{"id":251196,"date":"2023-06-12T06:59:48","date_gmt":"2023-06-11T22:59:48","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=251196"},"modified":"2023-06-11T21:01:31","modified_gmt":"2023-06-11T13:01:31","slug":"%e9%99%b6%e5%8f%8b%e5%8d%8e%e5%9b%a2%e9%98%9fangew%ef%bc%9a%e9%80%9a%e8%bf%87%e9%93%9d%e5%82%ac%e5%8c%96%e4%ba%8c%e7%a1%ab%e4%bb%a3%e5%86%85%e9%85%af%e5%bc%80%e7%8e%af%e8%81%9a%e5%90%88%e5%ae%9e","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=251196","title":{"rendered":"\u9676\u53cb\u534e\u56e2\u961fAngew\uff1a\u901a\u8fc7\u94dd\u50ac\u5316\u4e8c\u786b\u4ee3\u5185\u916f\u5f00\u73af\u805a\u5408\u5b9e\u73b0\u7684\u6027\u80fd\u4f18\u52bf\u578b\u7acb\u4f53\u89c4\u5219\u53ef\u56de\u6536\u5851\u6599"},"content":{"rendered":"<p><strong>\u4e00\u3001\u3010\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p>\u5851\u6599\uff0c\u662f\u65e0\u5904\u4e0d\u5728\u7684\u8010\u7528\u6750\u6599\u3002\u7136\u800c\uff0c\u5851\u6599\u4ea7\u751f\u7684\u5e9f\u7269\u7f3a\u4e4f\u540e\u7eed\u7684\u7ba1\u7406\uff0c\u52a0\u4e4b\u5176\u751f\u4ea7\u901f\u5ea6\u8fc7\u5feb\uff0c\u7531\u6b64\u4ea7\u751f\u7684\u4e0d\u53ef\u964d\u89e3\u7684\u5851\u6599\u5e9f\u7269\u5feb\u901f\u7d2f\u79ef\uff0c\u5bf9\u73af\u5883\u4ea7\u751f\u4e86\u4e25\u91cd\u7684\u8d1f\u9762\u5f71\u54cd\u3002\u89e3\u51b3\u5851\u6599\u53ef\u6301\u7eed\u6027\u53d1\u5c55\u6210\u4e3a\u6784\u5efa\u7eff\u8272\u751f\u6001\u73af\u5883\u7684\u6311\u6218\uff0c\u4e00\u79cd\u6f5c\u5728\u7684\u7eff\u8272\u73af\u4fdd\u65b9\u6cd5\u662f\u7528\u5316\u5b66\u53ef\u56de\u6536\u7684\u805a\u5408\u7269\u53d6\u4ee3\u5f53\u524d\u7684\u805a\u5408\u7269\uff0c\u8fd9\u4e9b\u805a\u5408\u7269\u53ef\u4ee5\u89e3\u805a\u6210\u5176\u7ec4\u6210\u5355\u4f53\uff0c\u4ece\u800c\u5b9e\u73b0\u7f29\u77ed\u805a\u5408\u7269\u5faa\u73af\u7684\u751f\u547d\u5468\u671f\u3002\u6700\u5148\u8fdb\u7684\u53ef\u56de\u6536\u805a\u5408\u7269\u5728\u6027\u80fd\uff08\u7ed3\u6676\u5ea6\u3001\u5e94\u529b\/\u5e94\u53d8\u7b49\uff09\u4e0a\u4e0e\u4f20\u7edf\u5546\u4e1a\u5316\u7684\u805a\u5408\u7269\u76f8\u5f62\u89c1\u7ecc\uff0c\u4f20\u7edf\u805a\u5408\u7269\u901a\u5e38\u53d7\u5230\u53ef\u56de\u6536\u5851\u6599\u4e2d\u89e3\u805a\u6027\/\u6027\u80fd\u4e4b\u95f4\u7684\u6743\u8861\u9650\u5236\u3002\u56e0\u6b64\uff0c\u751f\u4ea7\u5316\u5b66\u53ef\u56de\u6536\u805a\u5408\u7269\u81f3\u5173\u91cd\u8981\uff0c\u8fd9\u4e9b\u805a\u5408\u7269\u5177\u6709\u4e0e\u4f20\u7edf\u805a\u70ef\u70c3\u76f8\u5f53\u7684\u6027\u80fd\uff0c\u540c\u65f6\u5728\u62a5\u5e9f\u65f6\u89e3\u805a\u6210\u5176\u7ec4\u6210\u5355\u4f53\uff0c\u56e0\u6b64\u9700\u8981\u5728\u53ef\u56de\u6536\u6027\u548c\u8010\u7528\u6027\u4e4b\u95f4\u53d6\u5f97\u72ec\u7279\u7684\u5e73\u8861\u3002\u5728\u8fd9\u65b9\u9762\uff0c\u5316\u5b66\u53ef\u56de\u6536\u7684\u7acb\u4f53\u590d\u5408\u805a\u5408\u7269\u6781\u4e3a\u7f55\u89c1\u3002<\/p>\n<p>\u8102\u80aa\u65cf\u805a\u786b\u916f\u56e0\u5176\u7279\u6027\uff0c\u6700\u8fd1\u5f15\u8d77\u4e86\u7814\u7a76\u4eba\u5458\u76f8\u5f53\u5927\u7684\u5174\u8da3\u3002\u76f4\u5230\u6700\u8fd1\uff0c\u4e8c\u786b\u4ee3\u5185\u916f\uff08\u5373\u4e8c\u5185\u916f\uff08\u5373\u4e59\u4ea4\u916f\u3001\u4e19\u4ea4\u916f\u7c7b\u4f3c\u7269\uff09\u624d\u88ab\u63a2\u7d22\u4e3a\u53ef\u56de\u6536\u7684\u805a\u786b\u916f\u3002\u4e8c\u786b\u4ee3\u5185\u916f\u7684\u89e3\u805a\u805a\u5408\u7269\u901a\u5e38\u540c\u65f6\u8868\u73b0\u51fa\u9ad8\u805a\u5408\u6027\u548c\u89e3\u805a\u6027\uff0c\u901a\u5e38\u5728\u4e00\u79cd\u805a\u5408\u7269\u7ed3\u6784\u4e2d\u76f8\u4e92\u51b2\u7a81\u3002\u7136\u800c\uff0c\u8fd9\u79cd\u65b9\u6cd5\u6709\u5176\u5c40\u9650\u6027\u3002\u6b64\u5916\uff0c\u91d1\u5c5e\u50ac\u5316\u662f\u63d0\u4f9b\u7acb\u4f53\u9009\u62e9\u6027\u805a\u5408\u7684\u4e00\u79cd\u4e3b\u8981\u7b56\u7565\uff0c\u4e8c\u786b\u4ee3\u5185\u916f\u7684\u5f00\u53d1\u4ecd\u7136\u4e0d\u8db3\uff0c\u5176\u4e2d\u786b\u4e2d\u6bd2\u5bf9\u91d1\u5c5e\u57fa\u50ac\u5316\u5242\u63d0\u51fa\u4e86\u91cd\u5927\u6311\u6218\u3002\u603b\u4f53\u800c\u8a00\uff0c\u5f00\u53d1\u50ac\u5316\u9a71\u52a8\u6280\u672f\u4ee5\u751f\u4ea7\u6027\u80fd\u4f18\u8d8a\u7684\u7acb\u4f53\u89c4\u5219\uff0c\u5bf9\u4e8e\u6fc0\u52b1\u53ef\u56de\u6536\u805a\u786b\u916f\uff0c\u63d0\u9ad8\u5851\u6599\u53ef\u6301\u7eed\u6027\u81f3\u5173\u91cd\u8981\u3002<\/p>\n<p><strong>\u4e8c\u3001\u3010\u6210\u679c\u63a0\u5f71\u3011<\/strong><\/p>\n<p>\u5316\u5b66\u53ef\u56de\u6536\u805a\u5408\u7269\u53ef\u4ee5\u89e3\u805a\u6210\u5176\u7ec4\u6210\u5355\u4f53\uff0c\u662f\u66ff\u4ee3\u4e0d\u53ef\u56de\u6536\u77f3\u6cb9\u884d\u751f\u5851\u6599\u7684\u65b0\u65b9\u5f0f\u3002\u7136\u800c\uff0c\u53ef\u89e3\u805a\u805a\u5408\u7269\u7684\u7269\u7406\u6027\u80fd\u548c\u673a\u68b0\u5f3a\u5ea6\u901a\u5e38\u4e0d\u8db3\u4ee5\u6ee1\u8db3\u5b9e\u9645\u5e94\u7528\u3002\u5728\u8fd9\u91cc\uff0c\u4e2d\u79d1\u9662\u957f\u6625\u5e94\u5316\u6240\u9676\u53cb\u534e\u56e2\u961f\u8bc1\u660e\u4e86\u901a\u8fc7\u9002\u5f53\u7684\u914d\u4f53\u8bbe\u8ba1\u548c\u4fee\u9970\uff0c\u94dd\u914d\u5408\u7269\u53ef\u4ee5\u50ac\u5316\u4e8c\u786b\u4ee3\u5185\u916f\u7684\u7acb\u4f53\u4fdd\u7559\u5f00\u73af\u805a\u5408\uff0c\u4ea7\u751f\u6469\u5c14\u8d28\u91cf\u9ad8\u8fbe45.5 kDa\u7684\u9ad8\u5ea6\u7b49\u540c\u89c4\u805a\u786b\u916f\u3002\u8fd9\u79cd\u6750\u6599\u53ef\u4ee5\u5f62\u6210\u6676\u4f53\u7acb\u4f53\u7edc\u5408\u7269\uff0c\u5177\u6709Tm94.5\u00b0C\uff0c\u673a\u68b0\u6027\u80fd\u53ef\u4e0e\u77f3\u6cb9\u57fa\u4f4e\u5bc6\u5ea6\u805a\u4e59\u70ef\u76f8\u5ab2\u7f8e\u3002\u5c06\u805a\u786b\u916f\u66b4\u9732\u4e8e\u7528\u4e8e\u5408\u6210\u5b83\u7684\u94dd\u9884\u50ac\u5316\u5242\u4e2d\uff0c\u5bfc\u81f4\u89e3\u805a\u4e3a\u539f\u59cb\u624b\u6027\u4e8c\u786b\u4ee3\u5185\u916f\u3002\u5b9e\u9a8c\u548c\u8ba1\u7b97\u7814\u7a76\u8868\u660e\uff0c\u94dd\u914d\u5408\u7269\u4e0e\u786b\u5316\u7269\u5408\u6210\u7269\u8d28\u5177\u6709\u9002\u5f53\u7684\u7ed3\u5408\u4eb2\u548c\u529b\uff0c\u4ece\u800c\u907f\u514d\u4e86\u50ac\u5316\u5242\u4e2d\u6bd2\u5e76\u6700\u5927\u9650\u5ea6\u5730\u51cf\u5c11\u4e86\u4f7f\u7528\u5176\u4ed6\u91d1\u5c5e\u50ac\u5316\u5242\u65e0\u6cd5\u5b9e\u73b0\u7684\u5dee\u5411\u5f02\u6784\u5316\u53cd\u5e94\u3002\u603b\u4f53\u800c\u8a00\uff0c\u94dd\u50ac\u5316\u63d0\u4f9b\u4e86\u6027\u80fd\u4f18\u52bf\u7684\u7acb\u4f53\u53ef\u56de\u6536\u5851\u6599\uff0c\u4f5c\u4e3a\u77f3\u5316\u5851\u6599\u7684\u6709\u524d\u9014\u7684\u66ff\u4ee3\u54c1\uff0c\u4ece\u800c\u6fc0\u52b1\u63d0\u9ad8\u5851\u6599\u7684\u53ef\u6301\u7eed\u6027\u3002\u8be5\u9879\u5de5\u4f5c\u4ee5\u6807\u9898\u4e3a\uff1a\u201cPerformance-Advantaged Stereoregular Recyclable Plastics Enabled by Aluminum-Catalytic Ring-Opening Polymerization of Dithiolactone\u201d\uff0c\u53d1\u8868\u5728\u671f\u520aAngew\u4e0a\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-251197\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/0-10.png\" alt=\"\" width=\"1485\" height=\"458\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/0-10.png 1485w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/0-10-300x93.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/0-10-768x237.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/0-10-1024x316.png 1024w\" sizes=\"(max-width: 1485px) 100vw, 1485px\" \/><\/p>\n<p><strong>\u4e09\u3001\u3010\u6838\u5fc3\u521b\u65b0\u70b9\u3011<\/strong><\/p>\n<p>1.\u9996\u5148\uff0c\u6839\u636e\u8f6f\u786c\u9178\u78b1\uff08HSAB\uff09\u7406\u8bba\uff0c\u9009\u62e9\u8f83\u786c\u7684\u91d1\u5c5e\u53ef\u4ee5\u964d\u4f4e\u5176\u4e0e\u8f83\u8f6f\u7684\u786b\u5316\u7269\u94fe\u7aef\u7684\u5f3a\u7ed3\u5408\u4eb2\u548c\u529b\uff0c\u4ece\u800c\u907f\u514d\u50ac\u5316\u5242\u4e2d\u6bd2\u3002<\/p>\n<p>2.\u5176\u6b21\uff0c\u9002\u5f53\u7684\u914d\u4f53\u8bbe\u8ba1\u548c\u4fee\u9970\u53ef\u4ee5\u5f71\u54cd\u91d1\u5c5e\u7684\u8def\u6613\u65af\u9178\u5ea6\uff0c\u4ee5\u6700\u5927\u9650\u5ea6\u5730\u51cf\u5c11\u5dee\u5411\u5f02\u6784\u5316\u526f\u53cd\u5e94\uff0c\u4ece\u800c\u63d0\u4f9b\u6027\u80fd\u4f18\u8d8a\u7684\u7acb\u4f53\u89c4\u5219\u805a\u786b\u916f\u3002<\/p>\n<p><strong>\u56db\u3001\u3010\u6570\u636e\u6982\u89c8\u3011<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-251198\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/1-14.png\" alt=\"\" width=\"1234\" height=\"861\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/1-14.png 1234w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/1-14-300x209.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/1-14-768x536.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/1-14-1024x714.png 1024w\" sizes=\"(max-width: 1234px) 100vw, 1234px\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe1.\u5dee\u5411\u5f02\u6784\u5316\u526f\u53cd\u5e94\u53ca\u94dd\u50ac\u5316\u7b56\u7565\u7684\u63d0\u51fa\u3002\u00a92023 Angew<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-251199\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/2-13.png\" alt=\"\" width=\"816\" height=\"327\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/2-13.png 816w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/2-13-300x120.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/2-13-768x308.png 768w\" sizes=\"(max-width: 816px) 100vw, 816px\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe2.\u57fa\u4e8e\u76f8\u540c\u914d\u4f53\u7684\u4e0d\u540c\u91d1\u5c5e\u50ac\u5316\u5242\u7684\u6ce2\u51fd\u6570\u5206\u6790\u4e0b\u8ba1\u7b97CCA\u3002\u00a92023 Angew<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-251200\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/3-15.png\" alt=\"\" width=\"1590\" height=\"688\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/3-15.png 1590w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/3-15-300x130.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/3-15-768x332.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/3-15-1024x443.png 1024w\" sizes=\"(max-width: 1590px) 100vw, 1590px\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe3.\uff08A\uff09\u94dd\u50ac\u5316\u5242\u7684\u7b5b\u9009\u3002\uff08B\uff09\u5355\u4f53\u7684\u7ed3\u6784\u3002\uff08C\uff09\u5f15\u53d1\u5242\u7684\u7ed3\u6784\u3002\u00a92023 Angew<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-251201\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/4-14.png\" alt=\"\" width=\"1345\" height=\"555\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/4-14.png 1345w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/4-14-300x124.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/4-14-768x317.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/4-14-1024x423.png 1024w\" sizes=\"(max-width: 1345px) 100vw, 1345px\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe4. \uff08A\uff09\u50ac\u5316\u5242\u7684\u53d6\u4ee3\u57fa\u548c\u9aa8\u67b6\u8fde\u63a5\u57fa\u5bf9\u03b1-\u78b3\u5171\u632f\u7684\u5f71\u54cd\u3002\uff08B\uff09 \u57fa\u4e8e\u4e00\u9636\u9a6c\u5c14\u53ef\u592b\u7edf\u8ba1\uff0c\u5168\u540c\u7acb\u6784D-PTEG\u7684<sup>13<\/sup>C NMR\u5149\u8c31\u3002\u00a92023 Angew<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-251202\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/5-10.png\" alt=\"\" width=\"1085\" height=\"855\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/5-10.png 1085w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/5-10-300x236.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/5-10-768x605.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/5-10-1024x807.png 1024w\" sizes=\"(max-width: 1085px) 100vw, 1085px\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe5. \uff08R\uff0cR\uff09-TEG\u7684\u94dd\u50ac\u5316\u7acb\u4f53\u4fdd\u6301ROP\u3002\u00a92023 Angew<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-251203\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/6-8.png\" alt=\"\" width=\"657\" height=\"780\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/6-8.png 657w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/6-8-253x300.png 253w\" sizes=\"(max-width: 657px) 100vw, 657px\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe6. (A)\uff08R\uff0cR\uff09-TEG\u53ef\u4ee5\u805a\u5408\u6210\u9ad8\u5ea6\u5168\u540c\u7acb\u6784\u7684\u7ed3\u6676\u805a\u786b\u916f\u5e76\u5316\u5b66\u518d\u5faa\u73af\u6210\u624b\u6027\u5355\u4f53\u3002(B)\u8d77\u59cb\u7684\uff08R\uff0cR\uff09-TEG\uff08\u9876\u90e8\uff09\u3001\u6765\u81ea\u901a\u8fc7DMAP\u89e3\u805a\u7684D-PTEG\u7684\u518d\u5faa\u73af\u7684\u5916\u6d88\u65cb-TEG\uff08\u4e2d\u4e0a\u90e8\uff09\u3001\u6765\u81ea\u901a\u8fc72c\u89e3\u805a\u7684D-PTEG\u7684\u518d\u5faa\u73af\u7684\uff08R\uff0cR\uff09-TEG\uff08\u4e2d\u4e0b\u90e8\uff09\u548cD-PTEG\uff08\u5e95\u90e8\uff09\u5728CDCl 3\u4e2d\u76841H NMR\u5149\u8c31\u7684\u53e0\u52a0\u3002(C)\u901a\u8fc7DMAP\u89e3\u805a\u6765\u81eaD-PTEG\u7684\u518d\u5faa\u73af\u7684\u5916\u6d88\u65cb-TEG\uff08\u9876\u90e8\uff09\u3001\u901a\u8fc72c\u89e3\u805a\u6765\u81eaD-PTEG\u7684\u518d\u5faa\u73af\u7684\uff08R\uff0cR\uff09-TEG\uff08\u4e2d\u95f4\uff09\u548c\u901a\u8fc72c\u89e3\u805a\u6765\u81eaL-PTEG\u7684\u518d\u5faa\u73af\u7684\uff08S\uff0cS\uff09-TEG\uff08\u5e95\u90e8\uff09\u7684HPLC\u8272\u8c31\u56fe\u7684\u91cd\u53e0\u56fe\u3002\u00a92023 Angew<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-251204\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/7-4.png\" alt=\"\" width=\"811\" height=\"567\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/7-4.png 811w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/7-4-300x210.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/7-4-768x537.png 768w\" sizes=\"(max-width: 811px) 100vw, 811px\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe7. TEG\u9009\u62e9\u6027ROP\u7684\u91cf\u5b50\u5316\u5b66\u6a21\u62df\u3002\u00a92023 Angew<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-251205\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/8-1.png\" alt=\"\" width=\"819\" height=\"571\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/8-1.png 819w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/8-1-300x209.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/05\/8-1-768x535.png 768w\" sizes=\"(max-width: 819px) 100vw, 819px\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe8. (A)\uff08a\uff09\u65e0\u89c4\u7acb\u6784PTEG\uff08Mn=19.9 kg mol<sup>-1<\/sup>\uff09\uff0c\uff08b\uff09D-PTEG\uff08Mn=18.9 kg mol<sup>-1<\/sup>\uff09\uff0c\uff08c\uff09L-PTEG\uff08Mn=17.6 kg mol<sup>-1<\/sup>\uff09\u548c\uff08d\uff09\u4e24\u79cd\u805a\u5408\u7269\u7684\u7acb\u4f53\u7edc\u5408\u6df7\u5408\u7269\u7684DSC\u70ed\u5206\u6790\u56fe\u3002(B)D-PTEG\u3001L-PTEG\u548csc-PTEG\u7684\u7c89\u672bXRD\u56fe\u8c31\u3002(C)\u4f5c\u4e3a\u54d1\u94c3\u5f62\u8bd5\u6837\u7684\u5168\u540c\u7acb\u6784PTEG\u7684\u7167\u7247\u548c\u5168\u540c\u7acb\u6784PTEG\u3002\u00a92023 Angew<\/p>\n<p><strong>\u4e94\u3001\u3010\u6210\u679c\u542f\u793a\u3011<\/strong><\/p>\n<p>\u5728\u672c\u6587\u4e2d\uff0c\u516c\u5f00\u4e86\u4e00\u79cd\u6709\u6548\u7684\u91d1\u5c5e\u50ac\u5316\u4e8c\u786b\u4ee3\u5185\u916f\u7684\u7acb\u4f53\u4fdd\u7559 ROP\uff0c\u4ece\u800c\u4ea7\u751f\u4e86\u6027\u80fd\u4f18\u8d8a\u7684\u7b49\u89c4\u805a\u786b\u916f\u3002\u4e3a\u4e86\u5efa\u7acb\u8fd9\u79cd\u65b9\u6cd5\uff0c\u63d0\u51fa\u4e86\u4e24\u4e2a\u5047\u8bbe\u3002\u53d1\u73b0\u4e86\u6709\u673a\u91d1\u5c5e\u94dd\u50ac\u5316\u5242\uff0c\u7528\u4e8e\u4e8c\u786b\u4ee3\u5185\u916f\u7684\u5316\u5b66\u9009\u62e9\u6027\u805a\u5408\uff0c\u5176\u7279\u5f81\u662f\u6700\u5c0f\u7684\u5dee\u5411\u5f02\u6784\u5316\u3002\u901a\u8fc7\u9002\u5f53\u7684\u914d\u4f53\u8bbe\u8ba1\u548c\u4fee\u9970\uff0c \u94dd\u50ac\u5316\u5242\u80fd\u591f\u751f\u4ea7\u51fa\u9ad8\u5ea6\u7b49\u89c4\u7684\u7acb\u4f53\u7edc\u5408\u805a\u786b\u916f\uff0c\u5e76\u83b7\u5f97\u4e86\u9ad8\u5206\u5b50\u91cf\u805a\u5408\u7269\u3002\u5b9e\u9a8c\u548c\u8ba1\u7b97\u7814\u7a76\u8868\u660e\uff0c\u94dd\u914d\u5408\u7269\u4e0e\u786b\u5316\u7269\u5408\u6210\u7269\u79cd\u5177\u6709\u9002\u5f53\u7684\u7ed3\u5408\u4eb2\u548c\u529b\uff0c\u907f\u514d\u4e86\u50ac\u5316\u5242\u4e2d\u6bd2\u5e76\u6700\u5927\u9650\u5ea6\u5730\u51cf\u5c11\u4e86\u5dee\u5411\u5f02\u6784\u5316\u53cd\u5e94\uff0c\u8fd9\u662f\u4f7f\u7528\u5176\u4ed6\u91d1\u5c5e\u50ac\u5316\u5242\u65e0\u6cd5\u5b9e\u73b0\u7684\u3002\u6240\u83b7\u5f97\u7684\u4e8c\u786b\u4ee3\u5185\u916f\u57fa\u5851\u6599\u662f\u4e00\u79cd\u575a\u97e7\u7684\u534a\u7ed3\u6676\u6750\u6599\uff0c\u5e76\u8868\u73b0\u51fa\u5b8c\u5168\u7684\u53ef\u56de\u6536\u6027\uff0c\u4f7f\u5851\u6599\u53ef\u4ee5\u56de\u6536\u5e76\u518d\u6b21\u4f7f\u7528\u3002\u8fd9\u79cd\u9ad8\u6548\u7684\u94dd\u50ac\u5316\u6280\u672f\u548c\u6700\u7ec8\u4ea7\u54c1\u4f53\u73b0\u4e86\u4ece\u6447\u7bee\u5230\u6447\u7bee\u7684\u5faa\u73af\uff0c\u4e3a\u751f\u4ea7\u6027\u80fd\u4f18\u8d8a\u7684\u53ef\u56de\u6536\u5851\u6599\u63d0\u4f9b\u4e86\u65b0\u7684\u673a\u4f1a\u3002<\/p>\n<p><strong>\u539f\u6587\u8be6\u60c5\uff1a<\/strong>https:\/\/onlinelibrary.wiley.com\/doi\/abs\/10.1002\/ange.202302898<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u4e00\u3001\u3010\u5bfc\u8bfb\u3011 \u5851\u6599\uff0c\u662f\u65e0\u5904\u4e0d\u5728\u7684\u8010\u7528\u6750\u6599\u3002\u7136\u800c\uff0c\u5851\u6599\u4ea7\u751f\u7684\u5e9f\u7269\u7f3a\u4e4f\u540e\u7eed\u7684\u7ba1\u7406\uff0c\u52a0\u4e4b\u5176\u751f\u4ea7\u901f\u5ea6\u8fc7\u5feb\uff0c\u7531\u6b64\u4ea7\u751f\u7684\u4e0d\u53ef\u964d\u89e3\u7684\u5851\u6599\u5e9f\u7269\u5feb\u901f\u7d2f\u79ef\uff0c\u5bf9\u73af\u5883\u4ea7\u751f\u4e86\u4e25\u91cd\u7684\u8d1f\u9762\u5f71&#8230;<\/p>\n","protected":false},"author":35611,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-251196","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/251196"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/35611"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=251196"}],"version-history":[{"count":3,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/251196\/revisions"}],"predecessor-version":[{"id":251961,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/251196\/revisions\/251961"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=251196"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=251196"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=251196"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}