{"id":250725,"date":"2023-05-29T06:01:38","date_gmt":"2023-05-28T22:01:38","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=250725"},"modified":"2023-05-27T09:01:51","modified_gmt":"2023-05-27T01:01:51","slug":"scripta-materialia%ef%bc%9a%e6%bf%80%e5%85%89%e7%b2%89%e6%9c%ab%e5%ba%8a%e7%86%94%e5%90%88cu-ni-al%e5%90%88%e9%87%91%e7%9a%84%e6%88%90%e5%88%86%e6%a2%af%e5%ba%a6%e6%96%b9%e6%b3%95","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=250725","title":{"rendered":"Scripta Materialia\uff1a\u6fc0\u5149\u7c89\u672b\u5e8a\u7194\u5408Cu-Ni-Al\u5408\u91d1\u7684\u6210\u5206\u68af\u5ea6\u65b9\u6cd5"},"content":{"rendered":"<p>\u5f20\u7199\u7199<\/p>\n<p><strong>\u4e00\u3001 \u3010\u5bfc\u8bfb\u3011\u00a0 <\/strong><\/p>\n<p>\u589e\u6750\u5236\u9020(AM)\u6709\u9650\u7684\u9002\u7528\u5408\u91d1\u6570\u91cf\u4e25\u91cd\u963b\u788d\u4e86\u8be5\u6280\u672f\u7684\u5e7f\u6cdb\u5e94\u7528\u3002\uff0c\u56e0\u6b64\u9700\u8981\u9ad8\u901a\u91cf\u65b9\u6cd5\u8fdb\u884c\u6210\u5206\u7b5b\u9009\u3002\u5176\u4e2d\uff0c\u76f4\u63a5\u80fd\u91cf\u6c89\u79ef(DED)\u548c\u6fc0\u5149\u7c89\u672b\u5e8a\u7194\u878d(LPBF)\u6280\u672f\u5df2\u7ecf\u88ab\u7528\u4e8e\u4f7f\u7528\u6df7\u5408\u7c89\u672b(\u800c\u975e\u5355\u4e00\u7c7b\u578b\u7684\u9884\u5408\u91d1\u7c89\u672b)\u6784\u5efa\u6210\u5206\u68af\u5ea6\u5408\u91d1\uff0c\u8fd9\u4e9b\u6280\u672f\u53ef\u4ee5\u5feb\u901f\u68c0\u67e5\u591a\u79cd\u6210\u5206\u7684\u53ef\u6253\u5370\u6027\uff0c\u5fae\u89c2\u7ed3\u6784\u548c\u673a\u68b0\u6027\u80fd\u3002<\/p>\n<p>\u5728LPBF\u4e2d\uff0c\u6210\u5206\u68af\u5ea6\u53ef\u4ee5\u8bbe\u8ba1\u6210\u5e73\u6ed1\u8fde\u7eed\u7684\uff0c\u4e5f\u53ef\u4ee5\u8bbe\u8ba1\u6210\u9636\u68af\u5f0f\u7684\u3002\u5176\u4e2d\u9636\u68af\u5f0f\u7684\u8bbe\u8ba1\u65b9\u6cd5\u4ecd\u6709\u8f83\u591a\u63a3\u8098\uff0c\u4f8b\u5982i\uff09\u4e3a\u786e\u4fdd\u6210\u5206\u5747\u5300\uff0c\u6210\u5206\u7c89\u672b\u9700\u8981\u63d0\u524d\u5145\u5206\u6df7\u5408\uff0c\u9700\u8981\u82b1\u8d39\u5927\u91cf\u65f6\u95f4\u3002ii\uff09\u4e3a\u907f\u514d\u6210\u5206\u7684\u7a81\u7136\u53d8\u5316\u5bfc\u81f4\u7684\u53f0\u9636\u754c\u9762\u5f00\u88c2\u3002\u53ef\u80fd\u9700\u8981\u5bf9LPBF\u8bbe\u7f6e\u8fdb\u884c\u4fee\u6539\uff0c\u5c06\u7ed9\u7c89\u7cfb\u7edf\u4ece\u56fa\u5b9a\u7684\u4f9b\u6599\u4ed3\u6539\u9020\u4e3a\u5177\u6709\u591a\u4e2a\u4e0d\u540c\u7c89\u4ed3\u7684\u79fb\u52a8\u6599\u6597\uff0c\u96be\u5ea6\u8f83\u5927\u3002iii\uff09\u7f3a\u4e4f\u9002\u5f53\u7684\u6df7\u5408\u4f1a\u5bfc\u81f4\u5fae\u89c2\u7684\u5316\u5b66\u504f\u6790\u3002\u7531\u4e8e\u5bf9\u6ce2\u957f\u5927\u4e8e1\u00b5m(LPBF\u4e2d\u6700\u5e38\u7528\u7684\u6ce2\u957f)\u7684\u6fc0\u5149\u5668\u5177\u6709\u8f83\u9ad8\u7684\u53cd\u5c04\u7387\uff0c\u70ed\u5bfc\u7387\u548c\u6613\u5f62\u6210\u6c27\u5316\u7269\uff0c\u4f7f\u7528LPBF\u5236\u9020\u94dc\u53ca\u5176\u5408\u91d1\u6781\u5177\u6311\u6218\u6027\u3002\u56e0\u6b64\uff0c\u6709\u5fc5\u8981\u63a2\u7d22\u4fdd\u8bc1\u94dc\u5408\u91d1\u53ef\u9760\u6253\u5370\u7684\u6700\u4f4e\u5408\u91d1\u542b\u91cf\u3002<\/p>\n<p><strong>\u4e8c\u3001\u3010\u6210\u679c\u63a0\u5f71\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c\u5357\u6d0b\u7406\u5de5\u5927\u5b66Siyuan Wei\uff0c\u65b0\u52a0\u5761\u6750\u6599\u7814\u7a76\u4e0e\u5de5\u7a0b\u7814\u7a76\u6240\u79d1\u5b66\u3001\u6280\u672f\u4e0e\u7814\u7a76\u5c40Pei Wang\u8bbe\u8ba1\u4e86\u4e00\u79cd\u7b80\u5355\u6709\u6548\u7684\u6210\u5206\u68af\u5ea6\u5408\u91d1\u5236\u5907\u65b9\u6cd5\uff0c\u5e76\u6210\u529f\u5236\u5907\u51fa\u4e86Ni\u542b\u91cf\u57280.6 ~ 9.8 wt.%\u8303\u56f4\u5185\u7684\u5747\u5300\u68af\u5ea6\u4e8c\u5143Cu-Ni\u5408\u91d1\u3002\u8fd9\u4e9b\u5408\u91d1\u5728\u7ed3\u6784\u548c\u529f\u80fd\u4e0a\u90fd\u6709\u91cd\u8981\u7684\u5e94\u7528\uff0c\u5e76\u4e14\u4f7f\u7528LPBF\u5236\u9020\u7684Cu-Ni\u5408\u91d1\u5728\u53ef\u5370\u5237\u6027\u3001\u5fae\u89c2\u7ed3\u6784\u548c\u673a\u68b0\u6027\u80fd\u4e0a\u4ecd\u6709\u6781\u5927\u7684\u63a2\u7d22\u7a7a\u95f4\u3002\u901a\u8fc7\u5236\u5907\u5177\u6709\u8fde\u7eed\u6210\u5206\u68af\u5ea6\u7684\u5408\u91d1\u76f8\u6bd4\u4e8e\u968f\u673a\u6210\u5206\u5408\u91d1\uff0c\u53ef\u4ee5\u66f4\u51c6\u786e\u5730\u83b7\u5f97\u4e34\u754c\u5408\u91d1\u5143\u7d20Ni\u7684\u542b\u91cf\u3002\u5728\u6b64\u57fa\u7840\u4e0a\uff0c\u7814\u7a76\u8005\u91c7\u7528LPBF\u5236\u5907\u4e86\u5177\u4f53\u7ec4\u6210\u4e3aCu-7.6Ni-3Al (wt.%)\u7684\u5408\u91d1\uff0c\u5e76\u5bf9\u5176\u8fdb\u884c\u4e86\u65f6\u6548\u8868\u5f81\u3002<\/p>\n<p>\u76f8\u5173\u7814\u7a76\u5de5\u4f5c\u4ee5\u201c<strong>Laser powder bed fusion of a Cu-Ni-Al alloy using the compositional grading approach<\/strong>\u201d\u4e3a\u9898\u53d1\u8868\u5728\u56fd\u9645\u9876\u7ea7\u671f\u520a<em>Scripta Materialia<\/em>\u4e0a\u3002<\/p>\n<p><strong><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-250726\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/1-7.png\" alt=\"\" width=\"1100\" height=\"533\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/1-7.png 1100w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/1-7-300x145.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/1-7-768x372.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/1-7-1024x496.png 1024w\" sizes=\"(max-width: 1100px) 100vw, 1100px\" \/>\u00a0<\/strong><strong>\u4e09\u3001\u3010\u6838\u5fc3\u521b\u65b0\u70b9\u3011<\/strong><\/p>\n<p>\u91c7\u7528\u6539\u8fdb\u7684\u6fc0\u5149\u7c89\u672b\u5e8a\u7194\u5408(LPBF)\u6280\u672f\u5236\u5907\u4e86\u4e00\u79cd\u6210\u5206\u68af\u5ea6\u7684Cu-Ni\u5408\u91d1\u3002\u901a\u8fc7\u5bf9\u4ece\u4e2d\u63d0\u53d6\u7684\u6837\u54c1\u8fdb\u884c\u663e\u5fae\u7ec4\u7ec7\u548c\u529b\u5b66\u8868\u5f81\uff0c\u786e\u5b9a\u4e86\u6dfb\u52a07.6 wt.%Ni\u7684Cu-Ni\u5408\u91d1\u662f\u4f7f\u7528LPBF\u83b7\u5f97\u65e0\u88c2\u7eb9\u548c\u63a5\u8fd1\u5168\u81f4\u5bc6\u7684\u8bd5\u6837\u6240\u9700\u7684\u6700\u5c0f\u503c\u3002\u968f\u540e\uff0c\u5728Cu-7.6 wt.%\u5408\u91d1\u4e2d\u52a0\u51653wt .% Al\uff0c\u4f7fLPBF Cu-Ni-Al\u5408\u91d1\u5728\u65f6\u6548\u8fc7\u7a0b\u4e2d\u6790\u51faNi<sub>3<\/sub>Al\uff0c\u4ece\u800c\u8017\u5c3d\u57fa\u4f53\u4e2d\u7684\u6eb6\u8d28Ni\u539f\u5b50\uff0c\u540c\u65f6\u63d0\u9ad8\u4e86\u5408\u91d1\u7684\u5f3a\u5ea6\u548c\u5bfc\u7535\u6027\u3002\u5c55\u793a\u4e86\u901a\u8fc7\u5236\u9020\u6210\u5206\u68af\u5ea6\u5408\u91d1\u548c\u968f\u540e\u7684\u5408\u91d1\u8bbe\u8ba1\u4ee5\u83b7\u5f97\u6700\u4f73\u6027\u80fd\u7ec4\u5408\u6765\u9ad8\u901a\u91cf\u7b5b\u9009\u9002\u5408LPBF\u7684\u5408\u91d1\u7684\u6f5c\u529b\u3002<\/p>\n<p><strong>\u00a0<\/strong><\/p>\n<p><strong>\u00a0<\/strong><strong>\u56db\u3001\u3010\u6570\u636e\u6982\u89c8\u3011 <\/strong><\/p>\n<p><strong>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-250727\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/2-6.png\" alt=\"\" width=\"1074\" height=\"566\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/2-6.png 1074w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/2-6-300x158.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/2-6-768x405.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/2-6-1024x540.png 1024w\" sizes=\"(max-width: 1074px) 100vw, 1074px\" \/><\/strong><\/p>\n<p>\u56fe1 (a)\u672c\u7814\u7a76\u4e2d\u7528\u4e8e\u5236\u5907\u6210\u5206\u68af\u5ea6\u7684Cu-Ni\u5408\u91d1\u7684LPBF\u88c5\u7f6e\u793a\u610f\u56fe\u3002(a)\u91c7\u7528(b)\u5de5\u827a\u5236\u5907\u7684Cu-Ni\u5408\u91d1\u3002\u6807\u8bb0\u51fa\u6784\u5efa\u65b9\u5411(BD)\u3001\u68af\u5ea6\u65b9\u5411(GD)\u548c\u6a2a\u5411\u65b9\u5411(TD)\u3002<strong>\u00a0 \u00a9 2023 Acta Materialia Inc.<\/strong><\/p>\n<p><strong>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-250728\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/3-7.png\" alt=\"\" width=\"786\" height=\"755\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/3-7.png 786w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/3-7-300x288.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/3-7-768x738.png 768w\" sizes=\"(max-width: 786px) 100vw, 786px\" \/><\/strong><\/p>\n<p>\u56fe2 \u5229\u7528EDS\u7ebf\u626b\u63cf\u8fdb\u884c\u8868\u5f81\u7684\u6cbf(a)\u68af\u5ea6\u65b9\u5411(GD)\u3001(b) \u6784\u5efa\u65b9\u5411(BD)\u548c(c)\u6a2a\u5411\u65b9\u5411(TD)\u7ed8\u5236\u68af\u5ea6\u6837\u54c1\u4f4d\u7f6e\u7684Ni\u542b\u91cf\u56fe\u3002(a)\u4e2d\u7684\u63d2\u56fe\u662fCu(\u7ea2\u8272)\u548cNi(\u84dd\u8272)\u7684\u4ee3\u8868\u6027EDS\u6620\u5c04\uff0c\u4ee5\u53ca\u4e8c\u6b21\u7535\u5b50\u56fe\u50cf\u3002(d)\u4f7f\u7528\u7535\u5b50\u80cc\u6563\u5c04\u884d\u5c04(EBSD)\u83b7\u5f97\u76840.6\u30014.6\u548c7.6 wt.% Ni\u6837\u54c1\u7684\u9006\u6781\u56fe(IPFs)\u3002\u6bcf\u5f20\u56fe\u7247\u90fd\u6807\u6ce8\u4e86Ni\u7684\u542b\u91cf<strong>\u00a9 2023 Acta Materialia Inc.<\/strong><\/p>\n<p><strong>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-250729\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/4-7.png\" alt=\"\" width=\"489\" height=\"688\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/4-7.png 489w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/4-7-213x300.png 213w\" sizes=\"(max-width: 489px) 100vw, 489px\" \/><\/strong><\/p>\n<p>\u56fe3 (a)\u786c\u5ea6\u548c\u7535\u5bfc\u7387\u968fNi\u542b\u91cf\u7684\u53d8\u5316\u3002(b) 6\u79cdCu-Ni\u5408\u91d1\u7684\u5de5\u7a0b\u5e94\u529b-\u5de5\u7a0b\u5e94\u53d8\u56fe\uff0c\u6bcf\u4e2a\u56fe\u9644\u8fd1\u90fd\u6807\u6709Ni\u542b\u91cf\uff0c\u5355\u4f4d\u4e3awt.%\u3002\u63d2\u56fe\u662f5.5\u548c7.6 wt.% Cu-Ni\u6837\u54c1\u65ad\u53e3\u7684\u4ee3\u8868\u6027\u4e8c\u6b21\u7535\u5b50\u56fe\u50cf\u3002<strong>\u00a0 \u00a9 2023 Acta Materialia Inc. <\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-250730\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/5-5.png\" alt=\"\" width=\"850\" height=\"616\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/5-5.png 850w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/5-5-300x217.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/5-5-768x557.png 768w\" sizes=\"(max-width: 850px) 100vw, 850px\" \/><\/p>\n<p>\u56fe4 (a) Cu-7.6Ni-3Al\u6837\u54c1\u5177\u6709\u4ee3\u8868\u6027\u7684\u540e\u5411\u6563\u5c04\u7535\u5b50\u56fe\u50cf\u3002(b)\u70ed\u5904\u7406\u65f6\u95f4\u4e0d\u540c\u7684Cu-7.6Ni-3Al\u6837\u54c1\u7684\u786c\u5ea6\u548c\u7535\u5bfc\u7387\u3002(c) Cu-7.6Ni\u548cCu-7.6Ni- 3al\u6837\u54c1(\u6253\u5370\u3001\u65f6\u65484 h\u548c\u65f6\u654824 h)\u7684\u5de5\u7a0b\u5e94\u529b-\u5e94\u53d8\u56fe\u3002<strong>\u00a9 2023 Acta Materialia Inc.<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-250731\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/6-4.png\" alt=\"\" width=\"950\" height=\"786\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/6-4.png 950w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/6-4-300x248.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/6-4-768x635.png 768w\" sizes=\"(max-width: 950px) 100vw, 950px\" \/>\u56fe5 (a) AP\u6837\u54c1\u7684\u626b\u63cf\u900f\u5c04\u7535\u5b50\u663e\u5fae\u955c(STEM)\u4eae\u573a(BF)\u56fe\u50cf\u548c(b)\u5176\u5bf9\u5e94\u7684\u9009\u5b9a\u533a\u57df\u7535\u5b50\u884d\u5c04\u56fe(SAED)\u6a21\u5f0f\u3002(c-d)\u8001\u53164 h\u6837\u54c1\u7684STEM-BF\u3001SAED\u548cTEM-\u6697\u573a(DF)\u56fe\u50cf\u3002(f-h) 24h\u8001\u5316\u6837\u54c1\u7684STEM-BF\u3001SAED\u548cTEM-DF\u56fe\u50cf\u3002\u8bf7\u6ce8\u610f\uff0c(e)\u548c(h)\u7684DF\u56fe\u50cf\u5206\u522b\u4f7f\u7528(d)\u548c(g)\u4e2d\u9ec4\u8272\u5706\u5708\u7a81\u51fa\u7684\u70b9\u83b7\u5f97\u3002\u5728\u6bcf\u4e2aSAED\u6a21\u5f0f\u4e2d\u6807\u8bb0\u533a\u57df\u8f74\u3002<\/p>\n<p><strong>\u00a0<\/strong><\/p>\n<p><strong>\u4e94\u3001\u3010\u6210\u679c\u542f\u793a\u3011<\/strong><\/p>\n<p>\u5728LPBF\u4e2d\u4f7f\u7528\u6539\u8fdb\u7684\u7c89\u672b\u4f9b\u5e94\u7cfb\u7edf\u5236\u5907\u4e86Ni\u542b\u91cf\u57280.6 ~ 9.8 wt.%\u4e4b\u95f4\u7684\u6210\u5206\u68af\u5ea6Cu-Ni\u5408\u91d1\u3002\u4ece\u68af\u5ea6\u5408\u91d1\u4e2d\u63d0\u53d6\u7684\u6837\u54c1\u7684\u663e\u5fae\u7ec4\u7ec7\u548c\u529b\u5b66\u7279\u6027\u8868\u660e\uff0c\u5728Cu\u4e2d\u6dfb\u52a0\u6700\u5c0f\u76847.6 wt.%\u7684Ni\u662f\u5236\u9020\u65e0\u88c2\u7eb9\u548c\u63a5\u8fd1\u5168\u81f4\u5bc6\u5408\u91d1\u7684\u5fc5\u8981\u6761\u4ef6\u3002Cu-7.6 wt.%\u5408\u91d1\u5177\u6709\u826f\u597d\u7684\u5f3a\u5ea6\u548c\u5ef6\u5c55\u6027\uff0c\u4f46\u5176\u4f53\u7535\u963b\u8f83\u5dee\u3002\u56e0\u6b64\uff0c\u52a0\u51653wt .%\u7684Al\uff0c\u5728LPBF\u540e\u65f6\u6548\u8fc7\u7a0b\u4e2d\u5f62\u6210Ni<sub>3<\/sub>Al\u6790\u51fa\u7269\uff0c\u663e\u8457\u63d0\u9ad8\u4e86\u786c\u5ea6\u3001\u5f3a\u5ea6\u548c\u5bfc\u7535\u6027\u3002\u9664\u4e86\u6790\u51fa\u786c\u5316\u5916\uff0c\u4f4d\u9519\u5bc6\u5ea6\u548c\u6c27\u5316\u7269\u9897\u7c92\u7684\u589e\u52a0\u4e5f\u6709\u52a9\u4e8eLPBF\u548c\u65f6\u6548\u5408\u91d1\u7684\u5f3a\u5ea6\u3002<\/p>\n<p><strong>\u00a0<\/strong><\/p>\n<p><strong>\u539f\u6587\u8be6\u60c5<\/strong>\uff1ahttps:\/\/www.sciencedirect.com\/science\/article\/abs\/pii\/S1359646223001653<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u5f20\u7199\u7199 \u4e00\u3001 \u3010\u5bfc\u8bfb\u3011\u00a0 \u589e\u6750\u5236\u9020(AM)\u6709\u9650\u7684\u9002\u7528\u5408\u91d1\u6570\u91cf\u4e25\u91cd\u963b\u788d\u4e86\u8be5\u6280\u672f\u7684\u5e7f\u6cdb\u5e94\u7528\u3002\uff0c\u56e0\u6b64\u9700\u8981\u9ad8\u901a\u91cf\u65b9\u6cd5\u8fdb\u884c\u6210\u5206\u7b5b\u9009\u3002\u5176\u4e2d\uff0c\u76f4\u63a5\u80fd\u91cf\u6c89\u79ef(DED)\u548c\u6fc0\u5149\u7c89\u672b&#8230;<\/p>\n","protected":false},"author":39557,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[2],"tags":[],"class_list":["post-250725","post","type-post","status-publish","format-standard","hentry","category-keji"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/250725"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/39557"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=250725"}],"version-history":[{"count":1,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/250725\/revisions"}],"predecessor-version":[{"id":250732,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/250725\/revisions\/250732"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=250725"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=250725"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=250725"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}