{"id":262240,"date":"2024-08-27T09:26:52","date_gmt":"2024-08-27T01:26:52","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=262240"},"modified":"2024-08-27T09:26:52","modified_gmt":"2024-08-27T01:26:52","slug":"%e6%b8%85%e5%8d%8e%e5%a4%a7%e5%ad%a6-%e9%84%82%e5%b0%94%e5%a4%9a%e6%96%af%e5%ae%9e%e9%aa%8c%e5%ae%a4%e9%ad%8f%e9%a3%9e-%e5%bc%a0%e6%99%a8%e6%9b%a6%e5%9b%a2%e9%98%9fafm%e9%94%82%e7%a3%b7%e6%b0%a7","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=262240","title":{"rendered":"\u6e05\u534e\u5927\u5b66-\u9102\u5c14\u591a\u65af\u5b9e\u9a8c\u5ba4\u9b4f\u98de-\u5f20\u6668\u66e6\u56e2\u961fAFM:\u9502\u78f7\u6c27\u6c2e\u56fa\u6001\u7535\u89e3\u8d28\u5728\u9ad8\u80fd\u9502\u91d1\u5c5e\u7535\u6c60\u4e2d\u7684\u5e94\u7528\u8fdb\u5c55"},"content":{"rendered":"<p><strong>\u4e00\u3001<\/strong> <strong>\u3010\u5bfc\u8bfb\u3011<\/strong><strong>\u00a0<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-262242\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72471-19.png\" alt=\"\" width=\"865\" height=\"314\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72471-19.png 865w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72471-19-300x109.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72471-19-768x279.png 768w\" sizes=\"(max-width: 865px) 100vw, 865px\" \/><\/p>\n<p>\u7814\u7a76\u666e\u904d\u8ba4\u4e3a\u4ee5LLZO\u4e3a\u4ee3\u8868\u7684\u4f20\u7edf\u65e0\u673a\u6c27\u5316\u7269\u56fa\u6001\u7535\u89e3\u8d28\u5728\u56fa\u6001\u7535\u6c60\u4e2d\u7684\u5b58\u5728\u663e\u8457\u7684\u754c\u9762\u95ee\u9898\uff0c\u5305\u62ec\u754c\u9762\u63a5\u89e6\u5dee\uff0c\u754c\u9762\u7535\u963b\u9ad8\uff0c\u5bb9\u6613\u4ea7\u751f\u9502\u679d\u6676\u7b49\u7f3a\u70b9\u3002LiPON\u4f5c\u4e3a\u4e00\u79cd\u4f18\u5f02\u7684\u77f3\u69b4\u77f3\u578b\u7535\u89e3\u8d28\u66ff\u4ee3\u54c1\uff0c\u7531\u4e8e\u5176\u5353\u8d8a\u7684\u754c\u9762\u76f8\u5bb9\u6027\u3001\u5bbd\u5e7f\u7684\u7535\u5316\u5b66\u7a33\u5b9a\u7a97\u53e3\u548c\u4f18\u5f02\u7684\u70ed\u7a33\u5b9a\u6027\uff0c\u5728\u5b66\u672f\u754c\u548c\u5de5\u4e1a\u754c\u5f15\u8d77\u4e86\u6781\u5927\u7684\u5174\u8da3\uff0c\u8fd9\u4f7f\u5f97\u5728\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u56fa\u6001\u9502\u91d1\u5c5e\u7535\u6c60\uff08SSLMBs\uff09\u4e2d\u6784\u7b51\u6781\u5176\u7a33\u5b9a\u7684\u7535\u89e3\u8d28\/\u7535\u6781\u754c\u9762\u6210\u4e3a\u53ef\u80fd\u3002\u7136\u800c\uff0c\u79bb\u5b50\u6269\u6563\u6027\u4e0d\u8db3\u3001\u5236\u5907\u56f0\u96be\u7b49\u95ee\u9898\u963b\u788d\u4e86\u5176\u5546\u4e1a\u5316\u8fdb\u7a0b\u3002<\/p>\n<p><strong>\u4e8c\u3001\u3010\u6210\u679c\u63a0\u5f71\u3011<\/strong><\/p>\n<p>\u672c\u6587\u7cfb\u7edf\u5730\u8ba8\u8bba\u4e86\u65e0\u5b9a\u5f62\u7ed3\u6784LiPON\u7684\u7279\u6027\u3001\u4f53\u76f8\u79bb\u5b50\u6269\u6563\u548c\u7535\u6781\/\u7535\u89e3\u8d28\u754c\u9762\u7684\u57fa\u7840\u7406\u89e3\uff0c\u5e76\u91cd\u70b9\u4ecb\u7ecd\u4e86\u63d0\u5347\u7535\u5316\u5b66\u6027\u80fd\u7684\u6539\u8fdb\u7b56\u7565\u3002\u968f\u540e\uff0c\u603b\u7ed3\u4e86\u521b\u65b0\u7684\u8868\u5f81\u548c\u8ba1\u7b97\u65b9\u6cd5\u7528\u4e8e\u63ed\u793aLiPON\u7684\u8bbe\u8ba1\u539f\u5219\u3002\u6b64\u5916\uff0c\u5206\u6790\u4e86\u5b9e\u73b0LiPON\u9ad8\u6548\u5236\u5907\u7684\u65b9\u6cd5\uff0c\u5e76\u63a2\u8ba8\u4e86LiPON\u5728\u5f53\u524d\u7535\u6c60\u4f53\u7cfb\u4e2d\u7684\u5e94\u7528\u73b0\u72b6\u3002\u6700\u540e\uff0c\u5bf9\u4e0eLiPON\u76f8\u5173\u7684\u57fa\u7840\u7406\u89e3\u3001\u7ed3\u6784\u548c\u754c\u9762\u8bbe\u8ba1\u7684\u5408\u7406\u9884\u6d4b\u3001\u9ad8\u6548\u5236\u5907\u7684\u5269\u4f59\u6311\u6218\u4ee5\u53ca\u5bf9\u4e8e\u672a\u6765\u5e94\u7528\u7684\u6f5c\u5728\u673a\u4f1a\u8fdb\u884c\u4e86\u9002\u5f53\u7684\u5c55\u671b\u3002\u76f8\u5173\u7814\u7a76\u4ee5\u9898\u76ee\u4e3a\u201cLithium Phosphorous Oxynitride as an advanced solid-state electrolyte to boost highenergy lithium metal battery\u201d\u53d1\u8868\u5728\u300aAdvanced Functional Materials\u300b\u3002\u901a\u8baf\u4f5c\u8005\u4e3a\u9102\u5c14\u591a\u65af\u5b9e\u9a8c\u5ba4\u4e3b\u4efb\u9b4f\u98de\u6559\u6388\uff0c\u5e38\u52a1\u526f\u4e3b\u4efb\u5f20\u6668\u66e6\u526f\u7814\u7a76\u5458\u548c\u8096\u54f2\u7199\u535a\u58eb\u3002\u8bba\u6587\u7b2c\u4e00\u4f5c\u8005\u4e3a\u6e05\u534e\u5927\u5b66\u535a\u58eb\u751f\u90b9\u6cfd\u709c\u3002\u672c\u7814\u7a76\u4e0d\u4ec5\u603b\u7ed3\u4e86LiPON\u5728\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u7535\u6c60\u4e2d\u7684\u6700\u65b0\u8fdb\u5c55\uff0c\u5e76\u5bf9\u4e8e\u8be5\u7c7b\u56fa\u6001\u7535\u89e3\u8d28\u5728\u5176\u4ed6\u7535\u5b50\u8bbe\u5907\u4e2d\u7684\u6f5c\u5728\u5e94\u7528\u53ef\u80fd\u505a\u51fa\u4e86\u5408\u7406\u5c55\u671b\u3002\u9102\u5c14\u591a\u65af\u5b9e\u9a8c\u5ba4\u5c06\u7ee7\u7eed\u81f4\u529b\u4e8e\u7a81\u7834\u56fa\u6001\u7535\u89e3\u8d28\u6280\u672f\u74f6\u9888\uff0c\u4e3a\u4e0b\u4e00\u4ee3\u9ad8\u5b89\u5168\u3001\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u7535\u6c60\u4f53\u7cfb\u7814\u53d1\u63d0\u4f9b\u91cd\u8981\u652f\u6301\u3002<\/p>\n<p><strong>\u4e09\u3001\u3010\u4e3b\u8981\u5185\u5bb9\u3011<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-262243\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72472-20.png\" alt=\"\" width=\"756\" height=\"295\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72472-20.png 756w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72472-20-300x117.png 300w\" sizes=\"(max-width: 756px) 100vw, 756px\" \/><\/p>\n<p>\u56fe1 LiPON\u56fa\u6001\u7535\u89e3\u8d28\u7684\u7ed3\u6784\u7279\u5f81<\/p>\n<p>LiPON\uff08Li<sub>x<\/sub>PO<sub>y<\/sub>N<sub>z<\/sub>\uff09\u4f5c\u4e3a\u4e00\u7c7b\u5178\u578b\u7684\u975e\u6676\u6001\u5316\u5408\u7269\uff0c\u5316\u5b66\u8ba1\u91cf\u7cfb\u6570\u4e3ax\u22483,z &lt; 0.5, 3 &lt; (y + z) &lt; 4\u3002\u975e\u6676\u7ed3\u6784\u5bf9\u4e8e\u7406\u89e3\u7ed3\u6784-\u6027\u80fd\u5173\u7cfb\u548c\u5236\u5b9a\u5408\u7406\u8bbe\u8ba1\u9ad8\u6027\u80fd\u6750\u6599\u7684\u6807\u51c6\u589e\u52a0\u4e86\u96be\u5ea6\u3002\u867d\u7136\u63ed\u793aLiPON\u7684\u7cbe\u786e\u7ed3\u6784\u8fd8\u6709\u5f88\u957f\u7684\u8def\u8981\u8d70\uff0c\u4f46\u666e\u904d\u8ba4\u4e3a\u6c2e\u78f7\u952e\u7684\u5b58\u5728\u4f1a\u663e\u8457\u5f71\u54cdLiPON\u7684\u6574\u4f53\u6027\u80fd\u3002\u968f\u7740\u65b0\u578b\u8868\u5f81\u6280\u672f\u7684\u53d1\u5c55\uff0cLiPON\u7684\u7ed3\u6784\u9010\u6b65\u88ab\u5168\u9762\u89e3\u6790\uff0c\u6c2e\u5728\u5206\u79bb\u7684P(O,N)<sub>4<\/sub>\u56db\u9762\u4f53\u4e2d\u6709\u4e24\u79cd\u5f62\u5f0f\uff0c\u4e00\u79cd\u662f\u9876\u7aef\u6c2e(N<sub>a<\/sub>)\uff0c\u53e6\u4e00\u79cd\u662f\u4e24\u4e2a\u78f7\u9178\u57fa\u56e2\u4e4b\u95f4\u7684\u6865(N<sub>b<\/sub>)\u3002\u8fdb\u4e00\u6b65\u7814\u7a76\u8868\u660e\uff0c\u9502\u79bb\u5b50\u4e0e\u9634\u79bb\u5b50\u7684\u76f8\u4e92\u4f5c\u7528\u5bf9\u79bb\u5b50\u7535\u5bfc\u7387\u6709\u663e\u8457\u5f71\u54cd\u3002\u5728\u9676\u74f7\u7535\u89e3\u8d28\u4e2d\u5f15\u5165\u6c2e\u57fa\u56e2\u53ef\u4ee5\u964d\u4f4e\u6269\u6563\u5c4f\u969c\uff0c\u800c\u5728\u57fa\u4f53\u4e2d\u5b58\u5728\u6c27\u53ef\u4ee5\u589e\u52a0\u4e0eLi<sup>+<\/sup>\u7684\u76f8\u4e92\u4f5c\u7528\u3002\u6b64\u5916\uff0cN\/P\u3001Li\/P\u6bd4\u503c\u5bf9\u7535\u89e3\u8d28\u7684\u6027\u80fd\u4e5f\u8d77\u7740\u91cd\u8981\u7684\u4f5c\u7528\u3002\u4e0a\u8ff0\u7814\u7a76\u8868\u660e\uff0c\u8c03\u6574\u5316\u5b66\u8ba1\u91cf\u53ef\u80fd\u662f\u6539\u53d8LiPON\u6027\u8d28\u7684\u6709\u6548\u65b9\u6cd5\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-262244\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72473-19.png\" alt=\"\" width=\"472\" height=\"627\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72473-19.png 472w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72473-19-226x300.png 226w\" sizes=\"(max-width: 472px) 100vw, 472px\" \/><\/p>\n<p>\u56fe2 LiPON\u56fa\u6001\u7535\u89e3\u8d28\u7684\u79bb\u5b50\u6269\u6563<\/p>\n<p>\u56fa\u6001\u7535\u89e3\u8d28\u4e2d\u79bb\u5b50\u8f93\u8fd0\u6027\u8d28\u4e0e\u7535\u89e3\u8d28\u7c7b\u578b\u606f\u606f\u76f8\u5173\u3002\u5b9e\u9a8c\u7ed3\u679c\u8868\u660e\uff0cLiPON\u4e2d\u7684\u79bb\u5b50\u8f93\u8fd0\u673a\u5236\u4e3b\u8981\u662f\u5728\u56fa\u5b9a\u6d53\u5ea6\u7684\u4e00\u79cd\u8f7d\u6d41\u5b50\u4e2d\u8fdb\u884c\u3002\u6b64\u5916\uff0c\u53ea\u6709\u90e8\u5206\u9502\u79bb\u5b50\u53c2\u4e0e\u4e86\u4f20\u5bfc\u8fc7\u7a0b\u3002\u79bb\u5b50\u7535\u5bfc\u7387\u5bf9\u5316\u5b66\u6210\u5206\u7684\u4f9d\u8d56\u6027\u8f83\u5f3a\uff0c\u5728\u4e0d\u540c\u7684Li\u542b\u91cf\u533a\u57df\uff0cLi\/P\u6bd4\u503c\u663e\u8457\u5f71\u54cd\u79bb\u5b50\u7535\u5bfc\u7387\uff0c\u4e14\u5728\u9876\u7aef\u6c2e\u3001\u4e8c\u6865\u6c2e\u548c\u4e09\u6865\u6c2e\u4e2d\u8868\u73b0\u51fa\u8f83\u5927\u5dee\u5f02\u3002\u78f7\u9178\u57fa\u6392\u5217\u4e0e\u79bb\u5b50\u7535\u5bfc\u7387\u5173\u7cfb\u7684\u76f8\u56fe\u8fdb\u4e00\u6b65\u8868\u660e\uff0c\u4e09\u914d\u4f4d\u6c2e\u7684\u5b58\u5728\u4e3b\u8981\u8868\u73b0\u5728\u504f\u78f7\u9178\u76d0\u548c\u7126\u78f7\u9178\u76d0\u6392\u5217\u4e2d\u3002\u540c\u65f6\uff0c\u7f3a\u9677\u5b58\u5728\u4e0e\u7ed3\u6676\u5316\u7a0b\u5ea6\u4e5f\u5bf9\u79bb\u5b50\u4f20\u8f93\u4ea7\u751f\u91cd\u8981\u5f71\u54cd\u3002\u867d\u7136\u5728\u63a2\u7d22LiPON\u4e2d\u7684\u79bb\u5b50\u8f93\u8fd0\uff0c\u7279\u522b\u662f\u5316\u5b66\u6210\u5206\u7684\u5f71\u54cd\u65b9\u9762\u5df2\u7ecf\u53d6\u5f97\u4e86\u7a81\u7834\uff0c\u4f46\u4ece\u5b9e\u9a8c\u548c\u8ba1\u7b97\u6280\u672f\u7684\u7ed3\u5408\u4e2d\u83b7\u5f97\u66f4\u76f4\u89c2\u7684\u7406\u89e3\uff0c\u4ecd\u7136\u9700\u8981\u5f00\u53d1\u66f4\u5148\u8fdb\u7684\u8868\u5f81\u548c\u5206\u6790\u65b9\u6cd5\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-262245\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72474-17.png\" alt=\"\" width=\"591\" height=\"539\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72474-17.png 591w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72474-17-300x274.png 300w\" sizes=\"(max-width: 591px) 100vw, 591px\" \/><\/p>\n<p>\u56fe3\u79bb\u5b50\u6269\u6563\u589e\u5f3a\u7b56\u7565<\/p>\n<p>\u5ba4\u6e29\u4e0b\u8fc7\u4f4e\u7684\u79bb\u5b50\u7535\u5bfc\u7387 (~10<sup>-6<\/sup> S cm<sup>-1<\/sup>)\u6781\u5927\u5730\u963b\u788d\u4e86LiPON\u5728\u56fa\u6001\u9502\u91d1\u5c5e\u7535\u6c60\u4e2d\u7684\u5e94\u7528\u3002\u63ba\u6742\u548c\u53d6\u4ee3\u88ab\u8ba4\u4e3a\u662f\u589e\u5f3a\u7535\u89e3\u8d28\u7535\u5bfc\u7387\u7684\u6709\u6548\u7b56\u7565\u3002\u589e\u52a0\u5176\u7ed3\u6784\u5185\u7684\u6c2e\u542b\u91cf\u4e4b\u5916\uff0c\u591a\u79cd\u91d1\u5c5e\u5143\u7d20\u5982\u9541\u3001\u9517\u3001\u94c1\u3001\u9530\u7b49\uff0c\u975e\u91d1\u5c5e\u5143\u7d20\u5982\u78b3\u3001\u787c\u3001\u7845\u7b49\u5747\u5bf9\u4e8e\u79bb\u5b50\u7535\u5bfc\u7387\u6709\u4e00\u5b9a\u63d0\u5347\u3002\u6b64\u5916\uff0c\u5176\u4ed6\u9633\u79bb\u5b50\u5982\u94a8\u3001\u94dd\u3001\u949b\u4e5f\u663e\u793a\u51fa\u589e\u52a0\u79bb\u5b50\u7535\u5bfc\u7387\u7684\u5de8\u5927\u6f5c\u529b\u3002\u5bf9\u6df7\u5408\u79bb\u5b50\u63ba\u6742\u7684\u589e\u5f3a\u673a\u7406\u4e5f\u6b63\u5728\u88ab\u6df1\u5165\u7814\u7a76\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-262246\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72475-16.png\" alt=\"\" width=\"591\" height=\"650\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72475-16.png 591w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72475-16-273x300.png 273w\" sizes=\"(max-width: 591px) 100vw, 591px\" \/><\/p>\n<p>\u56fe4 LiPON\/Li\u754c\u9762\u7279\u6027<\/p>\n<p>\u901a\u8fc7X\u5c04\u7ebf\u5149\u7535\u5b50\u80fd\u8c31\u8c31(XPS)\u548c\u4f4e\u6e29\u900f\u5c04\u7535\u955c(Cryo-TEM)\u5bf9\u4e8eLiPON\/Li\u754c\u9762\u8fdb\u884c\u4e86\u5b9e\u9a8c\u89c2\u5bdf\uff0c\u8fd8\u539f\u7535\u4f4d\u4e3a0.69 V\uff0c\u6700\u7ec8\u5206\u89e3\u4ea7\u7269\u4e3b\u8981\u4e3aLi<sub>3<\/sub>N\u3001Li<sub>2<\/sub>O\u548cLi<sub>3<\/sub>P\u3002\u5f62\u6210\u7684SEI\u4e3a\u591a\u5c42\u9576\u5d4c\u7ed3\u6784\uff0c\u5206\u89e3\u540e\u7684Li<sub>3<\/sub>N\u3001Li<sub>2<\/sub>O\u3001Li<sub>3<\/sub>PO<sub>4<\/sub>\u7b49\u7ec4\u5206\u7ed3\u6676\u5d4c\u5165\u65e0\u5b9a\u5f62\u57fa\u4f53\u4e2d\uff0c\u4e0d\u542b\u4efb\u4f55\u6709\u673a\u542b\u9502\u7269\u8d28\u6216LiF\uff0c\u4e0e\u4f20\u7edf\u6db2\u6001\u7535\u89e3\u8d28\u5f62\u6210\u7684\u7ed3\u6784\u660e\u663e\u4e0d\u540c\u3002SEI\u7684\u5f62\u6210\u51cf\u5c11\u4e86\u65bd\u52a0\u5728SSE\u4e0a\u7684\u9ad8\u5316\u5b66\u52bf\uff0c\u8fd9\u662fLiPON\u4e0eLi\u91d1\u5c5e\u9633\u6781\u826f\u597d\u76f8\u5bb9\u6027\u7684\u539f\u56e0\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-262247\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72476-8.png\" alt=\"\" width=\"591\" height=\"305\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72476-8.png 591w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72476-8-300x155.png 300w\" sizes=\"(max-width: 591px) 100vw, 591px\" \/><\/p>\n<p>\u56fe5 LiPON\u7528\u4e8e\u6539\u5584\u56fa\u6001\u7535\u6c60\u754c\u9762\u76f8\u5bb9\u6027<\/p>\n<p>\u7531\u4e8eLiPON\u4e0eLi\u8d1f\u6781\u7684\u826f\u597d\u7684\u754c\u9762\u76f8\u5bb9\u6027\uff0c\u8fd1\u5e74\u6765\u88ab\u5e94\u7528\u4e8e\u5176\u4ed6\u56fa\u6001\u7535\u89e3\u8d28\u4f53\u7cfb\u4e2d\u6784\u5efa\u66f4\u4f18\u5316\u7684\u56fa\u6001\u7535\u89e3\u8d28\/Li\u754c\u9762\u3002LiPON\u4f5c\u4e3a\u529f\u80fd\u4e2d\u95f4\u5c42\u6784\u7b51\u7684\u590d\u5408\u56fa\u6001\u7535\u89e3\u8d28\u5177\u6709\u8f83\u9ad8\u7684\u79bb\u5b50\u7535\u5bfc\u7387\uff0c\u4fc3\u8fdb\u4e86\u9502\u79bb\u5b50\u5728\u754c\u9762\u5904\u7684\u8fc1\u79fb\uff0c\u5e76\u4e14\u5176\u7535\u5b50\u7edd\u7f18\u6027\u80fd\u4e5f\u6709\u52a9\u4e8e\u6291\u5236\u9502\u679d\u6676\u751f\u957f\u3002\u826f\u597d\u7684\u67d4\u97e7\u6027\u6709\u52a9\u4e8e\u6539\u5584\u56fa\u6001\u7535\u89e3\u8d28\u4e0eLi\u91d1\u5c5e\u4e4b\u95f4\u7684\u673a\u68b0\u63a5\u89e6\u3002\u636e\u6b64\uff0c\u63d0\u51fa\u4e86\u7406\u60f3\u754c\u9762\u5c42\u7684\u5173\u952e\u7279\u5f81:(1)Li<sup>+<\/sup>\u901a\u91cf\u5747\u5300;(2)\u7535\u5b50\u7edd\u7f18;(3)\u5bf9\u91d1\u5c5e\u9502\u5177\u6709\u70ed\u529b\u5b66\u7a33\u5b9a\u6027;(4)\u826f\u597d\u7684\u6da6\u6e7f\u6027\uff0c\u4fdd\u8bc1\u65e0\u63a5\u89e6\u7f3a\u9677;(5)\u5177\u6709\u4e00\u5b9a\u7684\u67d4\u97e7\u6027\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-262248\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72477-4.png\" alt=\"\" width=\"591\" height=\"294\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72477-4.png 591w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72477-4-300x149.png 300w\" sizes=\"(max-width: 591px) 100vw, 591px\" \/><\/p>\n<p>\u56fe6\u754c\u9762\u529b\u5b66\u7a33\u5b9a\u6027\u5206\u6790\u4e0e\u6539\u5584<\/p>\n<p>LiPON\u867d\u7136\u5df2\u6210\u529f\u5e94\u7528\u4e8e\u9ad8\u6bd4\u80fd\u56fa\u6001\u7535\u6c60\u4e2d\uff0c\u4f46\u5176\u6709\u9650\u7684\u529b\u5b66\u6027\u8d28\u4f1a\u5bfc\u81f4\u91cd\u590d\u5faa\u73af\u8fc7\u7a0b\u4e2d\u8106\u6027\u5931\u6548\uff0c\u7279\u522b\u662f\u5728\u9ad8\u9762\u5bb9\u91cf\u6c89\u79ef\u6761\u4ef6\u4e0b\u3002\u5f15\u5165\u529b\u5b66\u589e\u5f3a\u57fa\u8d28\u9650\u5236\u5185\u90e8\u88c2\u7eb9\u6269\u5c55\u63d0\u9ad8\u6574\u4f53\u529b\u5b66\u7a33\u5b9a\u6027\u5c24\u4e3a\u5173\u952e\u3002\u7814\u7a76\u8868\u660e\uff0c\u5728Cu\/LiPON\u754c\u9762\u5904\u53d1\u751f\u7684\u9502\u6210\u6838\u4f1a\u5f15\u8d77Cu\u819c\u5c40\u90e8\u53d8\u5f62\uff0c\u5f62\u6210\u5706\u9876\u72b6\u7a81\u8d77\uff0c\u5f15\u53d1\u5c40\u90e8\u5e94\u529b\u5806\u79ef\u3002\u7531\u4e8eCu\/LiPON\u754c\u9762\u7f3a\u4e4f\u81ea\u7531\u7a7a\u95f4\uff0c\u5f62\u6210\u7684Li\u6838\u89e6\u53d1Cu\u819c\u4e0eLiPON\u5206\u79bb\uff0c\u5bfc\u81f4\u754c\u9762\u63a5\u89e6\u6076\u5316\u3002\u4e3a\u4e86\u89e3\u51b3\u9ad8\u901f\u7387\u957f\u5468\u671f\u5faa\u73af\u4e0b\u7684\u673a\u68b0\u5931\u6548\u95ee\u9898\uff0c\u4ee5LiF\u7b49\u4f5c\u4e3a\u529b\u5b66\u589e\u5f3a\u57fa\u8d28\u5f15\u5165SEI\u4e2d\uff0c\u80fd\u591f\u663e\u8457\u589e\u5f3aSEI\u65ad\u88c2\u97e7\u6027\uff0c\u63d0\u9ad8\u754c\u9762\u529b\u5b66\u7a33\u5b9a\u6027\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-262249\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72478-4.png\" alt=\"\" width=\"1217\" height=\"422\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72478-4.png 1217w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72478-4-300x104.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72478-4-768x266.png 768w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72478-4-1024x355.png 1024w\" sizes=\"(max-width: 1217px) 100vw, 1217px\" \/><\/p>\n<p>\u56fe7\u754c\u9762\u5316\u5b66\u7a33\u5b9a\u6027\u6539\u5584<\/p>\n<p>LiPON\u5728\u5b9e\u9645\u5e94\u7528\u4e2d\u53e6\u4e00\u4e2a\u5de8\u5927\u6311\u6218\u662f\u5bf9\u7a7a\u6c14\u73af\u5883\u6761\u4ef6\u4e2dH<sub>2<\/sub>O\u548cCO<sub>2<\/sub>\u7684\u9ad8\u654f\u611f\u6027\uff0c\u5bfc\u81f4\u5176\u754c\u9762\u5316\u5b66\u7a33\u5b9a\u6027\u5dee\u3002\u591a\u79cd\u529f\u80fd\u4fdd\u62a4\u5c42\u88ab\u5e94\u7528\u4e8e\u63d0\u9ad8LiPON\u754c\u9762\u5316\u5b66\u7a33\u5b9a\u6027\u3002\u867d\u7136\u5728\u6291\u5236LiPON\u7684\u5316\u5b66\u964d\u89e3\u65b9\u9762\u5df2\u7ecf\u53d6\u5f97\u4e86\u4e00\u4e9b\u8fdb\u5c55\uff0c\u4f46\u662f\u754c\u9762\u949d\u5316\u5177\u4f53\u673a\u7406\uff0c\u4ee5\u53ca\u5728LiPON\u8868\u9762\u6784\u7b51\u5b8c\u6574\u5747\u5300\u7684\u949d\u5316\u5c42\u6c89\u79ef\u4ecd\u7136\u662f\u672a\u6765\u7684\u5173\u952e\u6311\u6218\u3002\u540c\u65f6\uff0c\u53ef\u4ee5\u5c1d\u8bd5\u91c7\u7528\u6dfb\u52a0\u5242\u3001\u7ed3\u6784\u4f18\u5316\u3001\u5408\u6210\u540e\u5904\u7406\u7b49\u5e38\u7528\u7b56\u7565\u6765\u63d0\u9ad8\u754c\u9762\u5728\u73af\u5883\u4e0b\u7684\u5316\u5b66\u7a33\u5b9a\u6027\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-262250\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72479-4.png\" alt=\"\" width=\"591\" height=\"991\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72479-4.png 591w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u72479-4-179x300.png 179w\" sizes=\"(max-width: 591px) 100vw, 591px\" \/><\/p>\n<p>\u56fe8 LiPON\/\u6b63\u6781\u754c\u9762<\/p>\n<p>\u5229\u7528\u9ad8\u7535\u538b\u6b63\u6781\u6750\u6599\u53ef\u4ee5\u8fdb\u4e00\u6b65\u63d0\u9ad8\u6574\u4f53\u80fd\u91cf\u5bc6\u5ea6\uff0c\u4e86\u89e3\u5916\u52a0\u7535\u573a\u4f5c\u7528\u4e0bLiPON\/\u6b63\u6781\u754c\u9762\u6f14\u53d8\u5177\u6709\u91cd\u8981\u610f\u4e49\u3002\u7814\u7a76\u8868\u660eLiPON\u57284.3V\u4e0b\u5f00\u59cb\u5206\u89e3\uff0c\u4f34\u968f\u7740Li<sup>+<\/sup>\u7684\u91ca\u653e\uff0c\u751f\u6210Li<sub>4<\/sub>P<sub>2<\/sub>O<sub>7<\/sub>\u3001LiPO<sub>3<\/sub>\u7b49\u5bcc\u78f7\u5316\u5408\u7269\uff0c\u6700\u7ec8\u751f\u6210P<sub>4<\/sub>O<sub>10<\/sub>\u7ec4\u5206\uff0c\u540c\u65f6\u751f\u6210O<sub>2<\/sub>\u548cN<sub>2<\/sub>\u3002\u5e76\u4e14\u5176\u5206\u89e3\u4ee5\u6269\u6563\u53d7\u9650\u65b9\u5f0f\u8fdb\u884c\u3002LiPON\u4e0e\u4ee5\u9ad8\u538bLiCoO2\u3001\u5c16\u6676\u77f3\u7c7bLNMO\u3001\u4e09\u5143\u6750\u6599\u7b49\u5404\u7c7b\u9ad8\u538b\u6216\u5927\u5bb9\u91cf\u6b63\u6781\u7684\u590d\u5408\u4f7f\u7528\u4e2d\u4f53\u73b0\u51fa\u4e86\u826f\u597d\u7684\u76f8\u5bb9\u6027\uff0c\u53d6\u5f97\u4e86\u5f88\u5927\u7684\u8fdb\u5c55\uff0c\u4f46\u8fdb\u4e00\u6b65\u4e86\u89e3LiPON\/\u6b63\u6781\u754c\u9762\u7684\u6f14\u53d8\uff0c\u7279\u522b\u662f\u5728\u5faa\u73af\u8fc7\u7a0b\u4e2d\uff0c\u4ecd\u7136\u662f\u4e00\u4e2a\u975e\u5e38\u7d27\u8feb\u7684\u95ee\u9898\uff0c\u9700\u8981\u8c28\u614e\u8003\u8651\u5bf9\u754c\u9762\u6027\u80fd\u8fdb\u884c\u5408\u7406\u7684\u4fee\u6539\uff0c\u4ee5\u4f18\u5316\u754c\u9762\u6027\u80fd\uff0c\u8fdb\u4e00\u6b65\u63d0\u9ad8\u6574\u4f53\u6027\u80fd\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-262251\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u724710-4.png\" alt=\"\" width=\"866\" height=\"754\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u724710-4.png 866w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u724710-4-300x261.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u724710-4-768x669.png 768w\" sizes=\"(max-width: 866px) 100vw, 866px\" \/><\/p>\n<p>\u56fe9 \u5148\u8fdb\u8868\u5f81\u6280\u672f\u53d1\u5c55<\/p>\n<p>\u8fd1\u5e74\u6765\uff0c\u591a\u79cd\u5148\u8fdb\u539f\u4f4d\u8868\u5f81\u6280\u672f\u7ed3\u5408\u8ba1\u7b97\u6a21\u62df\u7684\u8fdb\u6b65\u6b63\u5728\u88ab\u7528\u6765\u5e2e\u52a9\u6df1\u5165\u4e86\u89e3\u56fa\u6001\u7535\u89e3\u8d28\u4f53\u76f8\u548c\u7535\u6781\/\u7535\u89e3\u8d28\u754c\u9762\u3002\u8ba1\u7b97\u6a21\u62df\u5728\u6750\u6599\u7814\u7a76\u4e2d\u540c\u6837\u8d77\u5230\u4e86\u91cd\u8981\u7684\u8865\u5145\u4f5c\u7528\uff0c\u901a\u8fc7\u63ed\u793a\u9502\u79bb\u5b50\u4e0e\u5b98\u80fd\u56e2\/\u5143\u7d20\u4e4b\u95f4\u7684\u76f8\u4e92\u4f5c\u7528\u3001\u5316\u5b66\u952e\u65ad\u88c2\u80fd\u3001\u79bb\u5b50\u4f20\u8f93\u9014\u5f84\u548c\u7535\u89e3\u8d28\/\u7535\u6781\u754c\u9762\u7684\u53cd\u5e94\u673a\u5236\uff0c\u6781\u5927\u5730\u4fc3\u8fdb\u4e86\u6027\u80fd\u9884\u6d4b\u3002\u7279\u522b\u662f\u5bc6\u5ea6\u6cdb\u51fd\u7406\u8bba\uff08DFT\uff09\u6a21\u62df\uff0c\u5728\u539f\u5b50\u5c42\u9762\u4e0a\u63d0\u4f9b\u4e86\u5bf9\u7f3a\u9677\u7279\u6027\u3001\u63ba\u6742\u5242\u6eb6\u89e3\u5ea6\u4ee5\u53ca\u9502\u63ba\u5165LiPON\u4e2d\u7684\u8be6\u7ec6\u89c1\u89e3\u3002\u540c\u65f6DFT\u6a21\u62df\u8fd8\u53ef\u4ee5\u786e\u5b9aLiPON\u7684\u7edd\u7f18\u6027\u548c\u5e26\u9699\u8d85\u8fc76 eV\uff0c\u4ee5\u53ca\u7a7a\u4f4d\u548c\u95f4\u9699\u8f85\u52a9\u7684Li\u79bb\u5b50\u7684\u8fc1\u79fb\u80fd\u3002\u8fdb\u4e00\u6b65\u7814\u7a76\u8868\u660e\uff0cDFT\u6a21\u62df\u548c\u8272\u6563\u6821\u6b63\u6280\u672f\u80fd\u591f\u6709\u6548\u63a2\u7d22LiPON\u7684\u672c\u5f81\u7f3a\u9677\u6027\u8d28\u548c\u53cd\u5e94\u80fd\u91cf\u5b66\u3002<\/p>\n<p>\u6b64\u5916\uff0c\u7406\u8bba\u7814\u7a76\u8fd8\u7528\u4e8e\u68c0\u67e5\u9634\u6781\u4e0e\u65e0\u673a\u7535\u89e3\u8d28\u4e4b\u95f4\u7684\u754c\u9762\u7279\u6027\u3002\u4f8b\u5982\uff0c\u901a\u8fc7DFT\u8ba1\u7b97LCO\/LYC\u754c\u9762\u7684\u7a33\u5b9a\u6027\uff0c\u4ee5\u53caDFT\u7535\u4f4d\u56fe\u7814\u7a76\u9634\u6781\/\u7535\u89e3\u8d28\u754c\u9762\u7684\u7535\u5316\u5b66\u884c\u4e3a\u3002\u5206\u5b50\u52a8\u529b\u5b66\uff08MD\uff09\u6a21\u62df\u5219\u7528\u4e8e\u7814\u7a76LiPON\u4e2d\u7684Li\u6269\u6563\u884c\u4e3a\u548c\u7535\u5bfc\u7387\u63a7\u5236\u56e0\u7d20\u3002\u901a\u8fc7\u8fd9\u4e9b\u6a21\u62df\uff0c\u7814\u7a76\u4eba\u5458\u80fd\u591f\u6df1\u5165\u7406\u89e3\u6750\u6599\u7684\u7ed3\u6784\u548c\u7535\u5316\u5b66\u7279\u6027\uff0c\u4ece\u800c\u63d0\u9ad8\u56fa\u6001\u7535\u6c60\u7684\u6027\u80fd\u548c\u7a33\u5b9a\u6027\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-262252\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u724711-2.png\" alt=\"\" width=\"591\" height=\"773\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u724711-2.png 591w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u724711-2-229x300.png 229w\" sizes=\"(max-width: 591px) 100vw, 591px\" \/><\/p>\n<p>\u56fe10 LiPON\u5236\u5907\u6280\u672f<\/p>\n<p>\u9ad8\u8d28\u91cfLiPON\u5236\u5907\u662f\u5b9e\u9645\u5e94\u7528\u4e2d\u7684\u53e6\u4e00\u4e2a\u5de8\u5927\u6311\u6218\u3002\u5c04\u9891\u78c1\u63a7\u6e85\u5c04\u6280\u672f\u4f5c\u4e3a\u6700\u5e7f\u6cdb\u91c7\u7528\u7684\u5236\u5907\u6280\u672f\u4e4b\u5916\uff0c\u591a\u79cd\u65b9\u6cd5\u5728\u886c\u5e95\u8868\u9762\u5f62\u6210LiPON\u5c42\uff0c\u5305\u62ecALD\u3001\u5316\u5b66\u6c14\u76f8\u6c89\u79ef(CVD)\u3001\u8109\u51b2\u79bb\u5b50\u675f\u8f85\u52a9\u6c89\u79ef(IBAD)\u3001\u8109\u51b2\u6fc0\u5149\u6c89\u79ef(PLD)\u548c\u7b49\u79bb\u5b50\u8f85\u52a9\u5b9a\u5411\u6c14\u76f8\u6c89\u79ef(PA-DVD)\u7b49\u5df2\u88ab\u6210\u529f\u5f00\u53d1\u3002\u591a\u79cd\u975e\u6676LiPON\u8584\u819c\u5236\u5907\u65b0\u65b9\u6cd5\u7684\u53d1\u5c55\u4e0d\u4ec5\u4e30\u5bcc\u4e86\u73b0\u6709\u6280\u672f\uff0c\u800c\u4e14\u62d3\u5c55\u4e86LiPON\u7684\u6f5c\u5728\u5e94\u7528\u3002\u8fd1\u5e74\u6765\uff0c\u5408\u6210LiPON\u7684\u6e7f\u5316\u5b66\u65b9\u6cd5\u5728\u5927\u89c4\u6a21\u5236\u9020\u4e2d\u663e\u793a\u51fa\u5de8\u5927\u6f5c\u529b\uff0c\u65e0\u9700\u771f\u7a7a\u6280\u672f\u5373\u53ef\u663e\u8457\u63d0\u9ad8\u5de5\u827a\u7ecf\u6d4e\u6027\uff0c\u4f46\u8be5\u9879\u65b9\u6cd5\u5c1a\u4e0d\u6210\u719f\uff0c\u4ecd\u5904\u4e8e\u8d77\u6b65\u9636\u6bb5\u3002\u6b64\u5916\uff0c\u91c7\u7528\u6d82\u8986\u6cd5\u548c\u5377\u5bf9\u5377\u6cd5\u5236\u5907LiPON\u8584\u819c\u5177\u6709\u9ad8\u5ea6\u7684\u5de5\u827a\u6027\u548c\u6210\u672c\u6548\u76ca\uff0c\u4f46\u96be\u4ee5\u63a7\u5236\u7c92\u5ea6\u548c\u819c\u539a\u3002<\/p>\n<p><strong>\u56db\u3001\u3010\u603b\u7ed3\u5c55\u671b\u3011<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-262253\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u724712-2.png\" alt=\"\" width=\"573\" height=\"452\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u724712-2.png 573w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2024\/08\/\u56fe\u724712-2-300x237.png 300w\" sizes=\"(max-width: 573px) 100vw, 573px\" \/><\/p>\n<p>\u56fe11 LiPON\u56fa\u6001\u7535\u89e3\u8d28\u5c55\u671b<\/p>\n<p>\u7efc\u4e0a\u6240\u8ff0\uff0cLiPON\u4f5c\u4e3a\u6700\u65e9\u5408\u6210\u7684\u65e0\u673a\u7c7b\u56fa\u6001\u7535\u89e3\u8d28\uff0c\u5728\u514b\u670d\u4f20\u7edf\u6db2\u6001\u7535\u6c60\u4f53\u7cfb\u7684\u5c40\u9650\u6027\u65b9\u9762\u53d6\u5f97\u4e86\u91cd\u5927\u8fdb\u5c55\u3002LiPON\u5177\u6709\u4f18\u5f02\u7684\u754c\u9762\u76f8\u5bb9\u6027\u3001\u5e7f\u6cdb\u7684\u7535\u5316\u5b66\u7a33\u5b9a\u7a97\u53e3\u548c\u4f18\u5f02\u7684\u70ed\u7a33\u5b9a\u6027\uff0c\u4e3a\u5176\u5728\u4e0b\u4e00\u4ee3\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u56fa\u6001\u7535\u6c60\u4e2d\u7684\u5e94\u7528\u5960\u5b9a\u4e86\u575a\u5b9e\u7684\u57fa\u7840\u3002\u7136\u800c\uff0c\u4ecd\u6709\u591a\u9879\u5173\u952e\u95ee\u9898\u503c\u5f97\u8fdb\u4e00\u6b65\u89e3\u51b3\uff1a<\/p>\n<p>(1)\u4ecd\u9700\u901a\u8fc7\u63ba\u6742\u548c\u53d6\u4ee3\u8fdb\u4e00\u6b65\u6539\u5584\u79bb\u5b50\u7535\u5bfc\u7387\u3002\u6df7\u5408\u79bb\u5b50\u63ba\u6742\u7684\u589e\u5f3a\u673a\u5236\u548c\u5bf9\u7ed3\u6784\u6027\u8d28\u7684\u6df1\u5165\u4e86\u89e3\u8fd8\u6709\u5f85\u8fdb\u4e00\u6b65\u63ed\u793a\u3002<\/p>\n<p>(2) \u65e0\u8d1f\u6781\u56fa\u6001\u7535\u6c60\u4f53\u7cfb\u4e2d\u9ad8\u901a\u91cfLi\u6c89\u79ef\u5f15\u53d1\u7684\u673a\u68b0\u5931\u6548\u4ecd\u9700\u8fdb\u4e00\u6b65\u5173\u6ce8\u3002\u5f15\u5165\u673a\u68b0\u589e\u5f3a\u57fa\u8d28\u83b7\u5f97\u5177\u6709\u4f18\u5f02\u79bb\u5b50\u4f20\u8f93\u6548\u7387\u548c\u673a\u68b0\u8010\u53d7\u6027\u7684\u4eba\u5de5\u590d\u5408SEI\uff0c\u662f\u7a33\u5b9a\u8fd0\u884c\u7684\u5173\u952e\u3002<\/p>\n<p>(3)\u754c\u9762\u949d\u5316LiPON\u7684\u5177\u4f53\u673a\u7406\uff0c\u4ee5\u53ca\u5728LiPON\u8868\u9762\u6784\u7b51\u5b8c\u6574\u5747\u5300\u7684\u949d\u5316\u5c42\u6c89\u79ef\u8fd8\u9700\u8981\u8fdb\u4e00\u6b65\u6df1\u5165\u7814\u7a76\u3002\u6dfb\u52a0\u5242\u3001\u7ed3\u6784\u4f18\u5316\u3001\u5408\u6210\u540e\u5904\u7406\u7b49\u662f\u53ef\u884c\u7684\u89e3\u51b3\u65b9\u6cd5\u3002<\/p>\n<p>(4)\u4e3a\u4e86\u5b9e\u73b0\u754c\u9762\u548c\u7ed3\u6784\u6f14\u5316\u7684\u5feb\u901f\u8bca\u65ad\uff0c\u9700\u8981\u66f4\u9ad8\u7684\u7a7a\u95f4\/\u65f6\u95f4\u5206\u8fa8\u7387\u7684\u539f\u4f4d\u534f\u540c\u8868\u5f81\u6280\u672f\u3002<\/p>\n<p>(5)\u591a\u79cd\u65b0\u578b\u5236\u5907\u65b9\u6cd5\u7684\u51fa\u73b0\u5e26\u6765\u4e86\u66f4\u9ad8\u7684\u5de5\u827a\u7ecf\u6d4e\u6027\u4f18\u52bf\uff0c\u4f46\u5728\u4ea7\u54c1\u8d28\u91cf\u65b9\u9762\u4ecd\u6709\u5f88\u5927\u7684\u63d0\u5347\u7a7a\u95f4\u3002\u65b0\u578b\u5236\u5907\u6280\u672f\u7684\u5f00\u53d1\uff0c\u5728\u5de5\u827a\u7ecf\u6d4e\u548c\u4ea7\u54c1\u8d28\u91cf\u4e4b\u95f4\u53d6\u5f97\u826f\u597d\u7684\u5e73\u8861\uff0c\u5bf9\u4e8eLiPON\u5728SSLMBs\u548c\u5176\u4ed6\u67d4\u6027\u5668\u4ef6\u4e2d\u7684\u5927\u89c4\u6a21\u5e94\u7528\u5177\u6709\u91cd\u8981\u610f\u4e49\u3002<\/p>\n<p>(6)\u6df1\u5165\u4e86\u89e3\u53cd\u5e94\u8fc7\u7a0b\u662f\u5b9e\u73b0LiPON\u5de5\u4e1a\u5316\u91cf\u4ea7\u7684\u8feb\u5207\u9700\u8981\u3002\u5e94\u4ed4\u7ec6\u8003\u8651\u6750\u6599\u7684\u8f93\u8fd0\u548c\u6c89\u79ef\u52a8\u529b\u5b66\uff0c\u5305\u62ec\u70ed\/\u8d28\/\u52a8\u91cf\u4f20\u9012\u3001\u5316\u5b66\u53cd\u5e94\u7684\u56fa\u6709\u6027\u8d28\u3002\u901a\u8fc7\u53cd\u5e94\u5668\u521b\u65b0\u548c\u8fc7\u7a0b\u8026\u5408\uff0c\u964d\u4f4e\u5de5\u827a\u6210\u672c\u83b7\u5f97\u5747\u5300\u7a33\u5b9a\u7684\u9ad8\u8d28\u91cf\u4ea7\u54c1\u662f\u6838\u5fc3\u76ee\u6807\u3002<\/p>\n<p><strong>\u539f\u6587\u8be6\u60c5<\/strong>\uff1a<\/p>\n<p>https:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/adfm.202409330<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u4e00\u3001 \u3010\u5bfc\u8bfb\u3011\u00a0 \u7814\u7a76\u666e\u904d\u8ba4\u4e3a\u4ee5LLZO\u4e3a\u4ee3\u8868\u7684\u4f20\u7edf\u65e0\u673a\u6c27\u5316\u7269\u56fa\u6001\u7535\u89e3\u8d28\u5728\u56fa\u6001\u7535\u6c60\u4e2d\u7684\u5b58\u5728\u663e\u8457\u7684\u754c\u9762\u95ee\u9898\uff0c\u5305\u62ec\u754c\u9762\u63a5\u89e6\u5dee\uff0c\u754c\u9762\u7535\u963b\u9ad8\uff0c\u5bb9\u6613\u4ea7\u751f\u9502\u679d\u6676\u7b49\u7f3a\u70b9\u3002Li&#8230;<\/p>\n","protected":false},"author":2,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[533],"tags":[],"class_list":["post-262240","post","type-post","status-publish","format-standard","hentry","category-zongshu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/262240"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/2"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=262240"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/262240\/revisions"}],"predecessor-version":[{"id":262254,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/262240\/revisions\/262254"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=262240"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=262240"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=262240"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}