{"id":244680,"date":"2022-12-08T06:15:16","date_gmt":"2022-12-07T22:15:16","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=244680"},"modified":"2022-12-07T19:31:32","modified_gmt":"2022-12-07T11:31:32","slug":"%e4%b8%9c%e5%8d%97%e7%ab%a0%e7%82%9c%e3%80%81%e5%8d%97%e5%a4%a7%e8%91%9b%e6%b5%b7%e9%9b%84%e3%80%81%e6%9d%ad%e7%94%b5%e5%bc%a0%e9%89%b4%e7%94%b5%e5%82%ac%e5%8c%96am","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=244680","title":{"rendered":"\u4e1c\u5357\u7ae0\u709c\u3001\u5357\u5927\u845b\u6d77\u96c4\u3001\u676d\u7535\u5f20\u9274\u7535\u50ac\u5316AM"},"content":{"rendered":"<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-244681\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/12\/\u5fae\u4fe1\u622a\u56fe_20221207191638.png\" alt=\"\" width=\"712\" height=\"304\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/12\/\u5fae\u4fe1\u622a\u56fe_20221207191638.png 712w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/12\/\u5fae\u4fe1\u622a\u56fe_20221207191638-300x128.png 300w\" sizes=\"(max-width: 712px) 100vw, 712px\" \/><\/p>\n<p><strong>\u521b\u65b0\u70b9<\/strong><\/p>\n<p>\u901a\u8fc7\u4eff\u751f\u6df1\u6d77\u6d77\u7ef5\u7684\u5f62\u8c8c\u7ed3\u6784\u548c\u8d28\u91cf\u4f20\u9012\u673a\u5236\uff0c\u5236\u5907\u51fa\u4e86\u4e00\u79cd\u65b0\u7684\u5206\u5c42\u7ed3\u6784\u50ac\u5316\u7535\u6781\uff0c\u4ee5\u63d0\u9ad8\u7535\u5316\u5b66\u6c34\u5206\u89e3\u6027\u80fd\u3002<\/p>\n<p><strong>\u5173\u952e\u8bcd<\/strong><\/p>\n<p>\u7535\u50ac\u5316\uff0c\u4eff\u751f\u6d77\u7ef5\uff0c\u8d28\u91cf\u4f20\u9012<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-244683\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/12\/\u56fe\u72471-1.jpg\" alt=\"\" width=\"699\" height=\"753\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/12\/\u56fe\u72471-1.jpg 699w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/12\/\u56fe\u72471-1-278x300.jpg 278w\" sizes=\"(max-width: 699px) 100vw, 699px\" \/><\/p>\n<p>\u56fe1 a)\u6d77\u7ef5\u7ba1\u901a\u8fc7\u5b83\u4eec\u7684\u8eab\u4f53\u4fdd\u6301\u6c34\u6d41\uff0c\u4ee5\u83b7\u5f97\u98df\u7269\u548c\u6c27\u6c14\uff0c\u5e76\u6e05\u9664\u5e9f\u7269\u3002b) NiFe-P<sub>Zn<\/sub>\u5305\u8986\u9ad8\u6df1\u5bbd\u6bd4PNTA\u7684\u4eff\u751f\u7ba1\u72b6\u6d77\u7ef5\u72b6\u50ac\u5316\u7535\u6781\u3002c) NiFe-P<sub>Zn<\/sub>@PNTA\u7535\u6781\u7684\u7535\u5b50\u4f20\u9012\u8def\u5f84(\u5de6)\u548cNiFe-P<sub>Zn<\/sub>\u8868\u9762\u7684OER\u8fc7\u7a0b(\u53f3)\u3002<\/p>\n<p>\u6c14\u6ce1\u91ca\u653e\u53d7\u963b\u548c\u7535\u5b50\u4f20\u5bfc\u8fc7\u7a0b\u53d7\u9650\u662f\u5927\u89c4\u6a21\u7535\u5316\u5b66\u6c34\u5206\u89e3\u7684\u4e3b\u8981\u74f6\u9888\u3002\u6700\u8fd1\uff0c\u53d7\u6df1\u6d77\u6d77\u7ef5\u7ba1\u72b6\u7ed3\u6784\u7684\u542f\u53d1\uff0c\u4e1c\u5357\u5927\u5b66\uff0c\u5357\u4eac\u5927\u5b66\u548c\u676d\u5dde\u7535\u5b50\u79d1\u6280\u5927\u5b66\u56e2\u961f\u901a\u8fc7\u7ed3\u5408\u70ed\u7eb3\u7c73\u538b\u5370\u548c\u7535\u9540\u7b49\u5de5\u827a\u5236\u5907\u51fa\u4e86\u591a\u5c3a\u5ea6\u7ed3\u6784\u5c42\u6b21\uff0c\u5b9e\u73b0\u4e86\u4eff\u751f\u50ac\u5316\u7535\u6781\u8868\u9762\u6c14\u6ce1\u7684\u89e3\u5438\u548c\u7535\u5b50\u7684\u8fde\u7eed\u4f20\u9012\u3002\u7535\u6781\u7531\u4e00\u79cd\u5f02\u5e38\u6d3b\u8dc3\u4e14\u65e0\u7c98\u7ed3\u5242\u7684\u591a\u5b54\u954d\u7ba1\u9635\u5217(PNTA)\u53ca\u5728\u5176\u8868\u9762\u8d1f\u8f7d\u7684\u591a\u5b54\u7eb3\u7c73\u7247(NiFe-P<sub>Zn<\/sub>)\u6784\u6210\u3002\u5176\u4e2d\uff0c\u6a21\u62df\u6d77\u7ef5\u8eaf\u5e72\u7684PNTA\u4fc3\u8fdb\u4e86\u6c14\u6ce1\u7684\u53bb\u9664\u548c\u7535\u5b50\u8f6c\u79fb\uff0c\u6a21\u62df\u6d77\u7ef5\u8868\u76ae\u7684NiFe-P<sub>Zn<\/sub>\u589e\u52a0\u4e86\u50ac\u5316\u6d3b\u6027\u4f4d\u70b9\u7684\u6570\u91cf\u3002\u901a\u8fc7\u6539\u8fdb\u5916\u90e8\u4f20\u8d28\u548c\u5185\u90e8\u7535\u5b50\u4f20\u9012\uff0c NiFe-P<sub>Zn<\/sub>@PNTA\u7535\u6781\u8868\u73b0\u51fa\u4f18\u8d8a\u7684\u6790\u6c27\u53cd\u5e94\u6027\u80fd\uff0c\u572810 mA\u2219cm<sup>-2<\/sup>\u65f6\u7684\u8fc7\u7535\u4f4d\u4e3a172 mV (Tafel\u659c\u7387\u4e3a50 mV\u2219dec<sup>-1<\/sup>)\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-244684\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/12\/\u56fe\u72472.jpg\" alt=\"\" width=\"699\" height=\"437\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/12\/\u56fe\u72472.jpg 699w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/12\/\u56fe\u72472-300x188.jpg 300w\" sizes=\"(max-width: 699px) 100vw, 699px\" \/><\/p>\n<p>\u56fe2 a) NiFe-P<sub>Zn<\/sub>@PNTA\u7535\u6781\u7684\u5236\u4f5c\u8fc7\u7a0b\u3002b-d)\u5bf9\u5e94\u7684NTA\u3001PNTA\u548cNiFe-P<sub>Zn<\/sub>@PNTA\u5fae\u89c2\u7ed3\u6784\u7684SEM\u56fe\u50cf\u3002<\/p>\n<p>\u5728\u7535\u89e3\u6db2\u4e2d\uff0cNiFe-P<sub>Zn<\/sub>@PNTA\u8868\u9762\u4e0e\u6c14\u6ce1\u4e4b\u95f4\u7ea6164.5\u00b0\u7684\u6c14\u6ce1\u63a5\u89e6\u89d2(CA)\u8868\u73b0\u51fa\u4e86\u8d85\u758f\u6c14\u6027\u3002\u540c\u4e00\u8868\u9762\u5728\u7a7a\u6c14\u4e2d\u7535\u89e3\u6db2\u6db2\u6ef4\u63a5\u89e6\u89d2\u4e3aCA ~1\u00b0\u5c55\u73b0\u51fa\u4eb2\u6c34\u6027\uff0c\u5f53\u7535\u89e3\u6db2\u6db2\u6ef4\u5230\u8fbe\u7535\u6781\u8868\u9762\u65f6\uff0c\u53ef\u8fc5\u901f\u88ab\u5438\u6536\u5e76\u6e17\u900f\u5230\u6574\u4e2a\u7535\u6781\u8868\u9762\u3002\u7ecf\u8fc7\u7535\u50ac\u5316\u6c34\u5206\u89e3\u53cd\u5e94\u540e\uff0c\u5728NiFe-P<sub>Zn<\/sub>@PNTA\u7535\u6781\u8868\u9762\u9664\u8fb9\u7f18\u5916\u672a\u89c2\u5bdf\u5230\u660e\u663e\u6c14\u6ce1\uff0c\u8868\u660e\u8d85\u758f\u6c14\/\u4eb2\u6c34\u8868\u9762\u786e\u5b9e\u4fc3\u8fdb\u4e86\u50ac\u5316\u53cd\u5e94\u4e2d\u7535\u6781\u8868\u9762\u7684\u6c14\u6ce1\u91ca\u653e\u3002\u7528\u539f\u4f4d\u5149\u5b66\u663e\u5fae\u955c\u89c2\u5bdf\u4e86\u7535\u6781\u4e0a\u6c14\u6ce1\u7684\u5f62\u6210\u548c\u5206\u79bb\u3002NiFe-P<sub>Zn<\/sub>@PNTA\u7535\u6781\u4e2d\u5f62\u6210\u7684\u6c14\u6ce1\u53ef\u4ee5\u5feb\u901f\u91ca\u653e\uff0c\u6c14\u6ce1\u5728\u7ba1\u5185\u4e0a\u5347\u8fc7\u7a0b\u4e2d\u76f8\u4e92\u878d\u5408\uff0c\u4f53\u79ef\u589e\u5927\u6240\u53d7\u6d6e\u529b\u589e\u5927\uff0c\u4ece\u800c\u52a0\u901f\u6c14\u6ce1\u5728\u7ba1\u5185\u5feb\u901f\u8fd0\u52a8\u3002\u5927\u91cf\u5feb\u901f\u79fb\u52a8\u7684\u6c14\u6ce1\u62d6\u52a8\u7535\u89e3\u6db2\u6d41\u52a8\uff0c\u5728PNTA\u5185\u4ea7\u751f\u8d1f\u538b\uff0c\u5bfc\u81f4\u5916\u90e8\u7535\u89e3\u6db2\u901a\u8fc7\u591a\u5b54\u7ba1\u58c1\u8fdb\u5165PNTA\uff0c\u7ef4\u6301\u5feb\u901f\u6c14\u6ce1\u91ca\u653e\u884c\u4e3a\u3002\u5728\u6b64\u8fc7\u7a0b\u4e2d\uff0c\u7535\u89e3\u6db2\u5f3a\u5236\u4e0eNiFe-P<sub>Zn<\/sub>@PNTA\u591a\u5b54\u5fae\u7ba1\u58c1\u5185\u7684\u6d3b\u6027\u4f4d\u70b9\u76f8\u4e92\u4f5c\u7528\uff0c\u5bfc\u81f4\u4e09\u76f8\u754c\u9762\u53cd\u5e94\u589e\u5f3a\uff0c\u6709\u6548\u751f\u6210O<sub>2<\/sub>\u3002NiFe-P<sub>Zn<\/sub>@PNTA\u7684\u6c14\u6ce1\u91ca\u653e\u8981\u6bd4NiFe-P<sub>Zn<\/sub>@NTA\u5feb\u5f97\u591a\uff0c\u662f\u7531\u4e8e\u540e\u8005\u7684\u56fa\u4f53\u7ba1\u58c1\u963b\u6321\u4e86\u5916\u90e8\u7535\u89e3\u8d28\u7684\u8fdb\u5165\u3002\u56e0\u6b64NiFe-P<sub>Zn<\/sub>@PNTA\u7684\u7535\u6d41\u5bc6\u5ea6\u503c\u6bd4NiFe-P<sub>Zn<\/sub>@NTA\u9ad8\u5f97\u591a\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-244685\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/12\/\u56fe\u72473.jpg\" alt=\"\" width=\"699\" height=\"607\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/12\/\u56fe\u72473.jpg 699w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/12\/\u56fe\u72473-300x261.jpg 300w\" sizes=\"(max-width: 699px) 100vw, 699px\" \/><\/p>\n<p>\u56fe3 a) NiFe-P<sub>Zn<\/sub>@PNTA\u7535\u6781\u7684\u6c14\u6ce1\u548c\u7535\u89e3\u8d28\u63a5\u89e6\u89d2(\u5de6)\u3002NiFe-P<sub>Zn<\/sub>@PNTA\u7535\u6781\u8868\u9762\u7535\u89e3\u6db2\u5feb\u901f\u5438\u6536\u8fc7\u7a0b\u7684\u7167\u7247(\u53f3)\u3002b) OER\u53cd\u5e94\u540eNiFe-P<sub>Zn<\/sub>@PNTA\u8868\u9762\u548c\u8fb9\u7f18\u7684\u7167\u7247\u3002c) NiFe-P<sub>Zn<\/sub>@PNTA\u7535\u6781\u4e0a\u6c14\u6ce1\u4ece\u4ea7\u751f\u5230\u5feb\u901f\u91ca\u653e\u8fc7\u7a0b\u7684\u5149\u5b66\u663e\u5fae\u955c\u56fe\u50cf\u3002d)\u6709\u7535\u89e3\u8865\u5145\u901a\u9053\u7684NiFe-P<sub>Zn<\/sub>@PNTA\u548c\u6ca1\u6709\u7535\u89e3\u8865\u5145\u901a\u9053\u7684NiFe-P<sub>Zn<\/sub>@NTA\u793a\u610f\u56fe\u3002e) NiFe-P<sub>Zn<\/sub>@PNTA\u548cNiFe-P<sub>Zn<\/sub>@NTA\u57281.3 V RHE -1.6 V RHE\u65f6\u7684\u7535\u6d41\u5bc6\u5ea6\u3002<\/p>\n<p>\u5728\u7535\u6d41\u5bc6\u5ea6\u4e3a10 mA\u2219cm<sup>-2<\/sup>\u65f6\uff0cNiFe-P<sub>Zn<\/sub>@PNTA\u7684\u8fc7\u7535\u4f4d\u8fbe\u5230172 mV\uff0c\u4f18\u4e8eNiFe@PNTA (260 mV)\u548c\u88f8PNTA (497 mV)\u3002\u540c\u65f6\uff0cNiFe-P<sub>Zn<\/sub>@PNTA\u5c55\u73b0\u51fa\u6700\u5c0f\u7684Tafel\u659c\u7387(50 mV\u2219dec<sup>-1<\/sup>)\uff0c\u8fd9\u662f\u7531\u4e8e\u5bf9\u542b\u6c27\u7269\u8d28\u66f4\u5bb9\u6613\u5438\u9644\/\u89e3\u5438\u3002\u7528\u7535\u5316\u5b66\u963b\u6297\u8c31(EIS)\u8bc4\u4f30\u4e86\u7535\u6781\u7684\u7535\u8377\u8f6c\u79fb\u884c\u4e3a\uff0cNiFe-P<sub>Zn<\/sub>@PNTA\u7684\u7535\u8377\u8f6c\u79fb\u7535\u963b(<em>R<\/em><sub>ct<\/sub>)\u7ea6\u4e3a0.2 \u03a9\uff0c\u5c0f\u4e8eNiFe@PNTA (0.3 \u03a9)\u548cPNTA (0.5 \u03a9)\u3002\u6b64\u5916\uff0cNiFe-P<sub>Zn<\/sub>@PNTA\u7535\u6781\u7684\u7535\u5316\u5b66\u6d3b\u6027\u8868\u9762\u79ef(ECSA)\u4e3a66.00 cm<sup>2<\/sup>\uff0c\u5927\u4e8eNiFe@PNTA (47.75 cm<sup>2<\/sup>)\u548c\u88f8PNTA (7.25 cm<sup>2<\/sup>)\u3002<\/p>\n<p>\u5236\u5907\u7684\u4eff\u751f\u50ac\u5316\u7535\u6781\u5177\u6709\u4f18\u5f02\u7684\u673a\u68b0\u6027\u80fd\u548c\u8010\u4e45\u6027\u3002\u6240\u5236\u5907\u7684\u50ac\u5316\u7535\u6781\u5728100 mA\u2219cm<sup>-2<\/sup>(\u7535\u4f4d\u4e3a1.52 V vs. RHE)\uff0c\u8fde\u7eed\u5de5\u4f5c360\u5c0f\u65f6\u8868\u73b0\u51fa\u826f\u597d\u7a33\u5b9a\u6027\u3002NiFe-P<sub>Zn<\/sub>@PNTA\u5728\u5377\u66f2\u548c\u5c55\u5f00\u5faa\u73af1000\u6b21\u540e\uff0cOER\u6027\u80fd\u548c\u7ed3\u6784\u4fdd\u6301\u4e0d\u53d8\u3002\u8fd9\u9879\u5de5\u4f5c\u4e3a\u8bbe\u8ba1\u9ad8\u6548\u6c34\u5206\u89e3\u7684\u5206\u5c42\u7ed3\u6784\u7535\u50ac\u5316\u7535\u6781\u63d0\u4f9b\u4e86\u4e00\u79cd\u65b0\u7b56\u7565\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-244686\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/12\/\u56fe\u72474.jpg\" alt=\"\" width=\"699\" height=\"743\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/12\/\u56fe\u72474.jpg 699w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2022\/12\/\u56fe\u72474-282x300.jpg 282w\" sizes=\"(max-width: 699px) 100vw, 699px\" \/><\/p>\n<p>\u56fe4 a) NiFe-P<sub>Zn<\/sub>@PNTA\u3001NiFe@PNTA\u548cPNTA\u7535\u6781\u7684LSV\u66f2\u7ebf\u3002b) Tafel\u56fe\u3002c) Nyquist\u56fe\u3002\u63d2\u56fe:\u7b49\u6548\u7535\u8def\u6a21\u578b\u3002d) ESCA\u3002e) NiFe-P<sub>Zn<\/sub>@PNTA\u7535\u6781\u5728\u4e00\u5b9a\u8fc7\u7535\u4f4d\u4e0b(290 mV vs RHE)\u6301\u7eed360\u5c0f\u65f6\u4ee5\u4e0a\u7684\u8ba1\u65f6\u5b89\u57f9\u6d4b\u8bd5\u548c5000 CV\u5faa\u73af\u524d\u540e\u7684LSV\u66f2\u7ebf(\u63d2\u56fe)\u3002f) NiFe-P<sub>Zn<\/sub>@PNTA\u7535\u6781\u57281000\u6b21\u5f2f\u66f2\u72b6\u6001\u4e0b\u7684LSV\u66f2\u7ebf\u548c\u7167\u7247\u3002g)\u7535\u6d41\u5bc6\u5ea6\u4e3a10 mA cm<sup>-2<\/sup>\u65f6\u7684\u8fc7\u7535\u4f4d\u6bd4\u8f83\u548c(h)\u4e0e\u6700\u8fd1\u62a5\u9053\u7684\u8fc7\u6e21\u91d1\u5c5e\u57fa\u50ac\u5316\u5242\u5728\u4e0d\u540c\u7535\u6d41\u5bc6\u5ea6\u4e0b\u7684\u50ac\u5316\u7a33\u5b9a\u6027\u3002<\/p>\n<p>\u8be5\u5de5\u4f5c\u4ee5\u201cTube-Sponge-Inspired Hierarchical Electrocatalysts with Boosted Mass and Electron Transfer for Efficient Oxygen Evolution\u201d\u4e3a\u9898\u53d1\u8868\u5728\u300a<em>Advanced Materials<\/em>\u300b\u4e0a\u3002\u6587\u7ae0\u7b2c\u4e00\u4f5c\u8005\u662f\u5357\u4eac\u5927\u5b662020\u7ea7\u535a\u58eb\u7814\u7a76\u751f\u5468\u4e9a\u4e9a\uff0c\u901a\u8baf\u4f5c\u8005\u662f\u4e1c\u5357\u5927\u5b66\u7ae0\u709c\u6559\u6388\u3001\u5357\u4eac\u5927\u5b66\u845b\u6d77\u96c4\u6559\u6388\u548c\u676d\u5dde\u7535\u5b50\u79d1\u6280\u5927\u5b66\u5f20\u9274\u6559\u6388\u3002\u8be5\u7814\u7a76\u5f97\u5230\u4e86\u56fd\u5bb6\u91cd\u70b9\u7814\u53d1\u8ba1\u5212\u3001\u56fd\u5bb6\u81ea\u7136\u79d1\u5b66\u57fa\u91d1\u7b49\u652f\u6301\u3002<\/p>\n<p>\u539f\u6587\u94fe\u63a5\uff1a<\/p>\n<p><a href=\"https:\/\/doi.org\/10.1002\/adma.202209500\">https:\/\/doi.org\/10.1002\/adma.202209500<\/a><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u521b\u65b0\u70b9 \u901a\u8fc7\u4eff\u751f\u6df1\u6d77\u6d77\u7ef5\u7684\u5f62\u8c8c\u7ed3\u6784\u548c\u8d28\u91cf\u4f20\u9012\u673a\u5236\uff0c\u5236\u5907\u51fa\u4e86\u4e00\u79cd\u65b0\u7684\u5206\u5c42\u7ed3\u6784\u50ac\u5316\u7535\u6781\uff0c\u4ee5\u63d0\u9ad8\u7535\u5316\u5b66\u6c34\u5206\u89e3\u6027\u80fd\u3002 \u5173\u952e\u8bcd \u7535\u50ac\u5316\uff0c\u4eff\u751f\u6d77\u7ef5\uff0c\u8d28\u91cf\u4f20\u9012 \u3010\u56fe\u6587\u5bfc\u8bfb\u3011 &#8230;<\/p>\n","protected":false},"author":2,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[2],"tags":[],"class_list":["post-244680","post","type-post","status-publish","format-standard","hentry","category-keji"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/244680"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/2"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=244680"}],"version-history":[{"count":1,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/244680\/revisions"}],"predecessor-version":[{"id":244687,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/244680\/revisions\/244687"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=244680"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=244680"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=244680"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}