{"id":253442,"date":"2023-08-12T06:53:13","date_gmt":"2023-08-11T22:53:13","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=253442"},"modified":"2023-08-11T22:33:18","modified_gmt":"2023-08-11T14:33:18","slug":"%e5%8d%97%e6%96%b9%e7%a7%91%e6%8a%80%e5%a4%a7%e5%ad%a6%e6%9b%be%e6%9e%97%e8%b5%b5%e5%a4%a9%e5%af%bf%e6%9c%80%e6%96%b0nc%ef%bc%9a3d%e5%88%86%e7%ba%a7%e7%9f%b3%e5%a2%a8%e7%83%af%e9%98%b5%e5%88%97","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=253442","title":{"rendered":"\u5357\u65b9\u79d1\u6280\u5927\u5b66\u66fe\u6797&#038;\u8d75\u5929\u5bff\u6700\u65b0NC\uff1a3D\u5206\u7ea7\u77f3\u58a8\u70ef\u9635\u5217\u4e3a\u6c34\u7cfb\u950c\u7535\u6c60\u63d0\u4f9b\u4e86\u7a33\u5b9a\u7684\u950c\u8d1f\u6781"},"content":{"rendered":"<p style=\"text-align: center;\"><strong><b>\u5357\u65b9\u79d1\u6280\u5927\u5b66\u66fe\u6797&amp;\u8d75\u5929\u5bff<\/b><\/strong><strong><b>\u6559\u6388<\/b><\/strong><strong><b>\u6700\u65b0NC\uff1a3D\u5206\u7ea7\u77f3\u58a8\u70ef<\/b><\/strong><strong><b>\u77e9\u9635<\/b><\/strong><strong><b>\u4e3a\u6c34\u7cfb\u950c\u7535\u6c60\u63d0\u4f9b\u4e86\u7a33\u5b9a\u7684\u950c\u8d1f\u6781<\/b><\/strong><\/p>\n<p style=\"text-align: center;\"><strong><b>\u4e00\u3001[\u5bfc\u8bfb]<\/b><\/strong><\/p>\n<p style=\"text-align: center;\">\u00a0<\/p>\n<p>\u91d1\u5c5e\u950c(Zn)\u7531\u4e8e\u5177\u6709\u8f83\u9ad8\u7684\u7406\u8bba\u5bb9\u91cf(820\u2009mAh\u2009g<sup>-1<\/sup>,5855\u2009mAh\u2009cm<sup>-3<\/sup>)\u3001\u8f83\u4f4e\u7684\u6c27\u5316\u8fd8\u539f\u7535\u4f4d(-0.76\u2009V vs.SHE)\u4ee5\u53ca\u73af\u5883\u53cb\u597d\u548c\u5b89\u5168\u7684\u7279\u6027\uff0c\u4f5c\u4e3a\u6c34\u7cfb\u950c\u79bb\u5b50\u7535\u6c60(AZIBs)\u7684\u8d1f\u6781\u6750\u6599\u53d7\u5230\u4e86\u5e7f\u6cdb\u7684\u5173\u6ce8\u3002\u8fd9\u4e9b\u4f18\u52bf\u4f7fAZIBs\u6210\u4e3a\u6700\u5177\u6709\u5b9e\u9645\u5e94\u7528\u524d\u666f\u7684\u50a8\u80fd\u6280\u672f\u4e4b\u4e00\u3002\u7136\u800c\uff0c\u950c\u679d\u6676\u751f\u957f\u3001\u6790\u6c22\u53cd\u5e94(HER)\u7b49\u526f\u53cd\u5e94\u4ee5\u53ca\u950c\u8150\u8680\u7b49\u95ee\u9898\u4e25\u91cd\u5f71\u54cd\u4e86\u8fd9\u4e9b\u7535\u6c60\u7684\u53ef\u9006\u6027\u548c\u5faa\u73af\u6027\u80fd\uff0c\u9650\u5236\u4e86\u5176\u5e7f\u6cdb\u7684\u5546\u4e1a\u5316\u5e94\u7528\u3002\u5728\u9ad8\u9762\u5bb9\u91cf\u548c\u9ad8\u7535\u6d41\u5bc6\u5ea6\u4e0b\uff0c\u6709\u5bb3\u950c\u679d\u6676\u7684\u5f62\u6210\u5c24\u5176\u56f0\u96be\uff0c\u5bfc\u81f4\u9540\u950c\/\u8131\u950c\u4e0d\u5747\u5300\uff0c\u679d\u6676\u751f\u957f\u5e7f\u6cdb\uff0c\u4f53\u79ef\u81a8\u80c0\u3002\u8fd9\u4e9b\u95ee\u9898\u8fdb\u4e00\u6b65\u52a0\u901f\u4e86\u6790\u6c22\u548c\u950c\u8150\u8680\uff0c\u56e0\u4e3a\u950c\u66b4\u9732\u9762\u79ef\u589e\u52a0\u3002<strong><b>\u6b64\u5916\uff0c\u5728\u9ad8\u7535\u6d41\u5bc6\u5ea6\u548c\u9ad8\u5bb9\u91cf\u4e0b\uff0c\u5feb\u901f\u7684\u5145\u653e\u7535\u8fc7\u7a0b\u52a0\u5267\u4e86\u8fd9\u4e00\u95ee\u9898\uff0c\u5bfc\u81f4\u539a\u7684\u950c\u9540\u5c42\u548c\u4e0d\u5b8c\u5168\u7684\u950c\u5265\u79bb<\/b><\/strong>\u3002<\/p>\n<p><strong><b>\u00a0<\/b><\/strong><\/p>\n<p style=\"text-align: center;\"><strong><b>\u4e8c\u3001[\u6210\u679c\u63a0\u5f71]<\/b><\/strong><\/p>\n<p><strong><b>\u00a0<\/b><\/strong><\/p>\n<p><strong><b>\u8fd1\u65e5\uff0c\u5357\u65b9\u79d1\u6280\u5927\u5b66\u66fe\u6797&amp;\u8d75\u5929\u5bff\u6559\u6388\u8bfe\u9898\u7ec4\u5f00\u53d1\u4e86\u4e24\u79cd\u7531\u6c2e\u63ba\u6742\u77f3\u58a8\u70ef\u7eb3\u7c73\u7ea4\u7ef4\u7c07\u951a\u5b9a\u5728\u6539\u6027\u591a\u901a\u9053\u78b3\u7684\u5782\u76f4\u77f3\u58a8\u70ef\u9635\u5217\u7ec4\u6210\u7684\u4e09\u7ef4\u5206\u7ea7\u77f3\u58a8\u70ef<\/b><\/strong><strong><b>\u77e9\u9635<\/b><\/strong>\u3002\u5177\u6709\u5f84\u5411\u78b3\u901a\u9053\u7684\u77f3\u58a8\u70ef\u77e9\u9635\u5177\u6709\u9ad8\u7684\u8868\u9762\u79ef\u548c\u5b54\u9699\u7387\uff0c\u6709\u6548\u5730\u51cf\u5c0f\u4e86\u8868\u9762\u5c40\u90e8\u7535\u6d41\u5bc6\u5ea6\uff0c\u8c03\u63a7\u4e86Zn<sup>2+<\/sup>\u79bb\u5b50\u6d53\u5ea6\u68af\u5ea6\uff0c\u5747\u5300\u5316\u4e86\u7535\u573a\u5206\u5e03\uff0c\u4ece\u800c\u8c03\u63a7\u4e86Zn\u7684\u6c89\u79ef\u3002\u56e0\u6b64\uff0c\u5728120\u2009mA\u2009cm<sup>-2<\/sup>\u7684\u7535\u6d41\u5bc6\u5ea6\u4e0b\uff0c\u7ecf\u8fc73000\u6b21\u5faa\u73af\u540e\uff0c\u8be5\u590d\u5408\u6750\u6599\u7684\u5e93\u4f26\u6548\u7387\u9ad8\u8fbe99.67%\uff0c\u572880\u2009mA\u2009cm<sup>-2<\/sup>\u548c80\u2009mAh\u2009cm<sup>-2<\/sup>\u7684\u7535\u6d41\u5bc6\u5ea6\u4e0b\uff0c\u5bf9\u79f0\u7535\u6c60\u53ef\u4ee5\u5b9e\u73b02600\u2009h\u7684\u65e0\u679d\u6676\u5faa\u73af\u3002\u6240\u8bbe\u8ba1\u7684\u5168\u7535\u6c60\u5177\u670916.91\u2009mAh\u2009cm<sup>-2<\/sup>\u7684\u4f18\u5f02\u5bb9\u91cf\u3002\u4e0e\u6d3b\u6027\u70ad\u5339\u914d\u7684Zn\u7535\u5bb9\u5668\u572840\u2009mA\u2009cm<sup>-2<\/sup>\u4e0b\u8868\u73b0\u51fa\u4f18\u5f02\u768420000\u6b21\u5faa\u73af\u7684\u957f\u671f\u5faa\u73af\u6027\u80fd\u3002<strong><b>\u8fd9\u79cd\u4e3a\u950c\u8d1f\u6781\u6784\u5efa\u4e09\u7ef4\u5206\u7ea7\u7ed3\u6784\u7684\u7b56\u7565\u53ef\u80fd\u4e3a\u91d1\u5c5e\u8d1f\u6781\u5728\u9ad8\u500d\u7387\u548c\u9ad8\u5bb9\u91cf\u4e0b\u8fd0\u884c\u5f00\u8f9f\u4e00\u6761\u65b0\u7684\u9014\u5f84<\/b><\/strong>\u3002\u76f8\u5173\u8bba\u6587\u4ee5\u9898\u4e3a\u201c<strong>3D hierarchical graphene matrices enable stable Zn anodes for aqueous Zn batteries<\/strong>\u201d\u7684\u8bba\u6587\u53d1\u8868\u5728<strong><em>Nature Communications<\/em><\/strong>\u4e0a\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-253453\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72471-8.png\" alt=\"\" width=\"733\" height=\"268\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72471-8.png 733w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72471-8-300x110.png 300w\" sizes=\"(max-width: 733px) 100vw, 733px\" \/><\/p>\n<p>&nbsp;<\/p>\n<p style=\"text-align: center;\"><strong><b>\u4e09\u3001[\u6838\u5fc3\u521b\u65b0\u70b9]<\/b><\/strong><\/p>\n<p>\u672c\u5de5\u4f5c\u5c55\u793a\u4e86\u4e00\u79cd\u65b0\u578b\u7684\u5177\u6709\u8d85\u9ad8Zn\u6c89\u79ef\/\u5265\u79bb\u901f\u7387\u548c\u5bb9\u91cf\u4ee5\u53ca\u4f18\u5f02\u7684\u957f\u671f\u5faa\u73af\u5bff\u547d\u76843D\u590d\u5408Zn\u8d1f\u6781\u3002\u8be5\u8d1f\u6781\u75313D\u6c2e\u63ba\u6742\u77f3\u58a8\u70ef\u7eb3\u7c73\u7ea4\u7ef4\u56e2\u7c07(GFs)\u951a\u5b9a\u5728\u5782\u76f4\u77f3\u58a8\u70ef\u9635\u5217(VGs)\u4fee\u9970\u7684\u591a\u901a\u9053\u78b3\u77e9\u9635(3D-FGC)\u4e2d\u6784\u6210\u3002\u66f4\u4ee4\u4eba\u9f13\u821e\u7684\u662f\uff0cAC@3D-LC\/3D-RFGC@Zn\u7535\u5bb9\u5668\u572840\u2009mA\u2009cm<sup>-2<\/sup>\u4e0b\u8868\u73b0\u51fa\u4f18\u5f02\u768420000\u5708\u7684\u957f\u671f\u5faa\u73af\u6027\u80fd\u3002<\/p>\n<p><strong><b>\u00a0<\/b><\/strong><\/p>\n<p style=\"text-align: center;\"><strong><b>\u56db\u3001[\u6570\u636e\u6982\u89c8]<\/b><\/strong><\/p>\n<ul>\n<li><b><\/b><strong><b>3D-FGC<\/b><\/strong><strong><b>\u77e9\u9635<\/b><\/strong><strong><b>\u7684\u5408\u6210\u4e0e\u8868\u5f81<\/b><\/strong><\/li>\n<\/ul>\n<p>&nbsp;<\/p>\n<p>\u4e0e\u5e73\u9762Zn\u7b94\u76f8\u6bd4\uff0c3D\u5206\u7ea7\u77f3\u58a8\u70ef\u7ed3\u6784\u6709\u5229\u4e8eZn\u91d1\u5c5e\u7684\u5747\u5300\u6c89\u79ef\uff0c\u6291\u5236\u4e86Zn\u679d\u6676\u7684\u751f\u957f\u3002Zn\u91d1\u5c5e\u5728\u88f8Zn\u548c3D\u77f3\u58a8\u70ef\u77e9\u9635\u4e0a\u7684\u6c89\u79ef\u884c\u4e3a\u5047\u8bbe\u5982<strong>\u56fe1<\/strong>\u6240\u793a\u3002\u5bf9\u4e8e\u88f8Zn\u7b94\u62162D Cu\u57fa\u677f\uff0cZn\u91d1\u5c5e\u5728\u9ad8Zn<sup>2+<\/sup>\u6d53\u5ea6\u4e0b\u5f62\u6838\u3002Zn\u679d\u6676\u5728\u53cd\u590d\u5faa\u73af\u8fc7\u7a0b\u4e2d\u8fc5\u901f\u751f\u957f\u5e76\u6700\u7ec8\u7a7f\u900f\u9694\u819c\uff0c\u4f7f\u7535\u6c60\u77ed\u8def\u5e76\u9020\u6210\u5b89\u5168\u9690\u60a3\uff0c\u5c24\u5176\u662f\u5728\u9ad8\u500d\u7387\u548c\u9ad8\u5bb9\u91cf\u4e0b\u3002\u76f8\u53cd\uff0cZn\u91d1\u5c5e\u57283D\u77e9\u9635\u4e0a\u7684\u6c89\u79ef\u60c5\u51b5\u5219\u4e0d\u540c\u3002Zn\u91d1\u5c5e\u7531\u4e8e\u5176\u4eb2\u950c\u6027\u6c89\u79ef\u5728\u4e30\u5bcc\u7684\u77f3\u58a8\u70ef\u9aa8\u67b6\u4e0a\uff0c\u9010\u6e10\u586b\u5145\u5b54\u9699\uff0c\u5f62\u6210\u81f4\u5bc6\u76843D Zn\u8d1f\u6781\u3002\u6b64\u5916\uff0c\u5bf9\u4e8e3D-LFGC(<strong>\u56fe1b<\/strong>)\u548c3D-RFGC(<strong>\u56fe1c<\/strong>)\u77f3\u58a8\u70ef\u77e9\u9635\uff0c\u7531\u4e8e\u5176\u8868\u9762\u5b58\u5728\u5927\u91cf\u5b54\u9699\uff0c\u6709\u8db3\u591f\u7684\u7a7a\u95f4\u50a8\u5b58Zn\uff0c\u5b9e\u73b0\u4e86\u77f3\u58a8\u70ef\u4fee\u9970\u5c42\u7684\u9ad8\u5229\u7528\u7387\uff0c\u4ece\u800c\u83b7\u5f97\u4e86\u8f83\u9ad8\u7684\u9762\u5bb9\u91cf\u3002\u5373\u4f7f\u5728\u9ad8\u7535\u6d41\u5bc6\u5ea6\u4e0b\uff0cZn\u91d1\u5c5e\u7684\u7535\u9540\u548c\u5265\u79bb\u4e5f\u4e0d\u80fd\u5931\u63a7\uff0c\u5bfc\u81f4\u679d\u6676\u751f\u957f\uff0c\u8fd9\u5f52\u56e0\u4e8e\u5176\u8f83\u5927\u7684\u6bd4\u8868\u9762\u79ef\u548c\u4e30\u5bcc\u7684\u6c89\u79ef\u4f4d\u70b9\uff0c\u5bfc\u81f4\u5c40\u90e8\u7535\u6d41\u5206\u5e03\u8f83\u4f4e\u3002\u6b64\u5916\uff0c\u8fde\u7eed\u7684\u591a\u5b54\u7ed3\u6784\u8fd8\u53ef\u4ee5\u7f13\u51b2\u6c89\u79efZn\u57283D-RFGC\u77e9\u9635\u5185\u90e8\u6c89\u79ef\u548c\u6eb6\u89e3\u8fc7\u7a0b\u4e2d\u7684\u4f53\u79ef\u53d8\u5316\u3002<\/p>\n<p>\u5229\u7528\u4e09\u7ef4\u6c2e\u63ba\u6742\u77f3\u58a8\u70ef\u7eb3\u7c73\u7ea4\u7ef4\u7c07(GFs)\u548c\u5782\u76f4\u77f3\u58a8\u70ef\u9635\u5217(VGs)\u4fee\u9970\u7684\u591a\u901a\u9053\u78b3\u77e9\u9635(3D-LFGC\/3DD-RFGC)\uff0c\u901a\u8fc7\u8fde\u7eed\u4e24\u6b65\u6cd5\u5f00\u53d1\u4e86\u5206\u5c42\u7ed3\u6784\u77f3\u58a8\u70ef\uff0c\u5982<strong><b>\u56fe2a<\/b><\/strong>\u6240\u793a\u3002\u626b\u63cf\u7535\u5b50\u663e\u5fae\u955c(SEM)\u548c\u900f\u5c04\u7535\u5b50\u663e\u5fae\u955c(TEM)\u89c2\u5bdf\u53d1\u73b0\uff0cGFs\u548cVGs\u53ef\u4ee5\u5f62\u6210\u5177\u6709\u5927\u7a7a\u95f4\u548c\u9ad8\u6548\u5bfc\u7535\u7f51\u7edc\u7684\u5206\u7ea7\u7ed3\u6784(<strong><b>\u56fe2b<\/b><\/strong>)\u30023D-LFGC\u7684\u5f62\u8c8c\u663e\u793a\u901a\u9053\u5c3a\u5bf8\u572810~30\u2009\u03bcm\u4e4b\u95f4\uff0c\u901a\u5e38\u4e3a20\u2009\u03bcm\u3002\u5177\u4f53\u6765\u8bf4\uff0c\u76f4\u5f84\u4e3a250\u2009nm\u7684GFs\u548cVGs\u7262\u56fa\u5730\u951a\u5b9a\u5728\u901a\u9053\u5185\u90e8\uff0c\u63d0\u4f9b\u4e86\u4e00\u4e2a3D\u4e92\u8054\u548c\u901a\u7528\u7684\u6846\u67b6(<strong><b>\u56fe2c-e<\/b><\/strong>)\u3002\u57fa\u4e8eIG\/ID\uff0c\u62c9\u66fc\u56fe\u8c31(<strong><b>\u56fe2o<\/b><\/strong>)\u8fdb\u4e00\u6b65\u8868\u660e\u4e86GFs\u548cVGs\u6d82\u5c42\u5728\u5206\u7ea7\u7ed3\u6784\u8bbe\u8ba1\u4e2d\u7684\u5747\u5300\u6027\uff0c\u4e0eSEM\u548cTEM\u89c2\u5bdf\u7ed3\u679c\u4e00\u81f4\u3002\u9ad8\u5206\u8fa8N 1s\u8c31\u7684X\u5c04\u7ebf\u5149\u7535\u5b50\u80fd\u8c31(XPS)\u6d4b\u91cf\u7ed3\u679c\u8bc1\u5b9e\u4e86\u6c2e\u63ba\u6742\u7684\u5b58\u5728(<strong><b>\u56fe2p<\/b><\/strong>)\u3002\u800c\u5728N\u63ba\u6742\u77f3\u58a8\u70ef\u4e0a\uff0c\u5bf9\u5e94\u7684\u7ed3\u5408\u80fd\u5206\u522b\u4e3a-0.0246\u2009eV(Top)\u3001-0.0270\u2009eV(Hollow)\u548c-0.0254\u2009eV(Bridge)(<strong><b>\u56fe2s<\/b><\/strong>)\u3002<strong><b>\u8fd9\u4e9b\u7ed3\u679c\u8868\u660e\uff0c\u6c2e\u63ba\u6742\u7684\u5f15\u5165\u6539\u53d8\u4e86\u950c\u4e0e\u78b3\u57fa\u5e95\u4e4b\u95f4\u7684\u76f8\u4e92\u4f5c\u7528\uff0c\u4f7f\u5176\u4ece\u758f\u950c\u8f6c\u53d8\u4e3a\u4eb2\u950c<\/b><\/strong>\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-253454\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72472-7.png\" alt=\"\" width=\"640\" height=\"502\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72472-7.png 640w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72472-7-300x235.png 300w\" sizes=\"(max-width: 640px) 100vw, 640px\" \/><\/p>\n<p><strong>\u56fe1<\/strong>\u00a0\u00a0\u4ee5\u7a33\u5b9a\u7684\u950c\u8d1f\u6781\u4e3a\u76ee\u6807\u7684\u4e09\u7ef4\u5206\u7ea7\u7ed3\u6784\u77f3\u58a8\u70ef\u77e9\u9635\u7684\u8bbe\u8ba1\u00a9 2023 The Authors<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-253455\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72473-6.png\" alt=\"\" width=\"588\" height=\"669\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72473-6.png 588w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72473-6-264x300.png 264w\" sizes=\"(max-width: 588px) 100vw, 588px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>2<\/strong>\u00a0\u00a0\u7ed3\u6784\u548c\u5f62\u6001\u8868\u5f81\u00a9 2023 The Authors<\/p>\n<p>&nbsp;<\/p>\n<ul>\n<li><b><\/b><strong><b>\u4e0d\u540c\u6761\u4ef6\u4e0bZn\u6c89\u79ef\/\u6eb6\u89e3\u6548\u7387\u7684\u6f14\u53d8<\/b><\/strong><\/li>\n<\/ul>\n<p><strong><b>\u00a0<\/b><\/strong><\/p>\n<p>\u57280.5\u2009mAh\u2009cm<sup>-2<\/sup>\u523010\u2009mAh\u2009cm<sup>-2<\/sup>\u7684\u4e0d\u540c\u7535\u6d41\u5bc6\u5ea6(1~120\u2009mA\u2009cm<sup>-2<\/sup>)\u4e0b\uff0c\u63a2\u7a76\u4e86Cu\u7b94\u3001Zn\u7b94\u30013D-LC\u30013D-RC\u30013D-LFGC\u548c3D-RFGC\u57fa\u5e95\u5728\u6052\u6d41\u5145\u653e\u7535\u8fc7\u7a0b\u4e2dZn\u6c89\u79ef\/\u6eb6\u89e3\u6548\u7387\u5f62\u8c8c\u7684\u6f14\u53d8\u3002\u5982<strong>\u56fe3a<\/strong>\u6240\u793a\uff0c\u57281.0\u2009mA\u2009cm<sup>-2<\/sup>\u4e0b\uff0c3D-LFGC\u548c3D-RFGC\u7535\u6781\u7684\u8fc7\u7535\u4f4d\u5206\u522b\u4e3a32\u548c30\u2009mV\u3002\u76f8\u6bd4\u4e4b\u4e0b\uff0cCu\u7b94\u7535\u6781\u5728\u6210\u6838\u9636\u6bb5\u8868\u73b0\u51fa\u76f8\u5f53\u5c16\u9510\u7684\u7535\u538b\u964d\uff0c\u8868\u73b0\u51fa52\u2009mV\u7684\u5927\u8fc7\u7535\u4f4d\u3002\u6b64\u5916\uff0c\u5373\u4f7f\u57282\u30015\u548c10\u2009mA\u2009cm<sup>-2<\/sup>\u7684\u9ad8\u7535\u6d41\u5bc6\u5ea6\u4e0b\uff0c3D-LFGC\u548c3D-RFGC\u77e9\u9635\u4e5f\u8868\u73b0\u51fa\u66f4\u7a33\u5b9a\u7684\u8fc7\u7535\u4f4d(<strong><b>\u56fe3b-d<\/b><\/strong>)\u3002\u7531\u4e8e\u4e30\u5bcc\u7684\u591a\u5b54\u7ed3\u6784\uff0c3D-LFGC\u548c3D-RFGC\u5177\u6709\u8f83\u4f4e\u7684\u5c40\u90e8\u7535\u6d41\u5bc6\u5ea6\u548c\u5747\u5300\u7684Zn<sup>2+<\/sup>\u5206\u5e03\uff0c\u56e0\u6b64\u53ef\u4ee5\u89c2\u5bdf\u5230\u5747\u5300\u81f4\u5bc6\u7684\u8868\u9762\u5f62\u8c8c\u3002<strong><b>\u5728\u9ad8\u8fbe120\u2009mA\u2009cm<\/b><\/strong><strong><sup><b>-2<\/b><\/sup><\/strong><strong><b>\u7684\u7535\u6d41\u5bc6\u5ea6\u4e0b\uff0c\u5bb9\u91cf\u4e3a40\u2009mAh\u2009cm<\/b><\/strong><strong><sup><b>-2 <\/b><\/sup><\/strong><strong><b>(\u56fe3e,f)\u76843D-RFGC\u4ecd\u7136\u53ef\u4ee5\u5b9e\u73b0\u4f18\u5f02\u7684\u6c89\u79ef\/\u6eb6\u89e3\u8fc7\u7535\u4f4d\u548c\u6548\u7387<\/b><\/strong>\u3002\u5728\u8d85\u8fc710\u2009mA\u2009cm<sup>-2<\/sup>\u7684\u9ad8\u7535\u6d41\u5bc6\u5ea6\u4e0b\uff0c3D-RFGC\u5728\u6c89\u79ef\/\u6eb6\u89e3\u6548\u7387\u65b9\u9762\u6bd43D-LFGC\u5177\u6709\u660e\u663e\u7684\u4f18\u52bf(<strong><b>\u56fe3j<\/b><\/strong>)\u3002\u4e0e3D-LFGC\u77e9\u9635\u76f8\u6bd4\uff0c3D-RFGC\u77e9\u9635\u5728\u4e0d\u540c\u7535\u6d41\u5bc6\u5ea6\u4e0b\u7b2c5\u6b21\u5faa\u73af\u7684\u5e73\u53f0\u8fc7\u7535\u4f4d\u8f83\u4f4e\uff0c\u8868\u73b0\u51fa\u4f4e\u7684\u5c40\u90e8\u7535\u6d41\u5bc6\u5ea6\u548c\u5747\u5300\u7684Zn<sup>2+<\/sup>\u79bb\u5b50\u5206\u5e03(<strong><b>\u56fe3k<\/b><\/strong>)\u3002\u5728\u6ca1\u6709GFs\u548cVGs\u7684\u60c5\u51b5\u4e0b\uff0c\u5f88\u660e\u663eZn\u53ea\u6c89\u79ef\u5728\u539f\u59cb3D-LC\u7684\u4e0a\u90e8\uff0c\u5bfc\u81f43D\u77e9\u9635\u7684\u7a7a\u95f4\u5229\u7528\u7387\u5f88\u5dee\u3002\u968f\u7740Zn\u6c89\u79ef\u539a\u5ea6\u7684\u589e\u52a0\uff0c\u7279\u522b\u662f\u5728\u9ad8\u500d\u7387\u548c\u9ad8\u5bb9\u91cf\u4e0b\uff0c\u53ef\u4ee5\u53d1\u751f\u5feb\u901f\u7684\u679d\u6676\u751f\u957f\u3002<strong><b>\u540c\u6837\uff0c\u5f53\u7535\u6d41\u5bc6\u5ea6\u8d85\u8fc710\u2009mA\u2009cm<\/b><\/strong><strong><sup><b>-2<\/b><\/sup><\/strong><strong><b>\u65f6\uff0c3D-LFGC<\/b><\/strong><strong><b>\u77e9\u9635<\/b><\/strong><strong><b>\u7684\u8fc7\u7535\u4f4d\u503c\u5f00\u59cb\u589e\u52a0\uff0c\u8fd9\u662f\u7531\u4e8e\u5782\u76f4\u6392\u5217\u7684\u901a\u9053\u4e2dZn\u7684\u7535\u9540\/\u5265\u79bb\u4e0d\u5b8c\u5168(\u56fe3k)<\/b><\/strong>\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-253456\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72474-6.png\" alt=\"\" width=\"662\" height=\"563\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72474-6.png 662w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72474-6-300x255.png 300w\" sizes=\"(max-width: 662px) 100vw, 662px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>3<\/strong>\u00a0Zn\/3D-LFGC\u3001Zn\/3D-RFGC\u548cZn\/Cu\u534a\u7535\u6c60\u4e2d\u4e0d\u540c\u7535\u6781\u7684\u7535\u5316\u5b66\u6027\u80fd\u00a9 2023 The Authors<\/p>\n<p>&nbsp;<\/p>\n<ul>\n<li><b><\/b><strong><b>\u5bf9\u79f0\u7535\u6c60\u4e2d\u4e09\u7ef4\u950c\u8d1f\u6781\u7684\u6027\u80fd<\/b><\/strong><strong><b>\u53ca\u6c89\u79ef\u673a\u7406<\/b><\/strong><\/li>\n<\/ul>\n<p>&nbsp;<\/p>\n<p>\u7ec4\u88c5\u5bf9\u79f0\u7535\u6c60\uff0c\u6839\u636e\u6052\u7535\u6d41\u5145\u653e\u7535(GCD)\u5728\u7535\u6d41\u5bc6\u5ea6\u4ece1\u523080\u2009mA\u2009cm<sup>-2<\/sup>\u548c\u9762\u79ef\u5bb9\u91cf\u4ece1\u523080\u2009mAh\u2009cm<sup>-2<\/sup>\u6d4b\u8bd53D-LFGC@Zn\u30013D-RFGC@Zn\u30013D Zn\u6ce1\u6cab\u548c\u88f8\u950c\u7b94\u7684\u957f\u671f\u5faa\u73af\u6027\u80fd\uff0c\u5982<strong><b>\u56fe4<\/b><\/strong>\u6240\u793a\u3002\u53ef\u4ee5\u770b\u51fa\uff0c\u4e0e\u88f8Zn\u548c3D Zn\u6ce1\u6cab(<strong><b>\u56fe4a\u3001b<\/b><\/strong>)\u76f8\u6bd4\uff0c3D-RFGC@Zn\u548c3D-LFGC@Zn\u8d1f\u6781\u7684\u7535\u538b\u6ede\u540e(21\u2009mV)\u51cf\u5c0f\uff0c\u5bff\u547d(3D-RFGC@Zn\u4e3a7300\u2009h,3D-LFGC@Zn\u4e3a4200\u2009h)\u663e\u8457\u5ef6\u957f\u3002\u5c063D-RFGC@Zn\u5bf9\u79f0\u7535\u6c60\u7684\u9ad8\u7ade\u4e89\u7535\u538b\u6ede\u540e\u548c\u8d85\u9ad8\u7535\u6d41\u5bc6\u5ea6\u4ee5\u53ca\u9762\u79ef\u5bb9\u91cf\u4e0e\u5148\u524d\u62a5\u9053\u76843D Zn\u5bbf\u4e3b(<strong><b>\u56fe4k,l<\/b><\/strong>)\u8fdb\u884c\u4e86\u6bd4\u8f83\uff0c\u8868\u660e<strong><b>\u672c\u5de5\u4f5c<\/b><\/strong><strong><b>\u65b0\u8bbe\u8ba1\u7684\u8868\u97623D\u5206\u7ea7\u77f3\u58a8\u70ef<\/b><\/strong><strong><b>\u77e9\u9635<\/b><\/strong><strong><b>\u5177\u6709\u4e30\u5bcc\u7684N\u63ba\u6742GFs\u548cVGs\u4ee5\u53ca\u5927\u7684\u4f53\u79ef\u901a\u9053\uff0c\u6709\u6548\u5730\u6291\u5236\u4e86\u679d\u6676\u751f\u957f\uff0c\u4ece\u800c\u5b9e\u73b0\u4e86\u9ad8\u5ea6\u53ef\u9006\u7684\u9540\u950c\/\u5265\u79bb\u8fc7\u7a0b<\/b><\/strong>\u3002<\/p>\n<p>\u4f7f\u7528\u5149\u5b66\u663e\u5fae\u955c\u5728\u7535\u6d41\u5bc6\u5ea6\u4e3a40\u2009mA\u2009cm<sup>-2<\/sup>\u7684\u6761\u4ef6\u4e0b\uff0c\u5bf9\u88f8\u950c\u7b94\u548c3D-RFGC\u77e9\u9635\u4e0a\u7684\u950c\u91d1\u5c5e\u7535\u9540\u8fc7\u7a0b\u8fdb\u884c\u4e86\u539f\u4f4d\u89c2\u5bdf\u3002\u5728\u88f8\u950c\u7b94\u4e0a\uff0c\u7ecf\u8fc710\u2009min\u540e\uff0c\u5728\u8868\u9762\u89c2\u5bdf\u5230\u5c0f\u4e14\u5f62\u72b6\u4e0d\u89c4\u5219\u7684Zn\u9897\u7c92\uff0c\u4f34\u968f\u7740\u4e0d\u5747\u5300\u7684Zn\u6c89\u79ef\u548c\u6c14\u6ce1\u7684\u5f62\u6210\uff0c\u8868\u660e\u53ef\u80fd\u7684\u4ea7\u6c22\u300220\u2009min\u540e\uff0c\u51fa\u73b0\u8089\u773c\u53ef\u89c1\u7684\u7a81\u8d77\uff0c\u7531\u4e8e\u6c89\u79ef\u4e0d\u5747\u5300\uff0c\u9010\u6e10\u5f62\u6210\u82d4\u85d3\u72b6Zn\u679d\u6676(<strong><b>\u56fe5a<\/b><\/strong>)\u3002\u76f8\u6bd4\u4e4b\u4e0b\uff0c3D-RFGC\u77e9\u9635\u5728\u6574\u4e2a\u7535\u9540\u8fc7\u7a0b\u4e2d\u53d8\u5316\u5f88\u5c0f\uff0c\u8868\u9762\u5149\u6ed1\uff0c\u5373\u4f7f\u5728\u6c89\u79ef60\u2009min\u540e\u4ecd\u4fdd\u6301\u65e0\u679d\u6676\u5f62\u8c8c(<strong><b>\u56fe5b<\/b><\/strong>)\u3002\u5faa\u73af200\u2009h\u540e\uff0c\u91c7\u7528\u4e09\u7ef4\u6fc0\u5149\u626b\u63cf\u5171\u805a\u7126\u663e\u5fae\u955c(LCSM)\u8868\u5f81Zn\u7535\u6781\u7684\u8868\u9762\u62d3\u6251\u7ed3\u6784\u3002\u88f8Zn\u8d1f\u6781\u51fa\u73b0\u6ce2\u5cf0\u548c\u6ce2\u8c37\uff0c\u8868\u9762\u660e\u663e\u7c97\u7cd9(<strong><b>\u56fe5c<\/b><\/strong>)\u3002\u8fd9\u4e9b\u65e0\u5e8f\u7684\u679d\u6676\u589e\u52a0\u4e86\u7535\u89e3\u8d28\/Zn\u7b94\u7684\u8868\u9762\u79ef\uff0c\u8fdb\u4e00\u6b65\u52a0\u901f\u4e86HER\u3002\u7136\u800c\uff0c\u5bf9\u4e8e3D-LFGC@Zn\u548c3D-RFGC@Zn\u8d1f\u6781\uff0c\u5728\u591a\u6b21\u5faa\u73af\u540e\uff0c\u7c97\u7cd9\u5ea6\u4ec5\u8868\u73b0\u51fa\u8f7b\u5fae\u7684\u53d8\u5316(<strong><b>\u56fe5d-e<\/b><\/strong>)\u3002\u6b64\u5916\uff0cSEM\u7167\u7247\u663e\u793a\uff0c\u5728\u88f8\u950c\u7b94\u4e0a\uff0c\u5206\u6563\u3001\u758f\u677e\u7684\u950c\u6676\u7c92\u4e0e\u5206\u5e03\u4e0d\u5747\u5300\u7684\u5927\u7247\u950c\u5171\u5b58\uff0c\u90e8\u5206\u950c\u9897\u7c92\u6e17\u900f\u5230\u73bb\u7483\u7ea4\u7ef4\u9694\u819c\u4e2d\uff0c\u8868\u660e\u950c\u679d\u6676\u751f\u957f\u4e25\u91cd(<strong><b>\u56fe5f<\/b><\/strong>)\u3002<strong><b>\u76f8\u6bd4\u4e4b\u4e0b\uff0c3D-RFGC<\/b><\/strong><strong><b>\u77e9\u9635<\/b><\/strong><strong><b>\u5728\u5faa\u73af\u540e\u5448\u73b0\u51fa\u81f4\u5bc6\u4e14\u65e0\u679d\u6676\u7684\u8868\u9762\uff0c\u5982\u56fe5g\uff0ch\u6240\u793a<\/b><\/strong>\u3002\u7136\u800c\uff0c3D-RFGC@Zn\u7535\u6781\u7684Rct\u6700\u521d\u964d\u4f4e\u5e76\u5728\u968f\u540e\u7684\u8bb0\u5f55\u5faa\u73af\u4e2d\u8d8b\u4e8e\u7a33\u5b9a\uff0c\u8868\u660e\u4e86\u9ad8\u6548\u7684\u754c\u9762\u4f20\u8f93\u52a8\u529b\u5b66\u3002<strong><b>\u8fd9\u4e9b\u7ed3\u679c\u8868\u660e\uff0c3D-RFGC<\/b><\/strong><strong><b>\u77e9\u9635<\/b><\/strong><strong><b>\u53ef\u4ee5\u5f15\u5bfc\u5747\u5300\u81f4\u5bc6\u7684\u9540\u950c\u5c42\uff0c\u4e14\u5177\u6709\u8f83\u9ad8\u7684\u53ef\u9006\u6027\uff0c\u4ece\u800c\u6291\u5236\u950c\u7684\u8150\u8680\u80fd\u529b<\/b><\/strong>\u3002<\/p>\n<p>\u4e3a\u4e86\u8fdb\u4e00\u6b65\u4e86\u89e3\u7a33\u5b9a\u7684\u7535\u6781-\u7535\u89e3\u8d28\u754c\u9762\u7684\u672c\u8d28\uff0c\u5728\u4e0d\u540c\u7684\u6e85\u5c04\u6df1\u5ea6\u4e0b\u8fdb\u884c\u4e86X\u5c04\u7ebf\u5149\u7535\u5b50\u80fd\u8c31(XPS)\u6d4b\u8bd5\uff0c\u4ee5\u63ed\u793a\u56fa\u4f53\u7535\u89e3\u8d28\u754c\u9762(SEI)\u5c42\u4e2d3D\u5143\u7d20\u7684\u5206\u5e03(<strong><b>\u56fe6a-d<\/b><\/strong>)\u3002\u4ee5C1\u2009s\u5cf0(\u5728284.8\u2009eV\u5904)\u4e3a\u53c2\u6bd4\uff0c\u5bf9\u7ed3\u5408\u80fd\u8fdb\u884c\u4e86\u6821\u6b63\u3002\u5728\u8fde\u7eed\u523b\u8680\u8fc7\u7a0b\u4e2d\uff0c\u53ef\u4ee5\u6e05\u6670\u5730\u89c2\u5bdf\u5230Zn\u91d1\u5c5e\u5cf0\u3002\u5982<strong><b>\u56fe6e<\/b><\/strong>\u6240\u793a\uff0c\u968f\u7740\u53cd\u5e94\u7684\u8fdb\u884c\uff0c3D-RFGC\u77e9\u9635\u5185\u5916\u7a7a\u95f4\u7684Zn<sup>2+<\/sup>\u79bb\u5b50\u6d53\u5ea6\u66f4\u52a0\u5747\u5300\u4e14\u4f4e\u4e8e3D-RC\uff0c\u8868\u660e\u5185\u90e8\u7a7a\u95f4\u9540\u950c\u5747\u5300\u3002<strong><b>\u56fe6k<\/b><\/strong>\u8868\u660e\uff0c\u4e0e\u539f\u59cb3D-RC\u7535\u6781(2.5\u2009mF\u2009cm<sup>2<\/sup>)\u76f8\u6bd4\uff0c\u539f\u59cb3D-LC\u7535\u6781\u7684\u53cc\u7535\u5c42\u7535\u5bb9(Cdl)\u663e\u8457\u964d\u4f4e\u3002\u4e0e3D-RFGC\u76f8\u5f53\u7684\u7535\u5316\u5b66\u6d3b\u6027\u8868\u9762\u79ef\u53ef\u5f52\u56e0\u4e8e\u5f15\u5165\u4e86\u6bd4\u8868\u9762\u79ef\u589e\u5927\u3001\u6d3b\u6027\u4f4d\u70b9\u4e30\u5bcc\u7684GFs\u548cVGs\u3002\u8f83\u5927\u7684ECSA\u53ef\u80fd\u8fdb\u4e00\u6b65\u4fc3\u8fdbZn<sup>2+<\/sup>\u6269\u6563\uff0c\u589e\u52a0DZn<sup>2+<\/sup>(Zn<sup>2+<\/sup>\u79bb\u5b50\u6269\u6563\u7cfb\u6570)\u3002<strong><b>\u56e0\u6b64\uff0c\u7406\u8bba\u6a21\u62df\u548c\u5b9e\u9a8c\u5747\u8bc1\u660e\u4e863D-RFGC<\/b><\/strong><strong><b>\u77e9\u9635<\/b><\/strong><strong><b>\u5728\u6c89\u79ef\u548c\u5265\u79bb\u8fc7\u7a0b\u4e2d\u53ef\u4ee5\u5b9e\u73b0Zn\u91d1\u5c5e\u7684\u5747\u5300\u9540\u8986\u5e76\u4fdd\u6301\u7a33\u5b9a\u7684\u7535\u89e3\u8d28-\u7535\u6781\u754c\u9762\uff0c\u4ece\u800c\u5b9e\u73b0\u4f4e\u963b\u6297\u503c\u3001\u5feb\u901f\u79bb\u5b50\u4f20\u8f93\u548c\u9ad8\u7a7a\u95f4\u5229\u7528\u7387\u7684<\/b><\/strong><strong><b>\u77e9\u9635<\/b><\/strong><strong><b>\u8868\u9762<\/b><\/strong>\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-253457\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72475-4.png\" alt=\"\" width=\"587\" height=\"642\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72475-4.png 587w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72475-4-274x300.png 274w\" sizes=\"(max-width: 587px) 100vw, 587px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>4<\/strong>\u00a0\u5404\u79cd\u950c\u8d1f\u6781\u5728\u5bf9\u79f0\u7535\u6c60\u4e2d\u7684\u7535\u5316\u5b66\u6027\u80fd\u00a9 2023 The Authors<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-253458\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72476-3.png\" alt=\"\" width=\"527\" height=\"545\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72476-3.png 527w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72476-3-290x300.png 290w\" sizes=\"(max-width: 527px) 100vw, 527px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>5<\/strong>\u00a0Zn\u6c89\u79ef\u673a\u7406\u7684\u63a2\u7d22\u00a9 2023 The Authors<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-253459\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72477-2.png\" alt=\"\" width=\"827\" height=\"549\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72477-2.png 827w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72477-2-300x199.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72477-2-768x510.png 768w\" sizes=\"(max-width: 827px) 100vw, 827px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>6<\/strong>\u00a0\u7535\u6781-\u7535\u89e3\u6db2\u754c\u9762\u76f8\u7ec4\u6210\u53ca\u4f20\u8f93\u52a8\u529b\u5b66\u7684\u7814\u7a76\u00a9 2023 The Authors<\/p>\n<p>&nbsp;<\/p>\n<ul>\n<li><b><\/b><strong><b>3D-RFGC@Zn<\/b><\/strong><strong><b>\u8d1f\u6781<\/b><\/strong><strong><b>\u4e0e\u4e0d\u540c3D<\/b><\/strong><strong><b>\u6b63\u6781<\/b><\/strong><strong><b>\u8026\u5408\u7684\u7535\u5316\u5b66\u6027\u80fd<\/b><\/strong><\/li>\n<\/ul>\n<p>&nbsp;<\/p>\n<p>\u4e3a\u4e86\u8bc1\u660e3D\u5206\u5c42\u77f3\u58a8\u70ef\u77e9\u9635\u5728\u5b9e\u9645\u7535\u6c60\u7cfb\u7edf\u4e2d\u7684\u53ef\u884c\u6027\uff0c\u4f7f\u7528Zn\u8d1f\u6781\u548cV<sub>2<\/sub>O<sub>5<\/sub>(MnO<sub>2<\/sub>\u3001AC)\u76843D\u77e9\u9635\u7ec4\u88c5\u5168\u7535\u6c60\uff0c\u5982<strong><b>\u56fe7a<\/b><\/strong>\u6240\u793a\u3002\u901a\u8fc7\u771f\u7a7a\u62bd\u6ee4\uff0c\u57281.0\u2009mg\u2009cm<sup>-2<\/sup>\u548c36\u2009mg\u2009cm<sup>-2<\/sup>\u4e4b\u95f4\u5b9e\u73b0\u4e86\u9ad8\u8d1f\u8f7d\u91cf\u7684V<sub>2<\/sub>O<sub>5<\/sub>@3D-LC\u6b63\u6781\u3002SEM\u7167\u7247\u548cEDS\u9762\u626b\u663e\u793aV<sub>2<\/sub>O<sub>5<\/sub>\u9897\u7c92\u5747\u5300\u5730\u586b\u5145\u57283D\u5b54\u9053\u4e2d(\u56fe7b)\u3002\u5982\u56fe7c\u6240\u793a\uff0cV<sub>2<\/sub>O<sub>5<\/sub>@3D-LC\/3D-RFGC@Zn\u5168\u7535\u6c60\u57282.0\u30014.0\u300120.0\u548c40.0\u2009mA\u2009cm<sup>-2<\/sup>\u7684\u500d\u7387\u4e0b\u5206\u522b\u5b9e\u73b0\u4e86256.55\u3001251.53\u3001199.13\u548c148.06\u2009mAh\u2009g<sup>-1<\/sup>\u7684\u5bb9\u91cf\u3002\u572840.0\u2009mA\u2009cm<sup>-2<\/sup>\u4e0b\uff0cV<sub>2<\/sub>O<sub>5<\/sub>@3D-LC\/3D-RFGC@Zn\u8868\u73b0\u51fa156.2\u2009mAh\u2009g<sup>-1<\/sup>\u7684\u9ad8\u5bb9\u91cf(\u56fe7d)\u3002Zn<sup>2+<\/sup>\u79bb\u5b50\u4f20\u8f93\u7684\u7535\u52a8\u529b\u5b66\u6539\u5584\u53ef\u4ee5\u901a\u8fc7\u539f\u4f4dEIS\u8fdb\u4e00\u6b65\u8bc1\u5b9e(\u56fe7e)\u3002V<sub>2<\/sub>O<sub>5<\/sub>@3D-LC\/\/3D-RFGC@Zn\u5168\u7535\u6c60\u5728\u7b2c\u4e00\u4e2a\u5faa\u73af\u4e2d\u53ef\u4ee5\u89c2\u5bdf\u5230\u8f83\u5c0f\u7684\u7535\u8377\u8f6c\u79fb\u7535\u963b(Rct)(200.61 \u03a9)\uff0c\u5728\u7b2c8\u300120\u548c27\u4e2a\u5faa\u73af\u4e2dRct\u9010\u6e10\u51cf\u5c0f\u523094.46\u300122.18\u548c16.91 \u03a9\u3002\u5982\u6b64\u5c0f\u7684Rct\u8868\u660e\u8f83\u4f4e\u7684\u7535\u8377\u8f6c\u79fb\u7535\u963b\u548c\u5feb\u901f\u7684Zn\u79bb\u5b50\u6269\u6563\u52a8\u529b\u5b66\u3002\u5982\u56fe7f\u6240\u793a\uff0c\u4e0d\u540c\u8d1f\u8f7d\u91cf\u7684V<sub>2<\/sub>O<sub>5<\/sub>@3D-LC\u6b63\u6781\u7684\u9762\u79ef\u6bd4\u5bb9\u91cf\u5206\u522b\u4e3a0.828\u30014.87\u300112.0\u548c16.69\u2009mAh\u2009cm<sup>-2<\/sup>\u3002<strong><b>\u5982\u6b64\u9ad8\u7684<\/b><\/strong><strong><b>\u6b63\u6781<\/b><\/strong><strong><b>\u9762\u79ef\u5bb9\u91cf\u4f18\u4e8e\u8fc4\u4eca\u4e3a\u6b62\u7684\u5927\u591a\u6570\u7814\u7a76\uff0c\u8fd9\u5f52\u56e0\u4e8e\u5177\u6709\u9ad8\u5bfc\u7535\u6027\u548c\u5feb\u901f\u79bb\u5b50\u4f20\u8f93\u901a\u9053\u76843D\u77f3\u58a8\u70ef<\/b><\/strong><strong><b>\u77e9\u9635<\/b><\/strong>\u3002<\/p>\n<p>\u4ee53D-RFGC@Zn\u4e3a\u8d1f\u6781\u7684ZHCs\u5728\u4e0d\u540c\u626b\u901f\u4e0b\u7684\u5faa\u73af\u4f0f\u5b89\u66f2\u7ebf(CV)\u8868\u660e\u5176\u5177\u6709\u4f18\u5f02\u7684\u7535\u5316\u5b66\u53ef\u9006\u6027\u548c\u7a33\u5b9a\u6027(<strong><b>\u56fe7h<\/b><\/strong>)\u3002\u8fd1\u77e9\u5f62\u7684\u8f6e\u5ed3\u8868\u660eAC@3D-LC\/3D-RFGC@Zn\u5177\u6709\u5178\u578b\u7684\u7535\u5bb9\u884c\u4e3a\u3002\u5728\u4e0d\u540c\u7535\u6d41\u5bc6\u5ea6\u4e0b\uff0cAC@3D-LC\/3D-RFGC@Zn\u8868\u73b0\u51fa\u4f18\u5f02\u7684\u5faa\u73af\u548c\u500d\u7387\u6027\u80fd\u3002\u5176\u4e2d\uff0cAC-3D-LC\/3D-RFGC@Zn\u7535\u5bb9\u5668\u57282.0\u300160.0\u548c120.0\u2009mA\u2009cm<sup>-2<\/sup>\u7535\u6d41\u5bc6\u5ea6\u4e0b\u7684\u6bd4\u5bb9\u91cf\u5206\u522b\u4e3a256\u3001152.5\u548c123.5\u2009mAh\u2009g<sup>-1<\/sup>\u3002<strong><b>\u5faa\u73af\u7a33\u5b9a\u6027\u6d4b\u8bd5\u8868\u660e\uff0c\u572840.0\u2009mA\u2009cm<\/b><\/strong><strong><sup><b>-2<\/b><\/sup><\/strong><strong><b>\u7684\u7535\u6d41\u5bc6\u5ea6\u4e0b\uff0c20000\u6b21\u5faa\u73af\u7684\u5bb9\u91cf\u4fdd\u6301\u7387\u4e3a75%\uff0c\u8868\u73b0\u51fa\u4f18\u5f02\u7684\u7a33\u5b9a\u6027(\u56fe7j)\u3002\u603b\u800c\u8a00\u4e4b\uff0c\u5bf9\u4e8eZn\u8d1f\u6781\uff0cGFs\u56e2\u7c07\u548cVGs\u7ec4\u6210\u76843D-RFGC<\/b><\/strong><strong><b>\u77e9\u9635<\/b><\/strong><strong><b>\u5177\u6709\u5927\u7684\u6bd4\u8868\u9762\u79ef\u548c\u9ad8\u6548\u7684\u5bfc\u7535\u7f51\u7edc\uff0c\u6709\u52a9\u4e8e\u51cf\u5c0f\u5c40\u90e8\u7535\u6d41\u5bc6\u5ea6\uff0c\u52a0\u901fZn<\/b><\/strong><strong><sup><b>2+<\/b><\/sup><\/strong><strong><b>\u79bb\u5b50\u7684\u4f20\u5bfc\uff0c\u4ece\u800c\u5b9e\u73b0\u5747\u5300\u7684Zn\u6c89\u79ef<\/b><\/strong>\u3002<\/p>\n<p>\u5bf9\u4e8e3D V<sub>2<\/sub>O<sub>5<\/sub>\u6216<em><i>\u03b1<\/i><\/em>-MnO<sub>2<\/sub>\u548cAC\u6b63\u6781\uff0c\u6574\u4e2a3D\u77f3\u58a8\u70ef\u9aa8\u67b6\u4f7f\u6b63\u6781\u7535\u6781\u5177\u6709\u9ad8\u5bfc\u7535\u7f51\u7edc\uff0c\u4e30\u5bcc\u7684\u591a\u5b54\u901a\u9053\u6709\u5229\u4e8eZn<sup>2+<\/sup>\u79bb\u5b50\u7684\u5feb\u901f\u4f20\u8f93\u3002\u663e\u8457\u7684\u591a\u5b54\u6027\u548c\u4eb2\u950c\u6027\u589e\u52a0\u4e86\u7535\u89e3\u6db2\u7684\u6da6\u6e7f\u6027\u548c\u50a8\u5b58\u6027\u3002<strong><b>\u56e0\u6b64\uff0c<\/b><\/strong><strong><b>\u672c\u5de5\u4f5c<\/b><\/strong><strong><b>\u8bbe\u8ba1\u76843D\u77f3\u58a8\u70ef<\/b><\/strong><strong><b>\u77e9\u9635<\/b><\/strong><strong><b>\u53ef\u4ee5\u6291\u5236AZIBs\u4e2dZn\u8d1f\u6781\u7684\u679d\u6676\u751f\u957f\u548c\u6b63\u6781\u7684\u5faa\u73af\u7a33\u5b9a\u6027\u95ee\u9898<\/b><\/strong>\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-253460\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72478-2.png\" alt=\"\" width=\"579\" height=\"624\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72478-2.png 579w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/\u56fe\u72478-2-278x300.png 278w\" sizes=\"(max-width: 579px) 100vw, 579px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>7<\/strong>\u00a0\u5168\u7535\u6c60\u548c\u7535\u5bb9\u5668\u75283D-RFGC@Zn\u8d1f\u6781\u7684\u7535\u5316\u5b66\u6027\u80fd\u00a9 2023 The Authors<\/p>\n<p>&nbsp;<\/p>\n<p style=\"text-align: center;\"><strong><b>\u4e94\u3001[\u6210\u679c\u542f\u793a]<\/b><\/strong><\/p>\n<p><strong><b>\u00a0<\/b><\/strong><\/p>\n<p><strong><b>\u603b\u4e4b\uff0c\u672c\u5de5\u4f5c\u63d0\u51fa\u4e86\u4e00\u79cd\u65b0\u9896\u7684\u65b9\u6cd5\uff0c\u5229\u7528\u81ea\u652f\u6491\u7684\u3001\u8f7b\u91cf\u7ea7\u7684\u3001\u4eb2\u950c\u76843D\u5206\u7ea7\u77f3\u58a8\u70ef<\/b><\/strong><strong><b>\u77e9\u9635<\/b><\/strong><strong><b>\uff0c\u5305\u62ecN\u63ba\u6742\u7684GF\u56e2\u7c07\u3001VGs\u548c\u591a\u901a\u9053\u78b3<\/b><\/strong><strong><b>\u77e9\u9635<\/b><\/strong><strong><b>\uff0c\u6784\u5efa\u5177\u6709\u4f18\u5f02\u500d\u7387\u548c\u5bb9\u91cf\u7684\u9ad8\u6027\u80fd\u548c\u7a33\u5b9a\u7684Zn\u590d\u5408\u8d1f\u6781<\/b><\/strong>\u3002\u901a\u8fc7\u4e00\u6b65\u70edCVD\u5de5\u827a\u5408\u6210\u76843D-RFGC\u77e9\u9635\u5177\u6709\u9ad8\u7684\u8868\u9762\u79ef\u3001\u5b54\u9699\u7387\u548c\u5747\u5300\u7684\u591a\u5b54\u7ed3\u6784\uff0c\u6709\u6548\u5730\u7f13\u89e3\u4e86\u5c40\u90e8\u7535\u6d41\u5bc6\u5ea6\uff0c\u964d\u4f4e\u4e86Zn<sup>2+<\/sup>\u79bb\u5b50\u6d53\u5ea6\u68af\u5ea6\uff0c\u5e76\u786e\u4fdd\u4e86\u5747\u5300\u7684\u7535\u573a\u5206\u5e03\u4ee5\u8c03\u8282Zn\u6c89\u79ef\u3002\u5bf9\u5177\u6709\u4e30\u5bcc\u4eb2\u950c\u4f4d\u70b9\u7684\u5782\u76f4\u77f3\u58a8\u70ef\u9635\u5217(VGs)\u548c\u77f3\u58a8\u70ef\u7eb3\u7c73\u7ea4\u7ef4\u56e2\u7c07(GFs)\u8fdb\u884c\u8868\u9762\u6539\u6027\uff0c\u53ef\u5b9e\u73b0\u517c\u5177\u9ad8\u7535\u6d41\u5bc6\u5ea6\u548c\u8868\u9762\u9762\u79ef\u5bb9\u91cf\u7684\u9ad8\u6027\u80fd\u950c\u91d1\u5c5e\u8d1f\u6781\u3002<strong><b>\u56e0\u6b64\uff0c\u5728120\u2009mA\u2009cm<\/b><\/strong><strong><sup><b>-2<\/b><\/sup><\/strong><strong><b>\u7684\u9ad8\u7535\u6d41\u5bc6\u5ea6\u4e0b\uff0c3D-RFGC@Zn\u8d1f\u6781\u57283000\u6b21\u5faa\u73af\u4e2d\u8868\u73b0\u51fa99.67%\u7684CE\u548c\u8f83\u4f4e\u7684\u8fc7\u7535\u4f4d<\/b><\/strong>\u3002<\/p>\n<p>\u6b64\u5916\uff0c\u5f53\u63ba\u5165\u5168\u7535\u6c60\uff0c\u5982V<sub>2<\/sub>O<sub>5<\/sub>@3D-LC\/3D-RFGC@Zn\uff0cMnO<sub>2<\/sub>@3D-LC\/3D-RFGC@Zn\u548cAC@3D-LC\/3D-RFGC@Zn\u7535\u5bb9\u5668\uff0c\u8fd9\u4e9b3D\u77f3\u58a8\u70ef\u77e9\u9635\u6709\u52a9\u4e8e\u4fc3\u8fdb\u5747\u5300\u7684Zn\u6c89\u79ef\uff0c\u4ece\u800c\u6709\u52a9\u4e8e\u4f18\u5f02\u7684\u500d\u7387\u6027\u80fd\u548c\u663e\u8457\u63d0\u9ad8\u7684\u5faa\u73af\u7a33\u5b9a\u6027\u3002<strong><b>\u8fd9\u79cd\u4f7f\u7528\u4e09\u7ef4\u77f3\u58a8\u70ef\u4f5c\u4e3a\u950c\u8d1f\u6781\u7684\u7b56\u7565\u4e3a\u5f00\u53d1\u80fd\u591f\u5728\u9ad8\u500d\u7387\u3001\u9ad8\u5bb9\u91cf\u548c\u653e\u7535\u6df1\u5ea6\u6761\u4ef6\u4e0b\u8fd0\u884c\u7684\u91d1\u5c5e\u8d1f\u6781\u63d0\u4f9b\u4e86\u4e00\u6761\u6709\u524d\u9014\u7684\u9014\u5f84<\/b><\/strong>\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u7b2c\u4e00\u4f5c\u8005\uff1aYongbiao Mu\u3001Zheng Li\u3001Bu-ke Wu<\/p>\n<p>\u901a\u8baf\u4f5c\u8005\uff1aLin Zeng\u3001Tianshou Zhao<\/p>\n<p>\u901a\u8baf\u5355\u4f4d\uff1a\u5357\u65b9\u79d1\u6280\u5927\u5b66<\/p>\n<p>\u8bba\u6587doi\uff1ahttps:\/\/doi.org\/10.1038\/s41467-023-39947-8<\/p>\n<p>&nbsp;<\/p>\n<p>\u672c\u6587\u7531\u6e29\u534e\u4f9b\u7a3f\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u5357\u65b9\u79d1\u6280\u5927\u5b66\u66fe\u6797&amp;\u8d75\u5929\u5bff\u6559\u6388\u6700\u65b0NC\uff1a3D\u5206\u7ea7\u77f3\u58a8\u70ef\u77e9\u9635\u4e3a\u6c34\u7cfb\u950c\u7535\u6c60\u63d0\u4f9b\u4e86\u7a33\u5b9a\u7684\u950c\u8d1f\u6781 \u4e00\u3001[\u5bfc\u8bfb] \u00a0 \u91d1\u5c5e\u950c(Zn)\u7531\u4e8e\u5177\u6709\u8f83\u9ad8\u7684\u7406\u8bba\u5bb9\u91cf(820\u2009&#8230;<\/p>\n","protected":false},"author":34419,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215,2],"tags":[3411,5081,5082],"class_list":["post-253442","post","type-post","status-publish","format-standard","hentry","category-jiedu","category-keji","tag-3411","tag-5081","tag-5082"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/253442"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/34419"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=253442"}],"version-history":[{"count":4,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/253442\/revisions"}],"predecessor-version":[{"id":253477,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/253442\/revisions\/253477"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=253442"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=253442"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=253442"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}