{"id":252479,"date":"2023-07-03T06:31:08","date_gmt":"2023-07-02T22:31:08","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=252479"},"modified":"2023-07-02T21:31:24","modified_gmt":"2023-07-02T13:31:24","slug":"scientific-reports%ef%bc%9a%e5%88%b6%e9%80%a0%e5%8a%9f%e8%83%bd%e6%a2%af%e5%ba%a6%e9%93%ac%e9%95%8d%e9%93%81%e5%90%88%e9%87%91-825-ss316l%e6%96%b0%e6%96%b9%e6%b3%95","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=252479","title":{"rendered":"Scientific Reports\uff1a\u5236\u9020\u529f\u80fd\u68af\u5ea6\u94ec\u954d\u94c1\u5408\u91d1 825\u2013SS316L\u65b0\u65b9\u6cd5"},"content":{"rendered":"<p style=\"text-align: center;\"><strong>\u4e00\u3001<\/strong> <strong>\u3010\u5bfc\u8bfb\u3011<\/strong><strong>\u00a0 <\/strong><\/p>\n<p>\u5728\u6574\u4e2a\u5386\u53f2\u4e2d\uff0c\u7406\u89e3\u548c\u64cd\u7eb5\u6750\u6599\u7684\u80fd\u529b\u5bf9\u6280\u672f\u7684\u8fdb\u6b65\u81f3\u5173\u91cd\u8981\u3002\u5982\u4eca\u7684\u79d1\u5b66\u5bb6\u548c\u5de5\u7a0b\u5e08\u4eec\u4ece\u7ecf\u6d4e\u548c\u73af\u5883\u7684\u89d2\u5ea6\u7406\u89e3\u65b0\u6750\u6599\u7684\u4ef7\u503c\u3002\u529f\u80fd\u68af\u5ea6\u6750\u6599\uff08FGMs\uff09\u662f\u96f6\u4ef6\u4e2d\u5177\u6709\u590d\u6742\u7ed3\u6784\u548c\u6781\u9ad8\u529f\u80fd\u6027\u7684\u533a\u57df\uff0c\u5176\u5143\u7d20\u7ec4\u6210\u5448\u6301\u7eed\u53d8\u5316\uff0c\u4ece\u800c\u4ea7\u751f\u65b0\u9896\u548c\u5b9a\u5236\u7684\u673a\u68b0\u6216\u70ed\u5b66\u6027\u8d28\u3002\u5f00\u53d1\u5177\u6709\u589e\u5f3a\u6027\u80fd\u5e76\u9002\u7528\u4e8e\u822a\u7a7a\u822a\u5929\u3001\u6d77\u6d0b\u3001\u6838\u5de5\u7a0b\u548c\u9ad8\u6e29\u9632\u62a4\u6d82\u5c42\u7b49\u5404\u79cd\u5e94\u7528\u7684\u6750\u6599\u80fd\u529b\uff0c\u5927\u5927\u589e\u52a0\u4e86\u5bf9FGMs\u7684\u5173\u6ce8\u3002\u5c3a\u5bf8\u548c\u7ed3\u6784\u7279\u5f81\u662f\u7528\u4e8e\u5bf9\u68af\u5ea6\u6750\u6599\u8fdb\u884c\u5206\u7c7b\u7684\u4e24\u4e2a\u56e0\u7d20\u3002\u68af\u5ea6\u53ef\u4ee5\u662f\u539a\u5b9e\u7684\u6216\u8584\u5c42\uff08\u4f8b\u5982\u8868\u9762\u6d82\u5c42\uff09\uff0c\u9700\u8981\u4e0d\u540c\u7684\u52a0\u5de5\u6280\u672f\u3002\u6839\u636e\u7ed3\u6784\u7684\u4e0d\u540c\uff0c\u5b83\u4eec\u5206\u4e3a\u8fde\u7eed\u548c\u95f4\u65ad\u4e24\u7ec4\u3002\u5728\u5177\u6709\u95f4\u65ad\u68af\u5ea6\u7684\u6750\u6599\u4e2d\uff0c\u5fae\u89c2\u7ed3\u6784\u6216\u5316\u5b66\u6210\u5206\u9010\u6e10\u53d8\u5316\uff0c\u754c\u9762\u901a\u5e38\u662f\u53ef\u89c2\u5bdf\u7684\u3002\u76f8\u53cd\uff0c\u5728\u5177\u6709\u8fde\u7eed\u68af\u5ea6\u7684\u6750\u6599\u4e2d\uff0c\u5316\u5b66\u6210\u5206\u6216\u5fae\u89c2\u7ed3\u6784\u968f\u4f4d\u7f6e\u4e0d\u65ad\u53d8\u5316\uff0c\u51e0\u4e4e\u4e0d\u53ef\u80fd\u611f\u77e5\u5230\u660e\u663e\u7684\u8fb9\u754c\u4f5c\u4e3a\u68af\u5ea6\u7ed3\u6784\u7684\u754c\u9762\u3002<\/p>\n<p style=\"text-align: center;\"><strong>\u4e8c\u3001\u3010\u6210\u679c\u63a0\u5f71\u3011<\/strong><\/p>\n<p>\u6700\u8fd1\uff0c\u5370\u5ea6\u6cf0\u7c73\u5c14\u7eb3\u5fb7\u90a6\u91d1\u5948\u5e02\u5b89\u7eb3\u5927\u5b66\u7684T. S. Senthil\u6559\u6388\u63d0\u51fa\u4e86\u4e00\u79cd\u65b0\u9896\u7684\u65b9\u6cd5\uff0c\u5229\u7528\u57fa\u4e8e\u51b7\u91d1\u5c5e\u4f20\u8f93\u7684\u7ebf\u5f27\u589e\u6750\u5236\u9020\u5de5\u827a\u6765\u5236\u9020\u529f\u80fd\u68af\u5ea6\u7684\u94ec\u954d\u94c1\u5408\u91d1 825-SS316L\u3002\u94ec\u954d\u94c1\u5408\u91d1 825\u7684\u5149\u5b66\u663e\u5fae\u56fe\u663e\u793a\u4e86\u8fde\u7eed\u548c\u95f4\u65ad\u7684\u6811\u679d\u72b6\u7ed3\u6784\u3002SS316L\u533a\u57df\u75315%\u7684\u03b4-\u94c1\u7d20\u4f53\u7ec4\u6210\uff0c\u5176\u4e2d\u4e3b\u8981\u7684\u5965\u6c0f\u4f53(\u03b3)\u6811\u679d\u72b6\u6676\u4f53\u901a\u8fc7C<sub>req<\/sub>\/N<sub>ieq<\/sub>\u6bd4\u503c\u4e3a1.305\u8fdb\u884c\u4e86\u786e\u8ba4\u3002\u529f\u80fd\u68af\u5ea6\u7684\u754c\u9762\u663e\u793a\u51fa\u90e8\u5206\u6df7\u5408\u533a\uff0c\u4ece\u7ec6\u957f\u7684\u6811\u679d\u72b6\u6676\u4f53\u8fc7\u6e21\u5230\u7ec6\u5c0f\u7684\u7b49\u8f74\u6676\u4f53\u3002\u5229\u7528\u4ece\u94ec\u954d\u94c1\u5408\u91d1 825\u3001SS316L\u548c\u754c\u9762\u533a\u57df\u63d0\u53d6\u7684\u8bd5\u6837\uff0c\u5728\u5ba4\u6e29\u4e0b\u786e\u5b9a\u4e86\u5236\u9020\u7684\u58c1\u7684\u62c9\u4f38\u6027\u80fd\u3002\u62c9\u4f38\u8bd5\u6837\u7684\u5f62\u6001\u5b66\u663e\u793a\u4e86\u663e\u8457\u7684\u5851\u6027\u53d8\u5f62\uff0c\u8868\u660e\u5c5e\u4e8e\u97e7\u6027\u7834\u574f\u3002\u901a\u8fc7\u91c7\u7528\u88c2\u7eb9\u5c16\u7aef\u5f20\u5f00\u4f4d\u79fb\uff08CTOD\uff09\u8bd5\u9a8c\uff0c\u5b9e\u9a8c\u6027\u5730\u7814\u7a76\u4e86\u58c1\u7684\u65ad\u88c2\u97e7\u6027\u3002\u65ad\u88c2\u5f62\u6001\u663e\u793a\u51fa\u4e00\u79cd\u97e7\u6027\u7834\u88c2\u6a21\u5f0f\uff0c\u88c2\u7eb9\u53d1\u5c55\u65b9\u5411\u5782\u76f4\u4e8e\u6761\u7eb9\u3002\u5143\u7d20\u6620\u5c04\u663e\u793a\u65ad\u88c2\u8868\u9762\u4e0a\u6ca1\u6709\u5143\u7d20\u504f\u6790\u7684\u8bc1\u636e\uff0c\u5143\u7d20\u5747\u5300\u5206\u6563\u3002CTOD\u503c\u5206\u522b\u5728\u94ec\u954d\u94c1\u5408\u91d1 825\u4fa7\u548cSS316L\u4fa7\u4e3a0.853\u6beb\u7c73\u548c0.873\u6beb\u7c73\u3002\u8bd5\u9a8c\u7ed3\u679c\u786e\u8ba4\uff0c\u94ec\u954d\u94c1\u5408\u91d1 825\u548cSS316L\u4e24\u4fa7\u5177\u6709\u826f\u597d\u7684\u65ad\u88c2\u97e7\u6027\u3002\u76f8\u5173\u6210\u679c\u4ee5 \u201c<strong>Mechanical, microstructural and fracture studies on Inconel 825\u2013SS316L functionally graded wall fabricated by wire arc additive manufacturing<\/strong>\u201d \u4e3a\u9898\u53d1\u8868\u5728<strong><em>Scientific Reports<\/em><\/strong>\u4e0a\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-252495\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/\u5c4f\u5e55\u622a\u56fe-2023-06-30-183054.png\" alt=\"\" width=\"907\" height=\"480\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/\u5c4f\u5e55\u622a\u56fe-2023-06-30-183054.png 907w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/\u5c4f\u5e55\u622a\u56fe-2023-06-30-183054-300x159.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/\u5c4f\u5e55\u622a\u56fe-2023-06-30-183054-768x406.png 768w\" sizes=\"(max-width: 907px) 100vw, 907px\" \/><\/p>\n<p style=\"text-align: center;\"><strong>\u00a0<\/strong><strong>\u4e09\u3001\u3010\u6838\u5fc3\u521b\u65b0\u70b9\u3011<\/strong><\/p>\n<p>\u8fd9\u9879\u7814\u7a76\u901a\u8fc7\u51b7\u91d1\u5c5e\u4f20\u8f93\u7684\u7ebf\u5f27\u589e\u6750\u5236\u9020\u5de5\u827a\u5b9e\u73b0\u529f\u80fd\u68af\u5ea6\u7684\u94ec\u954d\u94c1\u5408\u91d1825-SS316L\uff0c\u5728\u5149\u5b66\u663e\u5fae\u56fe\u548c\u5b9e\u9a8c\u7ed3\u679c\u4e2d\u5c55\u793a\u4e86\u8fde\u7eed\u548c\u95f4\u65ad\u7684\u6811\u679d\u72b6\u7ed3\u6784\uff0c\u6210\u529f\u5b9e\u73b0\u4e86\u5177\u6709\u826f\u597d\u65ad\u88c2\u97e7\u6027\u7684\u529f\u80fd\u68af\u5ea6\u754c\u9762\u3002<\/p>\n<p style=\"text-align: center;\"><strong>\u00a0<\/strong><strong>\u56db\u3001\u3010\u6570\u636e\u6982\u89c8\u3011<\/strong><\/p>\n<p><strong>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-252480\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig1_HTML_jpg.jpg\" alt=\"\" width=\"1774\" height=\"1602\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig1_HTML_jpg.jpg 1774w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig1_HTML_jpg-300x271.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig1_HTML_jpg-768x694.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig1_HTML_jpg-1024x925.jpg 1024w\" sizes=\"(max-width: 1774px) 100vw, 1774px\" \/><\/strong><\/p>\n<p><strong>\u56fe<\/strong><strong>1 <\/strong>\u5c55\u793a\u7684\u6784\u5efa\u540e\u7684\u6750\u6599\u663e\u793a\u4e86(a)\u9ad8\u5ea6 (b)\u5bbd\u5ea6 (c)\u539a\u5ea6\u3002\u00a9 2023 Springer Nature Limited<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-252481\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig2_HTML_jpg.jpg\" alt=\"\" width=\"2009\" height=\"682\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig2_HTML_jpg.jpg 2009w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig2_HTML_jpg-300x102.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig2_HTML_jpg-768x261.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig2_HTML_jpg-1024x348.jpg 1024w\" sizes=\"(max-width: 2009px) 100vw, 2009px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>2 <\/strong>(a) \u62c9\u4f38\u8bd5\u6837\u7684\u4f4d\u7f6e (b) \u62c9\u4f38\u8bd5\u6837\u7684\u89c4\u683c\u3002\u00a9 2023 Springer Nature Limited<\/p>\n<p><strong>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-252482\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig3_HTML_jpg.jpg\" alt=\"\" width=\"2007\" height=\"782\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig3_HTML_jpg.jpg 2007w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig3_HTML_jpg-300x117.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig3_HTML_jpg-768x299.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig3_HTML_jpg-1024x399.jpg 1024w\" sizes=\"(max-width: 2007px) 100vw, 2007px\" \/><\/strong><\/p>\n<p><strong>\u56fe<\/strong><strong>3<\/strong> (a) \u5728\u94ec\u954d\u94c1\u5408\u91d1825\u4e0a\u5236\u5907\u7684\u65ad\u88c2\u97e7\u6027\u8bd5\u6837\u7f3a\u53e3 (b) \u5728SS316L\u4e0a\u5236\u5907\u7684\u65ad\u88c2\u97e7\u6027\u8bd5\u6837\u7f3a\u53e3\u3002\u00a9 2023 Springer Nature Limited<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-252483\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig4_HTML_jpg.jpg\" alt=\"\" width=\"1769\" height=\"616\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig4_HTML_jpg.jpg 1769w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig4_HTML_jpg-300x104.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig4_HTML_jpg-768x267.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig4_HTML_jpg-1024x357.jpg 1024w\" sizes=\"(max-width: 1769px) 100vw, 1769px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>4<\/strong> (a) \u94ec\u954d\u94c1\u5408\u91d1 825\u7684\u5149\u5b66\u663e\u5fae\u56fe (b) SS316L\u7684\u5149\u5b66\u663e\u5fae\u56fe (c) \u754c\u9762\u7684\u5149\u5b66\u663e\u5fae\u56fe\u3002\u00a9 2023 Springer Nature Limited<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-252484\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig5_HTML_jpg.jpg\" alt=\"\" width=\"2009\" height=\"798\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig5_HTML_jpg.jpg 2009w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig5_HTML_jpg-300x119.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig5_HTML_jpg-768x305.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig5_HTML_jpg-1024x407.jpg 1024w\" sizes=\"(max-width: 2009px) 100vw, 2009px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>5<\/strong> (a) \u6784\u5efa\u540e\u7684\u94ec\u954d\u94c1\u5408\u91d1 825\u3001\u754c\u9762\u548cSS316L\u7684\u62c9\u4f38\u6027\u80fd\u5747\u503c (b) \u5e26\u6709\u8bef\u5dee\u68d2\u7684\u6807\u51c6\u504f\u5dee\u3002\u00a9 2023 Springer Nature Limited<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-252485\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig6_HTML.jpg\" alt=\"\" width=\"2010\" height=\"2344\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig6_HTML.jpg 2010w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig6_HTML-257x300.jpg 257w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig6_HTML-768x896.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig6_HTML-878x1024.jpg 878w\" sizes=\"(max-width: 2010px) 100vw, 2010px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>6<\/strong> (a) \u94ec\u954d\u94c1\u5408\u91d1 825\u7684\u65ad\u88c2\u8868\u9762 (b) \u754c\u9762\u7684\u65ad\u88c2\u8868\u9762 (c) SS316L\u7684\u65ad\u88c2\u8868\u9762\u9888\u90e8\u533a\u57df\u7684\u653e\u5927\u89c6\u56fe (d) \u94ec\u954d\u94c1\u5408\u91d1 825 (e) \u754c\u9762 (f) SS316L\u7684\u653e\u5927\u89c6\u56fe\u3002\u00a9 2023 Springer Nature Limited<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-252486\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig7_HTML.jpg\" alt=\"\" width=\"2010\" height=\"874\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig7_HTML.jpg 2010w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig7_HTML-300x130.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig7_HTML-768x334.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig7_HTML-1024x445.jpg 1024w\" sizes=\"(max-width: 2010px) 100vw, 2010px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>7<\/strong> (a) \u94ec\u954d\u94c1\u5408\u91d1 825\u7684\u88c2\u7eb9\u5c16\u7aef\u5f20\u5f00\u4f4d\u79fb\u66f2\u7ebf (b) SS316L\u7684\u88c2\u7eb9\u5c16\u7aef\u5f20\u5f00\u4f4d\u79fb\u66f2\u7ebf\u3002\u00a9 2023 Springer Nature Limited<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-252487\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig8_HTML.jpg\" alt=\"\" width=\"1770\" height=\"665\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig8_HTML.jpg 1770w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig8_HTML-300x113.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig8_HTML-768x289.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig8_HTML-1024x385.jpg 1024w\" sizes=\"(max-width: 1770px) 100vw, 1770px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>8<\/strong> (a) \u94ec\u954d\u94c1\u5408\u91d1 825\u88c2\u7eb9\u6269\u5c55\u7684\u4e0d\u540c\u533a\u57df\u7684\u626b\u63cf\u7535\u5b50\u663e\u5fae\u955c\u56fe\u50cf (b) SS316L\u88c2\u7eb9\u6269\u5c55\u7684\u4e0d\u540c\u533a\u57df\u7684\u626b\u63cf\u7535\u5b50\u663e\u5fae\u955c\u56fe\u50cf\u3002\u00a9 2023 Springer Nature Limited<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-252488\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig9_HTML.jpg\" alt=\"\" width=\"2010\" height=\"755\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig9_HTML.jpg 2010w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig9_HTML-300x113.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig9_HTML-768x288.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig9_HTML-1024x385.jpg 1024w\" sizes=\"(max-width: 2010px) 100vw, 2010px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>9<\/strong> (a) \u94ec\u954d\u94c1\u5408\u91d1 825\u7684\u626b\u63cf\u7535\u5b50\u663e\u5fae\u955c\u56fe\u50cf\u663e\u793a\u6761\u7eb9\u75d5\u8ff9 (b) SS316L\u7684\u626b\u63cf\u7535\u5b50\u663e\u5fae\u955c\u56fe\u50cf\u663e\u793a\u6761\u7eb9\u75d5\u8ff9\u3002\u00a9 2023 Springer Nature Limited<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-252489\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig10_HTML.jpg\" alt=\"\" width=\"1774\" height=\"658\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig10_HTML.jpg 1774w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig10_HTML-300x111.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig10_HTML-768x285.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig10_HTML-1024x380.jpg 1024w\" sizes=\"(max-width: 1774px) 100vw, 1774px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>10<\/strong> (a) \u94ec\u954d\u94c1\u5408\u91d1 825\u7684\u5feb\u901f\u65ad\u88c2\u8868\u9762\u7684\u626b\u63cf\u7535\u5b50\u663e\u5fae\u955c\u56fe\u50cf (b) SS316L\u7684\u5feb\u901f\u65ad\u88c2\u8868\u9762\u7684\u626b\u63cf\u7535\u5b50\u663e\u5fae\u955c\u56fe\u50cf\u3002\u00a9 2023 Springer Nature Limited<\/p>\n<p><strong>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-252490\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig11_HTML.jpg\" alt=\"\" width=\"1457\" height=\"2365\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig11_HTML.jpg 1457w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig11_HTML-185x300.jpg 185w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig11_HTML-768x1247.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig11_HTML-631x1024.jpg 631w\" sizes=\"(max-width: 1457px) 100vw, 1457px\" \/><\/strong><\/p>\n<p><strong>\u56fe<\/strong><strong>11<\/strong> (a-h) \u65ad\u88c2\u7684\u94ec\u954d\u94c1\u5408\u91d1 825\u533a\u57df\u7684EDS\u5143\u7d20\u6620\u5c04\u56fe\u3002\u00a9 2023 Springer Nature Limited<\/p>\n<p><strong>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-252491\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig12_HTML.jpg\" alt=\"\" width=\"1774\" height=\"723\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig12_HTML.jpg 1774w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig12_HTML-300x122.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig12_HTML-768x313.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig12_HTML-1024x417.jpg 1024w\" sizes=\"(max-width: 1774px) 100vw, 1774px\" \/><\/strong><\/p>\n<p><strong>\u56fe<\/strong><strong>12<\/strong> \u94ec\u954d\u94c1\u5408\u91d1 825\u533a\u57df\u7684EDS\u5143\u7d20\u8c31\u548c\u5b9a\u91cf\u5206\u6790\u3002\u00a9 2023 Springer Nature Limited<\/p>\n<p><strong>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-252492\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig13_HTML.jpg\" alt=\"\" width=\"1496\" height=\"2364\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig13_HTML.jpg 1496w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig13_HTML-190x300.jpg 190w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig13_HTML-768x1214.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig13_HTML-648x1024.jpg 648w\" sizes=\"(max-width: 1496px) 100vw, 1496px\" \/><\/strong><\/p>\n<p><strong>\u56fe<\/strong><strong>13<\/strong> (a-h) \u65ad\u88c2\u7684SS316L\u533a\u57df\u7684EDS\u5143\u7d20\u6620\u5c04\u56fe\u3002\u00a9 2023 Springer Nature Limited<\/p>\n<p><strong><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-252493\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig14_HTML.jpg\" alt=\"\" width=\"1774\" height=\"749\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig14_HTML.jpg 1774w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig14_HTML-300x127.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig14_HTML-768x324.jpg 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/06\/41598_2023_32124_Fig14_HTML-1024x432.jpg 1024w\" sizes=\"(max-width: 1774px) 100vw, 1774px\" \/>\u00a0<\/strong><\/p>\n<p><strong>\u56fe<\/strong><strong>14<\/strong> SS316L\u533a\u57df\u7684EDS\u5143\u7d20\u8c31\u548c\u5b9a\u91cf\u5206\u6790\u3002\u00a9 2023 Springer Nature Limited<\/p>\n<p>&nbsp;<\/p>\n<p style=\"text-align: center;\"><strong>\u4e94\u3001\u3010\u6210\u679c\u542f\u793a\u3011<\/strong><\/p>\n<p>\u603b\u7684\u6765\u8bf4\uff0c\u5229\u7528\u57fa\u4e8e\u51b7\u91d1\u5c5e\u8f6c\u79fb\u7684WAAM\u5de5\u827a\u6784\u5efa\u529f\u80fd\u68af\u5ea6\u58c1\uff0c\u91d1\u5c5e\u4f20\u8f93\u7279\u6027\u8868\u660eWAAM\u6210\u529f\u5730\u7528\u4e8e\u5236\u9020\u7ed3\u6784\u7a33\u5b9a\u7684\u96f6\u90e8\u4ef6\u3002\u91c7\u7528\u88c2\u7eb9\u5c16\u7aef\u5f00\u53e3\u4f4d\u79fb\u65b9\u6cd5\u548c\u5355\u8fb9\u7f3a\u53e3\u5f2f\u66f2\u8bd5\u6837\u51e0\u4f55\u5f62\u72b6\u8bc4\u4f30\u4e86\u5177\u6709\u7f3a\u53e3\u7684\u94ec\u954d\u94c1\u5408\u91d1 825\u548cSS316L\u4e24\u79cd\u529f\u80fd\u68af\u5ea6\u8bd5\u6837\u7684\u65ad\u88c2\u97e7\u6027\u3002\u6839\u636e\u7814\u7a76\u7ed3\u679c\uff0c\u94ec\u954d\u94c1\u5408\u91d1 825-SS316L\u58c1\u7684\u754c\u9762\u5177\u6709\u826f\u597d\u7684\u65ad\u88c2\u6027\u80fd\uff0c\u53ef\u5728\u6076\u52a3\u73af\u5883\u4e2d\u4f7f\u7528\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u539f\u6587\u8be6\u60c5\uff1aSenthil, T.S., Babu, S.R. &amp; Puviyarasan, M. Mechanical, microstructural and fracture studies on Inconel 825\u2013SS316L functionally graded wall fabricated by wire arc additive manufacturing. Sci Rep 13, 5321 (2023).<\/p>\n<p>https:\/\/doi.org\/10.1038\/s41598-023-32124-3<\/p>\n<p>\u672c\u6587\u7531jiojio\u4f9b\u7a3f<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u4e00\u3001 \u3010\u5bfc\u8bfb\u3011\u00a0 \u5728\u6574\u4e2a\u5386\u53f2\u4e2d\uff0c\u7406\u89e3\u548c\u64cd\u7eb5\u6750\u6599\u7684\u80fd\u529b\u5bf9\u6280\u672f\u7684\u8fdb\u6b65\u81f3\u5173\u91cd\u8981\u3002\u5982\u4eca\u7684\u79d1\u5b66\u5bb6\u548c\u5de5\u7a0b\u5e08\u4eec\u4ece\u7ecf\u6d4e\u548c\u73af\u5883\u7684\u89d2\u5ea6\u7406\u89e3\u65b0\u6750\u6599\u7684\u4ef7\u503c\u3002\u529f\u80fd\u68af\u5ea6\u6750\u6599\uff08FGMs\uff09\u662f\u96f6&#8230;<\/p>\n","protected":false},"author":34544,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-252479","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/252479"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/34544"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=252479"}],"version-history":[{"count":3,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/252479\/revisions"}],"predecessor-version":[{"id":252566,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/252479\/revisions\/252566"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=252479"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=252479"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=252479"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}