{"id":246017,"date":"2023-01-18T06:00:40","date_gmt":"2023-01-17T22:00:40","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=246017"},"modified":"2023-01-17T17:35:01","modified_gmt":"2023-01-17T09:35:01","slug":"%e7%bb%bc%e8%bf%b0%ef%bc%9a%e5%9f%ba%e4%ba%8e%e4%ba%8c%e7%bb%b4%e8%bf%87%e6%b8%a1%e9%87%91%e5%b1%9e%e7%a1%ab%e6%97%8f%e5%8c%96%e5%90%88%e7%89%a9%ef%bc%882d-tmds%ef%bc%89%e7%9a%84%e5%85%89%e5%82%ac","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=246017","title":{"rendered":"\u7efc\u8ff0\uff1a\u57fa\u4e8e\u4e8c\u7ef4\u8fc7\u6e21\u91d1\u5c5e\u786b\u65cf\u5316\u5408\u7269\uff082D TMDs\uff09\u7684\u5149\u50ac\u5316\u5242"},"content":{"rendered":"<ol>\n<li>\u5168\u6587\u901f\u89c8\uff1a<\/li>\n<\/ol>\n<p>\u4e8c\u7ef4\uff082D\uff09\u8fc7\u6e21\u91d1\u5c5e\u786b\u65cf\u5316\u5408\u7269\uff08TMDs\uff09\uff0c\u540e\u77f3\u58a8\u70ef\u65f6\u4ee3\u7684\u4e00\u9897\u65b0\u661f\uff0c\u5728\u5149\u50ac\u5316\u9886\u57df\u5177\u6709\u57fa\u7840\u6027\u548c\u6280\u672f\u6027\u7684\u5438\u5f15\u529b\u3002\u5b83\u4eec\u975e\u51e1\u7684\u7535\u5b50\u3001\u5149\u5b50\u548c\u5316\u5b66\u5c5e\u6027\u4f7f\u5b83\u4eec\u6210\u4e3a\u6709\u6548\u7684\u6355\u5149\u4f53\u548c\u5149\u50ac\u5316\u4f53\u3002\u672c\u6587\u5bf9\u7528\u4e8e\u5149\u50ac\u5316\u76842D TMDs\u6750\u6599\u8fdb\u884c\u4e86\u6559\u7a0b\u5f0f\u548c\u524d\u77bb\u5f0f\u7684\u56de\u987e\u548c\u5c55\u671b\uff0c\u6307\u51fa\u4e862D TMDs\u5728\u5149\u50ac\u5316\u9886\u57df\u4f5c\u4e3a\u52a9\u50ac\u5316\u5242\u548c\u6d3b\u6027\u5149\u50ac\u5316\u5242\u7684\u4f18\u52bf\u548c\u6311\u6218\uff0c\u4ee5\u53ca\u76f8\u5e94\u7684\u8bbe\u8ba1\u7b56\u7565\uff0c\u548c\u672a\u6765\u7684\u673a\u9047\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>2. \u80cc\u666f\u4ecb\u7ecd\uff1a<\/p>\n<p>2D TMDs\uff08\u4f8b\u5982MoS<sub>2<\/sub>, WS<sub>2<\/sub>, NbSe<sub>2<\/sub>\uff09\u6784\u6210\u4e86\u4e00\u4e2a\u8ff7\u4eba\u7684\u6750\u6599\u5e93\u3002\u5b83\u4eec\u662f\u77f3\u58a8\u70ef\uff08\u96f6\u5e26\u9699\uff09\u7684\u4e00\u79cd\u5f88\u6709\u524d\u9014\u7684\u66ff\u4ee3\u54c1\uff0c\u5e76\u4e14\u5728\u67d0\u4e9b\u65b9\u9762\u6709\u8d85\u8d8a\u77f3\u58a8\u70ef\u7684\u6f5c\u529b\uff0c\u56e0\u4e3a\u5b83\u4eec\u5177\u6709\u591a\u6837\u7684\u5316\u5b66\u6027\u8d28\uff0c\u4ece\u91d1\u5c5e\uff08\u5982NbS<sub>2<\/sub>\u548cVSe<sub>2<\/sub>\uff09\u3001\u534a\u91d1\u5c5e\uff08\u5982WTe<sub>2<\/sub>\u548cTiSe<sub>2<\/sub>\uff09\u3001\u534a\u5bfc\u4f53\uff08\u5982MoS<sub>2<\/sub>\u548cWS<sub>2<\/sub>\uff09\u5230\u7edd\u7f18\u4f53\uff08\u5982HfS<sub>2<\/sub>\uff09\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u8fd9\u7c7b\u6750\u6599\u6700\u8fd1\u5728\u7535\u5b50\u3001\u5149\u5b50\u3001\u5149\u7535\u5b50\u3001\u80fd\u91cf\u8f6c\u6362\u3001\u7535\u50ac\u5316\u3001\u73af\u5883\u4fee\u590d\u3001\u751f\u7269\u4f20\u611f\u548c\u751f\u7269\u6210\u50cf\u7b49\u9886\u57df\u5f15\u8d77\u4e86\u5e7f\u6cdb\u7684\u5174\u8da3\uff0c\u56e0\u4e3a\u5b83\u4eec\u5177\u6709\u975e\u51e1\u7684\u6027\u8d28\uff0c\u5305\u62ec\u539f\u5b50\u8584\u5c42\u3001\u5f3a\u81ea\u65cb\u8f68\u9053\u8026\u5408\u3001\u53ef\u8c03\u5e26\u9699\u3001\uff0c\u5f3a\u70c8\u7684\u6fc0\u5b50\u6548\u5e94\u7b49\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u5728\u8fc7\u53bb\u7684\u5341\u5e74\u4e2d\uff0c2D TMDs\u5728\u5149\u50ac\u5316\u9886\u57df\u4e5f\u4ece\u6280\u672f\u4e0a\u5438\u5f15\u4e86\u7814\u7a76\u8005\u7684\u597d\u5947\u5fc3\u3002\u81ea2008\u5e74\u674e\u707f\u9662\u58eb\u53d1\u8868\u7684\u5f00\u521b\u6027\u5de5\u4f5c\uff08\u4f7f\u7528MoS<sub>2<\/sub>\u4f5c\u4e3a\u5149\u50ac\u5316\u5236\u6c22\u7684\u52a9\u50ac\u5316\u5242\uff0c<em>J. Am. Chem. Soc.<\/em> <strong>2008<\/strong>, 130, 7176\uff09\u4ee5\u6765\uff0c\u5173\u4e8e\u8be5\u4e3b\u9898\u7684\u51fa\u7248\u7269\u6025\u5267\u7684\u589e\u957f\uff08<strong>\u56fe<\/strong><strong>1<\/strong>\uff09\u3002\u5c3d\u7ba1\u8fd9\u662f\u4e00\u4e2a\u5e74\u8f7b\u7684\u9886\u57df\uff0c\u6311\u6218\u4f9d\u7136\u5b58\u5728\uff0c\u4f46\u5b83\u786e\u5b9e\u6307\u51fa\u4e86\u4e00\u4e2a\u7684\u5bcc\u6709\u6210\u6548\u7684\u73b0\u72b6\u548c\u5149\u660e\u7684\u672a\u6765\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u9274\u4e8e\u6b64\uff0c\u9999\u6e2f\u57ce\u5e02\u5927\u5b66\u66fe\u5fd7\u8fdc\u6559\u6388\uff0c\u9999\u6e2f\u4e2d\u6587\u5927\u5b66\u4f59\u6d4e\u7f8e\u6559\u6388\uff0c\u540d\u53e4\u5c4b\u5927\u5b66\u738b\u8c26\u6559\u6388\uff0c\u4ee5\u53ca\u54c8\u5c14\u6ee8\u5de5\u4e1a\u5927\u5b66\uff08\u6df1\u5733\uff09\u6731\u8363\u6dd1\u6559\u6388\u7b49\u4eba\uff0c\u603b\u7ed3\u548c\u5c55\u671b\u4e862D TMDs\u6750\u6599\u5728\u5149\u50ac\u5316\u9886\u57df\u7684\u4f18\u52bf\uff0c\u6311\u6218\uff0c\u7b56\u7565\u548c\u673a\u9047\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-246018\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe1-2.png\" alt=\"\" width=\"1269\" height=\"1134\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe1-2.png 1269w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe1-2-300x268.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe1-2-768x686.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe1-2-1024x915.png 1024w\" sizes=\"(max-width: 1269px) 100vw, 1269px\" \/><\/p>\n<p>\u56fe1 | \u7528\u4e8e\u5149\u50ac\u5316\u76842D TMDs\u7684\u7814\u7a76\u5de5\u4f5c\u548c\u5e74\u5ea6\u51fa\u7248\u7269\u6570\u91cf\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>3\u3001\u6b63\u6587\u89e3\u6790\uff1a<\/p>\n<p><strong><em>\uff08\u4e00\uff09\u57fa\u7840\u77e5\u8bc6<\/em><\/strong><\/p>\n<p><strong><em>\uff08<\/em><\/strong><strong><em>\u2160<\/em><\/strong><strong><em>\uff09<\/em><\/strong><strong><em>2D TMDs<\/em><\/strong><strong><em>\u7684\u57fa\u7840\u77e5\u8bc6<\/em><\/strong><\/p>\n<p>\u672c\u8282\u4ecb\u7ecd\u4e862D TMDs\u7684\u7ec4\u6210\u3001\u6676\u4f53\u7ed3\u6784\u548c\u7535\u5b50\u80fd\u5e26\u7ed3\u6784\uff0c\u65e8\u5728\u8ba9\u8bfb\u8005\u5bf9\u8be5\u6750\u6599\u5bb6\u65cf\u6709\u4e00\u4e2a\u521d\u6b65\u7684\u8ba4\u8bc6\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u7ec4\u6210\u3002<\/em><\/strong>TMDs\u901a\u5e38\u6807\u8bb0\u4e3aMX<sub>2<\/sub>\uff08M\uff1aIVB\u65cf\u81f3VIII\u65cf\u7684\u8fc7\u6e21\u91d1\u5c5e\u5143\u7d20\uff1bX\uff1aVIA\u65cf\u7684S\u3001Se\u548cTe\u5143\u7d20\uff09\uff08<strong>\u56fe<\/strong><strong>2a<\/strong>\uff09\uff0c\u662f\u5178\u578b\u76842D\u5c42\u72b6\u7eb3\u7c73\u6750\u6599\u3002\u6bcf\u4e2aTMD\u5355\u5c42\u5305\u542b\u4e09\u4e2a\u539f\u5b50\u5c42\uff0c\u5f62\u6210\u201cX-M-X\u201d\u5939\u5c42\u7ed3\u6784\u3002\u76f8\u90bb\u7684\u5355\u5c42\u4e4b\u95f4\u7684\u8ddd\u79bb\u4e3a6-7\u00c5\uff0c\u7531\u5fae\u5f31\u7684\u8303\u5fb7\u534e\u529b\u7ed3\u5408\u5728\u4e00\u8d77\uff0c\u8fd9\u4f7f\u5f97\u5b83\u4eec\u5f88\u5bb9\u6613\u88ab\u5265\u79bb\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u6676\u4f53\u7ed3\u6784\u3002<\/em><\/strong>TMDs\u5b58\u5728\u591a\u79cd\u6676\u4f53\u7ed3\u6784\uff08<strong>\u56fe<\/strong><strong>2b<\/strong>\uff09\u3002\u5177\u4f53\u5730\u8bf4\uff0c\u6709\u4e09\u79cd\u4f17\u6240\u5468\u77e5\u7684\u6676\u4f53\u7ed3\u6784\uff0c\u8fd9\u4e9b\u7ed3\u6784\u662f\u7531\u8fc7\u6e21\u91d1\u5c5e\u539f\u5b50\u7684\u4e0d\u540c\u914d\u4f4d\u51e0\u4f55\u7ed3\u6784\u6240\u5f62\u6210\u7684\uff0c\u53732H\uff08\u4e09\u68f1\u67f1\u5f62\uff09\u30011T\uff08\u516b\u9762\u4f53\uff09\u548c1T\u2032\uff08\u7578\u53d8\u516b\u9762\u4f53\u7684\uff09\u30022H TMDs\u8868\u73b0\u51faBernal\uff08ABA\uff09\u5806\u53e0\uff0c\u800c1T TMDs\u4e2d\u539f\u5b50\u5e73\u9762\u7684\u5806\u53e0\u987a\u5e8f\u662f\u83f1\u5f62ABC\u3002\u7ed3\u6784\u76f8\u7684\u591a\u6837\u6027\u5bfc\u81f4\u591a\u6837\u7684\u7535\u5b50\u6027\u8d28\u3002\u4f8b\u5982\uff0c2H-MoS<sub>2<\/sub>\u8868\u73b0\u51fa\u534a\u5bfc\u4f53\u5c5e\u6027\uff0c\u800c1T-MoS<sub>2<\/sub>\u5219\u8868\u73b0\u51fa\u91d1\u5c5e\u7279\u6027\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u7535\u5b50\u80fd\u5e26\u7ed3\u6784\u3002<\/em><\/strong>TMD\u5177\u6709\u53ef\u8c03\u8c10\uff08\u53d6\u51b3\u4e8e\u539a\u5ea6\uff09\u7684\u7535\u5b50\u5e26\u9699\uff08<strong>\u56fe<\/strong><strong>3a<\/strong>\uff09\uff0c\u8fd9\u662f\u7531\u91cf\u5b50\u9650\u57df\u6548\u5e94\u5f15\u8d77\u7684\u3002\u4ee52H-MoS<sub>2<\/sub>\u4e3a\u4f8b\uff0c\u5176\u8ba1\u7b97\u7684\u7535\u5b50\u5e26\u9699\u503c\u8303\u56f4\u4ece0.88 eV\uff08\u5757\u4f53\uff09\u52301.71 eV\uff08\u5355\u5c42\uff09\u3002\u6709\u8da3\u7684\u662f\uff0c\u5f53MoS<sub>2<\/sub>\u7684\u539a\u5ea6\u964d\u4f4e\u5230\u5355\u5c42\u65f6\uff0c\u5b83\u4ece\u95f4\u63a5\u5e26\u9699\u534a\u5bfc\u4f53\u53d8\u4e3a\u76f4\u63a5\u5e26\u9699\u534a\u5bfc\u4f53\uff0c\u540c\u65f6\u53d1\u5149\u7279\u6027\u53d1\u751f\u4e86\u620f\u5267\u6027\u7684\u8df3\u8dc3\uff08<strong>\u56fe<\/strong><strong>3b<\/strong>\uff09\u3002\u6b64\u5916\uff0c~2.16 eV\u662f\u5355\u5c42MoS<sub>2<\/sub>\u7684\u7535\u5b50\u5e26\u9699\u7684\u5b9e\u9a8c\u503c\u3002\u4e0d\u540cTMD\u5355\u5c42\u4e4b\u95f4\u7684\u5e26\u9699\u503c\u4e5f\u4e0d\u540c\uff08<strong>\u56fe<\/strong><strong>3c<\/strong>\uff09\uff0c\u8fd9\u8fdb\u4e00\u6b65\u5bfc\u81f4\u5b83\u4eec\u7684\u5149\u8c31\u54cd\u5e94\u7387\u4e0d\u540c\uff08<strong>\u56fe<\/strong><strong>3d<\/strong>\uff09\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-246019\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe2-1.png\" alt=\"\" width=\"1269\" height=\"1180\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe2-1.png 1269w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe2-1-300x279.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe2-1-768x714.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe2-1-1024x952.png 1024w\" sizes=\"(max-width: 1269px) 100vw, 1269px\" \/><\/p>\n<p>\u56fe2 | 2D TMDs\u7684\u7ec4\u6210\u548c\u6676\u4f53\u7ed3\u6784\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-246020\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe3-1.png\" alt=\"\" width=\"1266\" height=\"1745\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe3-1.png 1266w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe3-1-218x300.png 218w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe3-1-768x1059.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe3-1-743x1024.png 743w\" sizes=\"(max-width: 1266px) 100vw, 1266px\" \/><\/p>\n<p>\u56fe3 | 2D TMDs\u7684\u7535\u5b50\u80fd\u5e26\u7ed3\u6784\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\uff08<\/em><\/strong><strong><em>\u2161<\/em><\/strong><strong><em>\uff09\u5149\u50ac\u5316\u7684\u57fa\u7840\u77e5\u8bc6\uff1a<\/em><\/strong><\/p>\n<p>\u672c\u8282\u4ecb\u7ecd\u4e86\u5149\u50ac\u5316\u7684\u57fa\u7840\u77e5\u8bc6\uff0c\u65e8\u5728\u5e2e\u52a9\u8bfb\u8005\u5728\u5173\u6ce82D TMDs\u4e4b\u524d\u5bf9\u8be5\u50ac\u5316\u6280\u672f\u6709\u4e00\u4e2a\u521d\u6b65\u5370\u8c61\u3002\u672c\u8282\u5185\u5bb9\u5305\u62ec\uff1a\u5149\u50ac\u5316\u76f8\u6bd4\u4e8e\u5176\u4ed6\u50ac\u5316\u7684\u4f18\u52bf\uff0c\u5149\u50ac\u5316\u57fa\u672c\u539f\u7406\u548c\u8fc7\u7a0b\uff0c\u5149\u50ac\u5316\u7684\u70ed\u529b\u5b66\u9700\u6c42\uff0c\u5149\u50ac\u5316\u7684\u52a8\u529b\u5b66\u6311\u6218\uff0c\u5149\u50ac\u5316\u7684\u7cfb\u7edf\u914d\u7f6e\uff0c\u4ee5\u53ca\u8bc4\u4ef7\u5149\u50ac\u5316\u6027\u80fd\u7684\u53c2\u6570\u6307\u6807\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u5149\u50ac\u5316\u7684\u4f18\u52bf\u3002<\/em><\/strong>\u5149\u50ac\u5316\u5229\u7528\u592a\u9633\u80fd\uff08\u4e00\u79cd\u4e30\u5bcc\u3001\u65e0\u6c61\u67d3\u548c\u53ef\u518d\u751f\u7684\u81ea\u7136\u80fd\u6e90\uff09\uff0c\u6765\u9a71\u52a8\u5316\u5b66\u8fc7\u7a0b\uff0c\u88ab\u8ba4\u4e3a\u662f\u4e00\u79cd\u5f88\u6709\u524d\u9014\u7684\u6280\u672f\u3002\u4e0e\u4f20\u7edf\u7684\u70ed\u50ac\u5316\uff08\u901a\u5e38\u9700\u8981\u9ad8\u6e29\u548c\u9ad8\u538b\u64cd\u4f5c\u73af\u5883\uff09\u76f8\u6bd4\uff0c\u5927\u591a\u6570\u5149\u50ac\u5316\u662f\u5728\u73af\u5883\u6761\u4ef6\u4e0b\u64cd\u4f5c\u7684\uff0c\u4e14\u53ef\u4ee5\u907f\u514d\u8fc7\u5ea6\u6c27\u5316\u548c\u50ac\u5316\u5242\u5931\u6d3b\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u5149\u50ac\u5316\u57fa\u672c\u539f\u7406\u548c\u8fc7\u7a0b\u3002<\/em><\/strong>\u901a\u5e38\uff0c\u57fa\u672c\u7684\u5149\u50ac\u5316\u8fc7\u7a0b\u5305\u62ec\u4e09\u4e2a\u6b65\u9aa4\uff08<strong>\u56fe<\/strong><strong>4a<\/strong>\uff09\uff1a\uff081\uff09\u5149\u5438\u6536\uff1b\uff082\uff09 \u5149\u751f\u7535\u8377\u8f7d\u6d41\u5b50\u7684\u5206\u79bb\u548c\u8fc1\u79fb\uff1b\uff083\uff09\u8868\u9762\u6c27\u5316\u8fd8\u539f\u53cd\u5e94\u3002\u503c\u5f97\u6ce8\u610f\u7684\u662f\uff0c\u8f7d\u6d41\u5b50\u8fc1\u79fb\u8fc7\u7a0b\u603b\u662f\u4f34\u968f\u7740\u8f7d\u6d41\u5b50\u590d\u5408\uff0c\u5305\u62ec\u672c\u4f53\u590d\u5408\u548c\u8868\u9762\u590d\u5408\uff0c\u8fd9\u4e0d\u5229\u4e8e\u5149\u50ac\u5316\uff0c\u5e94\u5c3d\u53ef\u80fd\u907f\u514d\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u5149\u50ac\u5316\u7684\u70ed\u529b\u5b66\u9700\u6c42\u3002<\/em><\/strong>\u5149\u50ac\u5316\u53cd\u5e94\u7684\u53d1\u751f\u9700\u8981\u6ee1\u8db3\u70ed\u529b\u5b66\u8981\u6c42\uff1a\uff081\uff09\u5165\u5c04\u5149\u5b50\u7684\u80fd\u91cf\u5e94\u7b49\u4e8e\u6216\u5927\u4e8e\u534a\u5bfc\u4f53\u7684\u5149\u5b66\u5e26\u9699\uff08E<sub>g<\/sub>\uff09\uff1b\uff082\uff09 \u534a\u5bfc\u4f53\u7684\u4ef7\u5e26\u6700\u5927\u503c\uff08VBM\uff09\u9700\u8981\u6bd4\u7ed9\u4f53\u7684\u6c27\u5316\u7535\u4f4d\uff08E<sub>\uff08<\/sub><sub>D\/D<\/sub><sub>\u2212<\/sub><sub>\uff09<\/sub>\uff09\u66f4\u6b63\uff1b\uff083\uff09 \u800c\u5bfc\u5e26\u6700\u5c0f\u503c\uff08CBM\uff09\u9700\u8981\u6bd4\u53d7\u4f53\u7684\u8fd8\u539f\u7535\u4f4d\uff08E<sub>\uff08<\/sub><sub>A+\/A<\/sub><sub>\uff09<\/sub>\uff09\u66f4\u8d1f\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u5149\u50ac\u5316\u7684\u52a8\u529b\u5b66\u6311\u6218\u3002<\/em><\/strong>\u9664\u4e86\u4e0a\u8ff0\u70ed\u529b\u5b66\u8981\u6c42\uff0c\u5149\u50ac\u5316\u8fd8\u9762\u4e34\u8bb8\u591a\u52a8\u529b\u5b66\u6311\u6218\uff1a\uff081\uff09\u4e09\u4e2a\u57fa\u672c\u6b65\u9aa4\u8de8\u8d8a10<sup>\u2212<\/sup><sup>15<\/sup>\u81f310<sup>\u2212<\/sup><sup>1<\/sup> s\u7684\u5de8\u5927\u65f6\u95f4\u5c3a\u5ea6\uff0810<sup>\u2212<\/sup><sup>15<\/sup>-10<sup>\u2212<\/sup><sup>9<\/sup> s\u7684\u5149\u5438\u6536\u3001&lt;10<sup>\u2212<\/sup><sup>15<\/sup> s\u7684\u7535\u8377\u5206\u79bb\u548c\u4f20\u8f93\uff0c\u4ee5\u53ca10<sup>\u2212<\/sup><sup>3<\/sup>-10<sup>\u2212<\/sup><sup>1<\/sup> s\u8868\u9762\u53cd\u5e94\uff09\uff0c\u8fd9\u5bf9\u6700\u5927\u5316\u4e09\u6b65\u53cd\u5e94\u4e4b\u95f4\u7684\u534f\u540c\u4f5c\u7528\u63d0\u51fa\u4e86\u5de8\u5927\u6311\u6218\uff1b\uff082\uff09 \u6700\u4f73\u7684\u5149\u50ac\u5316\u5242\u9700\u8981\u540c\u65f6\u4fdd\u6301\u592a\u9633\u8f90\u5c04\u5149\u8c31\u4e2d\u7684\u5bbd\u5149\u5438\u6536\uff08\u9700\u8981\u7a84\u5e26\u9699\uff09\u548c\u5f3a\u6c27\u5316\u8fd8\u539f\u80fd\u529b\uff08\u9700\u8981\u5bbd\u5e26\u9699\uff09\uff0c\u4f46\u5b83\u4eec\u7684\u5b9e\u73b0\u672c\u8d28\u4e0a\u662f\u77db\u76fe\u7684\uff1b\uff083\uff09 \u534a\u5bfc\u4f53\u5149\u654f\u5242\u901a\u5e38\u7f3a\u4e4f\u6d3b\u6027\u4f4d\u70b9\u3002\u56e0\u6b64\uff0c\u901a\u5e38\u9700\u8981\u5728\u534a\u5bfc\u4f53\u8868\u9762\u8d1f\u8f7d\u52a9\u50ac\u5316\u5242\uff0c\u4ee5\u4fc3\u8fdb\u7535\u8377\u5206\u79bb\u548c\u8f6c\u79fb\uff0c\u5e76\u964d\u4f4e\u6d3b\u5316\u80fd\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u5149\u50ac\u5316\u7684\u7cfb\u7edf\u914d\u7f6e\u3002<\/em><\/strong>\u5149\u50ac\u5316\u7cfb\u7edf\u7684\u5408\u7406\u6784\u5efa\u5bf9\u4e8e\u5149\u50ac\u5316\u81f3\u5173\u91cd\u8981\u3002\u901a\u5e38\uff0c\u5149\u50ac\u5316\u4e2d\u6709\u4e24\u79cd\u7c7b\u578b\u7684\u7cfb\u7edf\u914d\u7f6e\uff1a \u201c\u60ac\u6d6e\u201d\u7cfb\u7edf\u548c\u201c\u56fa\u5b9a\u201d\u7cfb\u7edf\uff08<strong>\u56fe<\/strong><strong>4b<\/strong>\uff09\u3002\u5728\u201c\u60ac\u6d6e\u201d\u7cfb\u7edf\u4e2d\uff0c\u9897\u7c92\u5149\u50ac\u5316\u5242\u76f4\u63a5\u60ac\u6d6e\u5728\u53cd\u5e94\u6eb6\u6db2\u4e2d\u3002\u987e\u540d\u601d\u4e49\uff0c\u201c\u56fa\u5b9a\u201d\u7cfb\u7edf\u662f\u6307\u56fa\u5b9a\u5728\u57fa\u6750\u4e0a\u8fdb\u884c\u5149\u50ac\u5316\u53cd\u5e94\u7684\u5149\u50ac\u5316\u5242\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u8bc4\u4ef7\u5149\u50ac\u5316\u6027\u80fd\u7684\u53c2\u6570\u6307\u6807\u3002<\/em><\/strong>\u5149\u50ac\u5316\u7684\u6700\u7ec8\u8ffd\u6c42\u662f\u9ad8\u6548\u5229\u7528\u592a\u9633\u80fd\u3002\u56e0\u6b64\uff0c\u5982\u4f55\u8bc4\u4ef7\u7cfb\u7edf\u7684\u6548\u7387\u662f\u5f88\u91cd\u8981\u7684\u3002\u5728\u6b64\uff0c\u6587\u7ae0\u6982\u8ff0\u4e86\u8bc4\u4f30\u5149\u50ac\u5316\u6d3b\u6027\u7684\u5e38\u7528\u53c2\u6570\uff08<strong>\u56fe<\/strong><strong>4c<\/strong>\uff09\uff1a\u592a\u9633\u80fd\u5230\u5316\u5b66\u80fd\u8f6c\u5316\u6548\u7387\uff0c\u4f8b\u5982\uff0c\u592a\u9633\u80fd\u5230\u6c22\u8f6c\u5316\u6548\u7387\uff0c\uff08STH\uff09\u3001\u8868\u89c2\u91cf\u5b50\u4ea7\u7387\uff08AQY\uff09, \u548c\u8f6c\u6362\u9891\u7387\uff08TOF\uff09\u3002\u9664\u4e86\u4e0a\u8ff0\u53c2\u6570\uff0c\u7a33\u5b9a\u6027\u662f\u5149\u50ac\u5316\u5b9e\u9645\u5e94\u7528\u7684\u53e6\u4e00\u4e2a\u91cd\u8981\u6307\u6807\uff0c\u503c\u5f97\u5173\u6ce8\u3002\u7a33\u5b9a\u6027\u7684\u76f4\u63a5\u8bc4\u4f30\u7b56\u7565\u662f\u8fdb\u884c\u957f\u671f\u5149\u50ac\u5316\u53cd\u5e94\u6d4b\u8bd5\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-246021\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe4-1.png\" alt=\"\" width=\"1269\" height=\"1210\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe4-1.png 1269w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe4-1-300x286.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe4-1-768x732.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe4-1-1024x976.png 1024w\" sizes=\"(max-width: 1269px) 100vw, 1269px\" \/><\/p>\n<p>\u56fe4 | \u5149\u50ac\u5316\u7684\u57fa\u7840\u77e5\u8bc6\u3002<\/p>\n<p><strong><em><br \/>\n <\/em><\/strong><\/p>\n<p><strong><em>\u00a0<\/em><\/strong><\/p>\n<p><strong><em>\uff08<\/em><\/strong><strong><em>\u2162<\/em><\/strong><strong><em>\uff09<\/em><\/strong><strong><em>2D TMDs<\/em><\/strong><strong><em>\u7684\u5408\u6210\uff1a<\/em><\/strong><\/p>\n<p>\u672c\u8282\u4ecb\u7ecd\u4e862D TMD\u7684\u53ef\u9760\u5408\u6210\u65b9\u6cd5\uff0c\u4e3a\u8bfb\u8005\u63d0\u4f9b\u4e86\u6b64\u7c7b\u6750\u6599\u5408\u6210\u7684\u7b80\u660e\u6307\u5357\u3002\u7406\u60f3\u60c5\u51b5\u4e0b\uff0c2D TMDs\u7684\u5408\u6210\u65b9\u6cd5\u53ef\u5206\u4e3a\u4e24\u7c7b\uff1a\u81ea\u4e0a\u800c\u4e0b\u7684\u5265\u79bb\uff08\u4ece\u5927\u5757\u52302D\u7eb3\u7c73\u7247\uff1b\u4f8b\u5982\u673a\u68b0\u5265\u79bb-<strong>\u56fe<\/strong><strong>5a<\/strong>\uff0c\u76f4\u63a5\u6db2\u76f8\u5265\u79bb-<strong>\u56fe<\/strong><strong>5b<\/strong>\uff0c\u548c\u57fa\u4e8e\u63d2\u5c42\u6cd5\u7684\u6db2\u76f8\u5265\u79bb-<strong>\u56fe<\/strong><strong>5c<\/strong>\uff09\u548c\u81ea\u4e0b\u800c\u4e0a\u7684\u5408\u6210\uff08\u4ece\u5c0f\u6784\u5efa\u5206\u5b50\u52302D\u7eb3\u7c73\u7247\u6750\uff1b\u4f8b\u5982\u5316\u5b66\u6c14\u76f8\u6c89\u79ef\u751f\u957f-<strong>\u56fe<\/strong><strong>5d<\/strong>\uff0c\u6e7f\u5316\u5b66\u5408\u6210-<strong>\u56fe<\/strong><strong>5e<\/strong>\uff09\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u673a\u68b0\u5265\u79bb\u6cd5\u3002<\/em><\/strong>\u673a\u68b0\u5265\u79bb\uff08<strong>\u56fe<\/strong><strong>5a<\/strong>\uff09\uff0c\u4f7f\u7528\u900f\u660e\u80f6\u5e26\u5c06\u539f\u5b50\u5c42\u4ece\u5176\u5757\u72b6\u6676\u4f53\u4e0a\u5265\u79bb\uff0c\u662fTMD\u5265\u79bb\u7684\u4e00\u79cd\u7b80\u5355\u800c\u5e38\u89c1\u7684\u65b9\u6cd5\u3002\u751f\u4ea7\u76842D TMD\u5177\u6709\u5355\u6676\u3001\u9ad8\u7eaf\u5ea6\u548c\u6e05\u6d01\u5ea6\u7684\u7279\u70b9\uff0c\u9002\u7528\u4e8e\u5668\u4ef6\u5e94\u7528\u3002\u7406\u8bba\u4e0a\uff0c\u8be5\u65b9\u6cd5\u53ef\u7528\u4e8e\u5265\u79bb\u6240\u6709\u5206\u5c42\u7684\u5757\u72b6TMD\u4ee5\u751f\u6210\u8d85\u85842D\u5bf9\u5e94\u7269\uff0c\u4f46\u4e0d\u53ef\u5927\u89c4\u6a21\u751f\u4ea7\u3002\u6b64\u5916\uff0c\u7cfb\u7edf\u63a7\u5236\u6700\u7ec8\u4ea7\u54c1\u7684\u539a\u5ea6\u3001\u5c3a\u5bf8\u548c\u5f62\u72b6\u76f8\u5bf9\u56f0\u96be\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u76f4\u63a5\u6db2\u76f8\u5265\u79bb\u3002<\/em><\/strong>\u5bf9\u4e8e\u5927\u89c4\u6a21\u83b7\u5f97\u5265\u79bb\u76842D TMD\uff08\u673a\u68b0\u5265\u79bb\u4e0d\u53ef\u884c\uff09\uff0c\u6db2\u76f8\u5265\u79bb\u662f\u6709\u5e0c\u671b\u7684\u3002\u76f4\u63a5\u6db2\u4f53\u5265\u79bb\uff08<strong>\u56fe<\/strong><strong>5b<\/strong>\uff09\u662f\u6307\u5728\u6eb6\u5242\u4e2d\u901a\u8fc7\u8d85\u58f0\u6216\u526a\u5207\u529b\u7834\u574f\u5f31\u8303\u5fb7\u534e\u76f8\u4e92\u4f5c\u7528\uff0c\u5c06\u5757\u72b6TMD\u76f4\u63a5\u5265\u79bb\u6210\u5176\u8d85\u85842D\u5bf9\u5e94\u7269\u3002N-\u7532\u57fa\u5421\u54af\u70f7\u916e\uff08NMP\uff09\u548c\u4e8c\u7532\u57fa\u7532\u9170\u80fa\uff08DMF\uff09\u662f\u5e38\u7528\u7684\u4e24\u79cd\u6eb6\u5242\u3002\u7b80\u5355\u7684\u64cd\u4f5c\u6b65\u9aa4\u3001\u4f4e\u6210\u672c\u3001\u6eb6\u6db2\u53ef\u52a0\u5de5\u6027\u4ee5\u53ca\u5bf9\u7a7a\u6c14\u548c\u6c34\u7684\u4e0d\u654f\u611f\u6027\u4f7f\u5176\u5728\u5546\u4e1a\u5e94\u7528\u4e2d\u663e\u793a\u51fa\u5de8\u5927\u7684\u6f5c\u529b\u3002\u7136\u800c\uff0c\u76f4\u63a5\u6db2\u76f8\u5265\u79bb\u53d7\u5230\u5355\u5c42\u4ea7\u7387\u4f4e\u3001\u5265\u79bb\u8584\u7247\u6a2a\u5411\u5c3a\u5bf8\u5c0f\u548c\u6240\u7528\u6709\u673a\u6eb6\u5242\u6bd2\u6027\u7684\u56f0\u6270\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u57fa\u4e8e\u63d2\u5c42\u6cd5\u7684\u6db2\u76f8\u5265\u79bb\u3002<\/em><\/strong>\u57fa\u4e8e\u63d2\u5c42\u6cd5\u7684\u6db2\u76f8\u5265\u79bb\u7684\u57fa\u672c\u539f\u7406\u662f\u901a\u8fc7\u5d4c\u5165\u5916\u6765\u7269\u79cd\uff08\u79bb\u5b50\u6216\u5206\u5b50\uff09\u6765\u6269\u5927\u5c42\u95f4\u8ddd\uff0c\u4ece\u800c\u5728\u5265\u79bb\u4e4b\u524d\u524a\u5f31\u5939\u5c42\u7c98\u9644\u529b\u3002\u5178\u578b\u7a0b\u5e8f\u5305\u62ec\u5c06\u5916\u6765\u7269\u79cd\u5316\u5b66\u6216\u7535\u5316\u5b66\u5d4c\u5165TMD\u7684\u5c42\u95f4\uff0c\u7136\u540e\u8fdb\u884c\u6e29\u548c\u7684\u5265\u79bb\u8fc7\u7a0b\u3002\u9502\u79bb\u5b50\uff08Li<sup>+<\/sup>\uff09\u662f\u4e00\u79cd\u5e38\u7528\u7684\u63d2\u5c42\u5242\uff0c\u4f46\u603b\u662f\u5f15\u5165\u57fa\u9762\u7f3a\u9677\uff0c\u5e76\u5f15\u53d12H-1T\/1T&#8217;\u76f8\u53d8\u3002\u8f83\u5927\u7684\u79bb\u5b50\uff0c\u5982\u56db\u70f7\u57fa\u94f5\u9633\u79bb\u5b50\uff08R<sub>4<\/sub>N<sup>+<\/sup>\uff09\uff0c\u53ef\u4ee5\u907f\u514d\u8fd9\u79cd\u76f8\u53d8\uff0c\u4f46\u589e\u5927\u7684\u5c3a\u5bf8\u4e0d\u53ef\u907f\u514d\u5730\u5bfc\u81f4\u63d2\u5c42\u52bf\u5792\u7684\u589e\u52a0\uff0c\u4ece\u800c\u964d\u4f4e\u5757\u72b6TMDs\u6676\u4f53\u7684\u63d2\u5c42\u901f\u7387\uff0c\u4ece\u800c\u964d\u4f4e\u5265\u79bb\u901f\u7387\u548c\u5355\u5c42\u7684\u4ea7\u7387\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>CVD<\/em><\/strong><strong><em>\u751f\u957f\u3002<\/em><\/strong>CVD\u751f\u957f\uff08<strong>\u56fe<\/strong><strong>5d<\/strong>\uff09\u662f\u5728\u886c\u5e95\uff08\u4f8b\u5982\uff0c\u4f20\u7edf\u7684SiO<sub>2<\/sub>\/Si\uff09\u4e0a\u8fdb\u884c2D TMD\u7684\u6676\u5706\u89c4\u6a21\u5408\u6210\u7684\u7ecf\u5178\u81ea\u4e0b\u800c\u4e0a\u7b56\u7565\u3002\u5728\u4e00\u4e2a\u5178\u578b\u7684\u8fc7\u7a0b\u4e2d\uff0c\u84b8\u53d1\u7684\u53cd\u5e94\u6027\u524d\u9a71\u4f53\uff08\u4f8b\u5982\uff0c\u786b\u78fa\u7c89\u548cMoO3\u7c89\uff09\u5728\u9ad8\u6e29\u548c\u9ad8\u771f\u7a7a\u73af\u5883\u4e0b\u4ee5\u7279\u5b9a\u6c14\u6d41\u7a7f\u8fc7\u76ee\u6807\u886c\u5e95\u7684\u8868\u9762\uff0c\u5728\u6b64\u8fc7\u7a0b\u4e2d\uff0c\u524d\u9a71\u4f53\u5728\u886c\u5e95\u8868\u9762\u4e0a\u7ecf\u5386\u53cd\u5e94\u3001\u5206\u89e3\u3001\u539f\u4f4d\u6210\u6838\u548c\u751f\u957f\uff0c\u6700\u7ec8\u5f62\u62102D TMD\u8584\u7247\u3002\u751f\u4ea7\u76842D TMD\u5c3a\u5bf8\u5927\u3001\u7eaf\u5ea6\u9ad8\u3001\u7ed3\u6676\u5ea6\u9ad8\u3002\u7136\u800c\uff0c\u8fd9\u79cd\u65b9\u6cd5\u53d7\u5230\u6076\u52a3\u5de5\u4f5c\u73af\u5883\uff08\u9ad8\u6e29\u548c\u9ad8\u771f\u7a7a\uff09\u7684\u963b\u788d\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong>\u6e7f\u5f0f\u5316\u5b66\u5408\u6210\u3002<\/strong>2D TMD \u8584\u7247\u4e5f\u53ef\u4ee5\u901a\u8fc7\u6e7f\u5316\u5b66\u5408\u6210\u5de5\u827a\uff08\u53e6\u4e00\u79cd\u8457\u540d\u7684\u81ea\u4e0b\u800c\u4e0a\u7b56\u7565\uff09\u5236\u5907\uff0c\u4f8b\u5982\u6c34\/\u6eb6\u5242\u70ed\u5408\u6210\uff08<strong>\u56fe<\/strong><strong>5e<\/strong>\u7684\u5de6\u4fa7\u9762\u677f\uff09\u548c\u70ed\u6ce8\u5c04\u5408\u6210\uff08<strong>\u56fe<\/strong><strong>5 e<\/strong>\u7684\u53f3\u4fa7\u9762\u677f\uff09\u3002\u8be5\u65b9\u6cd5\u6bd4CVD\u751f\u957f\u66f4\u7b80\u5355\u3001\u66f4\u5bb9\u6613\u64cd\u4f5c\uff0c\u4f46\u4ea7\u54c1\u8d28\u91cf\u548c\u7ed3\u6676\u5ea6\u4e0d\u5982CVD\u751f\u957f\u83b7\u5f97\u7684\u4ea7\u54c1\u30022D TMDs\u7684\u6c34\/\u6eb6\u5242\u70ed\u5408\u6210\u5728\u5bc6\u5c01\u5bb9\u5668\u4e2d\u7684\u9ad8\u6e29\u548c\u9ad8\u538b\u4e0b\u8fdb\u884c\uff0c\u5e76\u4f7f\u7528\u6c34\/\u6709\u673a\u6eb6\u5242\u4f5c\u4e3a\u53cd\u5e94\u4ecb\u8d28\uff0c\u5728\u6b64\u8fc7\u7a0b\u4e2d\u91d1\u5c5e\u524d\u9a71\u4f53\uff08\u5982\u94bc\u9178\uff09\u548c\u786b\u65cf\u524d\u9a71\u4f53\uff08\u4f8b\u5982\u786b\u8132\uff09\u76f8\u4e92\u53cd\u5e94\u5f62\u6210TMD\u6676\u4f53\u3002\u6240\u5f97\u5230\u76842D TMD\u8584\u7247\u5177\u6709\u4e30\u5bcc\u7684\u7f3a\u9677\u548c\u6d3b\u6027\u8fb9\u7f18\u4f4d\u70b9\uff0c\u663e\u793a\u51fa\u7a81\u51fa\u7684\u50ac\u5316\u6027\u80fd\uff0c\u4f46\u5176\u539a\u5ea6\u5e76\u672a\u6700\u7ec8\u663e\u793a\u4e3a\u5355\u5c42\u3002\u8fd9\u79cd\u65b9\u6cd5\u7b80\u5355\u4e14\u53ef\u6269\u5c55\uff0c\u4f46\u4ea7\u54c1\u8d28\u91cf\u5bf9\u53cd\u5e94\u6761\u4ef6\u654f\u611f\uff0c\u5982\u64cd\u4f5c\u6e29\u5ea6\u3001\u65f6\u95f4\u3001\u524d\u9a71\u4f53\u3001\u6eb6\u5242\u548c\u8868\u9762\u6d3b\u6027\u5242\u7684\u7c7b\u578b\u548c\u6d53\u5ea6\u3002\u70ed\u6ce8\u5c04\u6cd5\u662f2D TMDs\u80f6\u4f53\u5408\u6210\u7684\u6709\u6548\u7b56\u7565\uff0c\u5176\u901a\u8fc7\u5c06\u6d3b\u6027\u53cd\u5e94\u7269\u5206\u5b50\uff08\u4f8b\u5982CS<sub>2<\/sub>\u548cWCl<sub>6<\/sub>\u524d\u4f53\uff09\u5feb\u901f\u6ce8\u5c04\u5230\u542b\u6709\u7279\u6b8a\u8868\u9762\u6d3b\u6027\u5242\uff08\u957f\u94fe\u6cb9\u80fa\u548c\/\u6216\u6cb9\u9178\uff09\u7684\u70ed\u6eb6\u6db2\u4e2d\u6765\u8bf1\u5bfc\u5316\u5b66\u53cd\u5e94\u3002\u8fd9\u79cd\u70ed\u6ce8\u5c04\u65b9\u6cd5\u4ea7\u751f\u5177\u6709\u826f\u597d\u5206\u6563\u6027\u3001\u9ad8\u7eaf\u5ea6\u548c\u5747\u5300\u5c3a\u5bf8\u548c\u5f62\u72b6\u76842D TMD\uff0c\u4f46\u4ecd\u6709\u5c40\u9650\u6027\u3002\u4f7f\u7528\u96be\u53bb\u9664\u8868\u9762\u6d3b\u6027\u5242\uff08\u957f\u94fe\u6cb9\u80fa\u548c\u6cb9\u9178\uff09\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong>\u5176\u4ed6\u3002<\/strong>\u9664\u4e86\u4e0a\u8ff0\u5e38\u7528\u65b9\u6cd5\u4e4b\u5916\uff0c\u8fc7\u53bb\u51e0\u5e74\u8fd8\u51fa\u73b0\u4e86\u4e00\u4e9b\u7528\u4e8e\u751f\u4ea72D TMD\u7684\u65b0\u7b56\u7565\uff0c\u4f8b\u5982\u5206\u5b50\u675f\u5916\u5ef6\uff08MBE\uff09\u3001\u539f\u5b50\u5c42\u6c89\u79ef\uff08ALD\uff09\u3001\u8109\u51b2\u6fc0\u5149\u6c89\u79ef\u3001\u548c\u901a\u8fc7\u5e73\u9762\u8868\u9762\u7b49\u79bb\u5b50\u4f53\u6fc0\u5143\uff08SPPs\uff09\u8fdb\u884c\u7684\u539f\u5b50\u5c42\u8680\u523b\u3002\u8fd9\u4e9b\u6280\u672f\u7684\u51fa\u73b0\u4e30\u5bcc\u4e862D TMD\u5236\u5907\u7684\u5de5\u5177\u7bb1\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-246022\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe5-1.png\" alt=\"\" width=\"1055\" height=\"1432\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe5-1.png 1055w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe5-1-221x300.png 221w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe5-1-768x1042.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe5-1-754x1024.png 754w\" sizes=\"(max-width: 1055px) 100vw, 1055px\" \/><\/p>\n<p>\u56fe5 | 2D TMDs\u7684\u5408\u6210\u3002<\/p>\n<p><strong><em>\uff08\u4e8c\uff09<\/em><\/strong><strong><em>2D TMDs<\/em><\/strong><strong><em>\u5728\u5149\u50ac\u5316\u4e50\u56ed\u4e2d\u7684\u4f18\u52bf<\/em><\/strong><\/p>\n<p><strong><em>\uff08<\/em><\/strong><strong><em>\u2160<\/em><\/strong><strong><em>\uff09<\/em><\/strong><strong><em>2D TMDs<\/em><\/strong><strong><em>\u4f5c\u4e3a\u52a9\u50ac\u5316\u5242\u7684\u4f18\u52bf<\/em><\/strong><\/p>\n<p>2D TMDs\uff08\u7279\u522b\u662f\u5176\u91d1\u5c5e\u76f8\u6676\u4f53\uff0c\u4f8b\u59821T-MoS<sub>2<\/sub>\uff09\u662f\u5149\u50ac\u5316\u4e2d\u6709\u524d\u9014\u7684\u52a9\u50ac\u5316\u5242\u3002\u5b83\u4eec\u662f\u8d35\u91d1\u5c5e\u7684\u7406\u60f3\u66ff\u4ee3\u54c1\uff0c\u751a\u81f3\u6709\u53ef\u80fd\u5728\u6027\u80fd\u4e0a\u8d85\u8d8a\u8d35\u91d1\u5c5e\u3002\u4f8b\u5982\uff0c\u4f5c\u4e3a\u52a9\u50ac\u5316\u5242\u76842D MoS<sub>2<\/sub>\u548cWS<sub>2<\/sub>\u663e\u793a\u51fa\u6bd4\u8d35\u91d1\u5c5e\uff08\u5305\u62ecPt\u3001Pd\u3001Rh\u3001Ru\u548cAu\uff09\u66f4\u597d\u7684\u4fc3\u8fdbCdS\u5149\u50ac\u5316\u4ea7H<sub>2<\/sub>\u7684\u6548\u679c\uff08<strong>\u56fe<\/strong><strong>6a<\/strong>\uff09\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u826f\u597d\u7684\u5bfc\u7535\u6027\u3002<\/em><\/strong>\u91d1\u5c5e\u76f82D TMD\u5177\u6709\u826f\u597d\u7684\u5bfc\u7535\u6027\uff08<strong>\u56fe<\/strong><strong>6b<\/strong>\uff09\uff0c\u4f7f\u5176\u80fd\u591f\u4e3a\u5149\u751f\u7535\u8377\u63d0\u4f9b\u6355\u83b7\u4f4d\u70b9\uff0c\u5e76\u4fc3\u8fdb\u7535\u8377\u5206\u79bb\u3001\u8fc1\u79fb\u548c\u6536\u96c6\uff0c\u4ece\u800c\u63d0\u9ad8\u91cf\u5b50\u6548\u7387\uff08<strong>\u56fe<\/strong><strong>6c<\/strong>\uff09\u3002\u4f8b\u5982\uff0c\u91d1\u5c5e1T\u76f8MoS<sub>2<\/sub>\uff08\u5177\u6709\u9ad8\u7684\u7535\u5bfc\u7387\u200910-100S\u2219cm<sup>-1<\/sup>\uff09\u7684\u5bfc\u7535\u6027\u51e0\u4e4e\u662f\u5176\u534a\u5bfc\u75352H\u76f8\u768410<sup>7<\/sup>\u500d\uff0c\u5e76\u4e14\u63a5\u8fd1\u77f3\u58a8\u70ef\uff08~100\u2009S\u2219cm<sup>-1<\/sup>\uff09\uff0c\u8fd9\u8d4b\u4e88\u4e86\u5b83\u5728\u5149\u50ac\u5316\u4e2d\u7684\u7406\u60f3\u52a9\u50ac\u5316\u5242\u4f5c\u7528\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u5728\u8fb9\u7f18\u548c\u57fa\u5e95\u5e73\u9762\u4e0a\u90fd\u6709\u4e30\u5bcc\u7684\u6d3b\u6027\u4f4d\u70b9\u3002<\/em><\/strong>\u91d1\u5c5e\u76f82D TMDs\u5728\u8fb9\u7f18\u548c\u57fa\u9762\u4e0a\u90fd\u5177\u6709\u4e30\u5bcc\u7684\u6d3b\u6027\u4f4d\u70b9\uff08<strong>\u56fe<\/strong><strong>6e<\/strong>\uff09\uff0c\u8fd9\u8d4b\u4e88\u5b83\u4eec\u4f5c\u4e3a\u53cd\u5e94\u7269\u5206\u5b50\u7684\u5438\u9644\u3001\u6d3b\u5316\u548c\u53cd\u5e94\u4f4d\u70b9\u53d1\u6325\u6d3b\u6027\u4f5c\u7528\uff0c\u4ee5\u964d\u4f4e\u6d3b\u5316\u80fd\u5e76\u52a0\u901f\u53cd\u5e94\u52a8\u529b\u5b66\uff08<strong>\u56fe<\/strong><strong>6f<\/strong>\uff09\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u5bc6\u96c6\u754c\u9762\u7ed3\u3002<\/em><\/strong>\u5b83\u4eec\u7684\uff082D TMD\uff09\u539f\u5b50\u8584\u5c42\u7684\u7279\u6027\u4f7f\u5b83\u4eec\u80fd\u591f\u4e0e\u5149\u6536\u96c6\u534a\u5bfc\u4f53\u5f62\u6210\u5bc6\u96c6\u7684\u754c\u9762\u7ed3\uff0c\u8fd9\u4fdd\u8bc1\u4e86\u5149\u8bf1\u5bfc\u7535\u8377\u7684\u5feb\u901f\u8f6c\u79fb\u3002\u8fd9\u79cd\u5bc6\u96c6\u7684\u754c\u9762\u8fde\u63a5\u662f\u7531\u5316\u5b66\u952e\u6865\u6216\u8303\u5fb7\u534e\u529b\u6784\u6210\u7684\u3002<\/p>\n<p>2D TMD\u548c\u5149\u91c7\u96c6\u534a\u5bfc\u4f53\u4e4b\u95f4\u5bb9\u6613\u5f62\u6210\u5316\u5b66\u952e\u6865\uff0c\u5982Bi<sub>12<\/sub>O<sub>17<\/sub>Cl<sub>2<\/sub>-MoS<sub>2<\/sub>\u754c\u9762\u4e2d\u7684Bi-S\u952e\u6865\uff08<strong>\u56fe<\/strong><strong>8a<\/strong>\uff09\u3001ZnIn<sub>2<\/sub>S<sub>4<\/sub>-MoS<sub>2<\/sub>\u754c\u9762\u7684Zn-S\u952e\u6865\uff08<strong>\u56fe<\/strong><strong>8b<\/strong>\uff09\u3001\u548cTiO<sub>2<\/sub>-ReS<sub>2<\/sub>\u6216TiO<sub>2<\/sub>-MoS<sub>2<\/sub>\u754c\u9762\u4e2dO-Re\uff08\u6216O-Mo\uff09\u952e\u6865\uff08\u89c1<strong>\u56fe<\/strong><strong>8c<\/strong>\uff09\u3002\u8fd9\u6837\u7684\u6865\u4e3a\u7535\u5b50\u8fc1\u79fb\u63d0\u4f9b\u4e86\u9ad8\u901f\u901a\u9053\uff0c\u4ece\u800c\u4fc3\u8fdb\u4e86\u5149\u751f\u7535\u5b50-\u7a7a\u7a74\u5bf9\u7684\u5206\u79bb\uff0c\u5ef6\u957f\u4e86\u8f7d\u6d41\u5b50\u5bff\u547d\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u5176\u4ed6\u4e00\u4e9b\u6709\u5438\u5f15\u529b\u7684\u754c\u9762\u8868\u9762\u6027\u8d28\u548c\u884c\u4e3a\u3002<\/em><\/strong>\u91d1\u5c5e\u76f82D TMDs\u8fd8\u5177\u6709\u4e00\u4e9b\u5176\u4ed6\u6709\u5438\u5f15\u529b\u7684\u754c\u9762\u8868\u9762\u6027\u8d28\u548c\u884c\u4e3a\uff0c\u5305\u62ec\u6d3b\u6027\u4f4d\u70b9\u81ea\u4f18\u5316\u3001\u4f5c\u4e3a\u7535\u5b50\u5bcc\u96c6\u57df\u7684\u5bcc\u786b\u7a7a\u4f4d\u3001\u8bf1\u5bfc\u7684\u5149\u70ed\u6548\u5e94\u7b49\u3002\u8fd9\u4e9b\u6027\u8d28\u548c\u884c\u4e3a\u6fc0\u53d1\u4e86\u5b83\u4eec\u4f5c\u4e3a\u5149\u50ac\u5316\u52a9\u50ac\u5316\u5242\u7684\u66f4\u591a\u6f5c\u529b\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-246023\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe6-1.png\" alt=\"\" width=\"1240\" height=\"1550\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe6-1.png 1240w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe6-1-240x300.png 240w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe6-1-768x960.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe6-1-819x1024.png 819w\" sizes=\"(max-width: 1240px) 100vw, 1240px\" \/><\/p>\n<p>\u56fe6 | 2D TMDs\u4f5c\u4e3a\u52a9\u50ac\u5316\u5242\u7684\u4f18\u52bf\u548c\u529f\u80fd\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-246024\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe7-1.png\" alt=\"\" width=\"1266\" height=\"1297\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe7-1.png 1266w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe7-1-293x300.png 293w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe7-1-768x787.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe7-1-1000x1024.png 1000w\" sizes=\"(max-width: 1266px) 100vw, 1266px\" \/><\/p>\n<p>\u56fe7 | 2D TMDs\u4e0a\u6c22\u5438\u9644\u80fd\u7684\u7406\u8bba\u8ba1\u7b97\uff08\u57fa\u4e8e\u5bc6\u5ea6\u6cdb\u51fd\u7406\u8bba\uff09\u70ed\u529b\u5b66\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-246025\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe8-1.png\" alt=\"\" width=\"1270\" height=\"1597\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe8-1.png 1270w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe8-1-239x300.png 239w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe8-1-768x966.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe8-1-814x1024.png 814w\" sizes=\"(max-width: 1270px) 100vw, 1270px\" \/><\/p>\n<p>\u56fe8 | \u5728\u91d1\u5c5e\u76f82D TMD\u548c\u5149\u6536\u96c6\u534a\u5bfc\u4f53\u4e4b\u95f4\u5f62\u6210\u7684\u7535\u5b50\u6865\u3002<\/p>\n<p><strong><em>\u00a0<\/em><\/strong><\/p>\n<p><strong><em>\uff08<\/em><\/strong><strong><em>\u2161<\/em><\/strong><strong><em>\uff09<\/em><\/strong><strong><em>2D TMDs<\/em><\/strong><strong><em>\u4f5c\u4e3a\u6d3b\u6027\u5149\u50ac\u5316\u5242\u7684\u4f18\u52bf<\/em><\/strong><\/p>\n<p>\u534a\u5bfc\u4f53\u76f82D TMD\uff08\u4f8b\u59822H-MoS<sub>2<\/sub>\uff09\u662f\u6d3b\u6027\u5149\u50ac\u5316\u5242\uff08\u5149\u6536\u96c6\u6750\u6599\uff09\u7684\u6f5c\u5728\u5019\u9009\u8005\u3002\u5b83\u4eec\u4f5c\u4e3a\u6d3b\u6027\u5149\u50ac\u5316\u5242\u7684\u4f18\u52bf\u5982\u4e0b\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u7a84\u5e26\u9699\u3002<\/em><\/strong>\u5b83\u4eec\u5177\u6709\u7a84\u7684\u5e26\u9699\uff08\u901a\u5e38\u5c0f\u4e8e2.4eV\uff0c\u4f8b\u5982MoS<sub>2<\/sub>\u5355\u5c42\u76842.16eV\uff09\uff0c\u4e0e\u4f20\u7edf\u534a\u5bfc\u4f53\u76f8\u6bd4\uff0c\u5b83\u4eec\u5177\u6709\u66f4\u5bbd\u7684\u5149\u8c31\u5438\u6536\uff08\u622a\u6b62\u6ce2\u957f\u8303\u56f4\u4ece\u8fd1\u7ea2\u5916\u5230\u53ef\u89c1\u5149\u8c31\uff09\u548c\u66f4\u6709\u6548\u7684\u592a\u9633\u5149\u8c31\u5229\u7528\u7387\uff08\u4f8b\u5982\uff0c\u5c11\u5c42MoS<sub>2<\/sub>\u7684\u592a\u9633\u80fd\u5149\u8c31\u5229\u7528\u7387\u7ea6\u4e3a50%\uff09\uff08TiO<sub>2<\/sub>-3.2eV-4%\u7684\u592a\u9633\u5149\u8c31\u5229\u7528\u7387\uff0cWO<sub>3<\/sub>-2.8eV-10%\u7684\u592a\u9633\u6ce2\u8c31\u5229\u7528\u7387\uff0cCdS-2.4eV-20%\u7684\u592a\u9633\u9891\u8c31\u5229\u7528\u7387\uff09\uff08<strong>\u56fe<\/strong><strong>9<\/strong>\uff09\u3002\u6b64\u5916\uff0c\u5b83\u4eec\u7684\u7a84\u5e26\u9699\u5bfc\u81f4\u5b83\u4eec\u5f3a\u70c8\u7684\u5149-\u7269\u8d28\u76f8\u4e92\u4f5c\u7528\uff0c\u786e\u4fdd\u4e86\u5b83\u4eec\u5927\u91cf\u7684\u7535\u5b50\u7a7a\u7a74\u4ea7\u751f\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u5408\u9002\u7684\u80fd\u5e26\u4f4d\u7f6e\u3002<\/em><\/strong>\u540c\u65f6\uff0c\u5b83\u4eec\u5177\u6709\u5408\u9002\u7684\u80fd\u5e26\u4f4d\u7f6e\uff0c\u8fd9\u53ef\u4ee5\u6ee1\u8db3\u5404\u79cd\u5149\u50ac\u5316\u53cd\u5e94\u7684\u70ed\u529b\u5b66\u8981\u6c42\uff08<strong>\u56fe<\/strong><strong>10<\/strong>\uff09\uff0c\u5305\u62ec\u6c22\uff08H<sub>2<\/sub>\uff09\u751f\u4ea7\u3001\u4e8c\u6c27\u5316\u78b3\uff08CO<sub>2<\/sub>\uff09\u8fd8\u539f\u3001\u6c2e\u6c14\uff08N<sub>2<\/sub>\uff09\u56fa\u5b9a\u3001\u6740\u83cc\u3001\u6c61\u67d3\u964d\u89e3\u3001\u548c\u6709\u673a\u5408\u6210\uff0c\u8fd9\u4e9b\u5df2\u5728\u7406\u8bba\u548c\u5b9e\u9a8c\u4e0a\u5f97\u5230\u8bc1\u660e\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u539f\u5b50\u8584\u5c42\u7684\u5c5e\u6027\u3002<\/em><\/strong>\u66f4\u91cd\u8981\u7684\u662f\uff0c\u5b83\u4eec\u7684\u539f\u5b50\u8584\u5c42\u6027\u8d28\u8d4b\u4e88\u4e86\u5b83\u4eec\u4f5c\u4e3a\u5149\u50ac\u5316\u4e2d\u7684\u5149\u6536\u96c6\u6750\u6599\u66f4\u975e\u51e1\u7684\u6027\u80fd\uff0c\u5305\u62ec\u91cf\u5b50\u9650\u5236\u3001\u8f7d\u6d41\u5b50\u7684\u77ed\u4f20\u8f93\u8ddd\u79bb\u3001\u5927\u8868\u9762\u79ef\u4e0e\u4f53\u79ef\u6bd4\u7b49\u3002\u91cf\u5b50\u9650\u5236\u6548\u5e94\u8d4b\u4e88\u5b83\u4eec\u53ef\u8c03\u7684\u5e26\u7ed3\u6784\uff08<strong>\u56fe<\/strong><strong>11a<\/strong>\uff09\u3002\u8f7d\u6d41\u5b50\u4ece\u5185\u90e8\u5230\u8868\u9762\u7684\u77ed\u4f20\u8f93\u8ddd\u79bb\u6709\u5229\u4e8e\u6709\u6548\u6291\u5236\u8f7d\u6d41\u5b50\u7684\u4f53\u590d\u5408\uff0c\u5ef6\u957f\u5149\u91cf\u5b50\u7684\u5bff\u547d\uff0c\u4ece\u800c\u63d0\u9ad8\u91cf\u5b50\u6548\u7387\uff08<strong>\u56fe<\/strong><strong>11b<\/strong>\uff09\u3002\u5927\u7684\u8868\u9762\u79ef\u4e0e\u4f53\u79ef\u6bd4\u6709\u5229\u4e8e\u5149\u6355\u83b7\uff0c\u5e76\u4e14\u5bf9\u53cd\u5e94\u7269\u548c\u50ac\u5316\u4f4d\u70b9\u4e4b\u95f4\u7684\u5bcc\u70b9\u63a5\u89e6\u6709\u5f88\u5927\u8d21\u732e\uff0c\u5e76\u4e3a\u5f62\u6210\u63ba\u6742\u3001\u975e\u81f4\u547d\u7f3a\u9677\u548c\u5f02\u8d28\u7ed3\u63d0\u4f9b\u4e86\u826f\u597d\u7684\u5e73\u53f0\uff0c\u8fd9\u4e9b\u90fd\u6709\u5229\u4e8e\u8fdb\u4e00\u6b65\u589e\u5f3a\u5149\u50ac\u5316\u6027\u80fd\uff08<strong>\u56fe<\/strong><strong>11c<\/strong>\uff09\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u4f5c\u4e3a\u5149\u50ac\u5316\u57fa\u7840\u7814\u7a76\u7684\u7406\u60f3\u5e73\u53f0\u3002<\/em><\/strong>\u6b64\u5916\uff0c\u534a\u5bfc\u4f53\u76f82D TMD\uff0c\u7279\u522b\u662f\u5355\u5c42TMD\uff0c\u53ef\u4ee5\u4f5c\u4e3a\u4e00\u4e2a\u7406\u60f3\u7684\u5e73\u53f0\u6765\u6f14\u793a\u5149\u50ac\u5316\u4e2d\u7684\u4e00\u4e9b\u57fa\u672c\u539f\u7406\uff0c\u8fd9\u662f\u7531\u4e8e\u5b83\u4eec\u7684\u4e0a\u8ff0\u72ec\u7279\u7279\u6027\u3002\u4f8b\u5982\uff0c\u5b83\u4eec\u53ef\u4ee5\u7528\u4e8e\u6f14\u793a\u5f02\u8d28\u7ed3\u6784\u754c\u9762\u5904\u5149\u6fc0\u53d1\u540e\u8f7d\u6d41\u5b50\u8f6c\u79fb\u7684\u65b9\u5411\u548c\u65f6\u95f4\u3002\u5148\u524d\u7684\u7814\u7a76\u5df2\u7ecf\u901a\u8fc7\u5b9e\u9a8c\u9a8c\u8bc1\u4e86\u8fd9\u4e00\u70b9\u3002\u5728\u8fd9\u9879\u7814\u7a76\u4e2d\uff0c\u4f7f\u7528\u57fa\u4e8e2D TMDs\u7684\u8303\u5fb7\u534e\u5f02\u8d28\u7ed3\u6784\uff08\u7531MoS<sub>2<\/sub>\u5355\u5c42\u548cWS<sub>2<\/sub>\u5355\u5c42\u6784\u5efa\uff09\u4f5c\u4e3a\u6a21\u578b\uff0c\u8bc1\u660e\u4e86\u8f7d\u6d41\u5b50\u5728\u8303\u5fb7\u534e\u754c\u9762\u7684\u8d85\u5feb\u8f6c\u79fb\u3002\u5149\u81f4\u53d1\u5149\u6620\u5c04\u548c\u98de\u79d2\u6cf5\u6d66\u63a2\u9488\u5149\u8c31\u663e\u793a\uff0c\u5149\u6fc0\u53d1\u540e\uff0c\u5149\u8bf1\u5bfc\u7a7a\u7a74\u5728\u6781\u77ed\u7684\u65f6\u95f4\uff08~50 fs\uff09\u5185\u4eceMoS<sub>2<\/sub>\u5c42\u8fc1\u79fb\u5230WS<sub>2<\/sub>\u5c42\uff08<strong>\u56fe<\/strong><strong>11d<\/strong>\uff09\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-246026\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe9-1.png\" alt=\"\" width=\"1268\" height=\"840\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe9-1.png 1268w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe9-1-300x199.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe9-1-768x509.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe9-1-1024x678.png 1024w\" sizes=\"(max-width: 1268px) 100vw, 1268px\" \/><\/p>\n<p>\u56fe9 | \u534a\u5bfc\u4f53\u76f82D TMDs\u548c\u4e00\u4e9b\u4ee3\u8868\u6027\u5149\u50ac\u5316\u5242\u7684\u5e26\u9699\u548c\u5149\u5438\u6536\u7279\u6027\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-246027\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe10.png\" alt=\"\" width=\"1270\" height=\"1468\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe10.png 1270w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe10-260x300.png 260w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe10-768x888.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe10-886x1024.png 886w\" sizes=\"(max-width: 1270px) 100vw, 1270px\" \/><\/p>\n<p>\u56fe10 | 2D TMDs\u7684\u5408\u9002\u7684\u80fd\u5e26\u4f4d\u7f6e\u548c\u4e00\u4e9b\u5e38\u89c1\u5149\u50ac\u5316\u53cd\u5e94\u7684\u6c27\u5316\u8fd8\u539f\u7535\u52bf\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-246028\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe11.png\" alt=\"\" width=\"1268\" height=\"1483\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe11.png 1268w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe11-257x300.png 257w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe11-768x898.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe11-876x1024.png 876w\" sizes=\"(max-width: 1268px) 100vw, 1268px\" \/><\/p>\n<p>\u56fe11 | 2D TMDs\u4f5c\u4e3a\u5149\u654f\u5242\u7684\u4f18\u70b9\uff1a\u91cf\u5b50\u9650\u57df\u3001\u8f7d\u6d41\u5b50\u4f20\u8f93\u8ddd\u79bb\u77ed\u3001\u6bd4\u8868\u9762\u79ef\u5927\uff0c\u4f5c\u4e3a\u5149\u50ac\u5316\u57fa\u7840\u7814\u7a76\u7684\u7406\u60f3\u5e73\u53f0\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\uff08<\/em><\/strong><strong><em>\u2162<\/em><\/strong><strong><em>\uff09\u4e0e\u7ecf\u5178<\/em><\/strong><strong><em>2D<\/em><\/strong><strong><em>\u5149\u50ac\u5316\u6750\u6599\u76f8\u6bd4\uff0c<\/em><\/strong><strong><em>2D TMDs<\/em><\/strong><strong><em>\u7528\u4e8e\u5149\u50ac\u5316\u7684\u72ec\u7279\u4f18\u52bf<\/em><\/strong><\/p>\n<p>\u672c\u8282\u4ece\u5f53\u524d\u7684\u89d2\u5ea6\u89e3\u91ca\u4e86\u4e3a\u4ec0\u4e482D TMDs\u80fd\u591f\u5728\u5149\u50ac\u5316\u4e2d\u4ece\u8bb8\u591a\u7ecf\u51782D\u5149\u50ac\u5316\u6750\u6599\u4e2d\u8131\u9896\u800c\u51fa\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u4e0e\u77f3\u58a8\u70ef\u7684\u6bd4\u8f83\u3002<\/em><\/strong>\u867d\u7136\u77f3\u58a8\u70ef\u4f5c\u4e3a\u7ecf\u5178\u76842D\u52a9\u50ac\u5316\u5242\u5728\u7406\u8bba\u4e0a\u548c\u5b9e\u8df5\u4e0a\u90fd\u5177\u6709\u5438\u5f15\u529b\uff0c\u4f46\u5b83\u662f\u5316\u5b66\u60f0\u6027\u548c\u96f6\u5e26\u9699\u7684\u3002\u8fd9\u9650\u5236\u4e86\u77f3\u58a8\u70ef\u5728\u5149\u50ac\u5316\u4e2d\u5145\u5f53\u52a9\u50ac\u5316\u5242\uff0c\u5e76\u4e14\u603b\u662f\u9700\u8981\u901a\u8fc7\u6240\u9700\u5206\u5b50\u7684\u529f\u80fd\u5316\u6765\u6fc0\u6d3b\u30022D TMD\u5177\u6709\u591a\u79cd\u5316\u5b66\u6027\u8d28\uff0c\u4ece\u91d1\u5c5e\uff08\u96f6\u5e26\u9699\uff0c\u5982\u77f3\u58a8\u70ef\uff09\u3001\u534a\u91d1\u5c5e\uff08\u63a5\u8fd1\u96f6\u5e26\u9699\uff09\u5230\u534a\u5bfc\u4f53\uff08\u7a84\u5e26\u9699\uff09\u3002\u8fd9\u4e3a2D TMD\u63d0\u4f9b\u4e86\u5728\u5404\u79cd\u5149\u50ac\u5316\u53cd\u5e94\u4e2d\u8fdb\u884c\u5404\u79cd\u57fa\u7840\u548c\u6280\u672f\u7814\u7a76\u7684\u673a\u4f1a\uff0c\u8fd9\u4e9b\u53cd\u5e94\u65e2\u5145\u5f53\u52a9\u50ac\u5316\u5242\u53c8\u5145\u5f53\u6d3b\u6027\u5149\u50ac\u5316\u5242\u3002\u8fd9\u79cd\u591a\u6837\u6027\u662f2D TMDs\u5728\u5149\u50ac\u5316\u65b9\u9762\u4f18\u4e8e\u77f3\u58a8\u70ef\u7684\u6700\u660e\u663e\u4f18\u52bf\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\u4e0e\u77f3\u58a8\u78b3\u6c2e\u5316\u7269\u7684\u6bd4\u8f83\u3002<\/em><\/strong>\u77f3\u58a8\u78b3\u6c2e\u5316\u7269\uff08g-C<sub>3<\/sub>N<sub>4<\/sub>\uff09\u662f\u4e00\u79cd\u5178\u578b\u76842D\u534a\u5bfc\u4f53\u5149\u50ac\u5316\u5242\uff0c\u5df2\u6210\u4e3a\u5149\u50ac\u5316\u9886\u57df\u7684\u65b0\u7814\u7a76\u70ed\u70b9\u3002\u5b83\u7684\u5e26\u9699\u4e3a2.7eV\uff0c\u7406\u8bba\u4e0a\u53ef\u4ee5\u5229\u752810%-20%\u7684\u592a\u9633\u5149\u8c31\u3002\u5982\u524d\u6240\u8ff0\uff0c2D TMD\u5177\u6709\u8f83\u7a84\u7684\u5e26\u9699\uff08\u901a\u5e38&lt;2.4 eV\uff09\uff0c\u4f7f\u5176\u5177\u6709\u66f4\u5bbd\u7684\u5149\u8c31\u5438\u6536\u548c\u66f4\u6709\u6548\u7684\u592a\u9633\u5149\u8c31\u5229\u7528\u7387\uff08&gt;\u592a\u9633\u5149\u8c31\u5229\u7528\u768420%\uff09\u3002\u8fd9\u79cd\u6709\u6548\u7684\u592a\u9633\u5149\u8c31\u5229\u7528\u662f2D TMDs\u4f5c\u4e3a\u5149\u50ac\u5316\u6d3b\u6027\u5149\u50ac\u5316\u5242\u4f18\u4e8eg-C<sub>3<\/sub>N<sub>4<\/sub>\u7684\u4f18\u52bf\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u4e0d\u53ef\u5426\u8ba4\uff0c\u4ece\u76ee\u524d\u7684\u89d2\u5ea6\u6765\u770b\uff0c\u77f3\u58a8\u70ef\uff08\u4f5c\u4e3a\u52a9\u50ac\u5316\u5242\uff09\u548cg-C<sub>3<\/sub>N<sub>4<\/sub>\uff08\u4f5c\u4e3a\u6d3b\u6027\u5149\u50ac\u5316\u5242\uff09\u5728\u5149\u50ac\u5316\u65b9\u9762\u66f4\u53d7\u6b22\u8fce\u548c\u6210\u719f\u3002\u7136\u800c\uff0c2D TMDs\u662f\u4e00\u79cd\u6709\u524d\u9014\u7684\u5149\u50ac\u5316\u6750\u6599\uff0c\u7531\u4e8e\u5176\u591a\u6837\u6027\u548c\u6709\u6548\u7684\u5149\u8c31\u5229\u7528\uff0c\u6709\u671b\u6210\u4e3a\u4e0b\u4e00\u4e2a\u7814\u7a76\u70ed\u70b9\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\uff08\u4e09\uff09\u6311\u6218\u548c\u7b56\u7565<\/em><\/strong><\/p>\n<p><strong><em>\uff08<\/em><\/strong><strong><em>\u2160<\/em><\/strong><strong><em>\uff09\u6311\u6218<\/em><\/strong><\/p>\n<p>\u4f5c\u4e3a\u6d3b\u6027\u5149\u50ac\u5316\u5242\u7684\u534a\u5bfc\u4f53\u76f82D TMDs\u9762\u4e34\u50ac\u5316\u60f0\u6027\u57fa\u9762\u3001\u7f13\u6162\u7684\u8f7d\u6d41\u5b50\u52a8\u529b\u5b66\uff08\u6e90\u81ea\u5176\u963b\u788d\u7535\u8377\u8f6c\u79fb\u7684\u9ad8\u7535\u963b\uff09\u3001\u4ee5\u53ca\u5149\u8c31\u6536\u96c6\u8303\u56f4\u4e0e\u6c27\u5316\u8fd8\u539f\u7535\u4f4d\u7684\u76f8\u4e92\u59a5\u534f\u7b49\u6311\u6218\u3002\u4e00\u4e9b\u5de5\u7a0b\u7b56\u7565\uff0c\u5305\u62ec\u8fb9\u7f18\u4f4d\u7f6e\u3001\u76f8\u4f4d\u3001\u63ba\u6742\u548c\u7a7a\u4f4d\u4ee5\u53ca\u754c\u9762\u7684\u5de5\u7a0b\uff0c\u5df2\u7ecf\u7528\u4e8e\u5904\u7406\u8fd9\u4e9b\u95ee\u9898\uff0c\u5e76\u5728\u4e0b\u6587\u4e2d\u4ecb\u7ecd\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u6b64\u5916\uff0c2D TMD\u7531\u4e8e\u5176\u9ad8\u8868\u9762\u80fd\u548c\u4e30\u5bcc\u7684\u6d3b\u6027\u4f4d\u70b9\uff0c\u5728\u50a8\u5b58\u8fc7\u7a0b\u4e2d\u5bb9\u6613\u53d1\u751f\u56e2\u805a\u548c\u5316\u5b66\u53d8\u5316\uff0c\u7f3a\u4e4f\u957f\u671f\u7a33\u5b9a\u6027\u548c\u8010\u4e45\u6027\u3002\u901a\u8fc7\u4ee5\u60ac\u6d6e\u6db2\u7684\u5f62\u5f0f\u50a8\u5b582D TMD\uff0c\u5e76\u901a\u8fc7\u6d41\u53d8\u8c03\u63a7\u3001\u6216\u5171\u4ef7\u529f\u80fd\u5316\u4f7f\u5176\u7a33\u5b9a\uff0c\u53ef\u4ee5\u5e94\u5bf9\u8fd9\u4e00\u6311\u6218\u3002\u6b64\u5916\uff0c\u5728\u50ac\u5316\u53cd\u5e94\u671f\u95f4\uff0c2D TMD\u7684\u56e2\u805a\u4e5f\u9891\u7e41\u53d1\u751f\u3002\u89e3\u51b3\u8fd9\u4e2a\u95ee\u9898\u7684\u6709\u6548\u65b9\u6cd5\u662f\u5728\u886c\u5e95\u4e0a\u751f\u957f2D TMD\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\uff08<\/em><\/strong><strong><em>\u2161<\/em><\/strong><strong><em>\uff09\u8fb9\u4f4d\u70b9\u5de5\u7a0b<\/em><\/strong><\/p>\n<p>\u534a\u5bfc\u4f53\u76f82D TMD\u5177\u6709\u50ac\u5316\u60f0\u6027\u57fa\u9762\uff0c\u5176\u50ac\u5316\u6d3b\u6027\u4e2d\u5fc3\u901a\u5e38\u4f4d\u4e8e\u8fb9\u7f18\uff0c\u5728\u90a3\u91cc\u66b4\u9732\u51fa\u4e30\u5bcc\u7684\u4e0d\u9971\u548c\u539f\u5b50\u3002\u56e0\u6b64\uff0c\u521b\u5efa\u66b4\u9732\u826f\u597d\u7684\u6d3b\u6027\u8fb9\u7f18\u4f4d\u70b9\uff08\u79f0\u4e3a\u8fb9\u7f18\u4f4d\u70b9\u5de5\u7a0b\uff09\u662f\u589e\u5f3a2D TMDs\u5149\u50ac\u5316\u6d3b\u6027\u7684\u5408\u7406\u65b9\u6cd5\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u4f7f\u7528CVD\u65b9\u6cd5\u5728\u886c\u5e95\u4e0a\u6784\u5efa\u5782\u76f4\u751f\u957f\u76842D TMD\u5df2\u88ab\u8bc1\u660e\u662f\u521b\u5efa\u826f\u597d\u66b4\u9732\u7684\u6709\u6e90\u8fb9\u7f18\u4f4d\u7f6e\u7684\u6709\u6548\u7b56\u7565\uff08<strong>\u56fe<\/strong><strong>12a<\/strong>\uff09\u3002\u6216\u8005\uff0c\u901a\u8fc7\u7403\u78e8\u65b9\u6cd5\u57282D TMDs\u8868\u9762\u5f15\u5165\u5b54\u9699\u4e5f\u662f\u4e30\u5bcc\u8fb9\u754c\u548c\u8fb9\u7f18\u4f4d\u7f6e\u7684\u6709\u529b\u5de5\u5177\uff08<strong>\u56fe<\/strong><strong>12b<\/strong>\uff09\u3002\u6b64\u5916\uff0c\u8fd8\u5b58\u5728\u4e00\u4e9b\u6f5c\u5728\u53ef\u884c\u7684\u7b56\u7565\u6765\u521b\u5efa\u66b4\u9732\u826f\u597d\u7684\u6d3b\u6027\u8fb9\u7f18\u4f4d\u70b9\uff0c\u4ee5\u63d0\u9ad8\u5176\u5149\u50ac\u5316\u6027\u80fd\uff0c\u4f8b\u5982\u6784\u5efa\u87ba\u65cb\u87ba\u65cb\u7ed3\u67842D TMDs\uff08<strong>\u56fe<\/strong><strong>12c<\/strong>\uff09\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u5f88\u660e\u663e\uff0c\u521b\u5efa\u66b4\u9732\u826f\u597d\u7684\u6d3b\u6027\u8fb9\u7f18\u4f4d\u70b9\uff08\u8fb9\u7f18\u4f4d\u70b9\u5de5\u7a0b\uff09\u662f\u63d0\u9ad82D TMDs\u5149\u50ac\u5316\u6d3b\u6027\u7684\u53ef\u884c\u65b9\u6cd5\u3002\u5c3d\u7ba1\u5982\u6b64\uff0c\u8be5\u7b56\u7565\u4ecd\u5904\u4e8e\u8d77\u6b65\u9636\u6bb5\uff0c\u5176\u5b9e\u65bd\u901a\u5e38\u9700\u8981\u82db\u523b\u7684\u6761\u4ef6\uff08\u5982\u9ad8\u6e29\u548c\u9ad8\u771f\u7a7a\u6761\u4ef6\uff09\u3002\u5e94\u7ee7\u7eed\u81f4\u529b\u4e8e\u8fd9\u4e00\u9886\u57df\uff08\u5149\u50ac\u53162D TMDs\u7684\u8fb9\u7f18\u4f4d\u70b9\u5de5\u7a0b\uff09\uff0c\u5c06\u91cd\u5fc3\u653e\u5728\u5de7\u5999\u7684\u7ed3\u6784\u8bbe\u8ba1\u548c\u5bb9\u6613\u7684\u8fb9\u7f18\u4f4d\u70b9\u5408\u6210\u4e0a\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\uff08<\/em><\/strong><strong><em>\u2162<\/em><\/strong><strong><em>\uff09\u76f8\u5de5\u7a0b<\/em><\/strong><\/p>\n<p>\u5148\u524d\u7684\u7406\u8bba\u548c\u5b9e\u9a8c\u7814\u7a76\u8bc1\u660e\u4e86\u5177\u6709\u4e0d\u540c\u76f8\u4f4d\u76842D TMD\u7684\u4e0d\u540c\u7279\u6027\u3002\u4f8b\u5982\uff0c2H-MoS<sub>2<\/sub>\u5355\u5c42\u662f\u5177\u6709\u50ac\u5316\u60f0\u6027\u57fa\u9762\u7684\u534a\u5bfc\u4f53\uff0c\u7531\u4e8e\u9ad8\u7535\u963b\uff0c\u8f7d\u6d41\u5b50\u52a8\u529b\u5b66\u7f13\u6162\uff1b 1T-MoS<sub>2<\/sub>\u5355\u5c42\u5177\u6709\u96f6\u5e26\u9699\uff0c\u663e\u793a\u51fa\u91d1\u5c5e\u6027\u8d28\u3001\u548c\u9ad8\u5bfc\u7535\u6027\uff1b 1T&#8217;-MoS<sub>2<\/sub>\u53ea\u6709\u5f88\u5c0f\u7684\u5e26\u9699\uff0c\u662f\u4e00\u79cd\u51c6\u91d1\u5c5e\u76f8\uff0c\u5177\u6709\u4e0e\u91d1\u5c5e1T\u76f8\u7c7b\u4f3c\u7684\u6027\u8d28\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u56e0\u6b64\uff0c\u7406\u8bba\u4e0a\uff0c\u5c06\u91d1\u5c5e\/\u51c6\u91d1\u5c5e\u76f82D TMDs\uff08\u4f5c\u4e3a\u52a9\u50ac\u5316\u5242\uff09\u5f15\u5165\u5230\u534a\u5bfc\u4f53\u76f82D TMD\uff08\u4f5c\u4e3a\u5149\u654f\u5242\uff09\u4e2d\uff0c\u79f0\u4e3a\u76f8\u5de5\u7a0b\uff0c\u6709\u671b\u5b9e\u73b0\u4e92\u8865\u6027\u8d28\u548c\u534f\u540c\u50ac\u5316\u6548\u5e94\uff0c\u4ece\u800c\u63d0\u9ad8\u534a\u5bfc\u4f53\u76f82D TMDs\u7684\u5149\u50ac\u5316\u6d3b\u6027\u3002\u5176\u4e2d\uff0c\u91d1\u5c5e\u76f8TMDs\u4f5c\u4e3a\u52a9\u50ac\u5316\u5242\uff0c\u53ef\u4ee5\u52a0\u901f\u8f7d\u4f53\u52a8\u529b\u5b66\uff0c\u4e30\u5bcc\u50ac\u5316\u4f4d\u70b9\u3002\u6b64\u5916\uff0c\u5728\u5f62\u6210\u7684\u9762\u5185\u754c\u9762\u5904\uff0c\u5149\u8bf1\u5bfc\u7535\u5b50\u53ef\u4ee5\u5feb\u901f\u4ece\u534a\u5bfc\u4f53\u76f8\u8fc1\u79fb\u5230\u91d1\u5c5e\u76f8\uff0c\u4fc3\u8fdb\u5149\u751f\u7535\u5b50\u548c\u7a7a\u7a74\u7684\u5206\u79bb\uff0c\u5e76\u63d0\u9ad8\u91cf\u5b50\u6548\u7387\uff08<strong>\u56fe<\/strong><strong>12d<\/strong>\uff09\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u6beb\u65e0\u7591\u95ee\uff0c\u76f8\u5de5\u7a0b\u5bf9\u4e8e\u63d0\u9ad82D TMDs\u7684\u5149\u50ac\u5316\u6027\u80fd\u662f\u6709\u6548\u7684\uff0c\u4f46\u5176\u5b9e\u65bd\u9762\u4e34\u4e24\u4e2a\u5b9e\u8d28\u6027\u6311\u6218\u3002\u9996\u5148\uff0c\u91d1\u5c5e\u76f82D TMD\uff08\u4f8b\u59821T\/1T\u2019\u76f8MoS<sub>2<\/sub>\uff09\u901a\u5e38\u662f\u4e9a\u7a33\u6001\u7684\uff0c\u5f53\u7f6e\u4e8e\u73af\u5883\u4e2d\u6216\u50ac\u5316\u8fc7\u7a0b\u4e2d\u65f6\uff0c\u5bb9\u6613\u53d1\u751f\u76f8\u53d8\u3002\u8fd9\u5c06\u4f7f\u50ac\u5316\u5242\u53d8\u6027\uff0c\u5e76\u7ed9\u5176\u5149\u50ac\u5316\u7814\u7a76\u5e26\u6765\u4e0d\u786e\u5b9a\u6027\u3002\u5176\u6b21\uff0c\u65e0\u8bba\u662f\u76f4\u63a5\u5408\u6210\uff08\u901a\u8fc7\u6c34\u70ed\u6cd5\uff09\u8fd8\u662f\u901a\u8fc7\u90e8\u5206\u76f8\u53d8\uff08\u901a\u8fc7\u9502\u5d4c\u5165\u6216\u8d85\u4e34\u754cCO<sub>2<\/sub>\u8bf1\u5bfc\uff09\uff0c\u90fd\u4e0d\u5bb9\u6613\u7cbe\u786e\u63a7\u5236\u5177\u6709\u7cbe\u786e\u548c\u6309\u9700\u76f8\u6bd4\u7684\u591a\u76f82D TMD\u7684\u5408\u6210\u3002\u56e0\u6b64\uff0c\u5728\u672a\u6765\u7684\u7814\u7a76\u4e2d\uff0c\u5e94\u52aa\u529b\u89e3\u51b3\u8fd9\u4e24\u4e2a\u4e3b\u8981\u74f6\u9888\u3002\u4f8b\u5982\uff0c\u901a\u8fc7\u8868\u9762\u4fee\u9970\u6765\u6539\u5584\u91d1\u5c5e\u76f82D TMD\u7684\u7a33\u5b9a\u6027\uff0c\u4ee5\u89e3\u51b3\u76f8\u53d8\u7684\u6311\u6218\u3002\u540c\u65f6\uff0c\u589e\u5f3a\u76f8\u53d8\u7684\u53ef\u63a7\u6027\uff0c\u4ee5\u5408\u6210\u5177\u6709\u7cbe\u786e\u76f8\u7684\u50ac\u5316\u5242\u3002\u503c\u5f97\u6ce8\u610f\u7684\u662f\uff0c\u57fa\u4e8e\u7535\u5316\u5b66\u9502\u79bb\u5b50\u5d4c\u5165\u7684\u5265\u79bb\u662f\u4e00\u79cd\u5f88\u6709\u524d\u9014\u7684\u7b56\u7565\uff0c\u6709\u671b\u901a\u8fc7\u63a7\u5236\u7535\u6d41\u6216\u622a\u6b62\u7535\u538b\u6765\u5b9e\u73b0\u76f8\u53d8\u7684\u7cbe\u786e\u8c03\u8282\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\uff08<\/em><\/strong><strong><em>\u2163<\/em><\/strong><strong><em>\uff09\u63ba\u6742\u548c\u7f3a\u9677\u5de5\u7a0b<\/em><\/strong><\/p>\n<p>\u5c06\u6742\u539f\u5b50\uff08\u547d\u540d\u4e3a\u63ba\u6742\u5de5\u7a0b\uff0c<strong>\u56fe<\/strong><strong>13a<\/strong>\uff09\u5f15\u5165\u534a\u5bfc\u4f532D TMD\u53ef\u4ee5\u4e3a\u5149\u50ac\u5316\u5e94\u7528\u5e26\u6765\u5404\u79cd\u8bf1\u4eba\u7684\u4f18\u52bf\u3002\u7406\u8bba\u8ba1\u7b97\u8868\u660e\uff0c\u5f15\u5165\u6742\u539f\u5b50\u5bfc\u81f4\u7684\u751f\u6210\u7f3a\u9677\u80fd\u7ea7\u53ef\u4ee5\u8c03\u65742D TMD\u7684\u5e26\u9699\uff0c\u4ece\u800c\u8c03\u6574\u5176\u6c27\u5316\u8fd8\u539f\u80fd\u529b\u3002\u968f\u540e\u7684\u5b9e\u9a8c\u7814\u7a76\u8bc1\u5b9e\u4e86\u8fd9\u4e00\u70b9\u3002\u4f8b\u5982\uff0c\u78b3\u63ba\u6742SnS<sub>2<\/sub>\u7684\u5e26\u9699\u503c\u4e3a2.54 eV\uff0c\u6bd4\u5176\u539f\u59cb\u5bf9\u5e94\u7269\uff082.43 eV\uff09\u7684\u5e26\u9699\u503c\u66f4\u5927\uff08<strong>\u56fe<\/strong><strong>13b<\/strong>\uff09\u3002\u6b64\u5916\uff0c\u5f15\u5165\u6742\u539f\u5b50\u8fd8\u53ef\u4ee5\u6709\u6548\u5730\u6539\u53d8\u5176\u5149\u7535\u6027\u80fd\uff08\u4f8b\u5982\uff0c\u6709\u6548\u5730\u589e\u5f3a\u5149\u5438\u6536\u5e76\u5ef6\u957f\u8f7d\u6d41\u5b50\u5bff\u547d\uff0c<strong>\u56fe<\/strong><strong>13c<\/strong>\uff09\uff0c\u4ece\u800c\u63d0\u9ad8\u5176\u5149\u50ac\u5316\u6027\u80fd\uff08<strong>\u56fe<\/strong><strong>13d<\/strong>\uff09\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u521b\u5efa\u7a7a\u4f4d\uff08\u547d\u540d\u4e3a\u7a7a\u4f4d\u5de5\u7a0b\uff0c<strong>\u56fe<\/strong><strong>14a<\/strong>\uff09\u4e5f\u662f\u4e00\u79cd\u666e\u904d\u7684\u7b56\u7565\uff0c\u4ee5\u91ca\u653e2D TMD\u5728\u5149\u50ac\u5316\u6027\u80fd\u6539\u5584\u65b9\u9762\u7684\u5de8\u5927\u6f5c\u529b\u3002\u8fd9\u662f\u56e0\u4e3a\u5b83\u53ef\u4ee5\u8c03\u65742D TMD\u7684\u7535\u5b50\u7ed3\u6784\uff08<strong>\u56fe<\/strong><strong>14b<\/strong>\uff09\u548c\u76f8\u90bb\u539f\u5b50\u6392\u5217\uff0c\u4ee5\u63d0\u9ad8\u56fa\u6709\u6d3b\u6027\u3002\u6b64\u5916\uff0c\u4f5c\u4e3a\u8f7d\u6d41\u5b50\u9631\uff0c\u5b83\u4e5f\u6709\u5229\u4e8e\u5206\u79bb\u5149\u751f\u7535\u5b50\u548c\u7a7a\u7a74\uff0c\u5ef6\u957f\u5176\u5bff\u547d\uff0c\u4ece\u800c\u63d0\u9ad8\u5149\u50ac\u5316\u6027\u80fd\uff08<strong>\u56fe<\/strong><strong>14c<\/strong>\uff09\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u503c\u5f97\u6ce8\u610f\u7684\u662f\uff0c\u4fee\u9970\u7a0b\u5ea6\uff08\u4f8b\u5982\u63ba\u6742\u6d53\u5ea6\u548c\u7a7a\u4f4d\uff09\u9700\u8981\u9002\u5ea6\u3002\u56e0\u4e3a\u8fc7\u5ea6\u4fee\u6539\u53ef\u80fd\u4f1a\u5bfc\u81f4\u76f8\u53cd\u7684\u7ed3\u679c\u3002\u4f8b\u5982\uff0c\u8fc7\u91cf\u7684\u7a7a\u4f4d\u53ef\u80fd\u6210\u4e3a\u8f7d\u6d41\u5b50\u590d\u5408\u7684\u4e2d\u5fc3\uff0c\u5e76\u6291\u5236\u5149\u50ac\u5316\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u63ba\u6742\u548c\u7a7a\u4f4d\u5de5\u7a0b\u786e\u5b9e\u6709\u52a9\u4e8e\u589e\u5f3a2D TMDs\u7684\u5149\u50ac\u5316\u6027\u80fd\u3002\u5c3d\u7ba1\u5982\u6b64\uff0c\u5728\u57fa\u4e8e2D TMDs\u7684\u5149\u50ac\u5316\u4e2d\u5229\u7528\u8fd9\u79cd\u7b56\u7565\u624d\u521a\u521a\u5f00\u59cb\u3002\u5c3d\u7ba1\u8fd9\u4e9b\u7b56\u7565\u5728\u50ac\u5316\u9886\u57df\u975e\u5e38\u53d7\u6b22\u8fce\u3002\u672a\u6765\u5e94\u5f00\u5c55\u9488\u5bf9\u8be5\u4e3b\u9898\u7684\u5176\u4ed6\u7814\u7a76\uff08\u57fa\u4e8e2D TMDs\u7684\u5149\u50ac\u5316\u4e2d\u7684\u63ba\u6742\u548c\u7a7a\u4f4d\u5de5\u7a0b\uff09\u3002\u8fd9\u662f\u4e00\u4e2a\u5145\u6ee1\u673a\u9047\u7684\u7814\u7a76\u9886\u57df\u3002\u4f8b\u5982\uff0c\u63ba\u6742\u548c\u7a7a\u4f4d\u5de5\u7a0b\u7684\u73b0\u4ee3\u6280\u672f\u5de5\u5177\u5305\u4e0d\u65ad\u4e30\u5bcc\u548c\u6539\u8fdb\uff08\u5982\u7b49\u79bb\u5b50\u4f53\u8bf1\u5bfc\u63ba\u6742\u3001\u6fc0\u5149\u8f85\u52a9\u63ba\u6742\u3001\u4e2d\u5b50\u5b17\u53d8\u63ba\u6742\u3001\u7535\u5b50\u675f\u5149\u523b\u8bf1\u5bfc\u7a7a\u4f4d\uff09\uff0c\u4e3a\u5c06\u6742\u539f\u5b50\u548c\u7a7a\u4f4d\u5f15\u5165\u5149\u50ac\u5316\u5242\u63d0\u4f9b\u4e86\u66f4\u4e3a\u590d\u6742\u7684\u6280\u672f\u3002\u57282D TMD\u4e2d\u5e94\u7528\u8fd9\u4e9b\u6700\u5148\u8fdb\u7684\u6280\u672f\u6765\u63d0\u9ad8\u5176\u5149\u50ac\u5316\u6027\u80fd\u662f\u4e00\u4e2a\u6709\u524d\u9014\u7684\u7814\u7a76\u8bfe\u9898\uff0c\u503c\u5f97\u52aa\u529b\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\uff08<\/em><\/strong><strong><em>\u2164<\/em><\/strong><strong><em>\uff09\u754c\u9762\u5de5\u7a0b<\/em><\/strong><\/p>\n<p>\u5f53\u754c\u9762\u5f62\u6210\u65f6\uff0c\u8f7d\u6d41\u5b50\u8fc1\u79fb\u5c06\u8868\u73b0\u51fa\u5f88\u5f3a\u7684\u65b9\u5411\u6027\u3002\u8fd9\u79cd\u5f3a\u65b9\u5411\u6027\u6709\u52a9\u4e8e\u5149\u751f\u8f7d\u6d41\u5b50\u7684\u6709\u6548\u5206\u79bb\uff0c\u4ece\u800c\u5ef6\u957f\u5176\u5bff\u547d\u5e76\u63d0\u9ad8\u5149\u91cf\u5b50\u6548\u7387\u3002\u56e0\u6b64\uff0c\u5f53\u6211\u4eec\u5f00\u59cb\u6784\u5efa\u57fa\u4e8e2D TMDs\u7684\u5f02\u8d28\u7ed3\u754c\u9762\u65f6\uff0c\u51fa\u73b0\u4e86\u5927\u91cf\u63d0\u9ad8\u5149\u50ac\u5316\u6027\u80fd\u7684\u673a\u4f1a\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u8bbe\u8ba1\u826f\u597d\u7684\u57fa\u4e8e\u4e8c\u7ef4TMDs\u7684\u5f02\u8d28\u7ed3\u754c\u9762\u80fd\u5e26\u5339\u914d\u3001\u5c3a\u5bf8\uff08\u51e0\u4f55\uff09\u5339\u914d\u548c\u5316\u5b66\u76f8\u5bb9\u6027\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u7406\u8bba\u4e0a\uff0c\u6839\u636e\u7535\u5b50\u8f6c\u79fb\u7684\u80fd\u5e26\u6392\u5217\u548c\u65b9\u5411\u6027\uff0c\u53ef\u4ee5\u5f62\u6210\u591a\u4e2a\u57fa\u4e8e\u4e8c\u7ef4TMDs\u7684\u5f02\u8d28\u7ed3\u754c\u9762\uff0c\u5305\u62ecI\u578b\uff08\u8de8\u9699\uff09\u3001II\u578b\uff08\u4ea4\u66ff\u9699\uff09\u3001Z\u578b\uff08\u4ea4\u66ff\u95f4\u9699\uff09\u3001III\u578b\uff08\u65ad\u9699\uff09\u548c\u8096\u7279\u57fa\u7ed3\uff08\u6216\u6b27\u59c6\u7ed3\uff09\uff08<strong>\u56fe<\/strong><strong>15a<\/strong>\uff09\u3002\u5176\u4e2d\uff0cII\u578b\u3001Z\u578b\u3001\u548c\u8096\u7279\u57fa\u7ed3\uff08\u6216\u6b27\u59c6\u7ed3\uff09\u7684\u80fd\u5e26\u5339\u914d\u826f\u597d\u3002\u5728\u8fd9\u4e9b\u5f02\u8d28\u7ed3\u754c\u9762\uff08II\u578b\u3001Z\u578b\u548c\u8096\u7279\u57fa\u7ed3\u6216\u6b27\u59c6\u7ed3\uff09\uff0c\u5149\u8bf1\u5bfc\u7684\u7535\u5b50\u6216\u7a7a\u7a74\u4ece\u4e00\u4e2a\u6784\u9020\u5757\u8f6c\u79fb\u5230\u53e6\u4e00\u4e2a\uff0c\u5e76\u5728\u4e0d\u540c\u7684\u6784\u9020\u5757\u4e2d\u5bcc\u96c6\u3002\u8fd9\u79cd\u7279\u5f81\u6709\u5229\u4e8e\u8f7d\u6d41\u5b50\u7684\u5206\u79bb\u3002\u6b64\u5916\uff0c\u5b83\u4e5f\u6709\u5229\u4e8e\u5728\u4e0d\u540c\u5730\u70b9\u53d1\u751f\u5149\u50ac\u5316\u6c27\u5316\u548c\u8fd8\u539f\u53cd\u5e94\uff0c\u4ece\u800c\u63d0\u9ad8\u53cd\u5e94\u6548\u7387\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u9664\u4e86\u80fd\u5e26\u5339\u914d\uff08\u5982\u4e0a\u6240\u8ff0\uff09\uff0c\u5c3a\u5bf8\uff08\u51e0\u4f55\uff09\u5339\u914d\u662f\u6784\u5efa\u9ad8\u6548\u5f02\u8d28\u7ed3\u754c\u9762\u7684\u53e6\u4e00\u4e2a\u5173\u952e\u56e0\u7d20\u3002\u826f\u597d\u5339\u914d\u7684\u5c3a\u5bf8\uff08\u51e0\u4f55\u5f62\u72b6\uff09\u6709\u5229\u4e8e\u5728\u4e24\u79cd\u6750\u6599\u4e4b\u95f4\u5f62\u6210\u81f4\u5bc6\u7684\u754c\u9762\u7ed3\uff0c\u4e3a\u8f7d\u6d41\u5b50\u8fc1\u79fb\u63d0\u4f9b\u9ad8\u901f\u901a\u9053\u3002\u56fe15c-f\u663e\u793a\u4e86\u5177\u67090D-2D\u30011D-2D\u30012D-2D\u3001\u548c3D-2D\u5339\u914d\u5c3a\u5bf8\u7684\u8bbe\u8ba1\u826f\u597d\u76842D TMDs\u57fa\u5f02\u8d28\u7ed3\u7684\u4e00\u4e9b\u4ee3\u8868\u6027\u793a\u4f8b\u3002\u5176\u4e2d\uff0c2D-2D\u5f02\u8d28\u7ed3\u754c\u9762\u662f\u8457\u540d\u7684\u754c\u9762\uff0c\u53ef\u5206\u4e3a\u5e73\u9762\u5185\u5f02\u8d28\u7ed3\u754c\u9762\uff08\u4ee5\u5e73\u9762\u5185MoS<sub>2<\/sub>-WS<sub>2<\/sub>\u5f02\u8d28\u7ed3\u754c\u9762\u4e3a\u4f8b\uff0c<strong>\u56fe<\/strong><strong>15g<\/strong>\uff09\u548c\u5782\u76f4\u5f02\u8d28\u7ed3\u754c\u9762\uff0c\u4ee5PtSe<sub>2<\/sub>\/Pt\u5782\u76f4\u5f02\u8d28\u7ed3\u6784\u754c\u9762\u4e3a\u4f8b\uff08<strong>\u56fe<\/strong><strong>15h<\/strong>\uff09\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u6b64\u5916\uff0c\u8fd8\u5e94\u5f3a\u8c03\u4e24\u79cd\u6784\u9020\u5757\uff082D TMD\u548c\u53e6\u4e00\u79cd\u6750\u6599\uff09\u7684\u5316\u5b66\u517c\u5bb9\u6027\u3002\u5c312D TMDs\u800c\u8a00\uff0c\u91d1\u5c5e\u786b\u5316\u7269\uff08\u5982CdS\u3001ZnIn<sub>2<\/sub>S<sub>4<\/sub>\u3001\u548cTMD\u672c\u8eab\uff09\u5c06\u4e0e\u5b83\u4eec\u5728\u5316\u5b66\u4e0a\u6700\u4e3a\u76f8\u5bb9\uff0c\u4ee5\u5236\u5907\u529f\u80fd\u6027\u6df7\u5408\u5149\u50ac\u5316\u5242\u3002\u8fd9\u662f\u56e0\u4e3a\u5b83\u4eec\u5177\u6709\u76f8\u540c\u6216\u719f\u6089\u7684\u975e\u91d1\u5c5e\u5143\u7d20\uff08\u4f8b\u5982MoS<sub>2<\/sub>\u548cCdS\u4e2d\u7684S\u5143\u7d20\uff09\uff0c\u8fd9\u4f7f\u5f97\u5b83\u4eec\u5f88\u5bb9\u6613\u901a\u8fc7\u5916\u5ef6\u751f\u957f\u6784\u5efa\u5177\u6709\u826f\u597d\u754c\u9762\u7684\u5f02\u8d28\u7ed3\u6784\u3002\u5728\u8fd9\u6837\u7684\u754c\u9762\u5904\uff0c\u7ecf\u5e38\u5f62\u6210\u5316\u5b66\u952e\uff08\u4f8b\u5982\uff0cMoS<sub>2<\/sub>\u548cCuS\u754c\u9762\u4e4b\u95f4\u5f62\u6210\u7684Mo-S-Cu\u952e\uff09\uff0c\u8fde\u63a5\u4e24\u4e2a\u6784\u5efa\u5757\uff0c\u8fd9\u5c06\u6709\u52a9\u4e8e\u8f7d\u6d41\u5b50\u7684\u5feb\u901f\u8f6c\u79fb\u5e76\u63d0\u9ad8\u5149\u91cf\u5b50\u6548\u7387\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-246029\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe12.png\" alt=\"\" width=\"1268\" height=\"1757\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe12.png 1268w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe12-217x300.png 217w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe12-768x1064.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe12-739x1024.png 739w\" sizes=\"(max-width: 1268px) 100vw, 1268px\" \/><\/p>\n<p>\u56fe12 | 2D TMDs\u7684\u8fb9\u4f4d\u70b9\u5de5\u7a0b\u548c\u76f8\u4f4d\u5de5\u7a0b\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-246031\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe13.png\" alt=\"\" width=\"1268\" height=\"1121\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe13.png 1268w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe13-300x265.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe13-768x679.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe13-1024x905.png 1024w\" sizes=\"(max-width: 1268px) 100vw, 1268px\" \/><\/p>\n<p>\u56fe13 | 2D TMDs\u7684\u63ba\u6742\u5de5\u7a0b\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-246032\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe14.png\" alt=\"\" width=\"1269\" height=\"1606\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe14.png 1269w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe14-237x300.png 237w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe14-768x972.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe14-809x1024.png 809w\" sizes=\"(max-width: 1269px) 100vw, 1269px\" \/><\/p>\n<p>\u56fe14 | 2D TMDs\u7684\u7f3a\u9677\u5de5\u7a0b\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-246033\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe15.png\" alt=\"\" width=\"1259\" height=\"1766\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe15.png 1259w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe15-214x300.png 214w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe15-768x1077.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe15-730x1024.png 730w\" sizes=\"(max-width: 1259px) 100vw, 1259px\" \/><\/p>\n<p>\u56fe15 | 2D TMDs\u7684\u754c\u9762\u5de5\u7a0b\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\uff08\u56db\uff09\u5c55\u671b<\/em><\/strong><\/p>\n<p>\u6beb\u65e0\u7591\u95ee\uff0c2D TMDs\uff0c\u65e0\u8bba\u662f\u4f5c\u4e3a\u52a9\u50ac\u5316\u5242\u8fd8\u662f\u6d3b\u6027\u5149\u50ac\u5316\u5242\uff08\u5149\u6536\u96c6\u6750\u6599\uff09\uff0c\u90fd\u6307\u5411\u4e00\u4e2a\u5bcc\u6709\u6210\u6548\u7684\u8fc7\u53bb\u3001\u4e00\u4e2a\u52a8\u4eba\u7684\u73b0\u5728\u548c\u4e00\u4e2a\u5149\u660e\u7684\u672a\u6765\u3002\u7136\u800c\uff0c\u6311\u6218\u4f9d\u7136\u5b58\u5728\uff0c\u4f46\u673a\u9047\u4e5f\u6709\u5f88\u591a\u3002\u5728\u6b64\uff0c\u6211\u4eec\u5c55\u671b\u4e862D TMDs\u7528\u4e8e\u5149\u50ac\u5316\u7684\u8bf1\u4eba\u65b9\u5411 \uff08<strong>\u56fe<\/strong><strong>16<\/strong>\uff09\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\uff08<\/em><\/strong><strong><em>\u2160<\/em><\/strong><strong><em>\uff09\u6269\u5c55\u6210\u5458<\/em><\/strong><\/p>\n<p>\u7528\u4e8e\u5149\u50ac\u5316\u76842D TMDs\u5bb6\u65cf\u6210\u5458\u4e0d\u65ad\u589e\u957f\uff0c\u4eceMoS<sub>2<\/sub>\uff08MoSe<sub>2<\/sub>\uff09\u548cWS<sub>2<\/sub>\uff08WSe<sub>2<\/sub>\uff09\u5f00\u59cb\uff0c\u7136\u540eReS<sub>2<\/sub>\u548cSnS<sub>2<\/sub>\uff0c\u73b0\u5728\u5df2\u7ecf\u53d1\u5c55\u5230PtS<sub>2<\/sub>\u3001PtSe<sub>2<\/sub>\uff0c\u548c\u5176\u4ed6\u3002\u770b\u8d77\u6765\u8fd9\u4e2a\u8fc7\u7a0b\u624d\u521a\u521a\u5f00\u59cb\uff0c\u5728\u9ad8\u901a\u91cf\u8ba1\u7b97\u9884\u6d4b\u7684\u4e0d\u4e45\u7684\u5c06\u6765\uff0c\u66f4\u591a\u76842D TMD\u6210\u5458\uff08\u4f8b\u5982\uff0cZrS<sub>2<\/sub>\u3001HfS<sub>2<\/sub>\u3001PdS<sub>2<\/sub>\uff09\u53ef\u80fd\u4f1a\u6d8c\u5165\u5149\u50ac\u5316\u3002\u672a\u6765\uff0c\u8fd9\u4e9b\u7406\u8bba\u4e0a\u53ef\u884c\u7684TMD\u9700\u8981\u8fdb\u884c\u5b9e\u9a8c\u9a8c\u8bc1\u3002\u503c\u5f97\u6ce8\u610f\u7684\u662f\uff0c\u5c3d\u7ba1ReS<sub>2<\/sub>\u5728\u5149\u50ac\u5316\u5e94\u7528\u4e2d\u5177\u6709\u4ee4\u4eba\u5174\u594b\u7684\u7269\u7406\u5316\u5b66\u6027\u8d28\uff0c\u4f46\u5176\u91d1\u5c5e\u5143\u7d20\uff08Re\uff09\u5e76\u4e0d\u4e30\u5bcc\uff08\u5730\u58f3\u4e2d\u6700\u7a00\u6709\u7684\u5143\u7d20\u4e4b\u4e00\uff09\u3002\u56e0\u6b64\uff0c\u5176\u5b9e\u9645\u5e94\u7528\u524d\u666f\u5c06\u53d7\u5230\u7ecf\u6d4e\u53ef\u884c\u6027\u7684\u9650\u5236\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\uff08<\/em><\/strong><strong><em>\u2161<\/em><\/strong><strong><em>\uff09\u6539\u8fdb\u73b0\u6709\u7b56\u7565<\/em><\/strong><\/p>\n<p>\u5f53\u901a\u8fc7\u8fb9\u7f18\u4f4d\u70b9\u3001\u76f8\u3001\u63ba\u6742\u3001\u7a7a\u4f4d\u3001\u548c\u754c\u9762\u7684\u5de5\u7a0b\u5bf92D TMDs\u8fdb\u884c\u6539\u6027\u65f6\uff0c\u5149\u50ac\u5316\u6027\u80fd\u5b9e\u73b0\u4e86\u5927\u5e45\u63d0\u5347\u3002\u7136\u800c\uff0c\u4e0e\u7535\u50ac\u5316\u76f8\u6bd4\uff0c2D TMDs\u5149\u50ac\u5316\u7684\u5927\u591a\u6570\u5de5\u7a0b\u6280\u672f\u4ecd\u5904\u4e8e\u8d77\u6b65\u9636\u6bb5\u3002\u5728\u672a\u6765\uff0c\u7ee7\u7eed\u6df1\u5165\u6316\u6398\u8fd9\u4e9b\u5de5\u7a0b\u7c7b\u522b\u81f3\u5173\u91cd\u8981\u3002\u4f8b\u5982\uff0c\u5236\u9020\u68af\u5f622D TMD\u4ee5\u4e30\u5bcc\u8fb9\u7f18\u4f4d\u7f6e\uff1b\u6267\u884c\u5c40\u90e8\u76f8\u53d8\u4ee5\u6784\u5efa\u5468\u671f\u6027\u5f02\u76f8\u754c\u9762\uff1b\u5e94\u7528\u6fc0\u5149\u56fe\u6848\u5316\u3001\u70ed\u8680\u523b\u548c\u5185\u5916\u5ef6\u751f\u957f\u5de5\u827a\u6765\u6784\u5efa\u9576\u5d4c\u5f02\u8d28\u7ed3\u6784\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\uff08<\/em><\/strong><strong><em>\u2162<\/em><\/strong><strong><em>\uff09\u5f00\u53d1\u65b0\u7b56\u7565<\/em><\/strong><\/p>\n<p>\u540c\u65f6\uff0c 2D TMDs\u5f00\u53d1\u65b0\u7684\u5149\u50ac\u5316\u5de5\u7a0b\u7b56\u7565\u4e5f\u9700\u8981\u6295\u5165\u6fc0\u60c5\u548c\u52aa\u529b\u3002\u4f8b\u5982\u5c06\u63d2\u5c42\u91d1\u5c5e\u5f15\u51652D TMD\u7684\u5939\u5c42\u4e2d\uff0c\u901a\u8fc7\u534f\u540c\u50ac\u5316\u548c\u9650\u57df\u50ac\u5316\u6548\u5e94\u6765\u63d0\u5347\u5149\u50ac\u5316\u6d3b\u6027\uff08\u9650\u57df\u50ac\u5316\uff1a\u4e00\u79cd\u65b0\u7684\u50ac\u5316\u6982\u5ff5\uff0c\u4e3a\u7eb3\u7c73\u7ea7\u7684\u50ac\u5316\u53cd\u5e94\u7cfb\u7edf\u63d0\u4f9b\u4e00\u4e2a\u53d7\u9650\u7684\u73af\u5883\uff0c\u4ece\u800c\u5b9e\u73b0\u50ac\u5316\u6027\u80fd\u7684\u7cbe\u786e\u8c03\u8282\uff0c\u5e76\u4f7f\u50ac\u5316\u201c\u5feb\u800c\u597d\u201d\uff09\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\uff08<\/em><\/strong><strong><em>\u2163<\/em><\/strong><strong><em>\uff09\u4e86\u89e3\u673a\u5236<\/em><\/strong><\/p>\n<p>\u4e0d\u5e94\u5ffd\u89c62D TMDs\u7684\u5149\u50ac\u5316\u673a\u5236\u3002\u4f8b\u5982\u8c01\u662f\u771f\u6b63\u7684\u6d3b\u8dc3\u573a\u6240\uff1f\u50ac\u5316\u53cd\u5e94\u8fc7\u7a0b\u4e2dTMDs\u7684\u76f8\u4f4d\u662f\u5426\u53d1\u751f\u53d8\u5316\uff1f\u7535\u5b50\u5982\u4f55\u5728\u754c\u9762\u8fc1\u79fb\uff1f\u6700\u5148\u8fdb\u7684\u539f\u4f4d\u8868\u5f81\u6280\u672f\u4e3a\u6df1\u5165\u5b9e\u65f6\u63a2\u7d22\u8fd9\u4e9b\u673a\u5236\u548c\u6027\u8d28\u63d0\u4f9b\u4e86\u5f3a\u5927\u7684\u5de5\u5177\u3002\u8fd9\u4e9b\u539f\u4f4d\u6280\u672f\u5305\u62ec\u4f46\u4e0d\u9650\u4e8e\u539f\u4f4d\u6db2\u76f8\u900f\u5c04\u7535\u5b50\u663e\u5fae\u955c\uff08TEM\uff09\u3001\u539f\u4f4dX\u5c04\u7ebf\u5438\u6536\u5149\u8c31\uff08XAS\uff09\u548c\u539f\u4f4d\u62c9\u66fc\u3002\u4f8b\u5982\uff0c\u539f\u4f4d\u6db2\u76f8TEM\u53ef\u4ee5\u5728\u539f\u5b50\u5c3a\u5ea6\u4e0a\u63d0\u4f9b\u50ac\u5316\u5242\u8868\u9762\u7684\u5b9e\u65f6\u89c6\u89c9\u68c0\u6d4b\uff0c\u53ef\u4ee5\u6253\u5f00\u57fa\u4e8e2D TMDs\u7684\u6750\u6599\u7684\u771f\u5b9e\u5149\u50ac\u5316\u4f4d\u70b9\u7684\u9ed1\u5323\u5b50\u3002\u9664\u4e86\u5148\u8fdb\u7684\u539f\u4f4d\u8868\u5f81\u6280\u672f\u4e4b\u5916\uff0c\u8d85\u5feb\u8f7d\u6d41\u5b50\u68c0\u6d4b\uff08\u4f8b\u5982\uff0c\u98de\u79d2\u6cf5\u6d66\u63a2\u9488\u5149\u8c31\uff09\u548c\u9ad8\u901a\u91cf\u7b2c\u4e00\u539f\u7406\u8ba1\u7b97\u4e5f\u662f\u5149\u50ac\u5316\u673a\u7406\u7814\u7a76\u7684\u6709\u6548\u5de5\u5177\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\uff08<\/em><\/strong><strong><em>\u2164<\/em><\/strong><strong><em>\uff09\u5f00\u53d1\u5668\u4ef6<\/em><\/strong><\/p>\n<p>\u5e94\u5236\u5b9a\u65b9\u6cd5\u548c\u534f\u8bae\uff0c\u5f00\u53d1\u57fa\u4e8e2D TMDs\u7684\u5149\u50ac\u5316\u88c5\u7f6e\uff0c\u5b9e\u73b0\u5149\uff08\u7535\uff09\u50ac\u5316\u53cd\u5e94\u3001\u4ea7\u54c1\u6536\u96c6\u548c\u5b9e\u65f6\u76d1\u63a7\u7684\u96c6\u6210\u3002\u6700\u8fd1\u5f00\u53d1\u7684\u7528\u4e8e\u53ef\u6269\u5c55\u592a\u9633\u80fd\u71c3\u6599\u751f\u4ea7\u7684\u9499\u949b\u77ff-BiVO<sub>4<\/sub>\u5668\u4ef6\u53ef\u4ee5\u63d0\u4f9b\u53c2\u8003\u3002\u73b0\u4ee3\u5fae\u7eb3\u7c73\u5236\u9020\u6280\u672f\uff08\u5982\u5149\u523b\u3001\u7269\u7406\u6c14\u76f8\u6c89\u79ef\uff09\u3001\u57fa\u4e8e\u6eb6\u6db2\u7684\u6c89\u79ef\u6280\u672f\uff08\u5982\u55b7\u58a8\u5370\u5237\u3001\u5de5\u4e1a\u8f8a\u5bf9\u8f8a\u6d82\u5c42\uff09\u7684\u53d1\u5c55\u4ee5\u53ca\u529f\u80fd\u6750\u6599\uff08\u5982\u67d4\u6027\u6750\u6599\u3001\u8d85\u5bfc\u4f53\uff09\u7684\u4e0d\u65ad\u53d1\u5c55\u4e3a\u6b64\u7c7b\u5668\u4ef6\u7684\u5236\u9020\u63d0\u4f9b\u4e86\u4fdd\u969c\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\uff08<\/em><\/strong><strong><em>\u2165<\/em><\/strong><strong><em>\uff09\u5b9e\u9a8c\u5ba4\u5230\u5de5\u5382\u7684\u8fc7\u6e21<\/em><\/strong><\/p>\n<p>\u5149\u50ac\u5316\u6280\u672f\u7684\u6700\u7ec8\u76ee\u6807\u662f\u4e3a\u751f\u4ea7\u548c\u751f\u6d3b\u670d\u52a1\u3002\u56e0\u6b64\uff0c\u5b9e\u73b02D TMDs\u57fa\u5149\u50ac\u5316\u5242\u7684\u5149\u50ac\u5316\u5e94\u7528\u4ece\u5b9e\u9a8c\u5ba4\u5230\u5de5\u5382\u7684\u8f6c\u53d8\u81f3\u5173\u91cd\u8981\u3002\u7136\u800c\uff0c\u5b9e\u73b0\u8fd9\u4e00\u8f6c\u53d8\u8fd8\u6709\u5f88\u957f\u7684\u8def\u8981\u8d70\u3002\u672a\u6765\u5b9e\u73b0\u8fd9\u79cd\u8f6c\u53d8\u9700\u8981\u4f9d\u6b21\u5b8c\u6210\u7684\u6b65\u9aa4\u5305\u62ec\uff1a\u6269\u5927\u5df2\u5f00\u53d1\u7684\u8bbe\u5907\uff0c\u548c\/\u6216\u4e32\u8054\u6216\u5e76\u8054\u7ec4\u88c5\uff0c\u7136\u540e\u5c06\u5176\u7f6e\u4e8e\u517c\u5bb9\u7684\u5de5\u4e1a\u7cfb\u7edf\u4e2d\u3002\u5728\u8fd9\u4e9b\u6b65\u9aa4\u4e2d\uff0c\u4e0d\u5e94\u5ffd\u89c6\u5b89\u5168\u56e0\u7d20\u3001\u7ecf\u6d4e\u56e0\u7d20\u548c\u5e02\u573a\u56e0\u7d20\u7684\u8bc4\u4f30\u3002\u6700\u8fd1\u5b9e\u73b0\u7684\u592a\u9633\u80fd\u5236\u6c22\u519c\u573a\u5c31\u662f\u8fd9\u6837\u4e00\u4e2a\u5148\u9a71\uff0c\u503c\u5f97\u6211\u4eec\u5b66\u4e60\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><em>\uff08<\/em><\/strong><strong><em>\u2166<\/em><\/strong><strong><em>\uff09\u5176\u4ed6<\/em><\/strong><\/p>\n<p>\u9664\u4e86\u6293\u4f4f\u4e0a\u8ff0\u673a\u9047\uff0c\u81f4\u529b\u4e8e\u4ee5\u4e0b\u95ee\u9898\u4e5f\u662f\u6709\u610f\u4e49\u7684\u3002\u4f8b\u5982 \uff081\uff09\u4e3a2D TMDs\u57fa\u5149\u50ac\u5316\u5242\u7684\u751f\u4ea7\u3001\u50a8\u5b58\u548c\u56de\u6536\u5efa\u7acb\u4e00\u4e2a\u5b8c\u6574\u7684\u3001\u73af\u5883\u53cb\u597d\u7684\u7cfb\u7edf\u3002\u56e0\u4e3a\uff0c\u5927\u591a\u65702D TMD\uff0c\u65e0\u8bba\u662f\u51c6\u5907\u597d\u7684\u8fd8\u662f\u4e22\u5f03\u7684\uff0c\u90fd\u4f1a\u6c61\u67d3\u73af\u5883\u3002\uff082\uff09\u8feb\u5207\u9700\u8981\u4e3a\u57fa\u4e8e2D TMDs\u7684\u5149\u50ac\u5316\u5242\u6784\u5efa\u5404\u79cd\u5149\u50ac\u5316\u53cd\u5e94\u7684\u6548\u7387\u8ba4\u8bc1\u548c\u6807\u51c6\u5316\u6d4b\u8bd5\u534f\u8bae\u3002\u76ee\u524d\uff0c\u6bcf\u4e2a\u7814\u7a76\u7ec4\u7684\u5b9e\u9a8c\u6570\u636e\u7f3a\u4e4f\u6a2a\u5411\u6bd4\u8f83\u7684\u53ef\u4fe1\u5ea6\u3002\u56e0\u4e3a\u5b83\u4eec\u7684\u5b9e\u9a8c\u6761\u4ef6\uff08\u5982\u5149\u7167\u6761\u4ef6\u3001\u73af\u5883\u6e29\u5ea6\u548c\u53cd\u5e94\u6eb6\u6db2\u7684pH\u503c\uff09\u901a\u5e38\u4e0d\u540c\u3002\u8fd9\u901a\u5e38\u4f1a\u5bfc\u81f4\u65e0\u6cd5\u9a8c\u8bc1\u4e14\u7ecf\u5e38\u8bef\u5bfc\u7684\u6570\u636e\u79ef\u7d2f\uff0c\u963b\u788d\u7814\u7a76\u9886\u57df\u7684\u8fdb\u6b65\u3002\u56e0\u6b64\uff0c\u9700\u8981\u6548\u7387\u8ba4\u8bc1\u548c\u6807\u51c6\u5316\u6d4b\u8bd5\u534f\u8bae\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u603b\u4e4b\uff0c\u5728\u8fd9\u4e2a\u8ff7\u4eba\u7684\u9886\u57df\uff0c\u673a\u9047\u4e0e\u6311\u6218\u5e76\u5b58\u3002\u6211\u4eec\u9884\u8ba1\uff0c2D TMDs\u5c06\u5728\u672a\u6765\u51e0\u5341\u5e74\u6210\u4e3a\u5149\u50ac\u5316\u7684\u6838\u5fc3\u65b0\u6750\u6599\uff0c\u5149\uff08\u7535\uff09\u50ac\u5316\u5c06\u6210\u4e3a\u89e3\u51b3\u672a\u6765\u65f6\u4ee3\u80fd\u6e90\u548c\u73af\u5883\u5371\u673a\u7684\u6838\u5fc3\u6280\u672f\u4e4b\u4e00\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-246034\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe16.png\" alt=\"\" width=\"1266\" height=\"1058\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe16.png 1266w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe16-300x251.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe16-768x642.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/01\/\u56fe16-1024x856.png 1024w\" sizes=\"(max-width: 1266px) 100vw, 1266px\" \/><\/p>\n<p>\u56fe16 | 2D TMDs\u5149\u50ac\u5316\u7684\u5c55\u671b\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u7b2c\u4e00\u4f5c\u8005\uff08\u6216\u8005\u5171\u540c\u7b2c\u4e00\u4f5c\u8005\uff09\uff1a\u6768\u9510\u6377\uff0c\u8303\u83b9\u83b9\uff1b\u901a\u8baf\u4f5c\u8005\uff08\u6216\u8005\u5171\u540c\u901a\u8baf\u4f5c\u8005\uff09\uff1a \u66fe\u5fd7\u8fdc\uff0c\u4f59\u6d4e\u7f8e\uff0c\u738b\u8c26\uff0c\u6731\u8363\u6dd1\uff1b\u901a\u8baf\u5355\u4f4d\uff1a\u9999\u6e2f\u57ce\u5e02\u5927\u5b66\uff0c\u9999\u6e2f\u4e2d\u6587\u5927\u5b66\uff0c\u540d\u53e4\u5c4b\u5927\u5b66\uff0c\u54c8\u5c14\u6ee8\u5de5\u4e1a\u5927\u5b66\uff08\u6df1\u5733\uff09 \u00a0\u8bba\u6587DOI\uff1a10.1002\/anie.202218016\u00a0\u00a0<\/p>\n<p><strong>\u00a0<\/strong><\/p>\n<p><strong>\u901a\u8baf\u4f5c\u8005\u4ecb\u7ecd\uff1a<\/strong><\/p>\n<p>\u66fe\u5fd7\u8fdc\uff0c2019\u5e74\u52a0\u5165\u9999\u6e2f\u57ce\u5e02\u5927\u5b66\u4efb\u52a9\u7406\u6559\u6388\uff0c\u535a\u58eb\u751f\u5bfc\u5e08\u3002(\u8bfe\u9898\u7ec4\u4e3b\u9875: <a href=\"https:\/\/www.zeng-lab.com\/\">https:\/\/www.zeng-lab.com\/<\/a>, \u8054\u7cfb\u65b9\u5f0f: <a href=\"mailto:zhiyzeng@cityu.edu.hk\">zhiyzeng@cityu.edu.hk<\/a>)\u3002\u4e3b\u8981\u4ece\u4e8bTMDs\u9502\u79bb\u5b50\u7535\u5316\u5b66\u63d2\u5c42\u5265\u79bb\u6280\u672f\u3001\u539f\u4f4d\u6db2\u76f8\u900f\u5c04\u7535\u955c\u6280\u672f\u3001\u80fd\u6e90\u4e0e\u73af\u5883\u7b49\u9886\u57df\u7684\u7814\u7a76\u3002<\/p>\n<p><strong>\u8fd1\u671f\u4ee3\u8868\u6027\u5de5\u4f5c\uff1a<\/strong><\/p>\n<ol>\n<li><a href=\"https:\/\/www.nature.com\/articles\/s41596-021-00643-w\">Yang, et. al., Shin*, Voiry*, <strong>Zeng*<\/strong>, <strong><em>Nature Protocols<\/em><\/strong>, 2022, 17, 358-377.<\/a> (Highly Cited Papers)<\/li>\n<li><a href=\"https:\/\/www.nature.com\/articles\/s41596-022-00762-y\">Yang, et. al., Li*, <strong>Zeng*<\/strong>, <strong><em>Nature Protocols<\/em><\/strong>, 2022, DOI: 10.1038\/s41596-022-00762-y.<\/a><\/li>\n<li>Yang, et. al., Li*, <strong>Zeng*<\/strong>, <strong><em>Nature Synthesis<\/em><\/strong>, 2023, DOI: 10.1038\/s44160-022-00232-z.<\/li>\n<li><a href=\"https:\/\/www.cell.com\/matter\/fulltext\/S2590-2385(22)00015-7\">Zhang, et. al., Li*, Li*, <strong>Zeng*<\/strong>, <strong><em>Matter<\/em><\/strong>, 2022, 5, 1235-1250.<\/a><\/li>\n<li><a href=\"https:\/\/www.sciencedirect.com\/science\/article\/abs\/pii\/S2590238522005379\">Peng, Wang*, et. al., Qian*, Voiry*, <strong>Zeng*<\/strong>, <strong><em>Matter<\/em><\/strong>, 2023, 2023, 6, 59-96.<\/a><\/li>\n<li><a href=\"https:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/adma.202201416\">Mei, et. al., Wang*, Farimani*, <strong>Zeng*<\/strong>, <strong><em>Advanced Materials<\/em><\/strong>, 2022, 34, 2201416.<\/a> (Rising Stars Series)<\/li>\n<li><a href=\"https:\/\/onlinelibrary.wiley.com\/doi\/full\/10.1002\/adma.202004862\">Yang, et. al., Cao*, Yin*, <strong>Zeng*<\/strong>, <strong><em>Advanced Materials<\/em><\/strong>, 2021, 33, 2004862.<\/a> (Highly Cited Papers)<\/li>\n<li><a href=\"https:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/anie.202218016\">Yang, Zhu*, et al., Wang*, Yu*, <strong>Zeng*<\/strong>, <strong><em>Angewandte Chemie International Edition<\/em><\/strong>, 2023, DOI: 10.1002\/anie.202218016.<\/a><\/li>\n<li><a href=\"https:\/\/www.sciencedirect.com\/science\/article\/abs\/pii\/S0079642522001372\">Tian, Ho*, et. al., Wang*, <strong>Zeng*<\/strong>, <strong><em>Progress in Materials Science<\/em><\/strong>, 2023, 133, 101056.<\/a><\/li>\n<li><a href=\"https:\/\/onlinelibrary.wiley.com\/doi\/full\/10.1002\/smll.202203759\">Zhang, et. al., Li*, <strong>Zeng*<\/strong>, <strong><em>Small<\/em><\/strong>, 2022, 18, 2203759.<\/a> (Rising Stars Series)<\/li>\n<li><a href=\"https:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/smll.202103052\">Yang, Zhu*, et. al., <strong>Zeng*<\/strong>, <strong><em>Small<\/em><\/strong>, 2021, 17, 2103052.<\/a> (Back Cover)<\/li>\n<\/ol>\n<p>\u672c\u6587\u7531\u4f5c\u8005\u4f9b\u7a3f<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u5168\u6587\u901f\u89c8\uff1a \u4e8c\u7ef4\uff082D\uff09\u8fc7\u6e21\u91d1\u5c5e\u786b\u65cf\u5316\u5408\u7269\uff08TMDs\uff09\uff0c\u540e\u77f3\u58a8\u70ef\u65f6\u4ee3\u7684\u4e00\u9897\u65b0\u661f\uff0c\u5728\u5149\u50ac\u5316\u9886\u57df\u5177\u6709\u57fa\u7840\u6027\u548c\u6280\u672f\u6027\u7684\u5438\u5f15\u529b\u3002\u5b83\u4eec\u975e\u51e1\u7684\u7535\u5b50\u3001\u5149\u5b50\u548c\u5316\u5b66\u5c5e\u6027\u4f7f\u5b83\u4eec\u6210\u4e3a&#8230;<\/p>\n","protected":false},"author":41672,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[2],"tags":[],"class_list":["post-246017","post","type-post","status-publish","format-standard","hentry","category-keji"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/246017"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/41672"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=246017"}],"version-history":[{"count":1,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/246017\/revisions"}],"predecessor-version":[{"id":246035,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/246017\/revisions\/246035"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=246017"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=246017"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=246017"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}