{"id":248215,"date":"2023-03-08T06:01:24","date_gmt":"2023-03-07T22:01:24","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=248215"},"modified":"2023-03-03T14:01:43","modified_gmt":"2023-03-03T06:01:43","slug":"%e4%b8%ad%e7%a7%91%e5%a4%a7%e5%88%98%e5%ba%86%e5%8d%8e%e6%9c%80%e6%96%b0nc%ef%bc%9a%e8%b0%83%e8%8a%82%e7%bc%a9%e6%94%be%e5%85%b3%e7%b3%bb%e4%bb%a5%e5%ae%9e%e7%8e%b0%e6%b0%a7%e8%bf%98%e5%8e%9f%e5%8f%8d","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=248215","title":{"rendered":"\u4e2d\u79d1\u5927\u5218\u5e86\u534e\u6700\u65b0NC\uff1a\u8c03\u8282\u7f29\u653e\u5173\u7cfb\u4ee5\u5b9e\u73b0\u6c27\u8fd8\u539f\u53cd\u5e94\u7684\u9ad8\u50ac\u5316\u52a8\u529b\u5b66\u548c\u9009\u62e9\u6027"},"content":{"rendered":"<p style=\"text-align: center;\"><strong><b>\u4e2d\u79d1\u5927\u5218\u5e86\u534e\u6700\u65b0Nature Communications\uff1a\u8c03\u8282\u7f29\u653e\u5173\u7cfb\u4ee5\u5b9e\u73b0\u6c27\u8fd8\u539f\u53cd\u5e94\u7684\u9ad8\u50ac\u5316\u52a8\u529b\u5b66\u548c\u9009\u62e9\u6027<\/b><\/strong><\/p>\n<p style=\"text-align: center;\"><strong><b>[\u5bfc\u8bfb]<\/b><\/strong><\/p>\n<p>&nbsp;<\/p>\n<p>\u6c27\u8fd8\u539f\u53cd\u5e94(ORR)\u662f\u53ef\u518d\u751f\u80fd\u6e90\u8f6c\u5316\u6280\u672f\u7684\u6838\u5fc3\uff0c\u5728\u91d1\u5c5e-\u7a7a\u6c14\u7535\u6c60\u3001\u71c3\u6599\u7535\u6c60\u7b49\u65b0\u5174\u7535\u5316\u5b66\u80fd\u6e90\u88c5\u7f6e\u4e2d\u53d1\u6325\u7740\u4e0d\u53ef\u66ff\u4ee3\u7684\u4f5c\u7528\u3002\u7136\u800c\uff0c\u53d1\u751f\u5728\u9634\u6781\u4e0a\u7684ORR\u7684\u7f13\u6162\u52a8\u529b\u5b66\u6d89\u53ca\u591a\u6b65\u8d28\u5b50\u8026\u5408\u7535\u5b50\u8f6c\u79fb\uff0c\u8fd9\u5bf9\u63d0\u9ad8\u80fd\u91cf\u8f6c\u6362\u5668\u4ef6\u7684\u6574\u4f53\u6548\u7387\u5177\u6709\u91cd\u5927\u5f71\u54cd\u3002\u57fa\u4e8e\u8d35\u91d1\u5c5e\u94c2\u7684\u50ac\u5316\u5242\u5177\u6709\u9ad8\u8fbe400\u2009\u03bcgPt cm<sup>-2<\/sup>\u7684\u91d1\u5c5e\u8d1f\u8f7d\u91cf\uff0c\u5bf9\u4e8e\u63d0\u9ad8ORR\u9a71\u52a8\u80fd\u6e90\u5668\u4ef6\u7684\u80fd\u91cf\u8f93\u51fa\u6548\u7387\u662f\u6700\u5b9e\u7528\u7684\uff0c\u4f46\u5176\u5e94\u7528\u4ecd\u7136\u53d7\u5230\u8d35\u91d1\u5c5e\u8d44\u6e90\u7a00\u7f3a\u548c\u7406\u60f3\u9ad8\u7535\u538b\u4e0b\u7a33\u5b9a\u6027\u6709\u9650\u7684\u963b\u788d\u3002\u5c06Pt\u4e0e\u7b2c\u4e8c\u91d1\u5c5e\u5408\u91d1\u5316\u53ef\u4ee5\u5728\u63d0\u9ad8\u6027\u80fd\u7684\u540c\u65f6\u51cf\u5c11Pt\u7684\u4f7f\u7528\u91cf\u3002\u7136\u800c\uff0cPt\u7684\u7528\u91cf\u4ecd\u4e0d\u4f4e\u4e8e40at.%\uff0c\u4e14\u5728ORR\u6761\u4ef6\u4e0b\uff0c\u4e8c\u6b21\u91d1\u5c5e\u9010\u6e10\u6d41\u5931\uff0c\u5bfc\u81f4\u6027\u80fd\u8fc5\u901f\u635f\u5931\uff0c\u8fd9\u8db3\u4ee5\u9650\u5236\u5927\u89c4\u6a21\u5546\u4e1a\u5316\u3002\u56e0\u6b64\uff0c\u8bbe\u8ba1\u5177\u6709\u5feb\u901f\u53cd\u5e94\u52a8\u529b\u5b66\u548c\u957f\u671f\u8010\u4e45\u6027\u7684\u4f4e\u8d1f\u8f7d\u6d3b\u6027\u8d35\u91d1\u5c5eORR\u7535\u50ac\u5316\u5242\u5bf9\u4e8e\u9ad8\u6548\u7684\u80fd\u91cf\u8f6c\u6362\u548c\u5b58\u50a8\u662f\u975e\u5e38\u5fc5\u8981\u7684\u3002<\/p>\n<p><strong><b>\u00a0<\/b><\/strong><\/p>\n<p style=\"text-align: center;\"><strong><b>[\u6210\u679c\u63a0\u5f71]<\/b><\/strong><\/p>\n<p><strong><b>\u00a0<\/b><\/strong><\/p>\n<p><strong><b>\u5728\u8fd9\u9879\u7814\u7a76\u4e2d\uff0c<\/b><\/strong><strong><b>\u4e2d\u56fd\u79d1\u5b66\u6280\u672f\u5927\u5b66\u5218\u5e86\u534e\u3001\u82cf\u5fbd<\/b><\/strong><strong><b>\u8bfe\u9898\u7ec4<\/b><\/strong><strong><b>\uff0c<\/b><\/strong><strong><b>\u63d0\u51fa\u4e86\u4e00\u79cd\u4f7f\u7528\u91d1\u5c5e\u95f4\u8ddd\u79bb\u8c03\u63a7\u7684\u539f\u5b50\u5c3a\u5ea6\u53cc\u91d1\u5c5e\u7ec4\u88c5\u4f53(ABA)\u7684\u7b56\u7565<\/b><\/strong>\uff0c\u8be5\u7ec4\u88c5\u4f53\u53ef\u4ee5\u50ac\u5316\u76f4\u63a5\u7684O-O\u81ea\u7531\u57fa\u65ad\u88c2\u800c\u4e0d\u5f62\u6210\u591a\u4f59\u7684*OOH\u4e2d\u95f4\u4f53\uff0c\u4ece\u800c\u8c03\u8282\u56fa\u6709\u7684\u7ebf\u6027\u6807\u5ea6\u5173\u7cfb\uff0c\u5e76\u4f7fABA\u4e0a\u7684ORR\u9075\u5faa\u5feb\u901f\u52a8\u529b\u5b66\u53cc\u4f4d\u70b9\u673a\u5236\u3002\u5229\u7528\u539f\u4f4d\u540c\u6b65\u8f90\u5c04\u5149\u8c31\uff0c\u672c\u5de5\u4f5c\u76f4\u63a5\u89c2\u5bdf\u5230\u81ea\u8c03\u8282\u7684N-\u6865\u8fdePt=N<sub>2<\/sub>=Fe\u7ec4\u88c5\u4f53\u5728ORR\u8fc7\u7a0b\u4e2d\u4fc3\u8fdb\u4e86\u5173\u952e\u4e2d\u95f4\u72b6\u6001(Pt-O-O-Fe)\u7684\u4ea7\u751f\uff0c\u4ece\u800c\u5bfc\u81f4\u9ad8\u7684\u53cd\u5e94\u52a8\u529b\u5b66\u548c\u9009\u62e9\u6027\u3002\u7cbe\u5fc3\u8bbe\u8ba1\u7684Pt=N<sub>2<\/sub>=Fe ABA\u50ac\u5316\u5242\u57280.95\u2009V\u7684\u534a\u6ce2\u7535\u4f4d\u4e0b\u76f8\u5bf9\u4e8e\u5546\u4e1aPt\/C\u5b9e\u73b0\u4e86\u8fd12\u4e2a\u6570\u91cf\u7ea7\u7684\u52a8\u529b\u5b66\u7535\u6d41\u5bc6\u5ea6\u63d0\u5347\uff0c4\u7535\u5b50\u9014\u5f84\u9009\u62e9\u6027\u6548\u7387\u63a5\u8fd199%\uff0c\u662f\u5e94\u7528\u4e8e\u950c\u7a7a\u6c14\u7535\u6c60\u80fd\u91cf\u88c5\u7f6e\u7684\u6f5c\u5728ORR\u50ac\u5316\u5242\u4e4b\u4e00\u3002<strong><b>\u672c\u7814\u7a76\u4e3a\u5f00\u53d1\u548c\u4f18\u5316\u5176\u4ed6\u9ad8\u6548ORR\u7535\u50ac\u5316\u5242\u63d0\u4f9b\u4e86\u6709\u76ca\u7684\u8bbe\u8ba1\u539f\u5219<\/b><\/strong>\u3002\u76f8\u5173\u8bba\u6587\u4ee5\u9898\u4e3a\uff1a\u201c<em><i>Regulating the scaling relationship for high catalytic kinetics and selectivity of the oxygen reduction reaction<\/i><\/em>\u201d\u53d1\u8868\u5728<em><i>Nature Communications<\/i><\/em>\u4e0a\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-248216\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72471-6.png\" alt=\"\" width=\"724\" height=\"297\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72471-6.png 724w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72471-6-300x123.png 300w\" sizes=\"(max-width: 724px) 100vw, 724px\" \/><\/p>\n<p>&nbsp;<\/p>\n<p style=\"text-align: center;\"><strong><b>[\u6838\u5fc3\u521b\u65b0\u70b9]<\/b><\/strong><\/p>\n<ul>\n<li>\u4e3a\u4e86\u6ee1\u8db3\u56db\u7535\u5b50ORR\u9ad8\u52a8\u529b\u5b66\u548c\u9ad8\u9009\u62e9\u6027\u7684\u53cc\u4f4d\u70b9\u673a\u7406\u8bbe\u8ba1\u89c4\u5219\uff0c<strong><b>\u672c\u5de5\u4f5c<\/b><\/strong><strong><b>\u521b\u65b0\u6027\u7684<\/b><\/strong><strong><b>\u901a\u8fc7\u53ef\u63a7\u7684&#8221;\u6c28\u57fa\u529f\u80fd\u5316\u78b3\u7eb3\u7c73\u7247&#8221;\u7b56\u7565<\/b><\/strong><strong><b>\uff0c<\/b><\/strong><strong><b>\u5f00\u53d1\u4e86\u5177\u6709\u5b9a\u5236\u51e0\u4f55\u6784\u578b\u7684N-\u6865\u8fdePt=N<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>=Fe\u539f\u5b50\u5c3a\u5ea6\u53cc\u91d1\u5c5e\u7ec4\u88c5(ABA)\u6a21\u578b\u50ac\u5316\u5242<\/b><\/strong>\uff0c\u5177\u6709\u5408\u9002\u7684\u91d1\u5c5e\u95f4\u539f\u5b50\u95f4\u8ddd\uff0c\u5b9e\u73b0\u53cc\u4f4d\u70b9\u673a\u5236\u3002<\/li>\n<li>\u672c\u5de5\u4f5c\u901a\u8fc7SR-FTIR\u76d1\u6d4b\u4e86Pt=N<sub>2<\/sub>=Fe ABA\u50ac\u5316\u5242\u5728\u64cd\u4f5c\u6761\u4ef6\u4e0b\u5173\u952e\u4e2d\u95f4\u72b6\u6001(Pt-O-O-Fe)\u7684\u5f62\u6210\uff0c\u8bc1\u660eORR\u9075\u5faa\u53cc\u4f4d\u70b9\u673a\u7406\uff0c\u6ca1\u6709*OOH\u4e2d\u95f4\u4f53\u7684\u4ea7\u751f\u3002<\/li>\n<li>\u672c\u5de5\u4f5c\u4e3a\u5f00\u53d1\u548c\u4f18\u5316\u5176\u4ed6\u9ad8\u6548ORR\u7535\u50ac\u5316\u5242\u63d0\u4f9b\u4e86\u6709\u76ca\u7684\u8bbe\u8ba1\u539f\u5219\u3002<\/li>\n<\/ul>\n<p><strong><b>\u00a0<\/b><\/strong><\/p>\n<p style=\"text-align: center;\"><strong><b>[\u6570\u636e\u6982\u89c8]<\/b><\/strong><\/p>\n<ul>\n<li><b><\/b><strong><b>\u539f\u5b50\u5c3a\u5ea6\u53cc\u91d1\u5c5e\u7ec4\u88c5\u4f53\u7684\u5408\u6210\u4e0e\u8868\u5f81<\/b><\/strong><\/li>\n<\/ul>\n<p><strong><b>\u00a0<\/b><\/strong><\/p>\n<p>\u901a\u8fc7\u529f\u80fd\u5316\u78b3\u7eb3\u7c73\u7247(CNF-NH<sub>2<\/sub>)\u7684\u72ec\u7279\u4e24\u6b65\u7b56\u7565\u548c\u968f\u540e\u7684\u70ed\u89e3\u8fc7\u7a0b\u5408\u6210\u4e86\u5bcc\u6c2e\u50ac\u5316\u5242\u524d\u9a71\u4f53\u3002\u5408\u6210\u7684Pt=N<sub>2<\/sub>=Fe ABA\u50ac\u5316\u5242\u7684\u5c42\u72b6\u5f62\u8c8c\u5982\u56fe1a\u6240\u793a\u3002\u901a\u8fc7Cs\u6821\u6b63\u7684\u626b\u63cf\u900f\u5c04\u7535\u5b50\u663e\u5fae\u955c\u9ad8\u89d2\u73af\u5f62\u6697\u573a(STEM-HAADF)\u56fe\u50cf\u63ed\u793a\u4e86Pt=N<sub>2<\/sub>=Fe ABA\u50ac\u5316\u5242\u4e2d\u539f\u5b50\u5206\u6563\u7684\u91d1\u5c5e\u4f4d\u70b9\u3002\u57fa\u4e8eSTEM-HAADF\u56fe\u50cf\u4e2d\u539f\u5b50\u7684\u5f3a\u5ea6\u9ad8\u5ea6\u4f9d\u8d56\u4e8e\u5b83\u4eec\u7684\u539f\u5b50\u5e8f\u6570(Z)\uff0c\u5728STEM-HAADF\u56fe\u50cf\u4e2d\u7684\u56db\u4e2a\u53cc\u4f4d\u70b9\u533a\u57df\u8fdb\u884c\u5f3a\u5ea6\u5206\u6790\uff0c\u4ee5\u660e\u786e\u53cc\u4f4d\u70b9\u7ed3\u6784\u7684\u7ec4\u6210(\u56fe1c)\u3002\u6cbf\u7740\u7bad\u5934\u7684\u4e24\u4e2a\u4eae\u70b9\u90fd\u663e\u793a\u51fa\u4e0d\u540c\u7684\u5f3a\u5ea6\uff0c\u8bc1\u5b9e\u4e86\u53cc\u4f4d\u70b9\u662f\u7531Pt\u548cFe\u539f\u5b50\u7ec4\u6210\u7684\u3002\u7edf\u8ba1\u5206\u6790\u7ed3\u679c\u8868\u660ePt\u4e0eFe\u4e4b\u95f4\u7684\u539f\u5b50\u8ddd\u79bb\u7ea6\u4e3a2.83-2.91\u2009\u00c5\u3002\u57fa\u4e8e\u968f\u673a\u9009\u53d6\u7684500\u4e2a\u91d1\u5c5e\u4f4d\u70b9\u7684\u7edf\u8ba1\u5206\u6790\u53d1\u73b0\uff0c\u91d1\u5c5e\u53cc\u4f4d\u70b9\u7ed3\u6784\u7ea6\u536072.6%\u3002\u5728X\u5c04\u7ebf\u884d\u5c04(XRD)\u56fe\u8c31\u4e2d(\u56fe1d)\uff0c\u6240\u6709\u6837\u54c1\u53ea\u663e\u793a\u78b3\u7684\u4e00\u4e2a\u4e3b\u5bfc\u884d\u5c04\u5cf0(~25\u00b0)\uff0c\u6ca1\u6709\u89c2\u5bdf\u5230\u7ed3\u6676\u91d1\u5c5e\u7eb3\u7c73\u9897\u7c92\u3002\u800cPt=N<sub>2<\/sub>=Fe ABA\u50ac\u5316\u5242\u4e2dPt\u3001Fe\u3001N\u548cC\u5143\u7d20\u7684\u5747\u5300\u5206\u5e03\u53ef\u4ee5\u901a\u8fc7\u80fd\u91cf\u8272\u6563X\u5c04\u7ebf(EDX) \u56fe\u50cf\u53cd\u6620\u51fa\u6765\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-248217\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72472-6.png\" alt=\"\" width=\"660\" height=\"513\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72472-6.png 660w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72472-6-300x233.png 300w\" sizes=\"(max-width: 660px) 100vw, 660px\" \/><\/p>\n<p>\u56fe1. \u5f62\u8c8c\u548c\u7ed3\u6784\u8868\u5f81\u00a9 The Author(s) 2022<\/p>\n<p>&nbsp;<\/p>\n<ul>\n<li><b><\/b><strong><b>\u7535\u5316\u5b66\u6c27\u8fd8\u539f\u6027\u80fd<\/b><\/strong><\/li>\n<\/ul>\n<p><strong><b>\u00a0<\/b><\/strong><\/p>\n<p>\u5728\u65cb\u8f6c\u5706\u76d8\u7535\u6781(RDE)\u7cfb\u7edf\u4e0a\u8bc4\u4ef7\u4e86\u5408\u6210\u7684Pt=N<sub>2<\/sub>=Fe ABA\u3001Pt AMS\u3001Fe AMS\u50ac\u5316\u5242\u548c\u5546\u4e1aPt\/C\u7684\u7535\u50ac\u5316ORR\u6d3b\u6027\u3002\u5728N<sub>2<\/sub>\u9971\u548c\u76840.1\u2009M KOH\u7535\u89e3\u6db2\u4e2d\uff0c\u5bf9\u6240\u5408\u6210\u7684\u94c2\u57fa\u50ac\u5316\u5242(Pt=N<sub>2<\/sub>=Fe ABA\u548cPt AMS)\u8fdb\u884c\u4e86\u5faa\u73af\u4f0f\u5b89\u66f2\u7ebf\u7684\u8bb0\u5f55\uff0c\u7531\u4e8e\u94c2\u5728\u6240\u5408\u6210\u7684\u50ac\u5316\u5242\u4e2d\u7684\u5355\u539f\u5b50\u5206\u6563\uff0c\u6ca1\u6709\u8868\u73b0\u51fa\u6c22\u5438\u9644\u548c\/\u6216\u8131\u9644\u7279\u6027\u3002<strong><b>\u56fe2a\u6240\u793a\u7684\u7ebf\u6027\u626b\u63cf\u4f0f\u5b89(LSV)\u66f2\u7ebf\u660e\u663e\u8868\u660e\uff0c\u4e0e\u53c2\u6bd4\u50ac\u5316\u5242\u76f8\u6bd4\uff0cPt=N<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>\u2009=Fe ABA\u5177\u6709\u66f4\u4f18\u5f02\u7684\u6027\u80fd<\/b><\/strong>\u3002\u5728\u53cd\u5e94\u52a8\u529b\u5b66\u65b9\u9762\uff0cPt=N<sub>2<\/sub>=Fe ABA\u57280.95\u2009V (\u56fe2b)\u663e\u793a\u51fa5.83\u2009mA\u2009cm<sup>-2<\/sup>\u7684\u8d85\u9ad8\u52a8\u529b\u5b66\u7535\u6d41\u5bc6\u5ea6(J<sub>k<\/sub>)\uff0c\u6bd4\u5546\u4e1aPt\/C(J<sub>k<\/sub>,0.09\u2009mA\u2009cm<sup>-2<\/sup>)\u9ad8\u51fa\u8fd1\u4e24\u4e2a\u6570\u91cf\u7ea7\u3002Pt=N<sub>2<\/sub>=Fe ABA\u57280.85\u2009V\u4e0b\u7684\u52a0\u901f\u7535\u6d41\u5bc6\u5ea6\u4ecd\u6bd4\u5546\u4e1aPt\/C (Pt=N<sub>2<\/sub>=Fe ABA , 106.3\u2009mA\u2009cm<sup>-2<\/sup>;Pt\/ C,9.83\u2009mA\u2009cm<sup>-2<\/sup>)\u9ad8\u6570\u5341\u500d\u3002\u8f83\u5c0f\u7684Tafel\u659c\u7387(53\u2009mV dec<sup>-1<\/sup>)\u8fdb\u4e00\u6b65\u8bc1\u5b9e\u4e86Pt=N<sub>2<\/sub>=Fe ABA\u4f18\u8d8a\u7684ORR\u52a8\u529b\u5b66\uff0c\u660e\u663e\u5c0f\u4e8e\u5546\u4e1aPt\/C(84\u2009mV dec<sup>-1<\/sup>)\u3001Fe AMS(75\u2009mV dec<sup>-1<\/sup>)\u548cPt AMS (90\u2009mV dec<sup>-1<\/sup>) (\u56fe2c)\u3002\u57fa\u4e8e\u6240\u5408\u6210\u50ac\u5316\u5242\u4e2d\u5927\u81f4\u76f8\u7b49\u7684\u6d3b\u6027\u4f4d\u70b9\u6570\u76ee\uff0c<strong><b>Pt=N<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>=Fe ABA\u50ac\u5316\u6027\u80fd\u7684\u63d0\u9ad8\u4e3b\u8981\u5f52\u56e0\u4e8e\u5f62\u6210\u7684Pt-N-Fe\u53cc\u4f4d\u70b9<\/b><\/strong>\u3002<\/p>\n<p>\u50ac\u5316\u9009\u62e9\u6027\u662f\u8bc4\u4ef7\u7535\u50ac\u5316\u5242\u6027\u80fd\u7684\u91cd\u8981\u6307\u6807\uff0c\u5c24\u5176\u662f\u7535\u50ac\u5316\u6c27\u8fd8\u539f\u53cd\u5e94\u3002\u901a\u8fc7\u4e0d\u540c\u8f6c\u901f\u4e0b\u7684\u6781\u5316\u66f2\u7ebf\u6d4b\u8bd5\u8bc4\u4f30ORR\u9014\u5f84(\u56fe2e)\u3002\u6839\u636e\u6269\u6563\u63a7\u5236\u533a\u57df(\u56fe2e\u7684\u63d2\u56fe)\u4e2d\u5e94\u7528\u7684Levich\u65b9\u7a0b\u8ba1\u7b97\u5f97\u5230\u7535\u5b50\u8f6c\u79fb\u6570(n)\u4e3a~3.98\uff0c<strong><b>\u8bc1\u660ePt=N<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>=Fe ABA\u50ac\u5316\u5242\u6709\u5229\u4e8e4e-\u9014\u5f84<\/b><\/strong>\u3002\u6b64\u5916\uff0c\u5728\u65cb\u8f6c\u73af\u76d8\u7535\u6781(RRDE)\u4e0a\u7684\u6d4b\u91cf\u4e5f\u8868\u660e\uff0cPt=N<sub>2<\/sub>=Fe ABA\u7684n\u4e3a~3.98(\u56fe2f )\uff0c\u4f18\u4e8ePt\/C\u548c\u53c2\u6bd4\u6837\u54c1\uff0c<strong><b>\u8bc1\u5b9e2e-\u9014\u5f84\u7684\u526f\u53cd\u5e94\u5f97\u5230\u4e86\u6709\u6548\u6291\u5236<\/b><\/strong>\u3002\u503c\u5f97\u6ce8\u610f\u7684\u662f\uff0cPt=N<sub>2<\/sub>=Fe ABA\u7684H<sub>2<\/sub>O<sub>2<\/sub>\u4ea7\u7387\u4f4e\u4e8e1.5%\uff0c\u5bf94\u7535\u5b50ORR\u5177\u6709\u8f83\u9ad8\u7684\u9009\u62e9\u6027\u3002\u5728Pt=N<sub>2<\/sub>=Fe ABA\u4e0a\u5b9e\u73b0\u4e86\u5feb\u901f\u7684O-O\u952e\u65ad\u88c2\uff0c\u5b9e\u73b0\u4e86\u9ad8\u6548\u76844\u7535\u5b50ORR\u8fc7\u7a0b\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-248218\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72473-6.png\" alt=\"\" width=\"823\" height=\"440\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72473-6.png 823w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72473-6-300x160.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72473-6-768x411.png 768w\" sizes=\"(max-width: 823px) 100vw, 823px\" \/><\/p>\n<p>\u56fe2. \u7535\u5316\u5b66\u6c27\u8fd8\u539f\u6027\u80fd\u6d4b\u8bd5\u00a9 The Author(s) 2022<\/p>\n<p>&nbsp;<\/p>\n<ul>\n<li><b><\/b><strong><b>\u539f\u4f4dXAFS\u5206\u6790<\/b><\/strong><\/li>\n<\/ul>\n<p>&nbsp;<\/p>\n<p>\u5229\u7528\u539f\u4f4dXANES\u548cEXAFS\u5149\u8c31\u53ef\u4ee5\u53cd\u6620\u5b9e\u9645\u53cd\u5e94\u8fc7\u7a0b\u4e2d\u6d3b\u6027\u4f4d\u70b9\u7684\u52a8\u6001\u6f14\u53d8\uff0c\u89e3\u91ca\u4e86\u9ad8ORR\u6d3b\u6027\u7684\u672c\u8d28\u3002\u56fe3a\u4e2d\u7684Pt L<sub>3<\/sub>-edge XANES\u548c\u76f8\u5e94\u7684\u56fe3b\u7684\u5c40\u90e8\u653e\u5927\u56fe\u663e\u793a\uff0c\u5f53\u65bd\u52a01.05\u2009V\u7684\u7535\u4f4d\u65f6\uff0c\u767d\u7ebf\u5f3a\u5ea6\u660e\u663e\u589e\u52a0\uff0c\u8fd9\u662f\u7531\u4e8e\u4e0e\u6c27\u7269\u79cd\u914d\u4f4d\u7684Pt\u4f4d\u70b9\u7684\u51fa\u73b0\u5bfc\u81f4\u4e86\u66f4\u9ad8\u7684\u6c27\u5316\u6001\u3002\u968f\u7740\u6c27\u8fd8\u539f\u7535\u4f4d\u7684\u65bd\u52a0\uff0c\u767d\u7ebf\u7684\u5f3a\u5ea6\u964d\u4f4e\uff0c\u610f\u5473\u7740\u7535\u5b50\u4ece\u9644\u8fd1\u7684\u539f\u5b50\u8f6c\u79fb\u5230Pt\u4f4d\u70b9\uff0c\u4ece\u800c\u52a0\u901f\u50ac\u5316\u53cd\u5e94\u8fc7\u7a0b\u3002\u6709\u8da3\u7684\u662f\uff0c\u5bf9\u4e8eFe K\u8fb9\u7f18\u7684XANES (\u56fe3b,c)\uff0c\u767d\u7ebf\u5f3a\u5ea6\u7684\u53d8\u5316\u4e0e\u7535\u52bf\u6ede\u540e\u7c7b\u4f3c\uff0c\u8868\u660eFe\u4f4d\u70b9\u4e0e\u6c27\u7684\u914d\u4f4d\u4e0ePt\u4f4d\u70b9\u7d27\u5bc6\u76f8\u90bb\u3002\u8fd9\u8868\u660ePt\u548cFe\u662f\u534f\u540c\u6d3b\u6027\u4e2d\u5fc3\uff0c\u4f5c\u4e3a\u6d3b\u6027\u7269\u79cd\u7684\u5438\u9644\/\u8131\u9644\u4f4d\u70b9\u3002<\/p>\n<p>\u4e3a\u4e86\u8fdb\u4e00\u6b65\u9610\u660e\u53cc\u91d1\u5c5e\u7ec4\u88c5\u6d3b\u6027\u4f4d\u70b9\u7684\u7ed3\u6784\u6f14\u53d8\uff0c\u672c\u5de5\u4f5c\u7ed9\u51fa\u4e86Pt L<sub>3<\/sub>-edge\u548cFe K-edge\u7684FT-EXAFS\u56fe\u8c31\u3002\u5bf9\u4e8e\u56fe3e\u4e2d\u4e0d\u540c\u53cd\u5e94\u6761\u4ef6\u4e0bPt L<sub>3<\/sub>-edge\u7684FT-EXAFS\u8c31\uff0c\u53ef\u4ee5\u5f52\u56e0\u4e8ePt-N\/O\u914d\u4f4d\u7684\u7b2c\u4e00\u58f3\u5c42\u5728~1.55\u2009\u00c5\u5904\u7684\u4e3b\u5bfc\u5cf0\u5f3a\u5ea6\u660e\u663e\u589e\u52a0\uff0c\u7279\u522b\u662f\u4eceKOH\u52301.05\u2009V\u5904\u3002\u7c7b\u4f3c\u5730\uff0c\u5728Fe K-edge\u7684FT-EXAFS\u8c31\u4e2d(\u56fe3f )\uff0c\u672c\u5de5\u4f5c\u89c2\u5bdf\u5230\u540c\u6837\u7684\u73b0\u8c61\uff0c\u57280.95\u2009V\u7535\u538b\u4e0b\uff0c~1.42\u2009\u00c5\u5904\u7684\u4e3b\u5bfc\u5cf0\u5f3a\u5ea6\u589e\u52a0\uff0c\u8868\u660ePt\u548cFe\u91d1\u5c5e\u4f4d\u70b9\u90fd\u53c2\u4e0e\u4e86\u53cd\u5e94\uff0c\u5e76\u4e14\u5728ORR\u8fc7\u7a0b\u4e2d\u5177\u6709\u76f8\u4f3c\u7684\u914d\u4f4d\u6f14\u53d8\u3002\u5728Pt=N<sub>2<\/sub>=Fe\u7ec4\u88c5\u4f53\u4e2d\uff0c\u4e24\u4e2a\u76f8\u90bb\u7684\u91d1\u5c5e\u539f\u5b50\u5206\u522b\u4e0e\u4e00\u4e2a\u53cc\u6c27(-O-O-O-)\u7684O\u539f\u5b50\u7ed3\u5408\uff0c\u53ef\u4ee5\u4e3a\u76f4\u63a5O-O\u952e\u65ad\u88c2\u63d0\u4f9b\u5f3a\u7684\u9a71\u52a8\u529b\uff0c\u8c03\u8282\u591a\u4e2a\u53cd\u5e94\u4e2d\u95f4\u4f53\u7684\u6807\u5ea6\u5173\u7cfb\uff0c\u4ece\u800c\u5b9e\u73b0\u5feb\u901f\u76844\u7535\u5b50ORR\u8fc7\u7a0b\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-248219\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72474-6.png\" alt=\"\" width=\"654\" height=\"499\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72474-6.png 654w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72474-6-300x229.png 300w\" sizes=\"(max-width: 654px) 100vw, 654px\" \/><\/p>\n<p>\u56fe3. \u901a\u8fc7\u539f\u4f4dXAFS\u786e\u5b9a\u4e86\u7ed3\u6784\u7684\u6f14\u53d8\u00a9 The Author(s) 2022<\/p>\n<p>&nbsp;<\/p>\n<ul>\n<li><b><\/b><strong><b>\u539f\u4f4dSR-FTIR\u5206\u6790<\/b><\/strong><strong><b>\u4ee5\u53ca\u5728\u53ef\u518d\u751f\u80fd\u6e90\u88c5\u7f6e\u4e2d\u7684\u5e94\u7528<\/b><\/strong><\/li>\n<\/ul>\n<p>&nbsp;<\/p>\n<p>\u5728ORR\u64cd\u4f5c\u6761\u4ef6\u4e0b\u8fdb\u884c\u4e86\u539f\u4f4dSR-FTIR\uff0c\u53ef\u4ee5\u7075\u654f\u5730\u6355\u83b7\u53cd\u5e94\u6d3b\u6027\u539f\u5b50\u5e76\u8bc6\u522b\u53cd\u5e94\u673a\u7406\u3002\u5982\u56fe4a\u6240\u793a\uff0c\u5728\u9010\u6e10\u65bd\u52a0\u7684\u7535\u4f4d\u4e0b\uff0c\u89c2\u5bdf\u5230\u4f4d\u4e8e1115\u2009cm<sup>-1<\/sup>\u7684\u7ea2\u5916\u5438\u6536\u5e26\u3002\u5df2\u77e51060~1150\u2009cm<sup>-1<\/sup>\u8303\u56f4\u5185\u7684\u5438\u6536\u5e26\u4e0eO-O\u7684\u7ea2\u5916\u5438\u6536\u6709\u5173\u3002\u56e0\u6b64\uff0c\u8fd9\u79cd\u7535\u538b\u4f9d\u8d56\u7684\u632f\u52a8\u8868\u660e\u5728ORR\u8fc7\u7a0b\u4e2d\uff0cPt=N<sub>2<\/sub>=Fe\u53cc\u4f4d\u70b9\u4e0a\u4ea7\u751f\u4e86\u5173\u952e\u7684\u4e2d\u95f4\u4f53O-O\uff0c\u5f62\u6210Pt-O-O-Fe\u6784\u578b\u3002\u7ed3\u5408\u539f\u4f4dXAFS\u7ed3\u679c\uff0c\u6709\u5229\u4e8eO<sub>2<\/sub>\u5206\u5b50\u5438\u9644\u7684Pt\u548cFe\u53cc\u4f4d\u70b9\u76f4\u63a5\u6f14\u53d8\u4e3aO-O\u81ea\u7531\u57fa\u3002\u4f5c\u4e3a\u53c2\u8003\uff0c\u56fe4b\u7ed9\u51fa\u4e86\u76f8\u540c\u6761\u4ef6\u4e0bPt AMS\u6837\u54c1\u7684FTIR\u6d4b\u91cf\u7ed3\u679c\u3002\u5f53\u5916\u52a0\u7535\u4f4d\u8d85\u8fc70.95\u2009V vs.RHE\u3002\u8003\u8651\u5230\u5438\u9644\u5728\u5355\u91d1\u5c5e\u4f4d\u70b9\u4e0a\u7684*OOH\u7684\u7ea2\u5916\u632f\u52a8\u5cf0\u901a\u5e38\u4f4d\u4e8e~900\u2009cm<sup>-1<\/sup>\u5904\uff0c\u56e0\u6b64965\u2009cm<sup>-1<\/sup>\u5904\u7684\u5438\u6536\u632f\u52a8\u53ef\u5f52\u5c5e\u4e3a*OOH\u4e2d\u95f4\u4f53\u7684\u51fa\u73b0\u3002\u5f53ORR\u7535\u4f4d\u8d85\u8fc71.05\u2009V\u65f6\uff0c-O-O-\u5e26\u7684\u632f\u52a8\u5f3a\u5ea6\u8fc5\u901f\u589e\u52a0\u3002\u76f8\u6bd4\u4e4b\u4e0b\uff0cPt AMS\u50ac\u5316\u5242\u7684*OOH\u7684\u5f3a\u5ea6\u4ec5\u57280.95\u2009V\u540e\u8868\u73b0\u51fa\u7f13\u6162\u7684\u589e\u5f3a\u3002<strong><b>\u8fd9\u4e00\u73b0\u8c61\u8bc1\u5b9e\u4e86\u539f\u5b50\u7ea7\u53cc\u91d1\u5c5e\u7ec4\u88c5\u50ac\u5316\u5242\u4e2dPt=N<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>=Fe\u53cc\u4f4d\u70b9\u663e\u8457\u52a0\u901fO<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>\u6f14\u53d8\u4e3a-O-O-\u81ea\u7531\u57fa\uff0c\u5f62\u6210Pt-O-O-Fe\u4e2d\u95f4\u7ed3\u6784\uff0c\u4f7fORR\u5728\u8f83\u4f4e\u7684\u8fc7\u7535\u4f4d\u4e0b\u53d1\u751f\u3002\u540c\u65f6\uff0cPt-O-O-Fe\u6d3b\u6027\u76f8\u53ef\u4ee5\u6709\u6548\u5730\u5207\u65adO-O\u952e\u800c\u4e0d\u4ea7\u751f*OOH\u6765\u8c03\u8282\u56fa\u6709\u7684\u6807\u5ea6\u5173\u7cfb\u4ee5\u5b9e\u73b0\u5feb\u901f\u52a8\u529b\u5b66<\/b><\/strong>\u3002<\/p>\n<p>\u672c\u5de5\u4f5c\u7ec4\u88c5\u4e86Pt=N<sub>2<\/sub>=Fe ABA\u4f5c\u4e3a\u521d\u7ea7\u950c-\u7a7a\u6c14\u7535\u6c60(ZAB)\u7684\u9634\u6781\u6765\u8bc4\u4f30\u50ac\u5316\u5242\u5728\u53ef\u518d\u751f\u80fd\u6e90\u88c5\u7f6e\u4e2d\u7684\u6548\u7387(\u56fe5a )\u3002\u5982\u56fe5b\u6240\u793a\uff0cPt=N<sub>2<\/sub>=Fe ABA\u63ba\u6742Zn-\u7a7a\u6c14\u7535\u6c60\u7684\u5f00\u8def\u7535\u538b(OCV)\u4e3a1.50\u2009V\uff0c\u9ad8\u4e8ePt\/C\u57faZn-\u7a7a\u6c14\u7535\u6c60(1.42\u2009V)\u3002\u503c\u5f97\u6ce8\u610f\u7684\u662f\uff0c\u4e0ePt=N<sub>2<\/sub>=Fe ABA\u50ac\u5316\u5242\u590d\u5408\u7684ZAB\u5728315.2\u2009mA\u2009cm<sup>-2<\/sup>\u65f6\u83b7\u5f97\u4e86198.4\u2009mW\u2009cm<sup>-2<\/sup>\u7684\u6700\u5927\u529f\u7387\u5bc6\u5ea6(\u56fe5c)\uff0c\u4f18\u4e8ePt\/C\u57faZAB(172.1\u2009m W\u2009cm<sup>-2<\/sup>,253\u2009m A\u2009cm<sup>-2<\/sup>)\u548c\u5176\u4ed6\u50ac\u5316\u5242\u5236\u5907\u7684ZAB\u3002\u6b64\u5916\uff0cPt=N<sub>2<\/sub>=Fe ABA\u7a7a\u6c14\u9634\u6781\u7684ZAB\u5728\u653e\u7535\u7535\u6d41\u5bc6\u5ea6\u4e3a10\u2009mA\u2009cm<sup>-2<\/sup>\u65f6\u7684\u6bd4\u5bb9\u91cf\u4e3a787.8 m Ah g Zn<sup>-1<\/sup>\uff0c\u5360ZAB (820 m Ah g Zn<sup>-1<\/sup>)\u7406\u8bba\u5bb9\u91cf\u768496.1% (\u56fe5d)\u3002\u589e\u5f3a\u7684\u6027\u80fd\u8bc1\u660e\u4e86Pt=N<sub>2<\/sub>=Fe ABA\u50ac\u5316\u5242\u53ef\u4ee5\u63d0\u4f9b\u8db3\u591f\u7684\u6548\u7387\u6765\u8bc1\u660e\u5176\u63ba\u5165Zn-\u7a7a\u6c14\u7535\u6c60\u3002\u4e0d\u540c\u7535\u6d41\u5bc6\u5ea6\u5e73\u53f0\u4e0b\u7684\u6052\u6d41\u653e\u7535\u6d4b\u8bd5\u7ed3\u679c\u5982\u56fe5e\u6240\u793a\u3002Pt=N<sub>2<\/sub>=Fe ABA\u7684ZAB\u5728\u5404\u7535\u6d41\u5bc6\u5ea6\u4e0b\u7684\u7535\u6c60\u7535\u538b\u54cd\u5e94\u660e\u663e\u9ad8\u4e8ePt\/C\u7535\u6c60\uff0c\u5f53\u7535\u6d41\u5bc6\u5ea6\u6062\u590d\u52302\u2009mA\u2009cm<sup>-2<\/sup>\u65f6\uff0cPt=N<sub>2<\/sub>=Fe ABA\u7684\u7535\u6c60\u7535\u538b\u6062\u590d\u5230\u539f\u6765\u7684\u6c34\u5e73\u3002\u8fd9\u8868\u660ePt=N<sub>2<\/sub>=Fe ABA\u4f5c\u4e3aZAB\u4e2d\u7684\u9634\u6781\u5177\u6709\u53ef\u89c2\u7684\u500d\u7387\u6027\u80fd\u548c\u7a33\u5b9a\u7684\u7a33\u5b9a\u6027\u3002\u6b64\u5916\uff0c\u8fd9\u79cdPt=N<sub>2<\/sub>=Fe ABA\u57faZAB\u53ef\u4ee5\u901a\u8fc7\u673a\u68b0\u5145\u7535\u7a33\u5b9a\u5de5\u4f5c\uff0c\u5e76\u4e14\u53ea\u9700\u8981\u8865\u5145\u6d88\u8017\u7684\u950c\u8d1f\u6781\u548c\u7535\u89e3\u6db2\u3002\u7ecf\u8fc7\u4e09\u4e2a\u5145\u7535\u5468\u671f\u540e\uff0c\u8f93\u51fa\u7535\u538b\u6ca1\u6709\u660e\u663e\u7684\u4e0b\u964d(\u56fe5f)\u3002<strong><b>\u8fd9\u4e9b\u7ed3\u679c\u8868\u660e\uff0c\u4e00\u79cd\u72ec\u7279\u7684Pt=N<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>=Fe ABA\u50ac\u5316\u5242\u5728\u5b9e\u9645\u8fd0\u884c\u4e2d\u4fdd\u6301\u4e86\u4ee4\u4eba\u6ee1\u610f\u7684\u50ac\u5316\u6d3b\u6027\uff0c\u5728\u5de5\u4e1aORR\u4e2d\u5177\u6709\u5de8\u5927\u7684\u5e94\u7528\u524d\u666f<\/b><\/strong>\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-248220\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72475-6.png\" alt=\"\" width=\"831\" height=\"543\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72475-6.png 831w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72475-6-300x196.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72475-6-768x502.png 768w\" sizes=\"(max-width: 831px) 100vw, 831px\" \/><\/p>\n<p>\u56fe4. \u539f\u4f4dSR-FTIR\u9274\u5b9a\u53cd\u5e94\u8def\u5f84\u00a9 The Author(s) 2022<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-248221\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72476-2.png\" alt=\"\" width=\"827\" height=\"460\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72476-2.png 827w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72476-2-300x167.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/03\/\u56fe\u72476-2-768x427.png 768w\" sizes=\"(max-width: 827px) 100vw, 827px\" \/><\/p>\n<p>\u56fe5. \u950c\u7a7a\u6c14\u7535\u6c60(ZAB)\u6027\u80fd\u00a9 The Author(s) 2022<\/p>\n<p>&nbsp;<\/p>\n<p style=\"text-align: center;\"><strong><b>[\u6210\u679c\u542f\u793a]<\/b><\/strong><\/p>\n<p><strong><b>\u00a0<\/b><\/strong><\/p>\n<p>\u7efc\u4e0a\u6240\u8ff0\uff0c\u901a\u8fc7\u53ef\u63a7\u7684\u6c28\u57fa\u529f\u80fd\u5316\u78b3\u7eb3\u7c73\u7247\u7b56\u7565\uff0c\u5f00\u53d1\u4e86\u5177\u6709\u9002\u5f53\u91d1\u5c5e\u95f4\u539f\u5b50\u95f4\u8ddd\u548c\u72ec\u7279\u7535\u5b50\u7ed3\u6784\u7684\u9ad8\u6548\u3001\u9ad8\u9009\u62e9\u6027N-\u6865\u8fdePt=N<sub>2<\/sub>=Fe\u53cc\u91d1\u5c5e\u7ec4\u88c5\u50ac\u5316\u5242\u3002\u7ed3\u5408\u539f\u4f4dXAFS\u548cSR-FTIR\u6280\u672f\uff0c\u672c\u5de5\u4f5c\u53d1\u73b0\u5728\u5de5\u4f5c\u6761\u4ef6\u4e0b\uff0c\u5728\u81ea\u8c03\u8282\u7684N-\u6865\u8fdePt=N<sub>2<\/sub>=Fe\u53cc\u91d1\u5c5e\u7ec4\u88c5\u4f4d\u70b9\u4e0a\u6210\u529f\u5f62\u6210\u4e86\u5173\u952e\u7684\u4e2d\u95f4\u72b6\u6001(Pt-O-O-Fe)\uff0c\u8be5\u53cc\u91d1\u5c5e\u7ec4\u88c5\u4f4d\u70b9\u9ad8\u6548\u50ac\u5316ORR\u9075\u5faa\u53cc\u4f4d\u70b9\u673a\u7406\uff0c\u4fc3\u8fdb\u4e86O-O\u81ea\u7531\u57fa\u4e2d\u95f4\u4f53\u7684\u751f\u6210\u548c\u5feb\u901f\u65ad\u88c2\uff0c\u800c\u4e0d\u5f62\u6210\u4f20\u7edf\u7684\u53cd\u5e94\u4ea7\u7269*OOH\u3002\u6709\u8da3\u7684\u662f\uff0cPt=N<sub>2<\/sub>=Fe ABA\u50ac\u5316\u5242\u5728\u950c-\u7a7a\u6c14\u7535\u6c60\u4e2d\u4fdd\u8bc1\u4e86\u9ad8\u6548\u7387\u548c\u5f3a\u7a33\u5b9a\u6027\u3002<strong><b>\u672c\u5de5\u4f5c<\/b><\/strong><strong><b>\u7684\u7ed3\u679c\u4e3a\u5f00\u53d1\u9ad8\u6d3b\u6027\u548c\u9ad8\u9009\u62e9\u6027\u7684ORR\u50ac\u5316\u5242\u63d0\u4f9b\u4e86\u6709\u7528\u7684\u8bbe\u8ba1\u539f\u5219<\/b><\/strong>\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u7b2c\u4e00\u4f5c\u8005\uff1aWanlin Zhou<\/p>\n<p>\u901a\u8baf\u4f5c\u8005\uff1a\u5218\u5e86\u534e\u3001\u82cf\u5fbd<\/p>\n<p>\u901a\u8baf\u5355\u4f4d\uff1a\u4e2d\u56fd\u79d1\u5b66\u6280\u672f\u5927\u5b66<\/p>\n<p>\u8bba\u6587doi\uff1a<\/p>\n<p><a href=\"https:\/\/doi.org\/10.1038\/s41467-022-34169-w\"><u>https:\/\/doi.org\/10.1038\/s41467-022-34169-w<\/u><\/a><\/p>\n<p>\u672c\u6587\u7531\u6e29\u534e\u4f9b\u7a3f\u3002<\/p>\n<p>&nbsp;<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u4e2d\u79d1\u5927\u5218\u5e86\u534e\u6700\u65b0Nature Communications\uff1a\u8c03\u8282\u7f29\u653e\u5173\u7cfb\u4ee5\u5b9e\u73b0\u6c27\u8fd8\u539f\u53cd\u5e94\u7684\u9ad8\u50ac\u5316\u52a8\u529b\u5b66\u548c\u9009\u62e9\u6027 [\u5bfc\u8bfb] &nbsp; \u6c27\u8fd8\u539f\u53cd\u5e94(ORR)\u662f\u53ef&#8230;<\/p>\n","protected":false},"author":34419,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215,4,2],"tags":[2966,2891,3066],"class_list":["post-248215","post","type-post","status-publish","format-standard","hentry","category-jiedu","category-ganhuo","category-keji","tag-2966","tag-2891","tag-3066"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/248215"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/34419"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=248215"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/248215\/revisions"}],"predecessor-version":[{"id":248281,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/248215\/revisions\/248281"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=248215"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=248215"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=248215"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}