{"id":242966,"date":"2022-10-10T07:35:50","date_gmt":"2022-10-09T23:35:50","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=242966"},"modified":"2022-10-09T20:01:20","modified_gmt":"2022-10-09T12:01:20","slug":"%e3%80%90%e9%80%9a%e8%ae%af%e6%a0%a1%e7%a8%bf%e6%9c%aa%e5%9b%9e%e5%a4%8d%e3%80%91%e4%bf%9e%e4%b9%a6%e5%ae%8f%e5%9b%a2%e9%98%9f%e6%9c%80%e6%96%b0am%ef%bc%9a-%e7%ba%b3%e7%b1%b3%e7%ba%bf%e8%96%84","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=242966","title":{"rendered":"\u4fde\u4e66\u5b8f\u56e2\u961f\u6700\u65b0AM\uff1a \u7eb3\u7c73\u7ebf\u8584\u819c\u53cc\u9762\u795e\u87ba\u65cb\u5e26\u7ed3\u6784\u53ef\u7528\u4e8e\u5236\u9020\u9ad8\u6027\u80fd\u67d4\u6027\u592a\u9633\u80fd\u70ed\u7535\u5668\u4ef6"},"content":{"rendered":"<p><strong>\u3010\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p>\u592a\u9633\u80fd\u70ed\u7535\uff08STE\uff09\u5668\u4ef6\u53ef\u5728\u4e0d\u4ea7\u751f\u6e29\u5ba4\u6c14\u4f53\u7684\u60c5\u51b5\u4e0b\u5c06\u5149\/\u70ed\u8f6c\u6362\u6210\u7535\u529b\u3002\u5728\u8fd9\u4e00\u4f53\u7cfb\u4e2d\uff0c\u5668\u4ef6\u7684\u80fd\u91cf\u8f6c\u6362\u6548\u7387\u4e0d\u4ec5\u53d6\u51b3\u4e8e\u70ed\u7535\u6750\u6599\uff0c\u4e5f\u9ad8\u5ea6\u4f9d\u8d56\u4e8e\u70ed\u7535\u81c2\u4e0a\u7684\u6e29\u5ea6\u68af\u5ea6\uff08\u0394T\uff09\u3002\u8fc7\u53bb\u5341\u5e74\u91cc\uff0c\u4eba\u4eec\u5df2\u7ecf\u5f00\u53d1\u4e86\u591a\u79cd\u7b56\u7565\uff08\u5305\u62ec\u70ed\u7535\u81c2\u4e0a\u5b9e\u73b0\u70ed\u963b\u6297\u4ee5\u53ca\u5728\u70ed\u7535\u5668\u4ef6\u7684\u51b7\u70ed\u4e24\u7aef\u8fdb\u884c\u6e29\u5ea6\u7ba1\u7406\u7b49\uff09\u4ee5\u5b9e\u73b0\u663e\u8457\u7684\u6e29\u5ea6\u68af\u5ea6\u3002\u7136\u800c\uff0c\u8fd9\u4e9b\u7b56\u7565\u5728\u5927\u5c3a\u5bf8\u5e94\u7528\u4e2d\u6210\u672c\u5267\u589e\uff0c\u4e14\u8fd8\u65e0\u6cd5\u5728\u5e72\u71e5\u73af\u5883\u4e2d\u4fdd\u6301\u8f83\u4f4e\u7684\u51b7\u7aef\uff08cold side\uff09\u6e29\u5ea6\uff0c\u4e5f\u5c31\u662f\u8bf4\uff0c\u5728\u5927\u5c3a\u5bf8\u5e94\u7528\u4e2d\u9ad8\u6548\u7ef4\u6301\u7406\u60f3\u7684\u6e29\u5ea6\u68af\u5ea6\u76ee\u524d\u6765\u770b\u4f9d\u7136\u662f\u4e00\u4e2a\u8270\u5de8\u7684\u6311\u6218\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u65e5\u95f4\u88ab\u52a8\u8f90\u5c04\u5236\u51b7\uff08PDRC\uff09\u6280\u672f\u662f\u4e00\u9879\u65b0\u5174\u7684\u53ef\u89c4\u6a21\u5316\u5236\u51b7\u6280\u672f\u3002\u5728\u8fd9\u4e00\u6280\u672f\u4e2d\uff0cPDRC\u6750\u6599\u80fd\u591f\u53cd\u5c04\u51e0\u4e4e\u5168\u592a\u9633\u5149\u8c31\uff080.28-2.5 \u03bcm\uff09\u4ee5\u6291\u5236\u6e29\u5ea6\u4e0a\u5347\uff0c\u751a\u81f3\u5728\u65e0\u9700\u989d\u5916\u80fd\u91cf\u8f93\u5165\u7684\u65f6\u5019\u8fd8\u80fd\u8fbe\u5230\u4f4e\u4e8e\u5468\u56f4\u6e29\u5ea6\u7684\u6c34\u5e73\u3002\u56e0\u6b64\uff0c\u901a\u8fc7\u67d4\u6027PDRC\u8584\u819c\u6709\u671b\u589e\u52a0\u70ed\u7535\u5668\u4ef6\u51b7\u7aef\u7684\u70ed\u8017\u6563\u3002\u4e0e\u6b64\u540c\u65f6\uff0c\u9009\u62e9\u6027\u592a\u9633\u80fd\u5438\u6536\u6280\u672f\uff08SSA\uff09\u7684\u51fa\u73b0\u5219\u6709\u5229\u4e8e\u62ac\u5347STE\u70ed\u7aef\uff08hot side\uff09\u7684\u6e29\u5ea6\u3002\u56e0\u6b64\uff0c\u5c06PDRC\u548cSSA\u6280\u672f\u7ed3\u5408\u5728\u4e00\u8d77\u6709\u671b\u83b7\u5f97\u66f4\u5927\u7684\u6e29\u5ea6\u68af\u5ea6\uff0c\u4ece\u800c\u6539\u5584STE\u5668\u4ef6\u6027\u80fd\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u63a0\u5f71\u3011<\/strong><\/p>\n<p>\u8fd1\u671f\uff0c<strong>\u4e2d\u79d1\u5927\u4fde\u4e66\u5b8f\u6559\u6388\u548c\u5218\u5efa\u4f1f\u6559\u6388<\/strong>\uff08\u5171\u540c\u901a\u8baf\u4f5c\u8005\uff09\u7b49\u4eba\u8bbe\u8ba1\u4e86\u4e00\u79cd\u67d4\u6027\u7684\u4e09\u7ef4\u53cc\u9762\u87ba\u65cb\u5e26\u7ed3\u6784\u3002\u5728\u8fd9\u4e00\u7ed3\u6784\u4e2d\uff0c\u6392\u5217\u826f\u597d\u7684\u78b2\uff08Te\uff09\u7eb3\u7c73\u7ebf\u8584\u819c\u4e0eAg<sup>+<\/sup>\u548cCu<sup>2+<\/sup>\u53d1\u751f\u539f\u4f4d\u6c27\u5316\u8fd8\u539f\u8fc7\u7a0b\uff0c\u6700\u7ec8\u5728\u4e00\u5f20\u8584\u819c\u4e0a\u540c\u65f6\u4ea7\u751f<em>n<\/em>\u578b\u3001<em>p<\/em>\u578b\u548c\u5149\u70ed\u7aef\u3002\u901a\u8fc7\u5c06\u51b7\u7aef\u4e0e\u88ab\u52a8\u8f90\u5c04\u5236\u51b7\u6280\u672f\u7ed3\u5408\u3001\u70ed\u7aef\u4e0eSSA\u6280\u672f\u7ed3\u5408\uff0c\u8be5\u7ed3\u6784\u53ef\u5b9e\u73b0\u5168\u5929\u5019\u53d1\u7535\u548c\u663e\u8457\u6e29\u5ea6\u68af\u5ea6\uff08\u0394T=29.5 K\uff09\u3002\u56e0\u6b64\uff0c\u4f5c\u8005\u8ba4\u4e3a\uff0c\u8fd9\u4e00\u8bbe\u8ba1\u7b56\u7565\u4e3a\u9ad8\u6548\u70ed\u7ba1\u7406\u63d0\u4f9b\u4e86\u4e00\u79cd\u65b0\u7684\u601d\u8def\u3002\u8be5\u6587\u5171\u540c\u7b2c\u4e00\u4f5c\u8005\u4e3aCheng Chen\u548cBin Zhao\uff0c\u6587\u7ae0\u4ee5\u9898\u4e3a<strong>\u201cJanus Helical Ribbon Structure of Ordered Nanowire Films for Flexible Solar Thermoelectric Devices\u201d<\/strong>\u53d1\u5e03\u5728\u56fd\u9645\u8457\u540d\u671f\u520a<strong><em>Advanced Materials<\/em><\/strong>\u4e0a\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-242973\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/\u9898\u56fe.jpg\" alt=\"\" width=\"600\" height=\"250\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/\u9898\u56fe.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/\u9898\u56fe-300x125.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u3010\u6838\u5fc3\u521b\u65b0\u70b9\u3011<\/strong><\/p>\n<p>1.\u7814\u7a76\u5229\u7528PDRC\u548cSSA\u6280\u672f\u5b9e\u73b0\u4e86\u9ad8\u8fbe29.5K\u7684\u70ed\u7535\u5668\u4ef6\u6e29\u5ea6\u68af\u5ea6\u3002<\/p>\n<ol start=\"2\">\n<li>\u4e3a\u4e86\u5c06PDRC\u548cSSA\u6280\u672f\u6574\u5408\u5230\u540c\u4e00\u5668\u4ef6\u4e0a\uff0c\u7814\u7a76\u63d0\u51fa\u4e86\u4e00\u79cd\u53cc\u9762\u795e\u87ba\u65cb\u7ed3\u6784\uff0c\u901a\u8fc7\u5728\u6709\u5e8f\u7eb3\u7c73\u7ebf\u8584\u819c\u4e0a\u8fdb\u884c\u539f\u4f4d\u6c27\u5316\u8fd8\u539f\u53cd\u5e94\u6784\u5efa\u4e86<em>n<\/em>\u578b\u3001<em>p<\/em>\u578b\u548c\u5149\u70ed\u7aef\u3002<\/li>\n<\/ol>\n<p><strong>\u3010\u56fe\u6587\u89e3\u8bfb\u3011<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-242967\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/1.jpg\" alt=\"\" width=\"568\" height=\"573\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/1.jpg 568w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/1-150x150.jpg 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/1-297x300.jpg 297w\" sizes=\"(max-width: 568px) 100vw, 568px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>1.<\/strong> <strong>\u87ba\u65cb\u592a\u9633\u80fd\u70ed\u7535\u5e26\u7684\u539f\u7406\u53ca\u5236\u9020\u8fc7\u7a0b\u3002<\/strong><strong>\u00a9 1999-2022 John Wiley &amp; Sons, Inc.<\/strong><\/p>\n<p>\uff08a\uff09\u87ba\u65cbSTE\u5668\u4ef6\u7684\u539f\u7406\u548c\u7ed3\u6784\uff1b<\/p>\n<p>\uff08b\uff09\u67d4\u6027\u87ba\u65cbSTE\u5668\u4ef6\u7684\u5236\u9020\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-242969\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/2.jpg\" alt=\"\" width=\"600\" height=\"337\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/2.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/2-300x169.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>2. <\/strong><strong>PDRC<\/strong><strong>\u8584\u819c\u7684\u8868\u5f81\u548c\u5ba4\u5916\u6d4b\u8bd5<\/strong><strong>\u3002<\/strong><strong>\u00a91999-2022 John Wiley &amp; Sons, Inc.<\/strong><\/p>\n<p>\uff08a\uff09ESR\u8584\u819c\u3001PDRC\u8584\u819c\u548c\u94f6\u8584\u819c\u7684\u8026\u5408\u9ad8\u53cd\u5c04\u6027\u8d28\uff1b<\/p>\n<p>\uff08b\uff09\u89d2\u5206\u5e03\u5206\u6790\uff1b<\/p>\n<p>\uff08c\uff09\u5bf9ESR\u8584\u819c\u3001PDRC\u8584\u819c\u548c\u94f6\u8584\u819c\u7684\u5b9e\u65f6\u6d4b\u91cf\uff1b<\/p>\n<p>\uff08d\uff09ESR\u8584\u819c\u3001PDRC\u8584\u819c\u548c\u94f6\u8584\u819c\u5728\u65e5\u95f4\u7684\u5b9e\u65f6\u6e29\u5ea6\uff1b<\/p>\n<p>\uff08e\uff09ESR\u8584\u819c\u3001PDRC\u8584\u819c\u548c\u94f6\u8584\u819c\u5728\u591c\u95f4\u7684\u5b9e\u65f6\u6e29\u5ea6\u3002<\/p>\n<p><strong>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-242970\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/3.jpg\" alt=\"\" width=\"600\" height=\"393\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/3.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/3-300x197.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/strong><\/p>\n<p><strong>\u56fe<\/strong><strong>3. SSA<\/strong><strong>\u8584\u819c\u8868\u5f81\u3002<\/strong><strong>\u00a9 1999-2022 John Wiley &amp; Sons, Inc.<\/strong><\/p>\n<p>\uff08a\uff09\u78b2\u7eb3\u7c73\u7ebf\u5c42SEM\u4fa7\u89c6\u56fe\uff1b<\/p>\n<p>\uff08b\uff09Ag<sub>2<\/sub>Te\u7ebf\u5c42\u7684\u4f4e\u500dSEM\uff1b<\/p>\n<p>\uff08c\uff09\u00a0Ag<sub>2<\/sub>Te\u7ebf\u5c42\u7684\u9ad8\u500dSEM\uff1b<\/p>\n<p>\uff08d\uff09\u94f6\u8584\u819c\u4e0e\u78b2\u7eb3\u7c73\u7ebf\u8584\u819c\u7684\u53cd\u5e94\u793a\u610f\u56fe\uff1b<\/p>\n<p>\uff08e\uff09SSA\u3001\u78b2\u7eb3\u7c73\u7ebf\u8584\u819c\u548cBB paint\u8584\u819c\u7684\u7279\u5f81\u5438\u6536\uff08\u4ece\u7d2b\u5916\u5230\u4e2d\u7ea2\u5916\uff09\uff1b<\/p>\n<p>\uff08f\uff09\u5728\u4e00\u4e2a\u592a\u9633\u5f3a\u5ea6\u4e0b\u8f90\u7167\u4e00\u6bb5\u65f6\u95f4\u7684SSA\u548cBB paint\u8584\u819c\u7684\u6e29\u5ea6\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-242971\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/4.jpg\" alt=\"\" width=\"600\" height=\"313\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/4.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/4-300x157.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>4. <\/strong><strong>\u5ba4\u6e29\u4e0b\u7eb3\u7c73\u7ebf\u7684\u8868\u5f81\u53ca<\/strong><strong>STE<\/strong><strong>\u6027\u80fd<\/strong><strong>\u00a0<\/strong><strong>\u3002<\/strong><strong>\u00a9 1999-2022 John Wiley &amp; Sons, Inc.<\/strong><\/p>\n<p>\uff08a\uff09<em>n<\/em>\u578bAg<sub>2<\/sub>Te\u7eb3\u7c73\u7ebf\u7684TEM\uff1b<\/p>\n<p>\uff08b\uff09<em>p<\/em>\u578bCu<sub>1.75<\/sub>Te\u7eb3\u7c73\u7ebf\u7684TEM\uff1b<\/p>\n<p>\uff08c\uff09\u00a0\u6709\u5e8f\/\u65e0\u5e8fCu<sub>1.75<\/sub>Te\u7eb3\u7c73\u7ebf\u8584\u819c\u4e0d\u540c\u53cd\u5e94\u65f6\u95f4\u7684\u7535\u5bfc\u7387\u53d8\u5316\uff1b<\/p>\n<p>\uff08d\uff09\u6709\u5e8f\/\u65e0\u5e8fAg<sub>2<\/sub>Te\u7eb3\u7c73\u7ebf\u8584\u819c\u4e0d\u540c\u53cd\u5e94\u65f6\u95f4\u7684\u7535\u5bfc\u7387\u53d8\u5316\uff1b<\/p>\n<p>\uff08e\uff09\u53cd\u5e94150s\u540e\u6709\u5e8f\/\u65e0\u5e8f\u7eb3\u7c73\u7ebf\u7684Seebeck\u7cfb\u6570\uff1b<\/p>\n<p>\uff08f\uff09\u53cd\u5e94150s\u540e\u6709\u5e8f\/\u65e0\u5e8f\u7eb3\u7c73\u7ebf\u7684\u529f\u7387\u56e0\u5b50\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-242972\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/5.jpg\" alt=\"\" width=\"600\" height=\"293\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/5.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/5-300x147.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>5. <\/strong><strong>STE<\/strong><strong>\u5ba4\u5916\u6027\u80fd<\/strong><strong>\u00a0<\/strong><strong>\u3002<\/strong><strong>\u00a9 1999-2022 John Wiley &amp; Sons, Inc.<\/strong><\/p>\n<p>\uff08a\uff09STE\u8bb0\u5f55\u53d1\u7535\u5b9e\u65f6\u6027\u80fd\u7684\u88c5\u7f6e\uff1b<\/p>\n<p>\uff08b\uff09STE\u5668\u4ef6\u6d4b\u91cfU<sub>oc<\/sub>\uff1b<\/p>\n<p>\uff08c\uff09\u00a0\u5168\u5929\u5b9e\u65f6I<sub>solar<\/sub>\uff1b<\/p>\n<p>\uff08d\uff09\u76f8\u5bf9\u6e7f\u5ea6\u548c\u5468\u56f4\u6e29\u5ea6\uff1b<\/p>\n<p>\uff08e\uff09STE\u5668\u4ef6\u5ba4\u5916\u6d4b\u91cf\u7684U<sub>oc<\/sub>\u6570\u636e\uff1b<\/p>\n<p>\uff08f\uff09\u70ed\u7535\u81c2\u7684\u6e29\u5ea6\u5206\u5e03\uff1b<\/p>\n<p>\uff08g\uff09STE\u5668\u4ef6\u7684\u0394T\u3002<\/p>\n<p><strong>\u3010\u7ed3\u8bba\u4e0e\u5c55\u671b\u3011<\/strong><\/p>\n<p>\u603b\u4e4b\uff0c\u8be5\u7814\u7a76\u901a\u8fc7\u7eb3\u7c73\u7ebf\u7684\u539f\u4f4d\u53cd\u5e94\uff0c\u5c06PDRC\u548cSSA\u6280\u672f\u76f8\u7ed3\u5408\uff0c\u5b9e\u73b0STE\u7684\u9ad8\u7535\u529b\u8f93\u51fa\u548c\u5168\u5929\u5019\u53d1\u7535\u3002\u4e00\u65b9\u9762\uff0c\u51b7\u7a7a\u95f4\u4f5c\u4e3a\u4e00\u4e2a\u5de8\u5927\u7684\u6563\u70ed\u5668\uff0c\u4f1a\u5f15\u53d1\u66f4\u591a\u7684\u51b7\u7aef\u70ed\u8f90\u5c04\u3002\u53e6\u4e00\u65b9\u9762\uff0cSSA\u6280\u672f\u5219\u53ef\u9632\u6b62\u70ed\u7aef\u70ed\u91cf\u635f\u5931\u5230\u51b7\u7a7a\u95f4\u4e2d\u3002\u56e0\u6b64\uff0c\u66f4\u9ad8\uff08\u592a\u9633\u8f90\u5c04\u4e3a614 W m<sup>-2<\/sup>\u65f6\u4e3a29.5 K\uff09\u548c\u5168\u5929\u5019\u0394T\u5c06\u5b9e\u73b0\u66f4\u591a\u548c\u6301\u7eed\u7684\u7535\u529b\u8f93\u51fa\u3002\u7814\u7a76\u8fd8\u6307\u51fa\uff0c\u5de5\u4e1a\u548c\u5efa\u7b51\u5e9f\u70ed\u4e5f\u53ef\u4ee5\u8fdb\u884c\u5f88\u597d\u7684\u5229\u7528\uff0c\u8fd9\u5c06\u8fdb\u4e00\u6b65\u6269\u5927\u5668\u4ef6\u7684\u5e94\u7528\u8303\u56f4\u3002\u4f5c\u8005\u6700\u540e\u8fd8\u5f3a\u8c03\uff0c\u8be5\u7814\u7a76\u6240\u63d0\u51fa\u7684\u5668\u4ef6\u8fd8\u8fdc\u672a\u8fbe\u5230\u6027\u80fd\u6781\u9650\uff0c\u5982\u82e5\u5728\u91c7\u7528\u8d85\u9ad8PF-TE\u6750\u6599\u3001\u4f18\u5316TE\u6a21\u5757\u7684\u7ed3\u6784\u548c\u5c3a\u5bf8\u3001\u6269\u5927PDRC\u548cSSA\u7684\u9762\u79ef\u7b49\u65b9\u9762\u80fd\u591f\u8fdb\u4e00\u6b65\u5b8c\u5584\u63d0\u5347\uff0c\u5668\u4ef6\u5c06\u6709\u671b\u8fdb\u4e00\u6b65\u63d0\u9ad8\u3002\u56e0\u6b64\uff0c\u7814\u7a76\u8ba4\u4e3a\u8be5\u5de5\u4f5c\u6240\u63d0\u51fa\u7684\u7b56\u7565\u53ef\u4ee5\u6700\u5927\u9650\u5ea6\u5730\u6355\u83b7\u548c\u6563\u53d1\u70ed\u91cf\uff0c\u4e3a\u5b9e\u73b0\u9002\u5e94\u6027\u548c\u9ad8\u6027\u80fd\u53d1\u7535\u8bbe\u5907\u63d0\u4f9b\u4e86\u4e00\u6761\u5168\u65b0\u7684\u9014\u5f84\u3002<\/p>\n<p><strong>\u00a0<\/strong><\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a<\/strong>https:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/adma.202206364<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5bfc\u8bfb\u3011 \u592a\u9633\u80fd\u70ed\u7535\uff08STE\uff09\u5668\u4ef6\u53ef\u5728\u4e0d\u4ea7\u751f\u6e29\u5ba4\u6c14\u4f53\u7684\u60c5\u51b5\u4e0b\u5c06\u5149\/\u70ed\u8f6c\u6362\u6210\u7535\u529b\u3002\u5728\u8fd9\u4e00\u4f53\u7cfb\u4e2d\uff0c\u5668\u4ef6\u7684\u80fd\u91cf\u8f6c\u6362\u6548\u7387\u4e0d\u4ec5\u53d6\u51b3\u4e8e\u70ed\u7535\u6750\u6599\uff0c\u4e5f\u9ad8\u5ea6\u4f9d\u8d56\u4e8e\u70ed\u7535\u81c2\u4e0a\u7684\u6e29\u5ea6\u68af&#8230;<\/p>\n","protected":false},"author":1076,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[2],"tags":[],"class_list":["post-242966","post","type-post","status-publish","format-standard","hentry","category-keji"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/242966"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/1076"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=242966"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/242966\/revisions"}],"predecessor-version":[{"id":243114,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/242966\/revisions\/243114"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=242966"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=242966"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=242966"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}