{"id":256110,"date":"2023-11-26T06:58:57","date_gmt":"2023-11-25T22:58:57","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=256110"},"modified":"2023-11-25T18:59:07","modified_gmt":"2023-11-25T10:59:07","slug":"%e9%83%ad%e7%8e%89%e5%9b%bd%e6%95%99%e6%8e%88nat-commun-%ef%bc%9a%e9%80%89%e6%8b%a9%e6%80%a7sei%e6%ba%b6%e8%a7%a3%e7%ad%96%e7%95%a5%e5%ae%9e%e7%8e%b0%e9%95%bf%e5%af%bf%e5%91%bd%e5%be%ae%e7%b1%b3","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=256110","title":{"rendered":"\u90ed\u7389\u56fd\u6559\u6388Nat. Commun.\uff1a\u9009\u62e9\u6027SEI\u6eb6\u89e3\u7b56\u7565\u5b9e\u73b0\u957f\u5bff\u547d\u5fae\u7c73\u7845\u8d1f\u6781"},"content":{"rendered":"<p><strong>\u4e00\u3001\u3010\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p>\u5bf9\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u7535\u6c60\u7684\u9700\u6c42\u4e0d\u65ad\u589e\u957f\uff0c\u8981\u6c42\u5728\u9502\u79bb\u5b50\u7535\u6c60\u4e2d\u4f7f\u7528\u77f3\u58a8\u4ee5\u5916\u7684\u65b0\u578b\u8d1f\u6781\u6750\u6599\u3002\u5177\u6709\u9ad8\u7406\u8bba\u6bd4\u5bb9\u91cf\u7684\u66ff\u4ee3\u7535\u6781\u6750\u6599\u6b63\u5728\u88ab\u6df1\u5165\u8ba8\u8bba\uff0c\u4f8b\u5982Li\u91d1\u5c5e\u8d1f\u6781\u548c\u5408\u91d1\u578b\u8d1f\u6781\u6750\u6599\uff0c\u5982\u7845\uff08Si\uff09\u3002\u5fae\u7c73\u7ea7Si\u8d1f\u6781\u5177\u6709\u6bd4\u4f20\u7edf\u77f3\u58a8\u8d1f\u6781\u9ad8\u5f97\u591a\u7684\u7406\u8bba\u5bb9\u91cf\u548c\u6bd4\u7eb3\u7c73\u7ea7Si\u8d1f\u6781\u66f4\u9ad8\u7684\u5e94\u7528\u524d\u666f\u3002\u7136\u800c\uff0c\u5176\u5728\u9502\u5316\u8fc7\u7a0b\u4e2d\u4e25\u91cd\u7684\u4f53\u79ef\u81a8\u80c0\u963b\u788d\u4e86\u5176\u5e94\u7528\uff0c\u56e0\u6b64\u9700\u8981\u5177\u6709\u589e\u5f3a\u673a\u68b0\u7a33\u5b9a\u6027\u7684\u56fa\u4f53\u7535\u89e3\u8d28\u754c\u9762\u76f8\uff08SEI\uff09\u6765\u7a33\u5b9a\u5176\u4f53\u79ef\u53d8\u5316\u3002\u5bf9\u4e8eSi\u8d1f\u6781\uff0c\u5176\u8d85\u9ad8\u7406\u8bba\u6bd4\u5bb9\u91cf\uff08Li<sub>15<\/sub>Si<sub>4<\/sub>\uff0c3579\u2009mAh\u2009g<sup>\u22121<\/sup>\uff09\u4f34\u968f\u7740\u5927\u91cf\u7684\u4f53\u79ef\u53d8\u5316\u548c\u754c\u9762\u95ee\u9898\u3002\u56e0\u6b64\uff0c\u5bf9\u4e8e\u957f\u5bff\u547d\u5fae\u7c73\u5c3a\u5bf8\u7684Si\u8d1f\u6781\uff0c\u5fc5\u987b\u63d0\u9ad8SEI\u7684\u6297\u4fb5\u8680\u7684\u673a\u68b0\u7a33\u5b9a\u6027\u3002<\/p>\n<p><strong>\u00a0<\/strong><strong>\u4e8c\u3001\u3010\u6210\u679c\u63a0\u5f71\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u4e2d\u56fd\u79d1\u5b66\u9662\u5316\u5b66\u7814\u7a76\u6240\u90ed\u7389\u56fd\u6559\u6388<\/strong>\u56e2\u961f\u63d0\u51fa\u4e86\u4e00\u79cd\u6eb6\u5242\u8bf1\u5bfc\u7684\u9009\u62e9\u6027\u6eb6\u89e3\u7b56\u7565\u6765\u539f\u4f4d\u8c03\u8282SEI\u7684\u673a\u68b0\u6027\u80fd\u3002\u901a\u8fc7\u5728\u5e38\u89c4\u7535\u89e3\u8d28\u4e2d\u52a0\u5165\u9ad8\u7ed9\u4f53\u6570\uff08DN\uff09\u6eb6\u5242\u2014\u4e01\u5185\u916f\uff0c\u53ef\u4ee5\u5728\u5faa\u73af\u65f6\u9009\u62e9\u6027\u6eb6\u89e3SEI\u7684\u4f4e\u6a21\u91cf\u7ec4\u5206\uff0c\u5982\u70f7\u57fa\u78b3\u9178\u9502\uff0c\u7559\u4e0b\u4e3b\u8981\u7531\u6c1f\u5316\u9502\u548c\u805a\u78b3\u9178\u916f\u7ec4\u6210\u7684\u575a\u56faSEI\u3002\u91c7\u7528\u8fd9\u79cd\u7b56\u7565\uff0c\u539f\u59cb\u5fae\u7c73\u7ea7\u7845\u8d1f\u6781\u57280.5 C(1500 mA g<sup>-1<\/sup>\uff0c25\u00b0C)\u4e0b\u5faa\u73af100\u6b21\u540e\u4ecd\u80fd\u4fdd\u630187.5%\u7684\u5bb9\u91cf\uff0c\u4f7f\u7528\u78b3\u6d82\u5c42\u5fae\u7c73\u7ea7\u7845\u8d1f\u6781\u53ef\u4ee5\u63d0\u9ad8\u5230300\u6b21\u5faa\u73af\u3002\u6b64\u5916\uff0c\u57280.5 C(90 mA g<sup>-1<\/sup>)\u4e0b\u5faa\u73af150\u6b21\u540e\uff0c\u4f7f\u7528\u5fae\u7c73\u7ea7Si\u8d1f\u6781\u548c\u9009\u62e9\u6027\u6eb6\u89e3SEI\u7684Si||LiNi<sub>0.8<\/sub>Co<sub>0.1<\/sub>Mn<sub>0.1<\/sub>O<sub>2<\/sub>\u7535\u6c60\u5bb9\u91cf\u4fdd\u6301\u572883.7%\u3002\u8be5SEI\u7684\u9009\u62e9\u6027\u6eb6\u89e3\u6548\u5e94\u4ee5\u53ca\u76f8\u5e94\u7684Si\u8d1f\u6781\u5faa\u73af\u5bff\u547d\u4e0e\u6eb6\u5242\u7684\u7ed9\u4f53\u6570\u5448\u6b63\u76f8\u5173\uff0c\u8868\u660e\u8bbe\u8ba1\u9ad8\u7ed9\u4f53\u6570\u7535\u89e3\u8d28\u53ef\u4ee5\u8c03\u63a7SEI\u4ee5\u7a33\u5b9a\u9ad8\u80fd\u91cf\u53ef\u5145\u7535\u7535\u6c60\u4e2d\u4f53\u79ef\u53d8\u5316\u8f83\u5927\u7684\u5408\u91d1\u578b\u8d1f\u6781\u3002\u7814\u7a76\u6210\u679c\u4ee5\u9898\u4e3a\u201c<strong>Tailoring chemical composition of solid electrolyte interphase by selective dissolution for long-life micron-sized silicon anode<\/strong>\u201d\u53d1\u8868\u5728\u77e5\u540d\u671f\u520a<strong><em>Nature Communications<\/em><\/strong>\u4e0a\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-256111\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/11\/0-11.png\" alt=\"\" width=\"600\" height=\"383\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/11\/0-11.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/11\/0-11-300x192.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u4e09\u3001\u3010\u6838\u5fc3\u521b\u65b0\u70b9\u3011<\/strong><\/p>\n<p>1\u3001\u63d0\u51fa\u4e86\u4e00\u79cd\u6eb6\u5242\u8bf1\u5bfc\u7684\u9009\u62e9\u6027\u6eb6\u89e3\u7b56\u7565\u6765\u539f\u4f4d\u8c03\u8282SEI\u7684\u673a\u68b0\u6027\u80fd\u3002<\/p>\n<p>2\u3001\u8be5\u7b56\u7565\u4e0b\u5fae\u7c73\u7ea7\u7845\u8d1f\u6781\u57280.5 C\u4e0b\u5faa\u73af100\u6b21\u540e\u4ecd\u80fd\u4fdd\u630187.5%\u7684\u5bb9\u91cf\uff0c\u4f7f\u7528\u78b3\u6d82\u5c42\u5fae\u7c73\u7ea7\u7845\u8d1f\u6781\u53ef\u4ee5\u63d0\u9ad8\u5230300\u6b21\u5faa\u73af\u3002<\/p>\n<p>3\u3001GBL\u57fa\u7535\u89e3\u8d28\u7684Si||NCM811\u5168\u7535\u6c60\u57280.2 C\u4e0b\u5faa\u73af150\u6b21\u540e\uff0c\u5bb9\u91cf\u4fdd\u6301\u7387\u9ad8\u8fbe83.7%\u3002<\/p>\n<p><strong>\u56db\u3001\u3010\u6570\u636e\u6982\u89c8\u3011<\/strong><\/p>\n<p><strong>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-256112\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/11\/1-8.png\" alt=\"\" width=\"600\" height=\"462\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/11\/1-8.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/11\/1-8-300x231.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/strong><\/p>\n<p><strong>\u56fe<\/strong><strong>1\u00a0 SEI<\/strong><strong>\u7ec4\u5206\u7684\u6eb6\u5242\u8bf1\u5bfc\u6eb6\u89e3\u6548\u5e94<\/strong><strong> \u00a9 2023 Springer Nature<\/strong><\/p>\n<p>\uff08a\uff09\u6eb6\u5242\u8bf1\u5bfc\u7684SEI\u9009\u62e9\u6027\u6eb6\u89e3\u793a\u610f\u56fe\u3002<\/p>\n<p>\uff08b\uff09\u7eafGBL\u6eb6\u5242\u548c\u6d78\u6ce1\u5faa\u73af\u7845\u7535\u6781\u540e\u7684GBL\u6838\u78c1\u5171\u632f\u6c22\u8c31\u3002<\/p>\n<p>\uff08c\uff09\u7535\u5316\u5b66\u5faa\u73af\u540e\u7528\u5404\u79cd\u6eb6\u5242\u6d78\u6ce1\u7684Si\u7535\u6781\u76f8\u5bf9\u5143\u7d20\u542b\u91cf\u3002<\/p>\n<p>\uff08d\uff09GBL\u57fa\u7535\u89e3\u8d28\u4e2dSD-SEI\u7684\u5f62\u6210\u8fc7\u7a0b\u793a\u610f\u56fe\u3002<\/p>\n<p>\uff08e-f\uff09MD\u6a21\u62df\u7684\u5feb\u7167\u6846\u663e\u793a\u4e86GBL\u6eb6\u5242\u548cEC\u6eb6\u5242\u4e2d\u7684\u4ee3\u8868\u6027SEI\u7269\u79cd\u3002<\/p>\n<p>\uff08g\uff09\u5728GBL\u548cEC\u6eb6\u5242\u4e2dLi-O\u7684g(<em>r<\/em>)\u3002<\/p>\n<p>\uff08h\uff09GBL\u548cEC\u6eb6\u5242\u4e2dCO<sub>3<\/sub>CH<sub>2<\/sub>CH<sub>2<\/sub>CO<sub>3<\/sub><sup>2\u2212<\/sup>(LEDC\u9634\u79bb\u5b50)\u3001Li<sup>+<\/sup>\u3001CH<sub>3<\/sub>CH<sub>2<\/sub>O<sup>\u2212<\/sup>\u3001CH<sub>3<\/sub>CH<sub>2<\/sub>CO<sub>3<\/sub><sup>\u2212<\/sup>(LEC\u9634\u79bb\u5b50)\u548cPF<sub>2<\/sub>O<sup>\u2212<\/sup>\u79bb\u5b50\u7684MSD\u5206\u6790\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-256113\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/11\/2-9.png\" alt=\"\" width=\"600\" height=\"539\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/11\/2-9.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/11\/2-9-300x270.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>2\u00a0 SEI<\/strong><strong>\u7684\u5316\u5b66\u6210\u5206<\/strong><strong> \u00a9 2023 Springer Nature<\/strong><\/p>\n<p>\uff08a-b\uff09SD-SEI\u51b7\u51bb\u900f\u5c04\u7535\u955c\u56fe\u50cf\u548c\u653e\u5927\u56fe\u50cf\u3002<\/p>\n<p>\uff08c\uff09SD-SEI\u7684\u5178\u578bLi K-edge EEL\u8c31\u3002<\/p>\n<p>\uff08d\uff09SD-SEI\u548cc-SEI\u7684MALDI-ToF-MS\u3002<\/p>\n<p>\uff08e\uff09\u4e0d\u540c\u6df1\u5ea6\u5404SEI\u4e2d\u6240\u9009\u7ec4\u5206\u7684\u76f8\u5bf9\u542b\u91cf\u3002<\/p>\n<p>\uff08f-j\uff09\u5728GBL\u57fa\u7535\u89e3\u8d28\u3001PC\u57fa\u7535\u89e3\u8d28\u548cEC\u57fa\u7535\u89e3\u8d28\u4e2d\u6e85\u5c04\u5f97\u5230\u7684\u5404\u79cd\u4e8c\u6b21\u79bb\u5b50\u7684\u6df1\u5ea6\u5206\u5e03\u56fe\uff0c\u4ee5\u53caGBL\u57fa\u7535\u89e3\u8d28\u4e2d\u5faa\u73af\u5fae\u7c73\u7ea7Si\u7535\u6781\u7684LiF<sub>2<\/sub><sup>\u2212<\/sup>\u548cO<sup>\u2212<\/sup>\u7684ToF-SIMS\u4e8c\u6b21\u79bb\u5b50\u56fe\u50cf\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-256114\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/11\/3-9.png\" alt=\"\" width=\"600\" height=\"438\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/11\/3-9.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/11\/3-9-300x219.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>3\u00a0 <\/strong><strong>\u5fae\u7c73\u7ea7\u7845\u7535\u6781\u7684\u5faa\u73af\u6027\u80fd<\/strong><strong> \u00a9 2023 Springer Nature<\/strong><\/p>\n<p>\uff08a\uff09\u5fae\u7c73\u7ea7\u7845\u8d1f\u6781\u5728GBL\u57fa\u7535\u89e3\u8d28\u4e2d0.05 C\u30010.06 V\u548c1.0 V\u7684\u5178\u578b\u5145\u653e\u7535\u66f2\u7ebf\u3002<\/p>\n<p>\uff08b\uff09\u5fae\u7c73\u7ea7\u7845\u8d1f\u6781\u57280.2 C\u4e0d\u540c\u7535\u89e3\u8d28\u4e2d\u7684\u5faa\u73af\u6027\u80fd\u548cCE\u3002<\/p>\n<p>\uff08c\uff09\u4e0d\u540c\u7535\u89e3\u8d28\u4e2d\u7684\u500d\u7387\u6027\u80fd\u5bf9\u6bd4\u3002<\/p>\n<p>\uff08d\uff090.2 C\u4e0bSi@C\u8d1f\u6781\u5728\u4e0d\u540c\u7535\u89e3\u8d28\u4e2d\u7684\u5faa\u73af\u6027\u80fd\u548cCE\u3002<\/p>\n<p>\uff08e-f\uff09\u57283.0 V\u548c4.2 V\u4e4b\u95f4\uff0c0.05 C\u4e0b\u4f7f\u7528\u4e0d\u540c\u7535\u89e3\u8d28\u7684Si||NCM811\u5168\u7535\u6c60\u5178\u578b\u5145\u653e\u7535\u66f2\u7ebf\u548c\u5faa\u73af\u6027\u80fd\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-256115\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/11\/4-8.png\" alt=\"\" width=\"600\" height=\"411\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/11\/4-8.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/11\/4-8-300x206.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>4\u00a0 SEI<\/strong><strong>\u7684\u673a\u68b0\u6027\u80fd<\/strong><strong> \u00a9 2023 Springer Nature<\/strong><\/p>\n<p>\uff08a-c\uff09SD-SEI\u3001F-SEI\u548cc-SEI\u7684Derjaguin-Muller-Toporov(DMT)\u6a21\u91cf\u5206\u5e03\u3002<\/p>\n<p>\uff08d-f\uff09\u5728SD-SEI\u3001F-SEI\u548cc-SEI\u4e0a\u5f97\u5230\u7684\u529b-\u4f4d\u79fb\u66f2\u7ebf\u3002<\/p>\n<p>\uff08g-i\uff09\u7845\u7535\u6781\u5728GBL\u57fa\u7535\u89e3\u8d28\u3001PC\u57fa\u7535\u89e3\u8d28\u548cEC\u57fa\u7535\u89e3\u8d28\u4e2d\u5faa\u73af100\u6b21\u540e\u7684SEM\u56fe\u50cf\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-256116\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/11\/5-6.png\" alt=\"\" width=\"600\" height=\"152\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/11\/5-6.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2023\/11\/5-6-300x76.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>5\u00a0 SEI<\/strong><strong>\u7684\u793a\u610f\u56fe\u548c\u5bf9\u6bd4<\/strong><strong> \u00a9 2023 Springer Nature<\/strong><\/p>\n<p>\uff08a\uff09\u4e0d\u540cSEI\u5404\u56e0\u7d20\u7684\u6bd4\u8f83\u3002<\/p>\n<p>\uff08b\uff09SD-SEI\u4e2d\u805a\u78b3\u9178\u916f\u548cLiF\u7ef4\u62a4\u754c\u9762\u7a33\u5b9a\u6027\u7684\u793a\u610f\u56fe\u3002<\/p>\n<p>\uff08c\uff09DN\u4e0e\u5404\u79cd\u6eb6\u5242\u7684\u76f8\u5bf9\u6eb6\u89e3\u5ea6\u53caSi@C\u8d1f\u6781\u5728\u76f8\u5e94\u7535\u89e3\u8d28\u4e2d\u5faa\u73af100\u6b21\u540e\u7684\u5bb9\u91cf\u4fdd\u6301\u7387\u7684\u5173\u7cfb\u3002<\/p>\n<p><strong>\u4e94\u3001\u3010\u6210\u679c\u542f\u793a\u3011<\/strong><\/p>\n<p>\u672c\u7814\u7a76\u63d0\u51fa\u4e86\u4e00\u79cd\u901a\u8fc7\u9ad8\u7ed9\u4f53\u6570\uff08DN\uff09\u6eb6\u5242\u9009\u62e9\u6027\u6eb6\u89e3\u4e0d\u5229\u7684SEI\u7ec4\u5206\u6765\u6784\u5efa\u5fae\u7c73\u7ea7\u7845\u8d1f\u6781\u65e0\u673a\u805a\u5408\u7269SEI\u7684\u7b56\u7565\u3002\u53d7\u6b64\u7b56\u7565\u7684\u542f\u53d1\uff0c\u9009\u62e9\u4e86\u4ee5GBL\u4e3a\u4ee3\u8868\u7684\u6eb6\u5242\u6765\u521b\u9020\u9ad8DN\u73af\u5883\uff0c\u5728\u5176\u4e2d\u6c89\u79ef\u5e76\u4fdd\u6301\u5927\u91cf\u805a\u78b3\u9178\u916f\u548c\u65e0\u673a\u7269\u8d28\uff0c\u4ee5\u6784\u5efa\u65e0\u673a\u805a\u5408\u7269SD-SEI\u3002\u7531\u4e8eSD-SEI\u4e2d\u7684\u65e0\u673a\u548c\u9ad8\u5206\u5b50\u4e3b\u8981\u6210\u5206\u5177\u6709\u8f83\u5f3a\u7684\u673a\u68b0\u97e7\u6027\uff0c\u57280.2 C\u4e0b\u5faa\u73af100\u6b21\u540e\uff0c\u539f\u5fae\u7c73\u7ea7Si\u8d1f\u6781\u7684\u5bb9\u91cf\u4fdd\u6301\u7387\u8fbe\u523087.5%\uff0c\u5f53\u4f7f\u7528\u78b3\u5305\u8986\u7684\u5fae\u7c73\u7ea7Si\u8d1f\u6781\u65f6\uff0c\u5faa\u73af\u5bff\u547d\u53ef\u4ee5\u8fdb\u4e00\u6b65\u6269\u5c55\u5230300\u6b21\u4ee5\u4e0a\u3002\u91c7\u7528GBL\u57fa\u7535\u89e3\u8d28\u7684Si||NCM811\u5168\u7535\u6c60\u57280.2 C\u4e0b\u5faa\u73af150\u6b21\u540e\uff0c\u5bb9\u91cf\u4fdd\u6301\u7387\u9ad8\u8fbe83.7%\u3002\u8fd9\u9879\u5de5\u4f5c\u4e0d\u4ec5\u63d0\u4f9b\u4e86\u4e00\u79cd\u8c03\u63a7\u5fae\u7c73\u7ea7\u7845\u8d1f\u6781SEI\u7684\u7b56\u7565\uff0c\u800c\u4e14\u63ed\u793a\u4e86\u6eb6\u5242\u7684\u7406\u5316\u6027\u8d28\u4e0e\u7535\u5316\u5b66\u6027\u80fd\u4e4b\u95f4\u7684\u5173\u7cfb\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong>\u539f\u6587\u8be6\u60c5<\/strong>\uff1a<a href=\"https:\/\/www.nature.com\/articles\/s41467-023-43093-6\" target=\"_blank\" rel=\"noopener\">Tailoring chemical composition of solid electrolyte interphase by selective dissolution for long-life micron-sized silicon anode<\/a> (<em>Nat. Commun.<\/em> <strong>2023<\/strong>, <em>14<\/em>, 7247)<\/p>\n<p>\u672c\u6587\u7531\u8d5b\u6069\u65af\u4f9b\u7a3f\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u4e00\u3001\u3010\u5bfc\u8bfb\u3011 \u5bf9\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u7535\u6c60\u7684\u9700\u6c42\u4e0d\u65ad\u589e\u957f\uff0c\u8981\u6c42\u5728\u9502\u79bb\u5b50\u7535\u6c60\u4e2d\u4f7f\u7528\u77f3\u58a8\u4ee5\u5916\u7684\u65b0\u578b\u8d1f\u6781\u6750\u6599\u3002\u5177\u6709\u9ad8\u7406\u8bba\u6bd4\u5bb9\u91cf\u7684\u66ff\u4ee3\u7535\u6781\u6750\u6599\u6b63\u5728\u88ab\u6df1\u5165\u8ba8\u8bba\uff0c\u4f8b\u5982Li\u91d1\u5c5e\u8d1f\u6781\u548c\u5408\u91d1&#8230;<\/p>\n","protected":false},"author":36791,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-256110","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/256110"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/36791"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=256110"}],"version-history":[{"count":1,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/256110\/revisions"}],"predecessor-version":[{"id":256117,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/256110\/revisions\/256117"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=256110"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=256110"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=256110"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}