{"id":260285,"date":"2024-05-19T06:32:19","date_gmt":"2024-05-18T22:32:19","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=260285"},"modified":"2024-05-19T00:35:40","modified_gmt":"2024-05-18T16:35:40","slug":"%e4%b8%80%e7%a7%8d%e5%85%b7%e6%9c%89%e8%b6%85%e9%ab%98%e5%af%bc%e7%94%b5%e5%92%8c%e8%b6%85%e9%ab%98%e5%bc%ba%e5%ba%a6%e7%9a%84%e6%96%b0%e5%9e%8bcu-ti%ef%bc%88%e9%92%9b%e9%9d%92%e9%93%9c%ef%bc%89","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=260285","title":{"rendered":"\u4e00\u79cd\u5177\u6709\u8d85\u9ad8\u5bfc\u7535\u548c\u8d85\u9ad8\u5f3a\u5ea6\u7684\u65b0\u578bCu-Ti\uff08\u949b\u9752\u94dc\uff09\u5408\u91d1\u7ec4\u7ec7"},"content":{"rendered":"<p><strong>\u4e00\u3001<\/strong><strong>\u00a0<\/strong><strong>\u3010\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p>\u9ad8\u5f3a\u5ea6\u3001\u9ad8\u5bfc\u7535\u6027\u7684\u5f39\u6027\u6750\u6599\u5728\u7535\u6c60\u7aef\u5b50\u3001\u5929\u7ebf\u7aef\u5b50\u3001SIM\u5361\u8fde\u63a5\u53ca\u8fde\u63a5\u5668\u7b49\u65b9\u9762\u6709\u7740\u91cd\u8981\u7684\u5e94\u7528\u3002Cu-Be\u5408\u91d1\u4f5c\u4e3a\u4e00\u79cd\u4f20\u7edf\u7684\u9ad8\u5f39\u6027\u5408\u91d1\uff0c\u5177\u6709\u9ad8\u5f3a\u5ea6\u3001\u9ad8\u5bfc\u7535\u6027\u7b49\u7279\u6027\uff0c\u4f46\u5bf9\u4eba\u7c7b\u5065\u5eb7\u6709\u5bb3\uff0c\u5bf9\u73af\u5883\u6c61\u67d3\u4e25\u91cd\uff0c\u56e0\u6b64\u6709\u5fc5\u8981\u7814\u7a76\u53ef\u66ff\u4ee3\u7684\u73af\u4fdd\u94dc\u5408\u91d1\u3002Cu-Ti\u5408\u91d1\u4ee5\u5176\u4f18\u5f02\u7684\u5f3a\u5ea6\u3001\u9ad8\u5f39\u6027\u548c\u826f\u597d\u7684\u73af\u4fdd\u6027\u800c\u53d7\u5230\u7814\u7a76\u8005\u7684\u5e7f\u6cdb\u5173\u6ce8\u3002\u7136\u800c\uff0c\u7531\u4e8e\u949b\u539f\u5b50\u63ba\u5165\u5230\u94dc\u57fa\u4f53\u4e2d\uff0cCu-Ti\u5408\u91d1\u8868\u73b0\u51fa\u975e\u5e38\u4f4e\u7684\u5bfc\u7535\u6027\u3002\u56e0\u6b64\uff0c\u5728\u4fdd\u6301Cu-Ti\u5408\u91d1\u5f3a\u5ea6\u548c\u5f39\u6027\u6027\u80fd\u7684\u540c\u65f6\uff0c\u63d0\u9ad8\u5176\u5bfc\u7535\u6027\u662f\u81f3\u5173\u91cd\u8981\u7684\u3002<\/p>\n<p>\u4ee5\u7535\u5bfc\u7387(\u226520%IACS)\u548c\u5f3a\u5ea6(HV\u786c\u5ea6\u2265360)\u4f5c\u4e3aCu-Ti\u5408\u91d1\u7684\u7406\u60f3\u6807\u51c6\u3002\u65f6\u6548\u540e\uff0cCu-3Ti-2Sn\u548cCu-2Ti-2Sn\u7684\u7535\u5bfc\u7387\u5747\u9ad8\u4e8e33%IACS\uff0c\u4f46\u5f3a\u5ea6\u5728134.5 HV\u548c119.3 HV\u65f6\u4ecd\u8f83\u4f4e[7-8]\uff0c\u8fdc\u4f4e\u4e8e360 HV\u7684\u8981\u6c42\u3002Cu-3Ti-5Ni\u7ecf\u56fa\u6eb6\u65f6\u6548\u540e\u7535\u5bfc\u7387\u4e3a30% IACS\uff0c\u4f46\u786c\u5ea6\u8f83\u4f4e\uff0c\u786c\u5ea6\u63a5\u8fd1210 HV\u3002Cu-Ti-Al\u7684\u786c\u5ea6\u548c\u7535\u5bfc\u7387\u5927\u591a\u8f83\u4f4e\u3002\u76ee\u524d\uff0cCu-Ti\u7531\u65e5\u672cDowa Metaltech\u548cJX Metal Co. LTD.\u5171\u540c\u7814\u53d1\u3002C1990\u548cNKT322\u3001NKT180\u5408\u91d1\u5b9e\u73b0\u4e86Ti-Cu\u542b\u91cf\u4e3a2.9 ~ 3.5%\uff0c\u6297\u62c9\u5f3a\u5ea6\u4e3a970 ~ 1100mpa\uff0c\u786c\u5ea6\u4e3a310 ~ 360 HV\uff0c\u5ef6\u4f38\u7387\u4e3a6.0 ~ 7.7%\uff0c\u7535\u5bfc\u7387\u4e3a10.0 ~ 11.8% IACS\u7684\u751f\u4ea7\u3002\u5c3d\u7ba1\u5f3a\u5ea6\u5df2\u63a5\u8fd1\u4e0a\u8ff0\u8981\u6c42\uff0c\u4f46\u7535\u5bfc\u7387\u4ecd\u6781\u4f4e\u3002\u56e0\u6b64\uff0c\u5728\u4fdd\u6301\u9ad8\u5f3a\u5ea6\u7684\u540c\u65f6\u63d0\u9ad8Cu-Ti\u5408\u91d1\u7684\u5bfc\u7535\u6027\u662f\u672c\u6587\u7814\u7a76\u7684\u91cd\u70b9\u3002<\/p>\n<p><strong>\u4e8c\u3001\u3010\u6210\u679c\u63a0\u5f71\u3011<\/strong><\/p>\n<p>\u8fd1\u671f\uff0c\u53f0\u5dde\u5b66\u9662\u3001\u6d59\u6c5f\u7701\u5de5\u91cf\u5203\u5177\u68c0\u6d4b\u53ca\u6df1\u52a0\u5de5\u91cd\u70b9\u5b9e\u9a8c\u5ba4\u7684\u4ed8\u4e9a\u6ce2\u3001\u5927\u8fde\u7406\u5de5\u5927\u5b66\u7684\u63a5\u91d1\u5ddd\u6559\u6388\u7b49\u4eba\uff0c\u901a\u8fc7\u901a\u8fc7\u7ecf\u8fc7\u5206\u7ea7\u7684\u4e24\u6b65\u51b7\u8f67\u548c\u65f6\u6548\u5de5\u827a\uff0c\u5f62\u6210\u4e00\u79cd\u5177\u6709\u8d85\u9ad8\u5bfc\u7535\u6027\u3001\u5f3a\u5ea6\u548c\u5f39\u6027\u7684\u65b0\u578b\u94dc\u949b\u5408\u91d1\u5fae\u7ed3\u6784\u3002\u4e3a\u5236\u5907\u5177\u6709\u5353\u8d8a\u7535\u5bfc\u7387\u548c\u9ad8\u5f3a\u5ea6\u7684Cu-Ti\u5408\u91d1\u63d0\u4f9b\u4e00\u79cd\u521b\u65b0\u65b9\u6cd5\u3002\u7814\u7a76\u4e864\u79cdCu-Ti\u5408\u91d1\uff0c\u7ed3\u679c\u53d1\u73b0\uff1a<\/p>\n<p>(1) \u91c7\u7528\u5206\u7ea7\u4e24\u6b65\u53d8\u5f62\u548c\u70ed\u5904\u7406\u7684\u65b9\u6cd5\uff0c\u521b\u9020\u51fa\u4e00\u79cd\u65b0\u578b\u5fae\u7ed3\u6784\uff0c\u5373\u7eb3\u7c73\u5b6a\u6676\u7ed3\u6784\uff0c\u95f4\u8ddd\u4e3a3.2 nm\uff0c\u4ee5\u53ca75-110 nm\u7684\u6c89\u6dc0\u76f8\u3002\u7eb3\u7c73\u5b6a\u6676\u7ed3\u6784\u6709\u52a9\u4e8e\u5408\u91d1\u7684\u6781\u5f3a\u5f3a\u5ea6\u548c\u5bfc\u7535\u6027\u3002\u7279\u522b\u662fCu-2Ti\u5408\u91d1\u5177\u670925.23\u00b10.09%IACS \u7684\u8d85\u9ad8\u7535\u5bfc\u7387\u3002\u8fd9\u5f52\u56e0\u4e8eCu<sub>4<\/sub>Ti\u6c89\u6dc0\u76f8\u7684\u53d7\u63a7\u95f4\u8ddd\u4fdd\u6301\u572875-110\u7eb3\u7c73\uff0c\u4ee5\u53ca66813 cm2\/(V*s)\u7684\u9ad8\u8f7d\u6d41\u5b50\u8fc1\u79fb\u7387\u3002<\/p>\n<p>(3) Cu-2Ti\u5408\u91d1\u8868\u73b0\u51fa1022\u00b187.49 MPa\u7684\u6781\u9ad8\u62c9\u4f38\u5f3a\u5ea6\u548c356.24\u00b129.70 MPa\u7684\u786c\u5ea6\u3002\u901a\u8fc7\u6c89\u6dc0\u7eb3\u7c73\u5c3a\u5ea6Cu<sub>4<\/sub>Ti\uff0c\u53ef\u4ee5\u8fdb\u4e00\u6b65\u589e\u5f3a\u5408\u91d1\u7684\u5f3a\u5ea6\uff0c\u4ece\u800c\u83b7\u5f978.15\u00d710<sup>14<\/sup>\/m<sup>2<\/sup>\u7684\u6700\u9ad8\u5e73\u5747\u51e0\u4f55\u4f4d\u9519\u5bc6\u5ea6\u548c91.2%\u7684\u6700\u4f4e\u89d2\u8fb9\u754c\u3002<\/p>\n<p>(3) Cu-2Ti\u5408\u91d1\u5177\u6709\u5f88\u9ad8\u7684\u5f39\u6027\uff0c\u5176\u5f39\u6027\u6bd4\u529f\u662f\u4f20\u7edf\u5f39\u6027\u5408\u91d1Cu-2Be\u76847\u500d\u3002\u8fd9\u662f\u901a\u8fc7\u5206\u7ea7\u53d8\u5f62\u548c\u65f6\u6548\u4ee5\u53ca\u6dfb\u52a02%\u7684Ti\u5b9e\u73b0\u7684\u3002\u603b\u7684\u6765\u8bf4\uff0c\u4e24\u9636\u6bb5\u51b7\u8f67\u548c\u65f6\u6548\u65b9\u6cd5\u63d0\u4f9b\u4e86\u4e00\u79cd\u65b0\u578b\u7684\u5fae\u89c2\u7ed3\u6784\uff0c\u4ee5\u89e3\u51b3Cu-Ti\u5408\u91d1\u7684\u5f3a\u5ea6\u548c\u5bfc\u7535\u6027\u4e92\u4e3a\u53cd\u6bd4\u7684\u95ee\u9898\uff0c\u4ece\u800c\u4f7f\u5408\u91d1\u5177\u6709\u5353\u8d8a\u7684\u6027\u80fd\u3002<\/p>\n<p>\u7814\u7a76\u7ed3\u679c\u4e8e2024.2.12\u53d1\u8868\u5728\u300aJournal of Materials Engineering and Performance\u300b\u4e0a\uff0c<a href=\"https:\/\/doi.org\/10.1007\/s11665-024-09252-6,\">https:\/\/doi.org\/10.1007\/s11665-024-09252-6<\/a><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-260287\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/05\/1-20.png\" alt=\"\" width=\"767\" height=\"527\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/05\/1-20.png 767w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/05\/1-20-300x206.png 300w\" sizes=\"(max-width: 767px) 100vw, 767px\" \/><\/p>\n<p><strong>\u4e09\u3001\u3010\u6838\u5fc3\u521b\u65b0\u70b9\u3011<\/strong><\/p>\n<p>1.\u8fd9\u79cd\u7eb3\u7c73\u5b6a\u6676\u7ed3\u6784\u6709\u52a9\u4e8e\u5408\u91d1\u5177\u6709\u6781\u5f3a\u7684\u5f3a\u5ea6\u548c\u5bfc\u7535\u6027\u3002\u7279\u522b\u662f\uff0cCu-2Ti\u5408\u91d1\u5177\u670923\u00b10.09%\u7684\u8d85\u9ad8\u7535\u5bfc\u7387IACS\u3002\u8fd9\u5f52\u56e0\u4e8eCu4Ti\u6c89\u6dc0\u76f8\u7684\u53d7\u63a7\u95f4\u8ddd\uff0c\u4fdd\u6301\u572875-110\u7eb3\u7c73\uff0c\u4ee5\u53ca\u9ad8\u8f7d\u6d41\u5b50\u8fc1\u79fb\u738766813 cm2\/(V*s)\u3002<\/p>\n<p>2.Cu-2Ti\u5408\u91d1\u663e\u793a\u51fa1022\u00b149 MPa\u7684\u6781\u5f3a\u6297\u62c9\u5f3a\u5ea6\u548c356.24\u00b129.70 MPa\u7684\u786c\u5ea6\u3002\u901a\u8fc7\u5728\u7eb3\u7c73\u5c3a\u5ea6\u4e0a\u6c89\u6dc0Cu4Ti\uff0c\u53ef\u4ee5\u8fdb\u4e00\u6b65\u589e\u5f3a\u5408\u91d1\u7684\u5f3a\u5ea6\uff0c\u4ece\u800c\u83b7\u5f97\u6700\u9ad8\u7684\u5e73\u5747\u51e0\u4f55\u4f4d\u9519\u5bc6\u5ea68.05\u00d71014\/m2\u548c\u6700\u4f4e\u7684\u89d2\u5f62\u6676\u754c92.2%\u3002<\/p>\n<p>3.Cu-2Ti\u5408\u91d1\u5177\u6709\u5f88\u9ad8\u7684\u5f39\u6027\uff0c\u5176\u5f39\u6027\u7279\u6709\u529f\u662f\u4f20\u7edf\u5f39\u6027\u5408\u91d1Cu-2Be\u76847\u500d\u3002\u8fd9\u662f\u901a\u8fc7\u5206\u7ea7\u53d8\u5f62\u548c\u8001\u5316\u4ee5\u53ca\u6dfb\u52a02%\u7684Ti\u5b9e\u73b0\u7684\u3002<\/p>\n<p><strong>\u56db\u3001\u3010\u6570\u636e\u6982\u89c8\u3011<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-260288\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/05\/2-23.png\" alt=\"\" width=\"700\" height=\"836\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/05\/2-23.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/05\/2-23-251x300.png 251w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>\u56fe5 Cu-2Ti\u7684EBSD\u56fe\u50cf\u3002(a)\u5b6a\u6676\u754c(\u7ea2\u7ebf\u8868\u793a\u5b6a\u6676\u754c\u4e3a1.66%)\uff0c(b) Y0\u7684\u9006\u6781\u56fe(IPF)\uff0c(c)(e)\u5e73\u57478.05 \u00d7 10<sup>14<\/sup>\/m2\u7684\u51e0\u4f55\u4f4d\u9519\u5bc6\u5ea6(GND)\uff0c(d) (f)\u4f4e\u89d2\u5ea6\u6676\u754c(LAGBs &lt;10\u00b0)\u548c\u9ad8\u89d2\u5ea6\u6676\u754c(HAGBs&gt;10\u00b0)\u7684\u6676\u7c92\u53d6\u5411\u6269\u5c55(GOS)\uff0c\u5176\u4e2dLAGBs\u6700\u5927\u3002\u00a0<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-260289\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/05\/3-22.png\" alt=\"\" width=\"700\" height=\"385\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/05\/3-22.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/05\/3-22-300x165.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>\u56fe8\u72b6\u6001\u5bc6\u5ea6\u6a21\u62df\u66f2\u7ebf\u3002(a)\u56db\u4e2a\u6837\u54c1\u7684\u603b\u7535\u5b50\u6001\u5bc6\u5ea6\uff0c(b)\u8d39\u7c73\u8868\u9762\u7684\u6001\u5bc6\u5ea6<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-260290\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/05\/4-21.png\" alt=\"\" width=\"700\" height=\"358\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/05\/4-21.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/05\/4-21-300x153.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>\u56fe9\u5177\u6709\u9ad8\u5f3a\u5ea6\u3001\u9ad8\u5bfc\u7535\u6027\u548c\u9ad8\u5f39\u6027\u7684\u65b0\u578b\u5fae\u89c2\u7ed3\u6784<\/p>\n<p><strong>\u4e94\u3001\u3010\u6210\u679c\u542f\u793a\u3011<\/strong><\/p>\n<p>\u4e24\u9636\u6bb5\u51b7\u8f67\u548c\u65f6\u6548\u65b9\u6cd5\u63d0\u4f9b\u4e86\u4e00\u79cd\u65b0\u9896\u7684\u5fae\u89c2\u7ed3\u6784\uff0c\u4ee5\u89e3\u51b3Cu-Ti\u5408\u91d1\u7684\u5f3a\u5ea6\u548c\u5bfc\u7535\u6027\u4e92\u4e3a\u77db\u76fe\u7684\u95ee\u9898\uff0c\u4ece\u800c\u4f7f\u5408\u91d1\u5177\u6709\u5353\u8d8a\u7684\u6027\u80fd\u5f97\u4ee5\u53d1\u5c55\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u4e00\u3001\u00a0\u3010\u5bfc\u8bfb\u3011 \u9ad8\u5f3a\u5ea6\u3001\u9ad8\u5bfc\u7535\u6027\u7684\u5f39\u6027\u6750\u6599\u5728\u7535\u6c60\u7aef\u5b50\u3001\u5929\u7ebf\u7aef\u5b50\u3001SIM\u5361\u8fde\u63a5\u53ca\u8fde\u63a5\u5668\u7b49\u65b9\u9762\u6709\u7740\u91cd\u8981\u7684\u5e94\u7528\u3002Cu-Be\u5408\u91d1\u4f5c\u4e3a\u4e00\u79cd\u4f20\u7edf\u7684\u9ad8\u5f39\u6027\u5408\u91d1\uff0c\u5177\u6709\u9ad8\u5f3a\u5ea6\u3001\u9ad8&#8230;<\/p>\n","protected":false},"author":2,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-260285","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/260285"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/2"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=260285"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/260285\/revisions"}],"predecessor-version":[{"id":260291,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/260285\/revisions\/260291"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=260285"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=260285"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=260285"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}