{"id":254159,"date":"2023-09-07T06:51:21","date_gmt":"2023-09-06T22:51:21","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=254159"},"modified":"2023-09-08T15:04:04","modified_gmt":"2023-09-08T07:04:04","slug":"%e6%96%b0%e5%8a%a0%e5%9d%a1%e5%9b%bd%e7%ab%8b%e5%a4%a7%e5%ad%a6%e5%90%95%e5%8a%9b%e6%95%99%e6%8e%88%e5%9b%a2%e9%98%9fadv-energy-mater-%e7%bb%bc%e8%bf%b0%ef%bc%9a%e7%94%a8%e4%ba%8e%e9%ab%98%e8%83%bd","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=254159","title":{"rendered":"\u65b0\u52a0\u5761\u56fd\u7acb\u5927\u5b66\u5415\u529b\u6559\u6388\u56e2\u961fAdv. Energy Mater.\u7efc\u8ff0\uff1a\u7528\u4e8e\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u9502\u7535\u6c60\u7684\u805a\u5408\u7269\u56fa\u6001\u7535\u89e3\u8d28"},"content":{"rendered":"<p><strong><b>\u4e00\u3001\u3010\u5bfc\u8bfb\u3011<\/b><\/strong><\/p>\n<p>\u8fd1\u5e74\u6765\uff0c\u9502\u7535\u6c60\u5df2\u88ab\u5e7f\u6cdb\u5e94\u7528\u4e8e\u79fb\u52a8\u7535\u5b50\u8bbe\u5907\uff0c\u7535\u52a8\u6c7d\u8f66\uff0c\u5927\u578b\u50a8\u80fd\u88c5\u7f6e\u548c\u536b\u661f\u7b49\u7279\u6b8a\u9886\u57df\u3002\u5176\u4e2d\uff0c\u79fb\u52a8\u7535\u5b50\u8bbe\u5907\u548c\u7535\u52a8\u6c7d\u8f66\u7684\u5feb\u901f\u53d1\u5c55\u4f7f\u5f97\u4eba\u4eec\u5bf9\u9502\u7535\u6c60\u7684\u80fd\u91cf\u5bc6\u5ea6\u548c\u5b89\u5168\u6027\u9700\u6c42\u4e0d\u65ad\u589e\u52a0\u3002\u4e0e\u4f7f\u7528\u4f20\u7edf\u6db2\u6001\u7535\u89e3\u6db2\u7684\u7535\u6c60\u76f8\u6bd4\uff0c\u56fa\u6001\u7535\u6c60\u7684\u5b89\u5168\u6027\u66f4\u9ad8\uff0c\u4e14\u901a\u8fc7\u51cf\u5c0f\u56fa\u6001\u7535\u89e3\u8d28\u4f53\u79ef\u3001\u6216\u8005\u72ec\u7279\u7535\u6c60\u8bbe\u8ba1\uff0c\u56fa\u6001\u7535\u6c60\u8fd8\u80fd\u83b7\u5f97\u66f4\u9ad8\u7684\u80fd\u91cf\u5bc6\u5ea6\u3002\u7136\u800c\uff0c\u5f53\u524d\u56fa\u6001\u7535\u6c60\u4e2d\u7684\u7535\u6781\/\u7535\u89e3\u8d28\u754c\u9762\u63a5\u89e6\/\u6da6\u6e7f\u4ecd\u662f\u4e00\u9879\u96be\u9898\u3002\u4e0e\u6db2\u6001\u7535\u89e3\u6db2\u4e0d\u540c\uff0c\u5927\u591a\u6570\u56fa\u6001\u7535\u89e3\u8d28\u96be\u4ee5\u6da6\u6e7f\u3001\u6e17\u900f\u7535\u6781\uff0c\u5bfc\u81f4\u7535\u6781\u5185\u90e8\u4ee5\u53ca\u7535\u6781\/\u7535\u89e3\u8d28\u754c\u9762\u7684\u79bb\u5b50\u4f20\u5bfc\u53d7\u9650\uff0c\u5e76\u963b\u788d\u4e86\u56fa\u6001\u7535\u6c60\u4e2d\u9ad8\u8d1f\u8f7d\u539a\u7535\u6781\u7684\u4f7f\u7528\u3002\u76f8\u6bd4\u4e8e\u5176\u4ed6\u56fa\u6001\u7535\u89e3\u8d28\uff0c\u805a\u5408\u7269\u7535\u89e3\u8d28\u7531\u4e8e\u5176\u67d4\u8f6f\u7279\u6027\uff0c\u53ef\u4e0e\u7535\u6781\u5f62\u6210\u8f83\u597d\u63a5\u89e6\u3002\u901a\u8fc7\u5728\u805a\u5408\u7269\u4e2d\u6dfb\u52a0\u6db2\u4f53\u6210\u5206\uff0c\u6216\u539f\u4f4d\u805a\u5408\u7535\u89e3\u8d28\u4ee5\u53ca\u6784\u5efa\u4e00\u4f53\u5316\u7535\u6781-\u7535\u89e3\u8d28\u90fd\u80fd\u589e\u5f3a\u805a\u5408\u7269\u7535\u89e3\u8d28\u5bf9\u7535\u6781\u7684\u6da6\u6e7f\u6027\uff0c\u8fdb\u4e00\u6b65\u63d0\u9ad8\u7535\u6c60\u7684\u80fd\u91cf\u5bc6\u5ea6\u3002\u9664\u6b64\u4e4b\u5916\uff0c\u7535\u6781\/\u7535\u89e3\u8d28\u754c\u9762\u7684\u7535\u5316\u5b66\/\u5316\u5b66\u7a33\u5b9a\u6027\u3001\u7a7a\u95f4\u7535\u8377\u5c42\u4ee5\u53ca\u679d\u6676\u751f\u957f\u95ee\u9898\u4ecd\u7136\u5f71\u54cd\u7740\u7535\u6c60\u7684\u80fd\u91cf\u5bc6\u5ea6\u548c\u5faa\u73af\u7a33\u5b9a\u6027\u3002\u56fe1\u603b\u7ed3\u4e86\u9502\u7535\u6c60\u7684\u5e94\u7528\u9886\u57df\u4e0e\u7535\u6781\/\u805a\u5408\u7269\u7535\u89e3\u8d28\u754c\u9762\u5b58\u5728\u7684\u95ee\u9898\u3002<\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-2.png\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-254161\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-2.png\" alt=\"\" width=\"800\" height=\"430\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-2.png 800w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-2-300x161.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-2-768x413.png 768w\" sizes=\"(max-width: 800px) 100vw, 800px\" \/><\/a><\/p>\n<p>\u56fe1\u00a0\u9502\u7535\u6c60\u7684\u5e94\u7528\u9886\u57df\u4e0e\u7535\u6781\/\u805a\u5408\u7269\u7535\u89e3\u8d28\u754c\u9762\u5b58\u5728\u7684\u95ee\u9898<\/p>\n<p><strong><b>\u4e8c\u3001\u3010\u6210\u679c\u63a0\u5f71\u3011<\/b><\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong><b>\u65b0\u52a0\u5761\u56fd\u7acb\u5927\u5b66\u5415\u529b\u6559\u6388\u56e2\u961f<\/b><\/strong>\u4ece\u9502\u7535\u6c60\u80fd\u91cf\u5bc6\u5ea6\u7684\u89d2\u5ea6\u51fa\u53d1\uff0c\u603b\u7ed3\u4e86\u805a\u5408\u7269\u56fa\u6001\u7535\u89e3\u8d28\u76f8\u5173\u7684\u7814\u7a76\u8fdb\u5c55\u3002\u76f8\u5173\u7efc\u8ff0\u5de5\u4f5c\u4ee5\u201cPolymer\u2010Based Solid\u2010State Electrolytes for High\u2010Energy\u2010Density Lithium\u2010Ion Batteries \u2013 Review\u201d\u4e3a\u9898\u53d1\u8868\u5728<em><i>Advanced Energy Materials<\/i><\/em>\uff08IF=27.8\uff09\u4e0a\uff0c\u65b0\u52a0\u5761\u56fd\u7acb\u5927\u5b66\u7855\u58eb\u751f\u5362\u9704\u548c\u65b0\u52a0\u5761\u56fd\u7acb\u5927\u5b66\u91cd\u5e86\u7814\u7a76\u9662\u738b\u7389\u7f8e\u7814\u7a76\u5458\u4e3a\u672c\u6587\u7b2c\u4e00\u4f5c\u8005\uff0c\u65b0\u52a0\u5761\u56fd\u7acb\u5927\u5b66\u5415\u529b\u6559\u6388\u4e3a\u672c\u6587\u901a\u8baf\u4f5c\u8005\u3002<\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-1.png\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-254162\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-1.png\" alt=\"\" width=\"800\" height=\"224\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-1.png 800w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-1-300x84.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-1-768x215.png 768w\" sizes=\"(max-width: 800px) 100vw, 800px\" \/><\/a><\/p>\n<p><strong><b>\u4e09\u3001\u3010\u4e3b\u8981\u5185\u5bb9\u3011<\/b><\/strong><\/p>\n<p>\u672c\u7efc\u8ff0\u9996\u5148\u603b\u7ed3\u4e86\u5404\u79cd\u7535\u89e3\u8d28\u7684\u7279\u6027\u548c\u9502\u79bb\u5b50\u5728\u5176\u4e2d\u7684\u4f20\u5bfc\u673a\u5236\uff0c\u4ee5\u6bd4\u8f83\u5b83\u4eec\u5bf9\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u9502\u7535\u6c60\u7684\u9002\u914d\u6027\u3002\u5176\u4e2d\uff0c\u805a\u5408\u7269\u56fa\u6001\u7535\u89e3\u8d28\u5404\u9879\u6027\u8d28\u4f18\u5f02\uff0c\u662f\u9ad8\u6bd4\u80fd\u56fa\u6001\u7535\u6c60\u7684\u6700\u4f73\u9009\u62e9\u3002\u968f\u540e\u8ba8\u8bba\u4e86\u56fa\u6001\u7535\u89e3\u8d28\u4e2d\u5e38\u7528\u805a\u5408\u7269\u6750\u6599\u7684\u6027\u80fd\u53ca\u9488\u5bf9\u5176\u7f3a\u9677\u7684\u5178\u578b\u6539\u6027\u4f18\u5316\u65b9\u6cd5\u3002\u6b64\u5916\uff0c\u4e3a\u4e86\u8fdb\u4e00\u6b65\u63d0\u9ad8\u9502\u7535\u6c60\u80fd\u91cf\u5bc6\u5ea6\u4ee5\u53ca\u5faa\u73af\u7a33\u5b9a\u6027\uff0c\u5bf9\u7535\u6c60\u4e2d\u6b63\u6781\/\u805a\u5408\u7269\u7535\u89e3\u8d28\u754c\u9762\u63a5\u89e6\u548c\u6da6\u6e7f\u3001\u754c\u9762\u7535\u5316\u5b66\u517c\u5bb9\u6027\u548c\u7a7a\u95f4\u7535\u8377\u5c42\uff0c\u4ee5\u53ca\u8d1f\u6781\/\u805a\u5408\u7269\u7535\u89e3\u8d28\u754c\u9762\u5316\u5b66\u7a33\u5b9a\u6027\u548c\u9502\u679d\u6676\u751f\u957f\u95ee\u9898\u8fdb\u884c\u4e86\u5168\u9762\u7684\u5206\u6790\u3002\u6700\u540e\uff0c\u5728\u73b0\u6709\u5de5\u4f5c\u57fa\u7840\u4e0a\uff0c\u63d0\u51fa\u4e86\u7528\u4e8e\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u9502\u7535\u6c60\u7684\u805a\u5408\u7269\u56fa\u6001\u7535\u89e3\u8d28\u7684\u672a\u6765\u53d1\u5c55\u65b9\u5411\u3002<\/p>\n<p><strong><b>\u56db\u3001\u3010\u56fe\u6587\u8be6\u60c5\u3011<\/b><\/strong><\/p>\n<p><strong><b>1<\/b><\/strong><strong><b>. <\/b><\/strong><strong><b>\u4e0d\u540c\u79cd\u7c7b\u7535\u89e3\u8d28\u7684\u6027\u80fd\u6bd4\u8f83<\/b><\/strong><\/p>\n<p>\u9502\u7535\u6c60\u7535\u89e3\u8d28\u5927\u4f53\u53ef\u5206\u4e3a\u6db2\u6001\u7535\u89e3\u6db2\uff08Liquid\u00a0Electrolytes\uff0cLEs\uff09\u548c\u56fa\u6001\u7535\u89e3\u8d28\uff08Solid-State\u00a0Electrolytes\uff0cSSEs\uff09\u4e24\u5927\u7c7b\uff0c\u5176\u4e2d\u56fa\u6001\u7535\u89e3\u8d28\u5305\u62ec\u56fa\u6001\u805a\u5408\u7269\u7535\u89e3\u8d28\uff08Solid\u00a0Polymer\u00a0Electrolytes\uff0cSPEs\uff09\u548c\u65e0\u673a\u9676\u74f7\u7535\u89e3\u8d28\uff08Inorganic\u00a0Ceramic\u00a0Electrolytes\uff0cICEs\uff09\u3002\u5b83\u4eec\u6709\u5404\u81ea\u663e\u8457\u7684\u4f18\u7f3a\u70b9\u3002\u4e3a\u4e86\u8fdb\u4e00\u6b65\u63d0\u9ad8\u7535\u89e3\u8d28\u7684\u7efc\u5408\u6027\u80fd\uff0c\u5e38\u5e38\u5c06\u5b83\u4eec\u7ec4\u5408\uff0c\u800c\u5f62\u6210\u590d\u5408\u7535\u89e3\u8d28\uff0c\u5982\u56fe2\u6240\u793a\u3002\u5176\u4e2d\uff0c\u57fa\u4e8e\u805a\u5408\u7269\u7684\u56fa\u6001\u7535\u89e3\u8d28\uff08\u865a\u7ebf\u6807\u6ce8\uff09\u62e5\u6709\u6700\u7efc\u5408\u7684\u5404\u9879\u6027\u8d28\uff0c\u6700\u9002\u4e8e\u9ad8\u6bd4\u80fd\u56fa\u6001\u7535\u6c60\u7684\u6784\u5efa\u3002<\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-3.png\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-254163\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-3.png\" alt=\"\" width=\"800\" height=\"820\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-3.png 800w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-3-293x300.png 293w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-3-768x787.png 768w\" sizes=\"(max-width: 800px) 100vw, 800px\" \/><\/a><\/p>\n<p>\u56fe2\u00a0\u5404\u79cd\u7535\u89e3\u8d28\u7684\u7279\u6027\u6bd4\u8f83<\/p>\n<p><strong><b>2<\/b><\/strong><strong><b>. <\/b><\/strong><strong><b>\u4e0d\u540c\u79cd\u7c7b\u7535\u89e3\u8d28\u4e2d\u9502\u79bb\u5b50\u7684\u4f20\u8f93\u673a\u7406<\/b><\/strong><\/p>\n<p><strong><b>\uff081\uff09\u5355\u7ec4\u5206\u7535\u89e3\u8d28<\/b><\/strong><\/p>\n<p>\u5728LE\u5185\uff0c\u9502\u79bb\u5b50\u88ab\u591a\u4e2a\u6eb6\u5242\u5206\u5b50\u5305\u56f4\uff0c\u5f62\u6210\u6eb6\u5242\u9798\u3002\u79bb\u5b50\u5e26\u7740\u6eb6\u5242\u9798\u8fc1\u79fb\uff0c\u5230\u8fbe\u53e6\u4e00\u7aef\u540e\uff0c\u8131\u53bb\u6eb6\u5242\u9798\u3002\u5176\u4e2d\uff0c\u53bb\u6eb6\u5242\u5316\u9700\u8981\u514b\u670d\u8f83\u5927\u7684\u80fd\u5792\uff0c\u5f71\u54cd\u754c\u9762\u9502\u79bb\u5b50\u4f20\u5bfc\u901f\u7387\u3002\u5728SPE\u5185\uff0c\u9502\u79bb\u5b50\u4e0e\u805a\u5408\u7269\u94fe\u4e0a\u7684\u57fa\u56e2\u6216\u539f\u5b50\u914d\u4f4d\uff0c\u968f\u7740\u94fe\u6bb5\u8fd0\u52a8\u800c\u8fc1\u79fb\u3002\u4f34\u968f\u7740\u914d\u4f4d\u952e\u7684\u65ad\u88c2\u4e0e\u5f62\u6210\uff0c\u9502\u79bb\u5b50\u5c06\u5728\u805a\u5408\u7269\u94fe\u5185\u6216\u94fe\u95f4\u8df3\u8dc3\u3002\u5728ICE\u4e2d\uff0c\u9502\u79bb\u5b50\u4f20\u5bfc\u5f88\u5927\u7a0b\u5ea6\u4e0a\u4f9d\u8d56\u4e8e\u6676\u4f53\u7ed3\u6784\u4e2d\u5b58\u5728\u7684\u7f3a\u9677\u3002\u591a\u6676\u9676\u74f7\u5219\u56e0\u5176\u8f83\u5927\u7684\u6676\u754c\u963b\u6297\uff0c\u6210\u4e3a\u9650\u5236\u79bb\u5b50\u5bfc\u901a\u7684\u4e3b\u8981\u56e0\u7d20\u3002<\/p>\n<p><strong><b>\uff082\uff09\u591a\u7ec4\u5206\u7535\u89e3\u8d28<\/b><\/strong><\/p>\n<p>\u591a\u7ec4\u5206\u7535\u89e3\u8d28\u4e3b\u8981\u5305\u62ec\u53cc\u7ec4\u5206\u7684\u9676\u74f7-\u6db2\u4f53\u7535\u89e3\u8d28\uff08Ceramic-Liquid\u00a0Electrolytes\uff0cCLEs\uff09\uff0c\u51dd\u80f6\u805a\u5408\u7269\u7535\u89e3\u8d28\uff08Gel\u00a0Polymer\u00a0Electrolytes\uff0cGPEs\uff09\uff0c\u590d\u5408\u805a\u5408\u7269\u7535\u89e3\u8d28\uff08Composite\u00a0Polymer\u00a0Electrolytes\uff0cCPEs\uff09\u4ee5\u53ca\u4e09\u7ec4\u5206\u7684\u590d\u5408\u51dd\u80f6\u805a\u5408\u7269\u7535\u89e3\u8d28\uff08Composite\u00a0Gel\u00a0Polymer\u00a0Electrolytes\uff0cCGPEs\uff09\u3002\u5728\u591a\u7ec4\u5206\u7535\u89e3\u8d28\u4e2d\uff0c\u56e0\u4e3a\u6bcf\u79cd\u6210\u5206\u90fd\u4f1a\u8d21\u732e\u5176\u5404\u81ea\u7684\u79bb\u5b50\u4f20\u5bfc\u9014\u5f84\uff0c\u5bfc\u81f4\u79bb\u5b50\u4f20\u5bfc\u673a\u5236\u66f4\u4e3a\u590d\u6742\u3002\u6b64\u5916\uff0c\u4e0d\u540c\u6210\u5206\u4e4b\u95f4\u7684\u76f8\u4e92\u4f5c\u7528\uff0c\u4e5f\u9020\u6210\u4e86\u79bb\u5b50\u4f20\u8f93\u7684\u534f\u540c\u4e0e\u7ade\u4e89\u6548\u5e94\uff0c\u56e0\u800c\u9700\u8981\u5177\u4f53\u7814\u7a76\u3002<\/p>\n<p><strong><b>3<\/b><\/strong><strong><b>. <\/b><\/strong><strong><b>\u5e38\u7528\u805a\u5408\u7269\u7684\u6027\u80fd\u53ca\u5176\u6539\u6027\u65b9\u6cd5<\/b><\/strong><\/p>\n<p>\u7ecf\u8fc7\u6570\u5341\u5e74\u7684\u53d1\u5c55\uff0c\u805a\u73af\u6c27\u4e59\u70f7\uff08PEO\uff09\u3001\u805a\u4e19\u70ef\u8148\uff08PAN\uff09\u3001\u805a\u504f\u4e8c\u6c1f\u4e59\u70ef\uff08PVDF\uff09\u548c\u805a\u7532\u57fa\u4e19\u70ef\u9178\u7532\u916f\uff08PMMA\uff09\u5df2\u6210\u4e3a\u805a\u5408\u7269\u56fa\u6001\u7535\u89e3\u8d28\u4e2d\u4f7f\u7528\u6700\u5e7f\u6cdb\u7684\u805a\u5408\u7269\u57fa\u4f53\u6750\u6599\u3002\u5b83\u4eec\u5404\u81ea\u7684\u7ed3\u6784\u53ca\u7279\u6027\u5982\u56fe3\u6240\u793a\u3002\u9488\u5bf9\u5b83\u4eec\u7684\u7f3a\u70b9\uff0c\u6587\u4e2d\u8fd8\u603b\u7ed3\u4e86\u8bb8\u591a\u5178\u578b\u7684\u6539\u6027\u7b56\u7565\u3002<\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-4.png\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-254164\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-4.png\" alt=\"\" width=\"800\" height=\"367\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-4.png 800w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-4-300x138.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-4-768x352.png 768w\" sizes=\"(max-width: 800px) 100vw, 800px\" \/><\/a><\/p>\n<p>\u56fe3\u00a0\u5404\u79cd\u805a\u5408\u7269\u57fa\u4f53\u6750\u6599\u7684\u6027\u80fd\u6bd4\u8f83<\/p>\n<p><strong><b>4<\/b><\/strong><strong><b>. <\/b><\/strong><strong><b>\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u9502\u7535\u6c60\u6b63\u6781<\/b><\/strong><strong><b>\/<\/b><\/strong><strong><b>\u805a\u5408\u7269\u56fa\u6001\u7535\u89e3\u8d28\u754c\u9762\u95ee\u9898\u53ca\u6539\u5584\u65b9\u6cd5<\/b><\/strong><\/p>\n<p><strong><b>\uff081\uff09\u754c\u9762\u63a5\u89e6\u4e0e\u6da6\u6e7f<\/b><\/strong><\/p>\n<p>\u67d4\u8f6f\u7684\u805a\u5408\u7269\u56fa\u6001\u7535\u89e3\u8d28\u62e5\u6709\u4e0e\u7535\u6781\u7684\u826f\u597d\u63a5\u89e6\u3002\u7136\u800c\uff0c\u5f53\u7535\u6c60\u4f7f\u7528\u9ad8\u8d1f\u8f7d\u6b63\u6781\u65f6\uff0c\u805a\u5408\u7269\u56fa\u6001\u7535\u89e3\u8d28\u4ecd\u96be\u4ee5\u6709\u6548\u6e17\u900f\u548c\u6da6\u6e7f\u6b63\u6781\uff0c\u5bfc\u81f4\u6b63\u6781\u5185\u90e8\u548c\u754c\u9762\u5904\u7684\u9502\u79bb\u5b50\u4f20\u5bfc\u4e0d\u7406\u60f3\u3002\u9664\u4e86\u5728\u7535\u89e3\u8d28\u5185\u52a0\u5165\u6db2\u4f53\u6210\u5206\u5916\uff0c\u539f\u4f4d\u805a\u5408\u548c\u4e00\u4f53\u5316\u6b63\u6781-\u7535\u89e3\u8d28\u7b56\u7565\u4e5f\u53ef\u4ee5\u6539\u5584\u8fd9\u4e2a\u95ee\u9898\u3002\u539f\u4f4d\u805a\u5408\u901a\u8fc7\u5c06\u542b\u6709\u5f15\u53d1\u5242\u7684\u6db2\u6001\u805a\u5408\u7269\u524d\u9a71\u4f53\/\u5355\u4f53\u76f4\u63a5\u6d82\u8986\u5230\u6b63\u6781\u4e0a\uff0c\u6216\u6ce8\u5165\u9884\u7ec4\u88c5\u7684\u7535\u6c60\u4e2d\uff0c\u4ece\u800c\u4f7f\u6db2\u4f53\u524d\u9a71\u4f53\/\u5355\u4f53\u6709\u6548\u6e17\u900f\u6b63\u6781\uff0c\u518d\u805a\u5408\u3002\u4e00\u4f53\u5316\u6b63\u6781-\u7535\u89e3\u8d28\u6307\u7684\u662f\u5c06\u67d0\u4e9b\u805a\u5408\u7269\u7535\u89e3\u8d28\u65e2\u4f5c\u4e3a\u79bb\u5b50\u5bfc\u4f53\u548c\u7c98\u7ed3\u5242\u63ba\u5165\u6b63\u6781\uff0c\u53c8\u4f5c\u4e3a\u7535\u89e3\u8d28\u7ec4\u6210\u7535\u6c60\u3002\u6b64\u65f6\uff0c\u6b63\u6781\u548c\u7535\u89e3\u8d28\u7c98\u5408\u5728\u4e00\u8d77\u521b\u5efa\u96c6\u6210\u6b63\u6781\/\u7535\u89e3\u8d28\u4e00\u4f53\u5316\u7ed3\u6784\u3002<\/p>\n<p><strong><b>\uff082\uff09\u754c\u9762\u7535\u5316\u5b66\u7a33\u5b9a\u6027<\/b><\/strong><\/p>\n<p>\u5c3d\u7ba1\u76f8\u6bd4\u4f20\u7edf\u6db2\u6001\u7535\u89e3\u6db2\uff0c\u805a\u5408\u7269\u7535\u89e3\u8d28\u901a\u5e38\u5177\u6709\u66f4\u5bbd\u7684\u7535\u5316\u5b66\u7a33\u5b9a\u7a97\u53e3\uff0c\u5b83\u4eec\u4ecd\u96be\u4ee5\u6ee1\u8db3\u9ad8\u7535\u538b\u6b63\u6781\u7684\u5339\u914d\u8981\u6c42\u3002\u6b63\u6781\/\u7535\u89e3\u8d28\u754c\u9762\u7684\u7535\u5316\u5b66\u4e0d\u7a33\u5b9a\u9650\u5236\u4e86\u9502\u7535\u6c60\u7684\u80fd\u91cf\u5bc6\u5ea6\u548c\u5faa\u73af\u6027\u80fd\u3002\u5728\u6b63\u6781\u548c\u805a\u5408\u7269\u7535\u89e3\u8d28\u4e4b\u95f4\u6784\u5efa\u7a33\u5b9a\u7684\u6b63\u6781-\u7535\u89e3\u8d28\u4e2d\u95f4\u76f8\uff08CEI\uff09\u662f\u63d0\u9ad8\u754c\u9762\u7535\u5316\u5b66\u517c\u5bb9\u6027\u7684\u6709\u6548\u7b56\u7565\u3002\u901a\u8fc7\u7535\u89e3\u8d28\u6539\u6027\uff0c\u5305\u62ec\u52a0\u5165\u9502\u76d0\u6dfb\u52a0\u5242\u3001\u589e\u5851\u5242\u548c\u9676\u74f7\u586b\u6599\u90fd\u6709\u52a9\u4e8e\u5f62\u6210\u7a33\u5b9a\u7684CEI\u3002\u6b64\u5916\uff0c\u9274\u4e8eICE\u5177\u6709\u51fa\u8272\u7684\u7535\u5316\u5b66\u7a33\u5b9a\u6027\uff0c\u56e0\u6b64\u5728\u6b63\u6781\u4e0a\u6784\u5efa\u4e00\u5c42ICE\u6d82\u5c42\u53ef\u7528\u4f5c\u5939\u5c42\u7ed3\u6784\u4e2d\u6b63\u6781\u548c\u805a\u5408\u7269\u7535\u89e3\u8d28\u4e4b\u95f4\u7684\u4eba\u9020\u7a33\u5b9aCEI\u3002\u67d0\u4e9b\u5177\u6709\u4f18\u5f02\u7535\u5316\u5b66\u7a33\u5b9a\u6027\u7684\u805a\u5408\u7269\u4e5f\u53ef\u4ee5\u7528\u4f5c\u6b63\u6781\u6d82\u5c42\u3002\u6784\u5efa\u591a\u5c42\u805a\u5408\u7269\u7535\u89e3\u8d28\u4e5f\u662f\u4e00\u79cd\u907f\u514d\u7535\u5316\u5b66\u4e0d\u517c\u5bb9\u7684\u76f4\u63a5\u65b9\u6cd5\u3002<\/p>\n<p><strong><b>\uff083\uff09\u754c\u9762\u7a7a\u95f4\u7535\u8377\u5c42<\/b><\/strong><\/p>\n<p>\u6b63\u6781\/\u7535\u89e3\u8d28\u754c\u9762\u4e0a\u7a7a\u95f4\u7535\u8377\u5c42\u7684\u5b58\u5728\u4e5f\u53ef\u80fd\u5bfc\u81f4\u5927\u7684\u754c\u9762\u963b\u6297\u3002\u8fd9\u662f\u56e0\u4e3a\u5f53\u4e24\u79cd\u5177\u6709\u4e0d\u540c\u5316\u5b66\u52bf\u7684\u6750\u6599\u63a5\u89e6\u65f6\uff0c\u4f8b\u5982\u7535\u6781\u548c\u805a\u5408\u7269\u7535\u89e3\u8d28\uff0c\u7a7a\u95f4\u7535\u8377\u4f1a\u5728\u754c\u9762\u5904\u79ef\u805a\u3002\u9664\u4e86\u4e0d\u540c\u7684\u5316\u5b66\u52bf\u4e4b\u5916\uff0c\u7535\u6781\u548c\u805a\u5408\u7269\u7535\u89e3\u8d28\u4e4b\u95f4\u7684\u7535\u52bf\u5dee\u4e5f\u5c06\u9a71\u52a8\u5e26\u7535\u7c92\u5b50\u91cd\u65b0\u5206\u5e03\uff0c\u5728\u754c\u9762\u5904\u5f62\u6210\u7a7a\u95f4\u7535\u8377\u5c42\u7d2f\u79ef\u3002\u754c\u9762\u5904\u7684\u7a7a\u95f4\u7535\u8377\u5c42\u4f1a\u963b\u788d\u79bb\u5b50\u4f20\u5bfc\uff0c\u63d0\u9ad8\u79bb\u5b50\u7684\u8fc1\u79fb\u80fd\u5792\uff0c\u589e\u5927\u754c\u9762\u963b\u6297\u3002\u5c06\u94c1\u7535\/\u4ecb\u7535\u6750\u6599\u5f15\u5165\u754c\u9762\u4e2d\u5219\u80fd\u591f\u5f88\u597d\u5730\u6291\u5236\u7a7a\u95f4\u7535\u8377\u7684\u7d2f\u79ef\u3002<\/p>\n<p><strong><b>5<\/b><\/strong><strong><b>. <\/b><\/strong><strong><b>\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u9502\u7535\u6c60\u8d1f\u6781<\/b><\/strong><strong><b>\/<\/b><\/strong><strong><b>\u805a\u5408\u7269\u56fa\u6001\u7535\u89e3\u8d28\u754c\u9762\u95ee\u9898\u53ca\u4fee\u9970\u65b9\u6cd5<\/b><\/strong><\/p>\n<p>\u5728\u9502\u7535\u6c60\u7684\u5404\u79cd\u8d1f\u6781\u6750\u6599\u4e2d\uff0c\u9502\u91d1\u5c5e\u62e5\u6709\u8f83\u9ad8\u7684\u6bd4\u5bb9\u91cf\uff083860 mAh g<sup>&#8211;<\/sup><sup>1<\/sup>\uff09\uff0c\u53ca\u8f83\u4f4e\u7684\u8fd8\u539f\u7535\u4f4d\uff083.04 V\uff0c\u6807\u51c6\u6c22\u7535\u6781\uff09\u3002\u56e0\u6b64\uff0c\u9502\u91d1\u5c5e\u7535\u6c60\u7684\u80fd\u91cf\u5bc6\u5ea6\u80fd\u591f\u6bd4\u4f7f\u7528\u77f3\u58a8\u8d1f\u6781\u7684\u7535\u6c60\u63d0\u9ad840%-50%\u3002\u7136\u800c\uff0c\u9502\u91d1\u5c5e\u8d1f\u6781\/\u7535\u89e3\u8d28\u754c\u9762\u4e5f\u5b58\u5728\u7740\u4e00\u4e9b\u95ee\u9898\uff0c\u5b83\u4eec\u4e0d\u4ec5\u5f71\u54cd\u9502\u7535\u6c60\u7684\u80fd\u91cf\u5bc6\u5ea6\uff0c\u8fd8\u5f71\u54cd\u5176\u5faa\u73af\u6027\u80fd\u548c\u5b89\u5168\u6027\u3002<\/p>\n<p><strong><b>\uff081\uff09\u754c\u9762\u5316\u5b66\u7a33\u5b9a\u6027<\/b><\/strong><\/p>\n<p>\u754c\u9762\u7a33\u5b9a\u6027\u662f\u9502\u7535\u6c60\u7a33\u5b9a\u5faa\u73af\u7684\u5148\u51b3\u6761\u4ef6\u3002\u7136\u800c\uff0c\u9502\u91d1\u5c5e\u8d1f\u6781\u603b\u662f\u4f1a\u4e0e\u542b\u6709\u7279\u5b9a\u57fa\u56e2\u6216\u5143\u7d20\u7684\u805a\u5408\u7269\u7535\u89e3\u8d28\u53cd\u5e94\u3002\u5728\u805a\u5408\u7269\u7535\u89e3\u8d28\u4e2d\u52a0\u5165\u6dfb\u52a0\u5242\uff0c\u53ef\u4ee5\u5728\u754c\u9762\u5904\u8bf1\u5bfc\u751f\u6210\u5bcc\u542b\u65e0\u673a\u7269\u7684\u56fa\u4f53-\u7535\u89e3\u8d28\u4e2d\u95f4\u76f8\uff08SEI\uff09\uff0c\u963b\u9694\u526f\u53cd\u5e94\u53d1\u751f\uff0c\u63d0\u9ad8\u754c\u9762\u5316\u5b66\u7a33\u5b9a\u6027\u3002\u6b64\u5916\u200b\u200b\uff0c\u4e0e\u6b63\u6781\u4fa7\u76f8\u540c\uff0c\u91c7\u7528\u591a\u5c42\u7535\u89e3\u8d28\u8bbe\u8ba1\u4e5f\u53ef\u4ee5\u5c06\u6613\u53cd\u5e94\u7684\u7535\u89e3\u8d28\u4e0e\u9502\u91d1\u5c5e\u8d1f\u6781\u8fdb\u884c\u7269\u7406\u5206\u9694\u3002<\/p>\n<p><strong><b>\uff082\uff09\u679d\u6676\u751f\u957f<\/b><\/strong><\/p>\n<p>\u9502\u79bb\u5b50\u5728\u8d1f\u6781\/\u7535\u89e3\u8d28\u754c\u9762\u5904\u7684\u4e0d\u5747\u5300\u6c89\u79ef\u4f1a\u5bfc\u81f4\u9502\u679d\u6676\u7684\u5f62\u6210\uff0c\u8fdb\u800c\u523a\u7a7f\u7535\u89e3\u8d28\u5e76\u5bfc\u81f4\u7535\u6c60\u77ed\u8def\u3002\u8fd9\u5bf9\u4f7f\u7528\u805a\u5408\u7269\u7535\u89e3\u8d28\u9502\u7535\u6c60\u7684\u5b89\u5168\u6027\u548c\u5faa\u73af\u6027\u80fd\u6784\u6210\u4e86\u91cd\u5927\u5a01\u80c1\u3002\u5728\u4e25\u91cd\u7684\u60c5\u51b5\u4e0b\uff0c\u5982\u679c\u7535\u89e3\u8d28\u4e2d\u542b\u6709\u6613\u71c3\u6210\u5206\uff0c\u751a\u81f3\u53ef\u80fd\u5f15\u53d1\u70ed\u5931\u63a7\u3002\u800c\u4e14\u4e3a\u4e86\u63d0\u9ad8\u9502\u7535\u6c60\u7684\u80fd\u91cf\u5bc6\u5ea6\uff0c\u901a\u5e38\u504f\u5411\u4e8e\u4f7f\u7528\u8f83\u8584\u7684\u805a\u5408\u7269\u7535\u89e3\u8d28\uff0c\u8fd9\u66f4\u52a0\u5927\u4e86\u8fd9\u79cd\u98ce\u9669\u3002\u5728\u805a\u5408\u7269\u56fa\u6001\u7535\u89e3\u8d28\u4e2d\u52a0\u5165\u9676\u74f7\u586b\u6599\uff0c\u63d0\u9ad8\u7535\u89e3\u8d28\u7684\u673a\u68b0\u5f3a\u5ea6\u80fd\u591f\u6709\u6548\u6291\u5236\u679d\u6676\u7684\u751f\u957f\u3002\u7136\u800c\uff0c\u8fc7\u9ad8\u7684\u9676\u74f7\u6dfb\u52a0\u91cf\u53ef\u80fd\u5f15\u8d77\u9676\u74f7\u9897\u7c92\u7684\u4e25\u91cd\u56e2\u805a\u73b0\u8c61\uff0c\u4ece\u800c\u5f71\u54cd\u7535\u89e3\u8d28\u7684\u79bb\u5b50\u7535\u5bfc\u7387\u3002\u6b64\u5916\uff0c\u901a\u8fc7\u6539\u53d8\u9676\u74f7\u586b\u6599\u7684\u5f62\u8c8c\/\u7ed3\u6784\uff0c\u4f8b\u5982\u4f7f\u7528\u9676\u74f7\u7eb3\u7c73\u7ebf\uff0c\u751a\u81f3\u5728\u7535\u89e3\u8d28\u5185\u90e8\u6784\u5efa3D\u9676\u74f7\u7f51\u7edc\uff0c\u53ef\u4ee5\u8fdb\u4e00\u6b65\u589e\u5f3a\u5176\u679d\u6676\u6291\u5236\u80fd\u529b\uff0c\u540c\u65f6\u589e\u5f3a\u7535\u89e3\u8d28\u7684\u79bb\u5b50\u7535\u5bfc\u7387\u3002\u53e6\u4e00\u65b9\u9762\uff0c\u539f\u4f4d\u5f62\u6210\u7684\u5177\u6709\u8f83\u9ad8\u673a\u68b0\u5f3a\u5ea6\u7684\u754c\u9762\u76f8\u4e5f\u53ef\u4ee5\u6709\u6548\u6291\u5236\u9502\u679d\u6676\u751f\u957f\u3002\u56fe4\u603b\u7ed3\u4e86\u9502\u7535\u6c60\u7535\u6781\/\u805a\u5408\u7269\u56fa\u6001\u7535\u89e3\u8d28\u7684\u754c\u9762\u95ee\u9898\u53ca\u4fee\u9970\u6539\u5584\u65b9\u6cd5\u3002<\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-5.png\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-254165\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-5.png\" alt=\"\" width=\"800\" height=\"799\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-5.png 800w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-5-150x150.png 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-5-300x300.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-5-768x767.png 768w\" sizes=\"(max-width: 800px) 100vw, 800px\" \/><\/a><\/p>\n<p>\u56fe4\u00a0\u9502\u7535\u6c60\u7535\u6781\/\u805a\u5408\u7269\u56fa\u6001\u7535\u89e3\u8d28\u7684\u754c\u9762\u95ee\u9898\u53ca\u4fee\u9970\u6539\u5584\u65b9\u6cd5<\/p>\n<p><strong><b>\u4e94\u3001\u3010\u672a\u6765\u5c55\u671b\u3011<\/b><\/strong><\/p>\n<p>\u5c3d\u7ba1\u73b0\u6709\u7684\u7535\u89e3\u8d28\u6539\u6027\u4ee5\u53ca\u754c\u9762\u4fee\u9970\u65b9\u6cd5\u5df2\u7ecf\u80fd\u591f\u5728\u4e00\u5b9a\u7a0b\u5ea6\u4e0a\u63d0\u9ad8\u9502\u7535\u6c60\u7684\u80fd\u91cf\u5bc6\u5ea6\uff0c\u672a\u6765\u4ecd\u9700\u8981\u66f4\u597d\u5730\u89e3\u51b3\u4ee5\u4e0b\u51e0\u4e2a\u6311\u6218\uff0c\u4ee5\u8fdb\u4e00\u6b65\u63d0\u9ad8\u7535\u6c60\u7684\u7efc\u5408\u6027\u80fd\uff1a<\/p>\n<p><strong><b>\uff081\uff09<\/b><\/strong>\u5bf9\u805a\u5408\u7269\u7535\u89e3\u8d28\uff0c\u5c24\u5176\u662f\u591a\u7ec4\u5206\u7535\u89e3\u8d28\u4e2d\u9502\u79bb\u5b50\u7684\u4f20\u5bfc\u673a\u7406\u8fdb\u884c\u8fdb\u4e00\u6b65\u63a2\u7a76\u3002<\/p>\n<p><strong><b>\uff082\uff09<\/b><\/strong>\u9700\u8981\u8fdb\u4e00\u6b65\u63d0\u9ad8\u805a\u5408\u7269\u56fa\u6001\u7535\u89e3\u8d28\u7684\u7535\u5316\u5b66\u7a33\u5b9a\u6027\u4e0e\u673a\u68b0\u5f3a\u5ea6\uff0c\u5e76\u5bf9\u7535\u89e3\u8d28\u8fdb\u884c\u66f4\u65b0\u9896\u7684\u7ed3\u6784\u8bbe\u8ba1\u3002<\/p>\n<p><strong><b>\uff083\uff09<\/b><\/strong>\u5728\u5c3d\u91cf\u63d0\u9ad8\u7535\u6781\u8d1f\u8f7d\u91cf\u7684\u524d\u63d0\u4e0b\uff0c\u4fdd\u8bc1\u7535\u6c60\u7684\u653e\u7535\u5bb9\u91cf\u4e0e\u5faa\u73af\u6027\u80fd\u4e0d\u53d7\u5f71\u54cd\u3002<\/p>\n<p><strong><b>\uff084\uff09<\/b><\/strong>\u4f18\u5316\u805a\u5408\u7269\u7535\u89e3\u8d28\u7684\u5236\u5907\u8fc7\u7a0b\uff0c\u5e76\u964d\u4f4e\u5236\u5907\u6210\u672c\uff0c\u9002\u5e94\u5927\u89c4\u6a21\u751f\u4ea7\u3002<\/p>\n<p><strong><b>\u516d\u3001\u3010\u6587\u7ae0\u94fe\u63a5\u3011<\/b><\/strong><\/p>\n<p>Xiao Lu, Yumei Wang, Xiaoyu Xu, Binggong Yan, Tian Wu, Li Lu<sup>*<\/sup>. Polymer\u2010Based Solid\u2010State Electrolytes for High\u2010Energy\u2010Density Lithium\u2010Ion Batteries \u2013 Review. <em><i>Advanced Energy Materials<\/i><\/em>, 2023, 2301746,\u00a0https:\/\/doi.org\/10.1002\/aenm.202301746<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u4e00\u3001\u3010\u5bfc\u8bfb\u3011 \u8fd1\u5e74\u6765\uff0c\u9502\u7535\u6c60\u5df2\u88ab\u5e7f\u6cdb\u5e94\u7528\u4e8e\u79fb\u52a8\u7535\u5b50\u8bbe\u5907\uff0c\u7535\u52a8\u6c7d\u8f66\uff0c\u5927\u578b\u50a8\u80fd\u88c5\u7f6e\u548c\u536b\u661f\u7b49\u7279\u6b8a\u9886\u57df\u3002\u5176\u4e2d\uff0c\u79fb\u52a8\u7535\u5b50\u8bbe\u5907\u548c\u7535\u52a8\u6c7d\u8f66\u7684\u5feb\u901f\u53d1\u5c55\u4f7f\u5f97\u4eba\u4eec\u5bf9\u9502\u7535\u6c60\u7684\u80fd\u91cf\u5bc6\u5ea6&#8230;<\/p>\n","protected":false},"author":2,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-254159","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/254159"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/2"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=254159"}],"version-history":[{"count":3,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/254159\/revisions"}],"predecessor-version":[{"id":254168,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/254159\/revisions\/254168"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=254159"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=254159"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=254159"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}