{"id":254573,"date":"2023-09-22T06:49:11","date_gmt":"2023-09-21T22:49:11","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=254573"},"modified":"2023-09-21T21:49:30","modified_gmt":"2023-09-21T13:49:30","slug":"%e6%b9%98%e6%bd%ad%e5%a4%a7%e5%ad%a6%e8%b4%b9%e4%bf%8a%e6%9d%b0carbon%ef%bc%9a%e5%85%89%e9%a9%b1%e5%8a%a8%e6%97%a0%e9%85%b6%e5%85%89%e7%94%b5%e5%8c%96%e5%ad%a6%e4%bc%a0%e6%84%9f%e5%99%a8%e7%94%a8","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=254573","title":{"rendered":"\u6e58\u6f6d\u5927\u5b66\u8d39\u4fca\u6770Carbon\uff1a\u5149\u9a71\u52a8\u65e0\u9176\u5149\u7535\u5316\u5b66\u4f20\u611f\u5668\u7528\u4e8e\u8d85\u7075\u654f\u68c0\u6d4b L-\u534a\u80f1\u6c28\u9178"},"content":{"rendered":"<p>\u3010\u80cc\u666f\u4ecb\u7ecd\u3011<\/p>\n<p>L-\u534a\u80f1\u6c28\u9178\uff08L-Cys\uff09\u662f\u4e00\u79cd\u975e\u5e38\u91cd\u8981\u7684\u5929\u7136\u6c28\u57fa\u9178\uff0c\u5b83\u542b\u6709\u786b\u4f5c\u4e3a\u6d3b\u6027\u4f4d\u70b9\uff0c\u56e0\u6b64\u53ef\u4ee5\u4e0e\u8bb8\u591a\u6709\u6bd2\u7269\u8d28\u5f62\u6210\u65e0\u6bd2\u914d\u5408\u7269\uff0c\u4ece\u4f53\u5185\u6d88\u9664\u3002\u56e0\u6b64\uff0c\u5bfb\u627e\u4e00\u79cd\u4f4e\u6210\u672c\u3001\u9ad8\u6027\u80fd\u7684L-Cys\u68c0\u6d4b\u65b9\u6cd5\uff0c\u4ee5\u5b9e\u73b0\u5bf9\u4eba\u4f53\u72b6\u51b5\u3001\u5de5\u4e1a\u6c61\u67d3\u7b49\u65b9\u9762\u7684\u76d1\u6d4b\u6210\u4e3a\u5f53\u52a1\u4e4b\u6025\u3002\u6c27\u5316\u4e9a\u94dc\u90fd\u662f\u00a0p \u578b\u534a\u5bfc\u4f53\uff0c\u5177\u6709\u76f8\u5bf9\u8f83\u7a84\u7684\u5e26\u9699\uff0c\u53ef\u4ee5\u6709\u5f88\u5f3a\u7684\u5149\u5438\u6536\u80fd\u529b\u3002\u77f3\u58a8\u78b3\u6c2e\u5316\u7269\u662f\u4e00\u79cd\u975e\u91d1\u5c5e\u805a\u5408\u7269\u534a\u5bfc\u4f53\uff0c\u4f1a\u4ea7\u751f\u66f4\u591a\u7684\u91d1\u5c5e\u914d\u4f4d\u4f4d\u70b9\uff0c\u4ece\u800c\u4e0e\u91d1\u5c5e\u6c27\u5316\u7269\u6709\u6548\u7ed3\u5408\u3002<\/p>\n<p>\u3010\u7814\u7a76\u51fa\u53d1\u70b9\u3011<\/p>\n<p>\u5927\u591a\u6570\u7684\u5f02\u8d28\u7ed3\u5149\u50ac\u5316\u5242\u4e0d\u80fd\u540c\u65f6\u5b9e\u73b0\u5f3a\u6c27\u5316\u8fd8\u539f\u80fd\u529b\u548c\u9ad8\u7535\u5b50-\u7a7a\u7a74\u5206\u79bb\u3002\u76f8\u6bd4\u4e4b\u4e0b\uff0c\u5e26\u6709\u7535\u5b50\u4ecb\u8d28\u7684 p-n \u5f02\u8d28\u7ed3\u5f80\u5f80\u5177\u6709\u51fa\u8272\u7684\u6c27\u5316\u8fd8\u539f\u80fd\u529b\u548c\u8d85\u9ad8\u7684\u5149\u751f\u7535\u8377\u5bf9\u5206\u79bb\u6548\u7387\u3002\u56e0\u6b64\u6784\u5efa\u5e26\u6709\u7535\u5b50\u4ecb\u8d28\u7684 p-n \u5f02\u8d28\u7ed3\u5149\u7535\u5316\u5b66\u4f20\u611f\u5668\uff0c\u63a2\u7d22\u4f20\u611f\u673a\u5236\u662f\u6781\u5177\u6311\u6218\u7684\u3002<\/p>\n<p>\u3010\u5168\u6587\u901f\u89c8\u3011<\/p>\n<p>\u8fd1\u671f\uff0c\u6e58\u6f6d\u5927\u5b66\u8d39\u4fca\u6770\u6559\u6388\u8bfe\u9898\u7ec4\u91c7\u7528\u7b80\u5355\u7684\u7269\u7406\u6df7\u5408\u6280\u672f\uff0c\u5c06\u6c27\u5316\u4e9a\u94dc\/\u94dc@\u5fae\u5b54\u78b3\uff08Cu2O\/Cu@mC\uff09\u5747\u5300\u56fa\u5b9a\u5728g-C3N4\uff08CNS\uff09\u8868\u9762\uff0c\u5f62\u6210\u4e86p-n\u5f02\u8d28\u7ed3\u3002\u4e0e\u5757\u72b6g-C3N4\uff08CNB\uff09\u76f8\u6bd4\uff0cg-C3N4 \u7247\uff08CNS\uff09\u5177\u6709\u66f4\u9ad8\u7684\u6bd4\u8868\u9762\u79ef\u3002\u70ed\u5904\u7406\u540e\u7684 Cu2O\/Cu@mC \u591a\u5b54\u7ed3\u6784\u6709\u5229\u4e8e\u7535\u8377\u5b58\u50a8\uff0c\u5176\u4e2d\u7684\u78b3\u5145\u5f53\u7535\u5b50\u4ecb\u8d28\u3002\u57fa\u4e8eL-Cys\u4e0eCu2O\/Cu@mC\u901a\u8fc7\u5f62\u6210Cu-S\u952e\u7684\u76f8\u4e92\u4f5c\u7528\uff0c\u6211\u4eec\u63d0\u51fa\u4e86Cu2O\/Cu@mC\/CNS\u4f5c\u4e3a\u68c0\u6d4bL-Cys\u7684\u5149\u9a71\u52a8\u65e0\u9176\u5149\u7535\u5316\u5b66\u4f20\u611f\u5668\u3002\u68c0\u6d4b\u9650\u4e3a1.26\u00d710-9\u202fM\uff0c\u7ebf\u6027\u8303\u56f4\u4e3a1.0\u00d710-8\u202fM\u202f- 4.0\u00d710-6\u202fM\u3002\u6587\u7ae0\u4ee5\u201cA light-driven enzyme-free photoelectrochemical sensor based on HKUST-1 derived Cu2O\/Cu@microporous carbon with g-C3N4\u00a0p-n heterojunction for ultra-sensitive detection of\u00a0L-cysteine\u201d\u4e3a\u9898\u53d1\u8868\u5728Carbon\u4e0a\u3002<\/p>\n<p>\u3010\u56fe\u6587\u89e3\u6790\u3011<\/p>\n<p>\u4e3a\u4e86\u6df1\u5165\u4e86\u89e3\u6837\u54c1\u7684\u8868\u9762\u5f62\u6001\u548c\u5fae\u89c2\u7ed3\u6784\uff0c\u5bf9\u626b\u63cf\u7535\u5b50\u663e\u5fae\u955c\uff08SEM\uff09\u56fe\u50cf\u8fdb\u884c\u4e86\u7814\u7a76\u3002\u56fe 1A \u663e\u793a\u4e86 CNB \u7684\u539a\u7247\u7ed3\u6784\u3002CNS \u7531\u8bb8\u591a\u4e0d\u89c4\u5219\u7684\u8584\u7247\u805a\u96c6\u5728\u4e00\u8d77\uff08\u56fe 1B\uff09\u3002\u56fe 1C \u663e\u793a\uff0c\u524d\u9a71\u4f53 HKUST-1 \u5448\u89c4\u5219\u7684\u516b\u9762\u4f53\u6676\u4f53\u7ed3\u6784\u3002\u53ef\u4ee5\u770b\u51faCu2O\/Cu@mC\u4e3a\u7403\u5f62\u7ed3\u6784\uff0c\u8868\u9762\u76f8\u5bf9\u7c97\u7cd9\uff08\u56fe 1D\uff09\u3002\u4ece\u56fe\u00a01E\u3001F \u4e2d\u53ef\u4ee5\u6e05\u695a\u5730\u770b\u5230 CNS \u4e0a\u7684\u7403\u5f62 Cu2O\/Cu@mC \u8d1f\u8f7d\u3002\u6b64\u5916\uff0c\u4ece\u56fe\u00a01G-K \u4e2d\u53ef\u4ee5\u770b\u51fa\uff0c\u5404\u5143\u7d20\u5206\u5e03\u5747\u5300\uff0c\u8fd9\u4e5f\u610f\u5473\u7740 Cu2O\/Cu@mC \u4e0e CNS \u6210\u529f\u5730\u7ed3\u5408\u5728\u4e00\u8d77\u3002EDS\uff08\u56fe 1L\uff09\u663e\u793a\uff0cCu2O\/Cu@mC\/CNS \u542b\u6709\u56db\u79cd\u5143\u7d20\uff0c\u5373\u78b3\uff08C\uff09\u3001\u6c2e\uff08N\uff09\u3001\u6c27\uff08O\uff09\u548c\u94dc\uff08Cu\uff09\uff0c\u6bd4\u4f8b\u5206\u522b\u4e3a 23.69%\u300169.72%\u30015.68% \u548c 0.91%\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-254575\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-11.png\" alt=\"\" width=\"600\" height=\"700\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-11.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-11-257x300.png 257w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u56fe\u00a01. CNB (A)\u3001CNS (B)\u3001HKUST-1 (C)\u3001Cu2O\/Cu@mC (D)\u3001Cu2O\/Cu@mC\/CNS (E, F) \u7684SEM\u56fe\u50cf\uff1bCu2O\/Cu@mC\/CNS (G-K) \u7684\u5143\u7d20\u5206\u5e03\u56fe\u50cf\uff1bCu2O\/Cu@mC\/CNS (L) \u7684 EDS \u5149\u8c31\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-254576\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-31.png\" alt=\"\" width=\"600\" height=\"685\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-31.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-31-263x300.png 263w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u5982\u56fe\u00a02A\u3001B \u6240\u793a\uff0c\u590d\u5408 Cu2O\/Cu@mC\/CNS \u7684\u5149\u7535\u6d41\u5206\u522b\u6bd4 Cu2O\/Cu@mC \u548c CNS \u7684\u5149\u7535\u6d41\u9ad8 250 \u500d\u548c 25 \u500d\uff0c\u800c\u5728\u542b\u6709 100 nM L-Cys \u7684\u6761\u4ef6\u4e0b\uff0cCu2O\/Cu@mC\/CNS \u7684\u5149\u7535\u6d41\u660e\u663e\u964d\u4f4e\u3002\u56fe 2C\u53ef\u4ee5\u770b\u51fa\uff0cCu2O\/Cu@mC \u548c CNS \u7684 zeta \u7535\u4f4d\u503c\u5206\u522b\u4e3a11.90 mV \u548c-6.90 mV\u3002\u8fd9\u6837\u5f97\u5230\u7684 Cu2O\/Cu@mC\/CNS\u7684zeta\u7535\u4f4d\u4e3a6.99 mV\uff0c\u9a8c\u8bc1\u4e86 Cu2O\/Cu@mC \u53ef\u4ee5\u8d1f\u8f7d\u5728 CNS \u8868\u9762\u3002\u5728\u5b58\u5728\u68c0\u6d4b\u7269\u00a0L-Cys\uff08-10.70 mV\uff09\u7684\u6761\u4ef6\u4e0b\uff0cCu2O\/Cu@mC\/CNS \u7684 zeta \u7535\u4f4d\u53d8\u4e3a -7.39 mV\uff0c\u8fd9\u53ef\u80fd\u662f\u7531\u4e8e\u5f3a\u5927\u7684\u9759\u7535\u5438\u5f15\u4f5c\u7528\u3002\u56fe 2D\u663e\u793a\uff0c\u9ed1\u6697\u4e2d\u6ca1\u6709\u53d1\u73b0\u00b7O2-\u7684\u4fe1\u53f7\uff0c\u5728\u53ef\u89c1\u5149\u7167\u5c04\u4e0b\u51fa\u73b0\u4e86\u00b7O2-\u7684\u7279\u5f81\u5cf0\u3002\u5982\u56fe 2E \u548c\u56fe2F\u6240\u793a\uff0cCu2O\/Cu@mC\/CNS\u5177\u6709\u5f88\u597d\u7684\u7535\u5b50\u8f6c\u79fb\u80fd\u529b\u3002<\/p>\n<p>\u56fe\u00a02\uff1a\uff08A\u3001B\uff09\u4e0d\u540c\u4fee\u9970\u7535\u6781\u5728 PBS \u4e2d\u7684\u5149\u7535\u6d41\u54cd\u5e94\u3002(C) \u4e0d\u540c\u6837\u54c1\u7684 Zeta \u7535\u4f4d\u503c\u3002(D) O2-\u00a0\u5728 Cu2O\/Cu@mC\/CNS \u5b58\u5728\u4e0b\u7684 EPR \u5149\u8c31\u3002(E) \u4e0d\u540c\u4fee\u9970\u7535\u6781\u7684\u7535\u5316\u5b66\u963b\u6297\u8c31\u3002(F) \u4e0d\u540c\u4fee\u9970\u7535\u6781\u7684 Bode \u56fe\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-254578\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-21.png\" alt=\"\" width=\"600\" height=\"240\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-21.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-21-300x120.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u56fe\u00a03A \u5c55\u793a\u4e86 Cu2O\/Cu@mC\/CNS\/GCE \u4f20\u611f\u5668\u5728\u4e0d\u540c L-Cys \u6d53\u5ea6\u68af\u5ea6\u7684\u6700\u4f73\u5b9e\u9a8c\u6d4b\u8bd5\u6761\u4ef6\u4e0b\u7684\u5b9e\u65f6\u5149\u7535\u6d41\u54cd\u5e94\u3002\u5728 10 nM &#8211; 4 \u00b5M \u8303\u56f4\u5185\uff0c\u5149\u7535\u6d41\u7684\u53d8\u5316\u503c\u4e0e L-Cys \u6d53\u5ea6\u7684\u5bf9\u6570\u4e4b\u95f4\u5b58\u5728\u4e24\u4e2a\u7ebf\u6027\u56de\u5f52\u65b9\u7a0b\uff08\u56fe\u00a07B\uff09\uff0c\u5982\u4e0b\u6240\u793a\u3002<\/p>\n<p>\u56fe\u00a03. (A) Cu2O\/Cu@mC\/CNS \u5bf9\u4e0d\u540c\u6d53\u5ea6 L-Cys \u7684\u5149\u7535\u6d41\u54cd\u5e94\uff08a \u81f3 k\uff1a0.01\u30010.02\u30010.04\u30010.08\u30010.1\u30010.2\u30010.4\u30010.8\u30011.6\u30012.0\u30014.0 \u03bcM\uff09\u3002(B) \u5149\u7535\u6d41\u4e0e L-Cys \u6d53\u5ea6\u4e4b\u95f4\u7684\u7ebf\u6027\u5173\u7cfb\u3002<\/p>\n<p>\u5982\u56fe4\u6240\u793a\uff0c\u5c55\u793a\u4e86\u57fa\u4e8e Cu2O\/Cu@mC\/CNS\/GCE \u7684 PEC \u4f20\u611f\u5668\u68c0\u6d4b L-Cys \u7684\u673a\u7406\u3002\u9996\u5148\uff0cCu2O\/Cu@mC \u548c CNS \u5728\u53ef\u89c1\u5149\u7684\u6fc0\u53d1\u4e0b\u4ea7\u751f\u7535\u5b50\u548c\u7a7a\u7a74\uff0c\u5f62\u6210 p-n \u5f02\u8d28\u7ed3\u540e\u83b7\u5f97\u5149\u7535\u6d41\u4fe1\u53f7\u3002\u7535\u5b50\u8fd8\u80fd\u8f6c\u5316 O2 \u751f\u6210 \u00b7O2-\uff0c\u8fd9\u4e00\u7ed3\u8bba\u4e5f\u5f97\u5230\u4e86 EPR \u5b9e\u9a8c\u7684\u8bc1\u5b9e\u3002\u78b3\u5143\u7d20\u5145\u5f53\u4e86\u7535\u5b50\u4ecb\u8d28\uff0c\u6269\u5927\u4e86 PEC \u7684\u53ef\u89c1\u5149\u5438\u6536\u8303\u56f4\u3002\u4e8b\u5b9e\u4e0a\uff0cCu2O\/Cu@mC \u4e2d Cu (I) \u7684\u4ef7\u7535\u5b50\u6784\u578b\u4e3a 3d10\uff0cCu (I) \u62e5\u6709\u4e00\u4e2a\u672a\u88ab\u5360\u7528\u7684 4s \u8f68\u9053\uff0c\u800c L-Cys \u7684\u786b\u9187\u57fa\u56e2\u4e2d\u7684\u5b64\u5bf9\u7535\u5b50\u8f6c\u79fb\u5230Cu (I)\u00a0\u7684\u7a7a\u95f2\u8f68\u9053\u4e0a\u4f1a\u5f62\u6210 Cu-S \u5171\u4ef7\u952e\uff0c\u7c98\u9644\u5728\u7535\u6781\u8868\u9762\uff0c\u4ece\u800c\u963b\u788d\u7535\u5b50\u7684\u8f6c\u79fb\u548c\u6d88\u8017\u3002CNS \u7684\u7247\u72b6\u7ed3\u6784\u548c\u9ad8\u6bd4\u8868\u9762\u79ef\u6210\u4e3a Cu2O\/Cu@mC \u4e0e L-Cys \u7ed3\u5408\u7684\u8f7d\u4f53\u3002\u56e0\u6b64\uff0c\u6240\u5f00\u53d1\u7684\u57fa\u4e8e\u00a0Cu2O\/Cu@mC\/CNS\/GCE \u7684 PEC \u4f20\u611f\u5668\u53ef\u7528\u4e8e\u9009\u62e9\u6027\u68c0\u6d4b L-Cys\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-254579\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-41.png\" alt=\"\" width=\"600\" height=\"381\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-41.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/09\/\u56fe\u7247-41-300x191.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u56fe\u00a04. \u57fa\u4e8e Cu2O\/Cu@mC\/CNS\/GCE \u7684\u5149\u7535\u5316\u5b66\u4f20\u611f\u5668\u68c0\u6d4b L-Cys \u7684\u673a\u7406\u793a\u610f\u56fe\u3002<\/p>\n<p>\u3010\u603b\u7ed3\u4e0e\u5c55\u671b\u3011<\/p>\n<p>\u603b\u4e4b\uff0c\u4f5c\u8005\u63d0\u51fa\u4e86\u4e00\u79cd\u57fa\u4e8eCu2O\/Cu@mC\/CNS\/GCE\u7684PEC\u4f20\u611f\u5668\u5e73\u53f0\uff0c\u5b9e\u73b0\u4e86\u5bf9L-Cys\u7684\u68c0\u6d4b\u3002\u5176\u4e2d\uff0cCu2O\/Cu@mC \u4e2d\u7684\u78b3\u5143\u7d20\u589e\u5f3a\u4e86\u6750\u6599\u7684\u6574\u4f53\u5bfc\u7535\u6027\uff0c\u4fc3\u8fdb\u4e86\u7535\u5b50\u4f20\u9012\u3002\u5728\u6700\u4f73\u5b9e\u9a8c\u6761\u4ef6\u4e0b\uff0cCu2O\/Cu@mC\/CNS\/GCE \u4f20\u611f\u5668\u5177\u6709\u8f83\u5bbd\u7684\u7ebf\u6027\u8303\u56f4\u548c\u8d85\u4f4e\u7684\u68c0\u6d4b\u9650\u3002\u7ebf\u6027\u8303\u56f4\u4ece 10 nM \u5230 4 \u00b5M\uff0c\u68c0\u6d4b\u9650\u4e3a 1.26 nM\u3002\u8fd9\u662f\u7531\u4e8e Cu2O\/Cu@mC \u4e0a\u7684\u94dc\u79bb\u5b50\u4e0e\u68c0\u6d4b\u5668 L-Cys \u4e0a\u7684\u786b\u539f\u5b50\u4e4b\u95f4\u5f62\u6210\u4e86 Cu-S \u952e\uff0c\u4ece\u800c\u5b9e\u73b0\u4e86\u5bf9 L-Cys \u7684\u7075\u654f\u68c0\u6d4b\u3002\u901a\u8fc7\u5c06\u68c0\u6d4b\u7ed3\u679c\u4e0e\u7d2b\u5916\u53ef\u89c1\u5206\u5149\u5149\u5ea6\u6cd5\u7684\u68c0\u6d4b\u7ed3\u679c\u8fdb\u884c\u6bd4\u8f83\uff0c\u8bc1\u660e\u4e86\u8be5\u4f20\u611f\u5668\u7684\u9ad8\u7cbe\u786e\u5ea6\u3002\u7279\u522b\u662f\uff0c\u5b9e\u9645\u6837\u54c1\u7ed3\u679c\u9a8c\u8bc1\u4e86 PEC \u4f20\u611f\u5668\u5728\u6709\u6548\u68c0\u6d4b\u81ea\u6765\u6c34\u548c\u4eba\u4f53\u8840\u6e05\u4e2d\u7684 L-Cys \u65b9\u9762\u5177\u6709\u51fa\u8272\u7684\u7a33\u5b9a\u6027\u548c\u53ef\u91cd\u590d\u6027\u3002<\/p>\n<p>\u3010\u8d39\u4fca\u6770\u6559\u6388\u7b80\u4ecb\u3011<\/p>\n<p>\u8d39\u4fca\u6770\u6559\u6388\uff0c\u4e8c\u7ea7\u6559\u6388\uff0c\u535a\u58eb\u751f\u5bfc\u5e08\uff0c\u6e56\u5357\u7701\u6770\u9752\uff0c\u6e56\u5357\u7701\u81ea\u7136\u79d1\u5b66\u4e8c\u7b49\u5956\u83b7\u5f97\u8005\uff0c\u6e56\u5357\u7701\u201c\u8299\u84c9\u5b66\u8005\u201d\u7279\u8058\u6559\u6388\u3002\u4e3b\u8981\u4ece\u4e8b\u5149\u7535\u5316\u5b66\u4f20\u611f\u5668\uff0c\u73af\u5883\u5206\u6790\u5316\u5b66\uff0c\u78b3\u57fa\u7535\u5316\u5b66\u4f20\u611f\u5668\uff0c\u7eb3\u7c73\u7535\u5206\u6790\u5316\u5b66\u7b49\u65b9\u9762\u7684\u7814\u7a76\u5de5\u4f5c\u3002\u8fd1\u5e74\u6765\u5728Science\u3001Angewandte Chemie International Edition\u3001Chemical Engineering Journal\u3001Carbon\u3001Analytical Chemistry\u3001Biosensors and Bioelectronics\u3001Nanoscale\u3001Journal of Colloid and Interface Science\u3001Sensors and Actuators B: Chemical\u7b49SCI\u671f\u520a\u4e0a\u53d1\u8868\u8bba\u6587100\u4f59\u7bc7\u3002\u73b0\u62c5\u4efb\u6559\u80b2\u90e8\u73af\u5883\u53cb\u597d\u5316\u5b66\u4e0e\u5e94\u7528\u91cd\u70b9\u5b9e\u9a8c\u5ba4\u526f\u4e3b\u4efb\uff0c\u6e56\u5357\u7701\u7eff\u8272\u6709\u673a\u5408\u6210\u4e0e\u5e94\u7528\u91cd\u70b9\u5b9e\u9a8c\u5ba4\u526f\u4e3b\u4efb\uff0c\u6e58\u6f6d\u5e02\u6d77\u6ce1\u77f3\u4ea7\u4e1a\u54a8\u8be2\u59d4\u5458\u4f1a\u59d4\u5458\u7b49\u804c\u52a1\u3002<\/p>\n<p>\u8bfe\u9898\u7ec4\u5b98\u7f51\uff1ahttps:\/\/www.x-mol.com\/groups\/fei_junjie<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1ahttps:\/\/www.sciencedirect.com\/science\/article\/pii\/S000862232300711X<\/p>\n<p>\u672c\u6587\u7531\u4f5c\u8005\u4f9b\u7a3f\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u80cc\u666f\u4ecb\u7ecd\u3011 L-\u534a\u80f1\u6c28\u9178\uff08L-Cys\uff09\u662f\u4e00\u79cd\u975e\u5e38\u91cd\u8981\u7684\u5929\u7136\u6c28\u57fa\u9178\uff0c\u5b83\u542b\u6709\u786b\u4f5c\u4e3a\u6d3b\u6027\u4f4d\u70b9\uff0c\u56e0\u6b64\u53ef\u4ee5\u4e0e\u8bb8\u591a\u6709\u6bd2\u7269\u8d28\u5f62\u6210\u65e0\u6bd2\u914d\u5408\u7269\uff0c\u4ece\u4f53\u5185\u6d88\u9664\u3002\u56e0\u6b64\uff0c\u5bfb\u627e\u4e00\u79cd\u4f4e\u6210\u672c&#8230;<\/p>\n","protected":false},"author":2,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-254573","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/254573"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/2"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=254573"}],"version-history":[{"count":4,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/254573\/revisions"}],"predecessor-version":[{"id":254582,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/254573\/revisions\/254582"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=254573"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=254573"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=254573"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}