\u9760\u7684\u673a\u68b0\u67d4\u6027\u548c\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u662f\u67d4\u6027\u50a8\u80fd\u5668\u4ef6\u7684\u4e24\u4e2a\u5173\u952e\u6307\u6807&#8230;<\/p>\n","protected":false},"author":36637,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215,67],"tags":[],"class_list":["post-242805","post","type-post","status-publish","format-standard","hentry","category-jiedu","category-zhoubao"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/242805"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/36637"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=242805"}],"version-history":[{"count":1,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/242805\/revisions"}],"predecessor-version":[{"id":242812,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/242805\/revisions\/242812"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=242805"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=242805"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=242805"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}