{"id":253830,"date":"2023-08-28T09:50:33","date_gmt":"2023-08-28T01:50:33","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=253830"},"modified":"2023-08-28T09:50:33","modified_gmt":"2023-08-28T01:50:33","slug":"%e5%8c%97%e7%90%86%e5%b7%a5adv-mater-%ef%bc%9a%e8%87%aa%e8%af%b1%e5%af%bc%e5%8f%8c%e5%b1%82%e5%9b%ba%e4%bd%93%e7%94%b5%e8%a7%a3%e8%b4%a8%e7%95%8c%e9%9d%a2%e5%ae%9e%e7%8e%b0%e8%b6%85%e7%a8%b3%e5%ae%9a","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=253830","title":{"rendered":"\u5317\u7406\u5de5Adv. Mater.\uff1a\u81ea\u8bf1\u5bfc\u53cc\u5c42\u56fa\u4f53\u7535\u89e3\u8d28\u754c\u9762\u5b9e\u73b0\u8d85\u7a33\u5b9a\u9502\u91d1\u5c5e\u7535\u6c60"},"content":{"rendered":"<p><strong>\u4e00\u3001\u3010\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p>\u968f\u7740\u4fbf\u643a\u5f0f\u3001\u67d4\u6027\u7535\u5b50\u8bbe\u5907\u7684\u5feb\u901f\u53d1\u5c55\uff0c\u9502\u79bb\u5b50\u7535\u6c60\u9010\u6e10\u4e0d\u80fd\u6ee1\u8db3\u65e5\u76ca\u589e\u957f\u7684\u5927\u529f\u7387\u50a8\u80fd\u8bbe\u5907\u7684\u9700\u6c42\u3002\u91d1\u5c5e\u9502\u88ab\u8ba4\u4e3a\u662f\u9ad8\u6bd4\u80fd\u7535\u6c60\u6700\u6709\u524d\u9014\u7684\u9633\u6781\u6750\u6599\u4e4b\u4e00\uff0c\u800c\u9502\u8868\u9762\u603b\u662f\u53d1\u751f\u4e0d\u53ef\u9006\u7684\u5316\u5b66\u53cd\u5e94\uff0c\u4e0d\u65ad\u6d88\u8017\u6d3b\u6027\u9502\u7535\u89e3\u8d28\u3002\u56fa\u4f53\u7535\u89e3\u8d28\u754c\u9762\u5c42\uff08SEI\uff09\u88ab\u8ba4\u4e3a\u662f\u4fdd\u62a4\u9502\u91d1\u5c5e\u9633\u6781\u7684\u5173\u952e\u90e8\u4ef6\u3002\u5faa\u73af\u540e\u5728\u9502\u91d1\u5c5e\u9633\u6781\u4e0a\u81ea\u7136\u5f62\u6210\u7684SEI\u8584\u819c\u5316\u5b66\u6210\u5206\u548c\u7269\u7406\u7ed3\u6784\u4e0d\u5747\u5300\u3001\u673a\u68b0\u5f3a\u5ea6\u5f31\u3001\u8106\u6027\u5927\uff0c\u96be\u4ee5\u9002\u5e94\u7535\u5316\u5b66\u5faa\u73af\u8fc7\u7a0b\u4e2d\u4f53\u79ef\u7684\u53d8\u5316\uff0c\u6781\u6613\u5bfc\u81f4\u7535\u6c60\u77ed\u8def\u548c\u7535\u6c60\u6027\u80fd\u4e0b\u964d\u3002\u8fd1\u5e74\u6765\u5f00\u53d1\u4e86\u591a\u79cd\u7b56\u7565\u6765\u8bbe\u8ba1\u9502\u9633\u6781\u7684\u754c\u9762\u5c42\uff0c\u7136\u800c\u4ee5\u53ef\u6269\u5c55\u548c\u4f4e\u635f\u8017\u7684\u65b9\u5f0f\u6784\u5efa\u53ef\u63a7\u7684\u53cc\u5c42SEI\u4ecd\u7136\u662f\u6539\u5584\u9502\u91d1\u5c5e\u9633\u6781\u6027\u80fd\u7684\u91cd\u8981\u95ee\u9898\u3002<\/p>\n<p><strong>\u00a0<\/strong><strong>\u4e8c\u3001\u3010\u6210\u679c\u63a0\u5f71\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u5317\u4eac\u7406\u5de5\u5927\u5b66\u9648\u4eba\u6770\u56e2\u961f<\/strong>\u4ee5\u53ef\u6269\u5c55\u3001\u4f4e\u635f\u8017\u7684\u65b9\u5f0f\u6784\u5efa\u4e86\u4e00\u79cd\u7528\u4e8e\u9502\u91d1\u5c5e\u9633\u6781\u7684\u53ef\u63a7\u53cc\u5c42SEI\u3002\u5728\u521d\u59cb\u5faa\u73af\u671f\u95f4\uff0cSEI\u7531\u9884\u6c89\u79ef\u7684LiAlO<sub>2<\/sub>\uff08LAO\uff09\u5c42\u81ea\u611f\u5e94\uff0c\u5176\u4e2d\u7531\u4e8e\u7535\u5b50\u96a7\u7a7fLAO\u800c\u4ea7\u751f\u5916\u90e8\u6709\u673a\u5c42\uff0c\u5bfc\u81f4\u7535\u89e3\u8d28\u8fd8\u539f\u3002\u575a\u56fa\u7684\u5185\u90e8LAO\u5c42\u7531\u4e8e\u5176\u826f\u597d\u7684\u673a\u68b0\u5f3a\u5ea6\u3001\u79bb\u5b50\u5bfc\u7535\u6027\u53ef\u4ee5\u4fc3\u8fdb\u5747\u5300\u7684Li\u6c89\u79ef\uff0c\u5916\u90e8\u6709\u673a\u5c42\u53ef\u4ee5\u8fdb\u4e00\u6b65\u63d0\u9ad8SEI\u7684\u7a33\u5b9a\u6027\u3002\u5f97\u76ca\u4e8e\u8fd9\u79cd\u53cc\u5c42SEI\u7684\u663e\u8457\u6548\u679c\uff0c\u63d0\u9ad8\u4e86LAO-Li\u9633\u6781\u7684\u7535\u5316\u5b66\u6027\u80fd\u3002\u6b64\u5916\uff0c\u53ef\u4ee5\u5bb9\u6613\u5730\u83b7\u5f97\u5927\u5c3a\u5bf8\u7684LAO-Li\u6837\u54c1\uff0c\u6539\u6027Li\u91d1\u5c5e\u9633\u6781\u7684\u5236\u5907\u663e\u793a\u51fa\u5927\u89c4\u6a21\u751f\u4ea7\u7684\u5de8\u5927\u6f5c\u529b\u3002\u8fd9\u9879\u5de5\u4f5c\u7a81\u51fa\u4e86\u8fd9\u79cd\u81ea\u8bf1\u5bfc\u53cc\u5c42SEI\u5728\u9502\u91d1\u5c5e\u9633\u6781\u5546\u4e1a\u5316\u65b9\u9762\u7684\u5de8\u5927\u6f5c\u529b\u3002\u7814\u7a76\u6210\u679c\u4ee5\u9898\u4e3a\u201c<strong>Self-Induced Dual-Layered Solid Electrolyte Interphase with High Toughness and High Ionic Conductivity for Ultra-Stable Lithium Metal Batteries<\/strong>\u201d\u53d1\u8868\u5728\u77e5\u540d\u671f\u520a<strong><em>Adv. Mater.<\/em><\/strong>\u4e0a\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-253831\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/0-11.png\" alt=\"\" width=\"600\" height=\"262\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/0-11.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/0-11-300x131.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u4e09\u3001\u3010\u6838\u5fc3\u521b\u65b0\u70b9\u3011<\/strong><\/p>\n<p>\u672c\u7814\u7a76\u4ee5\u53ef\u6269\u5c55\u548c\u4f4e\u635f\u8017\u7684\u65b9\u5f0f\u6784\u5efa\u4e86\u4e00\u79cd\u53ef\u63a7\u7684\u53cc\u5c42SEI\uff0c\u7531\u6b64\u5f00\u53d1\u7684\u5bf9\u79f0\u7535\u6c60\u8868\u73b0\u51fa\u5353\u8d8a\u7684\u957f\u671f\u5faa\u73af\u7a33\u5b9a\u6027\uff0c\u5728\u7535\u6d41\u5bc6\u5ea6\u4e3a1 mA cm<sup>-2<\/sup>\u548c\u9762\u79ef\u5bb9\u91cf\u4e3a1 mAh cm<sup>-2<\/sup>\u7684\u6761\u4ef6\u4e0b\uff0c\u53ef\u4fdd\u6301\u4f4e\u8fc7\u7535\u4f4d\u8fbe1800\u5c0f\u65f6\u3002<\/p>\n<p><strong>\u56db\u3001\u3010\u6570\u636e\u6982\u89c8\u3011<\/strong><\/p>\n<p><strong>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-253832\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/1-26.png\" alt=\"\" width=\"600\" height=\"658\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/1-26.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/1-26-274x300.png 274w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/strong><\/p>\n<p><strong>\u56fe<\/strong><strong>1\u00a0 <\/strong><strong>\u9502\u91d1\u5c5e\u9633\u6781\u4e0a<\/strong><strong>SEI<\/strong><strong>\u5f62\u6210\u793a\u610f\u56fe<\/strong><strong> \u00a9 2023 Wiley<\/strong><\/p>\n<p>\u9502\u91d1\u5c5e\u9633\u6781\u4e0a\u5f62\u6210\u7684\u81ea\u7136SEI\uff08\u4e0a\u56fe\uff09\u548c\u76ee\u6807\u53cc\u5c42SEI\uff08\u4e0b\u56fe\uff09\u793a\u610f\u56fe\uff0c\u4ee5\u53ca\u4e0d\u540cSEI\u7684\u9502\u91d1\u5c5e\u9633\u6781\u5728\u5faa\u73af\u540e\u7684\u76f8\u5e94\u5f62\u8c8c\u53d8\u5316\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-253833\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/2-23.png\" alt=\"\" width=\"600\" height=\"551\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/2-23.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/2-23-300x276.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>2\u00a0 LAO<\/strong><strong>\u819c\u7684\u8868\u5f81<\/strong><strong> \u00a9 2023 Wiley<\/strong><\/p>\n<p>\uff08a\uff09\u7528\u4e8e\u8bc4\u4f30LAO\u8584\u819c\u9502\u79bb\u5b50\u4f20\u5bfc\u6027\u7684\u7535\u6c60\u793a\u610f\u56fe\u3002<\/p>\n<p>\uff08b\uff09\u5305\u542b\u4ee5\u4e0d\u540c\u6e85\u5c04\u65f6\u95f4\u5236\u5907\u7684 LAO \u8584\u819c\u7684\u7535\u6c60\u7684Nyquist\u56fe\u3002<\/p>\n<p>\uff08c\uff09\u4ece(b)\u4e2d\u83b7\u5f97\u7684\u76f8\u5e94\u7535\u963b\u503c\u548c\u79bb\u5b50\u7535\u5bfc\u7387\u503c\u3002<\/p>\n<p>\uff08d-e\uff09\u672a\u6539\u6027\u7684Li\u548cLAO-Li\u7535\u6781\u7684SEM\u56fe\u50cf\u3002<\/p>\n<p>\uff08f\uff09LAO-Li\u9633\u6781\u7684EDS\u5143\u7d20\u56fe\u8c31\u3002<\/p>\n<p>\uff08g-i\uff09LAO-Li\u9633\u6781\u7684AFM\u5f62\u8c8c\u56fe\u50cf\u3001\u76f8\u5e94\u7684\u6768\u6c0f\u6a21\u91cf\u5206\u5e03\u53ca\u5176\u5b9a\u91cf\u5206\u5e03\u3002<\/p>\n<p>\uff08j\uff09\u672a\u6539\u6027\u9502\u9633\u6781\u548cLAO-Li\u9633\u6781\u66b4\u9732\u4e8e\u7a7a\u6c14\u4e2d2\u5929\u524d\u540e\u7684\u5149\u5b66\u7167\u7247\u3002<\/p>\n<p>\uff08k-m\uff09\u672a\u6539\u6027\u9502\u7535\u6781\u548cLAO\u9502\u7535\u6781\u7684\u5bf9\u79f0\u7535\u6c60\u572836\u5c0f\u65f6\u9759\u7f6e\u8fc7\u7a0b\u4e2d\u7684Nyquist\u56fe\u4ee5\u53ca\u76f8\u5e94\u7535\u963b\u503c\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-253834\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/3-23.png\" alt=\"\" width=\"600\" height=\"647\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/3-23.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/3-23-278x300.png 278w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>3\u00a0 LAO-Li<\/strong><strong>\u9633\u6781\u4e0a\u5f62\u6210\u7684<\/strong><strong>SEI<\/strong><strong>\u5c42\u7684\u53cc\u5c42\u7279\u5f81<\/strong><strong> \u00a9 2023 Wiley<\/strong><\/p>\n<p>\uff08a-b\uff09\u672a\u6539\u6027\u9502\u548cLAO-Li\u9633\u6781\u57283\u4e2a\u5468\u671f\u540e\u7684XPS\u56fe\u8c31\u3002<\/p>\n<p>\uff08c\uff09LAO-Li\u9633\u6781\u5728\u4e0d\u540c\u8680\u523b\u6df1\u5ea6\u4e0b\u7ecf\u8fc73\u4e2a\u5468\u671f\u540e\u7684C 1s\u3001N 1s\u3001O 1s\u3001Al 2p \u548cLi 1s XPS\u8c31\u3002<\/p>\n<p>\uff08d\uff09\u672a\u6539\u6027\u9502\u548cLAO-Li\u9633\u6781\u7ecf\u8fc73\u4e2a\u5468\u671f\u540e\u7684AFM\u5f62\u8c8c\u56fe\u3002<\/p>\n<p>\uff08e-f\uff09\u672a\u6539\u6027\u9502\u548cLAO-Li\u9633\u6781\u4e0aSEI\u5c42\u7684\u6768\u6c0f\u6a21\u91cf\u5b9a\u91cf\u5206\u5e03\u548c3\u4e2a\u5468\u671f\u540e\u7684\u529b-\u5206\u79bb\u8ddd\u79bb\u66f2\u7ebf\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-253835\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/4-22.png\" alt=\"\" width=\"600\" height=\"667\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/4-22.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/4-22-270x300.png 270w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>4\u00a0 Li<\/strong><strong>\u6c89\u79ef\u884c\u4e3a<\/strong><strong> \u00a9 2023 Wiley<\/strong><\/p>\n<p>\uff08a-b\uff09\u5bf9\u79f0\u900f\u660e\u7535\u6c60\u4e2d\u672a\u6539\u6027\u9502\u548cLAO-Li\u9633\u6781\u57281 mA cm<sup>-2<\/sup>\u7535\u6d41\u5bc6\u5ea6\u4e0b\u6c89\u79ef\u950230\u5206\u949f\u524d\u540e\u7684\u6a2a\u622a\u9762\u5149\u5b66\u663e\u5fae\u955c\u56fe\u50cf\u3002<\/p>\n<p>\uff08c-d\uff09\u9540\u950230\u5206\u949f\u540e\u76f8\u5e94\u7684\u4e09\u7ef4\u5149\u5b66\u8f6e\u5ed3\u6d4b\u91cf\u56fe\u50cf\u3002<\/p>\n<p>\uff08e\uff09\u5728\u7535\u6d41\u5bc6\u5ea6\u6539\u53d8\u65f6\uff0c\u4f7f\u7528\u672a\u6539\u6027\u9502\u548cLAO-Li\u9633\u6781\u7684\u5bf9\u79f0\u7535\u6c60\u7684\u9502\u5265\u79bb\u548c\u6c89\u79ef\u66f2\u7ebf\u3002<\/p>\n<p>\uff08f\uff09\u672a\u6539\u6027\u9502\u548cLAO-Li\u9633\u6781\u7684\u5bf9\u79f0\u7535\u6c60\u7684\u957f\u671f\u5faa\u73af\u7a33\u5b9a\u6027\u3002<\/p>\n<p>\uff08g-h\uff09\u672a\u6539\u6027\u9502\u9633\u6781\u548cLAO-Li\u9633\u6781\u5faa\u73af100\u6b21\u540e\u7684SEM\u56fe\u50cf\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-253836\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/5-18.png\" alt=\"\" width=\"600\" height=\"675\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/5-18.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/5-18-267x300.png 267w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>5\u00a0 <\/strong><strong>\u7535\u6c60\u6027\u80fd\u8bc4\u4f30<\/strong><strong> \u00a9 2023 Wiley<\/strong><\/p>\n<p>\uff08a-b\uff09\u91c7\u7528\u672a\u6539\u6027\u9502\u548cLAO-Li\u9633\u6781\u7684Li-S\u7535\u6c60\u57280.2 C\u65f6\u7684\u500d\u7387\u6027\u80fd\u548c\u5faa\u73af\u6027\u80fd\u3002<\/p>\n<p>\uff08c-d\uff09\u91c7\u7528\u672a\u6539\u6027\u9502\u548cLAO-Li\u9633\u6781\u7684Li-LTO\u7535\u6c60\u57285 C\u65f6\u7684\u500d\u7387\u6027\u80fd\u548c\u5faa\u73af\u6027\u80fd\u3002<\/p>\n<p>\uff08e-f\uff09\u91c7\u7528\u672a\u6539\u6027\u9502\u548cLAO-Li\u9633\u6781\u7684Li-LFP\u7535\u6c60\u57281 C\u65f6\u7684\u500d\u7387\u6027\u80fd\u548c\u5faa\u73af\u6027\u80fd\u3002<\/p>\n<p>\uff08g-h\uff09\u91c7\u7528\u672a\u6539\u6027\u9502\u548cLAO-Li\u9633\u6781\u7684Li-NCM811\u7535\u6c60\u57281 C\u65f6\u7684\u500d\u7387\u6027\u80fd\u548c\u5faa\u73af\u6027\u80fd\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-253837\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/6-10.png\" alt=\"\" width=\"600\" height=\"283\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/6-10.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/08\/6-10-300x142.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>6\u00a0 <\/strong><strong>\u53ef\u6269\u5c55\u6027\u7814\u7a76<\/strong><strong> \u00a9 2023 Wiley<\/strong><\/p>\n<p>\uff08a\uff09\u672a\u6539\u6027\u9502\u7b94\u548cLAO-Li\u7b94\u7684\u7167\u7247\u3002<\/p>\n<p>\uff08b\uff09LAO-Li\u7684\u8fde\u7eed\u5377\u5bf9\u5377\u5236\u9020\u793a\u610f\u56fe\u3002<\/p>\n<p>\uff08c-e\uff09\u5e26\u6709LAO-Li\u9633\u6781\u548cNCM532\u9634\u6781\u7684\u8f6f\u5305\u7535\u6c60\u7ed3\u6784\u793a\u610f\u56fe\uff0c\u4ee5\u53ca\u76f8\u5e94\u7684\u7535\u6c60\u7684\u5faa\u73af\u6027\u80fd\u548c\u5145\u653e\u7535\u66f2\u7ebf\u3002<\/p>\n<p><strong>\u00a0<\/strong><strong>\u00a0<\/strong><\/p>\n<p><strong>\u4e94\u3001\u3010\u6210\u679c\u542f\u793a\u3011<\/strong><\/p>\n<p>\u7efc\u4e0a\uff0c\u672c\u7814\u7a76\u4ee5\u53ef\u6269\u5c55\u548c\u4f4e\u635f\u8017\u7684\u65b9\u5f0f\u6784\u5efa\u4e86\u4e00\u79cd\u53ef\u63a7\u7684\u53cc\u5c42SEI\uff0c\u4ee5\u63d0\u9ad8\u9502\u91d1\u5c5e\u7535\u6c60\u7684\u6027\u80fd\u3002\u5728\u521d\u59cb\u5faa\u73af\u4e2d\uff0cLAO\u5c42\u4f5c\u4e3a\u5185\u5c42\u65e0\u673a\u5c42\uff0c\u800c\u5916\u5c42\u6709\u673a\u5c42\u5219\u662f\u7531\u4e8e\u7535\u5b50\u96a7\u7a7fLAO\u800c\u4ea7\u751f\u7684\uff0c\u4ece\u800c\u5bfc\u81f4\u7535\u89e3\u6db2\u8fd8\u539f\u3002\u7531\u4e8e\u5177\u6709\u826f\u597d\u7684\u673a\u68b0\u5f3a\u5ea6\u548c\u79bb\u5b50\u5bfc\u7535\u6027\uff0c\u575a\u56fa\u7684LAO\u5185\u5c42\u80fd\u6709\u6548\u6291\u5236\u9502\u679d\u6676\u7684\u751f\u957f\uff0c\u5e76\u5b9e\u73b0\u5747\u5300\u7684\u9502\u6c89\u79ef\u3002\u540c\u65f6\uff0c\u5916\u5c42\u6709\u673a\u5c42\u8fd8\u80fd\u8fdb\u4e00\u6b65\u63d0\u9ad8\u9502\u91d1\u5c5e\u9633\u6781\u548c\u7535\u89e3\u6db2\u4e4b\u95f4\u754c\u9762\u7684\u7a33\u5b9a\u6027\u3002\u5f97\u76ca\u4e8e\u8fd9\u79cd\u53cc\u5c42SEI\uff0c\u91c7\u7528LAO-Li\u7535\u6781\u7684\u9502\u5bf9\u79f0\u7535\u6c60\u8868\u73b0\u51fa\u5353\u8d8a\u7684\u957f\u671f\u5faa\u73af\u7a33\u5b9a\u6027\uff0c\u5728\u7535\u6d41\u5bc6\u5ea6\u4e3a1 mA cm<sup>-2<\/sup>\u548c\u9762\u79ef\u5bb9\u91cf\u4e3a1 mAh cm<sup>-2<\/sup>\u7684\u6761\u4ef6\u4e0b\uff0c\u53ef\u4fdd\u6301\u4f4e\u8fc7\u7535\u4f4d\u8fbe1800\u5c0f\u65f6\u3002\u5728\u4f7f\u7528S\u3001NCM811\u3001LTO\u548cLFP\u9634\u6781\u7684\u5168\u7535\u6c60\u4e2d\u4e5f\u8bc1\u660e\u4e86LAO-Li\u9633\u6781\u7684\u5353\u8d8a\u7684\u7535\u5316\u5b66\u6027\u80fd\u3002\u6b64\u5916\uff0cLAO-Li\u9633\u6781\u7684\u5236\u9020\u5177\u6709\u9ad8\u5ea6\u53ef\u6269\u5c55\u6027\u3002\u5373\u4f7f\u4f7f\u7528\u5b9e\u9a8c\u5ba4\u7ea7\u78c1\u63a7\u6e85\u5c04\u7cfb\u7edf\uff0c\u4e5f\u80fd\u8f7b\u677e\u83b7\u5f97\u5927\u5c3a\u5bf8\u7684LAOLi\u6837\u54c1\u3002\u672c\u5de5\u4f5c\u7684\u81ea\u8bf1\u5bfc\u53cc\u5c42SEI\u7684LAO-Li\u9633\u6781\u7684\u8bbe\u8ba1\u548c\u5236\u5907\u4e3aLMB\u7684\u5546\u4e1a\u5316\u5960\u5b9a\u4e86\u57fa\u7840\u3002<\/p>\n<p><strong>\u539f\u6587\u8be6\u60c5<\/strong>\uff1a<a href=\"https:\/\/onlinelibrary.wiley.com\/doi\/abs\/10.1002\/adma.202303710\" target=\"_blank\" rel=\"noopener\">Self-Induced Dual-Layered Solid Electrolyte Interphase with High Toughness and High Ionic Conductivity for Ultra-Stable Lithium Metal Batteries <\/a>(<em>Adv. Mater. <\/em><strong>2023<\/strong>, 2303710)<\/p>\n<p>\u672c\u6587\u7531\u5927\u5175\u54e5\u4f9b\u7a3f\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u4e00\u3001\u3010\u5bfc\u8bfb\u3011 \u968f\u7740\u4fbf\u643a\u5f0f\u3001\u67d4\u6027\u7535\u5b50\u8bbe\u5907\u7684\u5feb\u901f\u53d1\u5c55\uff0c\u9502\u79bb\u5b50\u7535\u6c60\u9010\u6e10\u4e0d\u80fd\u6ee1\u8db3\u65e5\u76ca\u589e\u957f\u7684\u5927\u529f\u7387\u50a8\u80fd\u8bbe\u5907\u7684\u9700\u6c42\u3002\u91d1\u5c5e\u9502\u88ab\u8ba4\u4e3a\u662f\u9ad8\u6bd4\u80fd\u7535\u6c60\u6700\u6709\u524d\u9014\u7684\u9633\u6781\u6750\u6599\u4e4b\u4e00\uff0c\u800c\u9502\u8868\u9762&#8230;<\/p>\n","protected":false},"author":1004,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-253830","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/253830"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/1004"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=253830"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/253830\/revisions"}],"predecessor-version":[{"id":253865,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/253830\/revisions\/253865"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=253830"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=253830"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=253830"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}