{"id":243050,"date":"2022-10-08T06:06:03","date_gmt":"2022-10-07T22:06:03","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=243050"},"modified":"2022-10-07T16:07:55","modified_gmt":"2022-10-07T08:07:55","slug":"%e7%a2%b3%e7%ba%b3%e7%b1%b3%e7%ae%a1%e5%8c%85%e8%a6%86fes2%e5%be%ae%e5%a4%9a%e9%9d%a2%e4%bd%93%e4%bd%9c%e4%b8%ba%e9%98%b3%e6%9e%81%e7%94%b5%e5%82%ac%e5%8c%96%e5%89%82%e7%94%a8%e4%ba%8e%e6%8f%90","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=243050","title":{"rendered":"\u78b3\u7eb3\u7c73\u7ba1\u5305\u8986FeS2\u5fae\u591a\u9762\u4f53\u4f5c\u4e3a\u9633\u6781\u7535\u50ac\u5316\u5242\u7528\u4e8e\u63d0\u9ad8\u5fae\u751f\u7269\u71c3\u6599\u7535\u6c60\u7684\u4ea7\u7535\u80fd\u529b"},"content":{"rendered":"<p><strong>\u3010\u7814\u7a76\u80cc\u666f\u3011<\/strong><\/p>\n<p>\u5fae\u751f\u7269\u71c3\u6599\u7535\u6c60\uff08MFCs\uff09\u53ef\u5229\u7528\u4ea7\u7535\u5fae\u751f\u7269\u6c27\u5316\u4ee3\u8c22\u6709\u673a\u7269\u7684\u8fc7\u7a0b\u4e2d\u56de\u6536\u7535\u80fd\uff0c\u662f\u4e00\u79cd\u751f\u6001\u53cb\u597d\u7684\u751f\u7269\u80fd\u6e90\u6536\u96c6\u548c\u5e9f\u6c34\u5904\u7406\u6280\u672f\u3002\u76ee\u524d\uff0cMFCs\u7684\u5546\u4e1a\u5316\u5e94\u7528\u4e3b\u8981\u53d7\u9650\u4e8e\u5176\u8f83\u4f4e\u7684\u8f93\u51fa\u529f\u7387\u5bc6\u5ea6\u3002\u9633\u6781\u4f5c\u4e3a\u4ea7\u7535\u5fae\u751f\u7269\u9644\u7740\u7684\u573a\u6240\u53ca\u7535\u5b50\u4f20\u8f93\u7684\u5a92\u4ecb\uff0c\u662f\u5f71\u54cdMFCs\u6027\u80fd\u7684\u91cd\u8981\u90e8\u4f4d\u4e4b\u4e00\u3002\u76ee\u524d\uff0c\u5e38\u7528\u7684\u9633\u6781\u6750\u6599\u4e3b\u8981\u4e3a\u5546\u4e1a\u78b3\u5e03\uff0c\u4f46\u5176\u4f5c\u4e3a\u9633\u6781\u6750\u6599\u65f6\uff0c\u5e38\u8868\u73b0\u51fa\u5fae\u751f\u7269\u9644\u7740\u91cf\u5c11\uff0c\u6302\u819c\u901f\u7387\u6162\uff0c\u6bd4\u7535\u5bb9\u5c0f\u7b49\u7f3a\u70b9\uff0c\u4e25\u91cd\u9650\u5236\u4e86\u9633\u6781\u4ea7\u7535\u91cf\u53ca\u5fae\u751f\u7269\u4e0e\u9633\u6781\u4e4b\u95f4\u7684\u7535\u5b50\u4f20\u8f93\u6548\u7387\u3002\u5bf9\u78b3\u5e03\u8868\u9762\u8fdb\u884c\u529f\u80fd\u5316\u6539\u6027\u662f\u89e3\u51b3\u4ee5\u4e0a\u95ee\u9898\u7684\u4e3b\u8981\u7b56\u7565\u3002<\/p>\n<p><strong>\u3010\u6587\u7ae0\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u57fa\u4e8e\u6b64\uff0c\u5317\u4eac\u79d1\u6280\u5927\u5b66\u674e\u4ece\u4e3e\u6559\u6388\u7684\u535a\u58eb\u751f\u5218\u8fdc\u5cf0\u5728\u5316\u5b66\u9886\u57dfTOP\u671f\u520aJournal of Colloid and Interface Science\u4e0a\u53d1\u8868\u9898\u4e3a\u201cCarbon nanotubes encapsulating FeS<sub>2<\/sub> micropolyhedrons as an anode electrocatalyst for improving the power generation of microbial fuel cells\u201d\u7684\u7814\u7a76\u6027\u6587\u7ae0\u3002\u8be5\u7814\u7a76\u8bbe\u8ba1\u4e86\u78b3\u7eb3\u7c73\u7ba1\u5305\u8986FeS<sub>2<\/sub>\u5fae\u591a\u9762\u4f53\u6750\u6599\u5e76\u7528\u4e8eMFC\u9633\u6781\uff0c\u53d1\u73b0\u76f8\u8f83\u4e8e\u7eaf\u78b3\u5e03\u9633\u6781\uff0c\u78b3\u7eb3\u7c73\u7ba1\u5305\u8986FeS<sub>2<\/sub>\u5fae\u591a\u9762\u4f53\u4fee\u9970\u7684\u78b3\u5e03\u8868\u9762\u4ea7\u7535\u5fae\u751f\u7269\u7684\u9644\u7740\u91cf\u3001\u5fae\u751f\u7269\u6d3b\u6027\u53ca\u80de\u5916\u7535\u5b50\u8f6c\u79fb\u6548\u7387\u5f97\u5230\u660e\u663e\u6539\u5584\uff0c\u6700\u5927\u8f93\u51fa\u529f\u7387\u9ad8\u8fbe1914 mW\/m<sup>2<\/sup>, \u7ea6\u662f\u7eaf\u78b3\u5e03\u9633\u6781MFC\u76844.5\u500d\uff0c\u4ea7\u751f\u7684\u7535\u80fd\u53ef\u4ee5\u6210\u529f\u9a71\u52a8LED\u706f\u53ca\u7535\u5b50\u8868\u3002\u5176\u4f18\u5f02\u7684\u6027\u80fd\u53ef\u5f52\u56e0\u4e8eFeS<sub>2<\/sub>\u53ca\u78b3\u7eb3\u7c73\u7ba1\u4e4b\u95f4\u7684\u534f\u540c\u4f5c\u7528\u3002FeS<sub>2<\/sub>\u5fae\u591a\u9762\u4f53\u53ef\u4ee5\u8c03\u63a7\u80de\u5916\u7535\u5b50\u4f20\u8f93\u8fc7\u7a0b\uff0c\u540c\u65f6\u53ef\u4ee5\u66f4\u597d\u7684\u534f\u52a9\u78b3\u7eb3\u7c73\u7ba1\u7684\u9644\u7740\uff0c\u800c\u78b3\u7eb3\u7c73\u7ba1\u53ef\u4ee5\u6539\u5584FeS<sub>2<\/sub>\u5fae\u591a\u9762\u4f53\u7684\u5bfc\u7535\u6027\u80fd\uff0c\u964d\u4f4e\u7535\u8377\u8f6c\u79fb\u5185\u963b\uff0c\u8fdb\u800c\u8d4b\u4e88\u9633\u6781\u66f4\u4f18\u5f02\u7684\u751f\u7269\u76f8\u5bb9\u6027\u53ca\u80de\u5916\u7535\u5b50\u8f6c\u79fb\u6548\u7387\u3002\u7531\u4e8e\u6210\u672c\u4f4e\u3001\u5236\u4f5c\u5de5\u827a\u7b80\u5355\u3001\u5bf9\u751f\u7269\u964d\u89e3\u6709\u673a\u7269\u5177\u6709\u826f\u597d\u7684\u7535\u50ac\u5316\u6027\u80fd\uff0c\u56e0\u6b64\uff0c\u5408\u6210\u7684FeS<sub>2<\/sub>@CNT\u5fae\u591a\u9762\u4f53\u662f\u4e00\u79cd\u5177\u6709\u5e94\u7528\u524d\u666f\u7684\u9ad8\u6027\u80fd\u3001\u4f4e\u6210\u672cMFC\u9633\u6781\u6750\u6599\u3002<\/p>\n<p><strong>\u3010\u672c\u6587\u8981\u70b9\u3011<\/strong><\/p>\n<p>\u8981\u70b9\u4e00\uff1aFeS<sub>2<\/sub>@CNT\u5fae\u591a\u9762\u4f53\u9633\u6781\u4fee\u9970\u5242\u5236\u5907\u793a\u610f\u56fe\u53ca\u5f62\u8c8c\u7ed3\u6784<\/p>\n<p>\u56fe 1\u3002(a)\u5fae\u591a\u9762\u4f53FeS<sub>2<\/sub>@CNT\u7684\u5236\u5907\u793a\u610f\u56fe;(b) FeS<sub>2<\/sub>@CNT\u7684SEM\u56fe\uff0c(c) TEM\u56fe\uff0c(d)\u9ad8\u5206\u8fa8\u7387TEM\u56fe\uff0c(e) SAED\u56fe\uff0c(f) XRD\u56fe\uff0c(g) N<sub>2<\/sub>\u5438\u9644-\u89e3\u5438\u7b49\u6e29\u7ebf\uff0c(h-k) EDS\u5143\u7d20\u56fe\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-243052\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/1-4.png\" alt=\"\" width=\"1207\" height=\"1240\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/1-4.png 1207w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/1-4-292x300.png 292w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/1-4-768x789.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/1-4-997x1024.png 997w\" sizes=\"(max-width: 1207px) 100vw, 1207px\" \/><\/p>\n<p>\u8981\u70b9\u4e8c\uff1aFeS<sub>2<\/sub>@CNT\u5fae\u591a\u9762\u4f53\u4fee\u9970\u9633\u6781\u4ea7\u7535\u6027\u80fd<\/p>\n<p>\u56fe2\u914d\u7f6e\u4e0d\u540c\u9633\u6781\u7684MFC\u7684\u53c2\u6570:(a)\u8f93\u51fa\u7535\u538b\uff0c(b)\u529f\u7387\u5bc6\u5ea6\u548c\u6781\u5316\u66f2\u7ebf\uff0c(c)\u5177\u6709\u4ee3\u8868\u6027\u7684\u9633\u6781\u7684MFC\u7684\u529f\u7387\u5bc6\u5ea6\uff0c(d) CV\u56fe\uff0c(e) Nyquist\u56fe\uff0c(f) COD\u53bb\u9664\u7387\u548c\u5e93\u4ed1\u6548\u7387\uff0c(g)FeS<sub>2<\/sub>@CNT\u9633\u6781MFC\u9a71\u52a8\u7535\u5b50\u8868\u548cLED\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-243053\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/2-4.png\" alt=\"\" width=\"1261\" height=\"940\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/2-4.png 1261w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/2-4-300x224.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/2-4-768x572.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/2-4-1024x763.png 1024w\" sizes=\"(max-width: 1261px) 100vw, 1261px\" \/><\/p>\n<p>\u8981\u70b9\u4e09\uff1aFeS<sub>2<\/sub>@CNT\u5fae\u591a\u9762\u4f53\u9633\u6781\u6750\u6599\u751f\u7269\u819c\u7ed3\u6784<\/p>\n<p>\u56fe3\u3002\u9644\u7740\u5728(a,b) CC\uff0c (d,e) CNT\u548c(g,h) FeS<sub>2<\/sub>@CNT\u9633\u6781\u4e0a\u7684\u751f\u7269\u819c\u5fae\u89c2\u5f62\u8c8c\u3002(c) CC\uff0c (f) CNT\u548c(i) FeS<sub>2<\/sub>@CNT\u9633\u6781\u4e0a\u5fae\u751f\u7269\u6d3b\u6027\u5206\u6790;(j-m) FeS<sub>2<\/sub>@CNT\u9633\u6781\u751f\u7269\u819c\u8868\u9762\u5143\u7d20\u5206\u5e03\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-243054\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/3-4.png\" alt=\"\" width=\"858\" height=\"827\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/3-4.png 858w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/3-4-300x289.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/10\/3-4-768x740.png 768w\" sizes=\"(max-width: 858px) 100vw, 858px\" \/><\/p>\n<p><strong>\u3010\u7ed3\u8bba\u3011<\/strong><\/p>\n<p>\u603b\u4e4b\uff0c\u6211\u4eec\u6210\u529f\u5408\u6210\u4e86\u4e00\u79cd\u9ad8\u6548\u7684CNTs\u5305\u8986FeS<sub>2<\/sub>\u5fae\u591a\u9762\u4f53\u9633\u6781\u7535\u50ac\u5316\u5242\uff0c\u4ee5\u63d0\u9ad8MFC\u7684\u6574\u4f53\u6027\u80fd\u3002\u5236\u5907\u7684FeS<sub>2<\/sub>@CNT\u7535\u50ac\u5316\u5242\u5177\u6709\u826f\u597d\u7684\u751f\u7269\u4eb2\u548c\u6027\uff0c\u5bfc\u7535\u6027\uff0c\u957f\u671f\u8fd0\u884c\u7a33\u5b9a\u6027\uff0c\u5bf9\u751f\u7269\u819c\u6c27\u5316\u4ee3\u8c22\u6709\u673a\u7269\u5177\u6709\u663e\u8457\u7684\u7535\u50ac\u5316\u6d3b\u6027\u3002\u6b64\u5916\uff0c\u5d4c\u5165\u751f\u7269\u819c\u7684FeS<sub>2<\/sub>@CNT\u5fae\u591a\u9762\u4f53\u6709\u5229\u4e8e\u751f\u7269\u819c\u9644\u7740\u3001\u5fae\u751f\u7269\u6d3b\u6027\u548c\u80de\u5916\u7535\u5b50\u4f20\u8f93\u3002\u57fa\u4e8e\u4ee5\u4e0a\u4f18\u70b9\uff0c\u672c\u5de5\u4f5c\u63cf\u8ff0\u4e86\u4e00\u79cd\u6709\u524d\u9014\u7684\u5236\u5907\u9ad8\u6548\u9633\u6781\u7535\u50ac\u5316\u5242\u7684\u65b9\u6cd5\uff0c\u4ee5\u63d0\u9ad8MFC\u7684\u6574\u4f53\u6027\u80fd\u3002<\/p>\n<p><strong>\u3010\u4f5c\u8005\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u672c\u7814\u7a76\u7684\u7b2c\u4e00\u4f5c\u8005\u4e3a\u5317\u4eac\u79d1\u6280\u5927\u5b66\u535a\u58eb\u751f\u5218\u8fdc\u5cf0\uff0c\u5e08\u4ece\u674e\u4ece\u4e3e\u6559\u6388\uff0c\u4e3b\u8981\u7814\u7a76\u65b9\u5411\u4e3a\u7eb3\u7c73\u7ea4\u7ef4\u6c14\u51dd\u80f6\u3001MOFs\u6750\u6599\u53ca\u5fae\u751f\u7269\u71c3\u6599\u7535\u6c60\u7684\u8bbe\u8ba1\u3002\u535a\u58eb\u671f\u95f4\u4ee5\u7b2c\u4e00\u4f5c\u8005\u5728Journal of Colloid and Interface Science\uff0c Journal of Power sources\uff0c Electrochimica Acta\u7b49\u671f\u520a\u7d2f\u8ba1\u53d1\u8868\u5b66\u672f\u8bba\u658710\u7bc7\uff0c\u6388\u6743\u53d1\u660e\u4e13\u5229\u4e00\u9879\u3002<\/p>\n<p><strong>\u6587\u7ae0\u4fe1\u606f<\/strong><\/p>\n<p>Yuanfeng Liu, Yaxin Sun, Min Zhang, Shiquan Guo, Zijing Su, Tingli Ren, Congju Li*. Carbon nanotubes encapsulating FeS<sub>2<\/sub> micropolyhedrons as an anode electrocatalyst for improving the power generation of microbial fuel cells, Journal of Colloid and Interface Science, https:\/\/doi.org\/10.1016\/j.jcis.2022.09.130.<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u7814\u7a76\u80cc\u666f\u3011 \u5fae\u751f\u7269\u71c3\u6599\u7535\u6c60\uff08MFCs\uff09\u53ef\u5229\u7528\u4ea7\u7535\u5fae\u751f\u7269\u6c27\u5316\u4ee3\u8c22\u6709\u673a\u7269\u7684\u8fc7\u7a0b\u4e2d\u56de\u6536\u7535\u80fd\uff0c\u662f\u4e00\u79cd\u751f\u6001\u53cb\u597d\u7684\u751f\u7269\u80fd\u6e90\u6536\u96c6\u548c\u5e9f\u6c34\u5904\u7406\u6280\u672f\u3002\u76ee\u524d\uff0cMFCs\u7684\u5546\u4e1a\u5316\u5e94\u7528\u4e3b&#8230;<\/p>\n","protected":false},"author":2,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-243050","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/243050"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/2"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=243050"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/243050\/revisions"}],"predecessor-version":[{"id":243055,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/243050\/revisions\/243055"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=243050"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=243050"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=243050"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}