{"id":267600,"date":"2025-07-26T10:51:40","date_gmt":"2025-07-26T02:51:40","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=267600"},"modified":"2025-07-26T11:00:54","modified_gmt":"2025-07-26T03:00:54","slug":"1-%e9%a2%98%e7%9b%ae%ef%bc%9a%e4%b8%ad%e5%8d%97%e5%a4%a7%e5%ad%a6%e9%be%9a%e6%b7%b1%e6%95%99%e6%8e%88%e5%9b%a2%e9%98%9f%e3%80%8acarbon%e3%80%8b-%e6%b9%8d%e6%b5%81%e5%86%b2%e5%87%bb%e5%9d%87%e5%8c%80","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=267600","title":{"rendered":"\u4e2d\u5357\u5927\u5b66\u9f9a\u6df1\u6559\u6388\u56e2\u961f\u300aCarbon\u300b: \u6e4d\u6d41\u51b2\u51fb\u5747\u5300\u94f8\u9020\u6cd5\u539f\u4f4d\u6784\u5efa\u9ad8\u5bfc\u70edCu\/\u78b3\u7ea4\u7ef4\u590d\u5408\u6750\u6599\u7684Cu\/Cr3C2\u00a0(ZrC) \/C\u5f02\u8d28\u754c\u9762"},"content":{"rendered":"\n<p>\u7814\u7a76\u5185\u5bb9\u7b80\u4ecb: \u7531\u4e8eCu\u548cC\u5bc6\u5ea6\u5dee\u5927\u4e14\u754c\u9762\u4e0d\u6da6\u6e7f\uff0c\u901a\u8fc7\u4f20\u7edf\u7684\u7194\u94f8\u65b9\u5f0f\u5f88\u96be\u5728Cu\u57fa\u4f53\u4e2d\u5747\u5300\u5206\u6563\u78b3\u586b\u6599\u3002\u8fd1\u671f\uff0c\u4e2d\u5357\u5927\u5b66\u9f9a\u6df1\u6559\u6388\u56e2\u961f\u5728\u975e\u63a5\u89e6\u5f0f\u6405\u62cc\u88c5\u7f6e\u7684\u57fa\u7840\u4e0a\uff0c\u5f00\u53d1\u4e86\u4e00\u79cd\u6e4d\u6d41\u51b2\u51fb\u5747\u8d28\u94f8\u9020\u7684\u65b0\u65b9\u6cd5\uff0c\u7ed3\u5408\u6570\u636e\u9a71\u52a8\u7b56\u7565\u6210\u529f\u8bbe\u8ba1\u5e76\u5236\u5907\u4e86\u9ad8\u5bfc\u70edCu-0.5Cr-0.5Zr\uff08wt.%\uff09\/\u78b3\u7ea4\u7ef4\uff08CFs\uff09\u590d\u5408\u6750\u6599\u3002\u5b9e\u9a8c\u7ed3\u679c\u8868\u660e\uff0c\u5f53\u8f6c\u901f\u8fbe\u5230800 rpm\uff0cCFs\u542b\u91cf\u4e3a18 vol%\u65f6\uff0c\u590d\u5408\u6750\u6599\u7684\u5e73\u9762\u5185\u548c\u5782\u76f4\u5e73\u9762\u65b9\u5411\u7684TC\u5206\u522b\u8fbe\u5230562 W m<sup>-1<\/sup>\u00a0K<sup>-1<\/sup>\u548c547 W m<sup>-1<\/sup>\u00a0K<sup>-1<\/sup>\u3002\u8d85\u91cd\u529b\u4f5c\u7528\u9a71\u52a8\u5408\u91d1\u7194\u4f53\u4ea7\u751f\u9ad8\u901f\u6e4d\u6d41\uff0c\u51b2\u51fb\u7834\u788eCF\u56e2\u805a\u4f53\u7684\u540c\u65f6\u5927\u5e45\u63d0\u5347\u4e86\u7194\u4f53\u4f20\u8d28\u6548\u7387\uff0c\u4fc3\u4f7f\u5408\u91d1\u5143\u7d20Cr\u3001Zr\u4e0eCFs\u7684\u8868\u9762\u78b3\u539f\u5b50\u53d1\u751f\u4e86\u5145\u5206\u7684\u754c\u9762\u53cd\u5e94\u3002\u7194\u4f53\u4e2d\u539f\u4f4d\u751f\u6210\u7684Cu\/Cr<sub>3<\/sub>C<sub>2 <\/sub>(ZrC) \/CF\u5f02\u8d28\u754c\u9762\u6781\u5927\u5730\u6539\u5584\u4e86Cu\/C\u754c\u9762\u7684\u6da6\u6e7f\u6027\uff0c\u786e\u4fdd\u4e86\u7194\u4f53\u51dd\u56fa\u540eCFs\u5728\u94dc\u57fa\u4f53\u4e2d\u7684\u5747\u5300\u5206\u6563\u5e76\u5f62\u6210\u4e92\u8fde\u7f51\u7edc\u3002\u901a\u8fc7\u6539\u8fdb\u7684Agari\u6a21\u578b\u5206\u6790\u4e86Cu-Cr-Zr\/CFs\u590d\u5408\u6750\u6599\u7684\u5bfc\u70ed\u673a\u7406\uff0c\u7ed3\u679c\u8868\u660e3D\u4e92\u8fde\u5bfc\u70ed\u7f51\u7edc\u548c\u4f4e\u70ed\u963bCu\/Cr<sub>3<\/sub>C<sub>2 <\/sub>(ZrC) \/CF\u5f02\u8d28\u754c\u9762\u662f\u590d\u5408\u6750\u6599\u5177\u6709\u4f18\u5f02\u5bfc\u70ed\u6027\u80fd\u7684\u4e3b\u8981\u539f\u56e0\u3002\u672c\u7814\u7a76\u4e3a\u5404\u5411\u540c\u6027\u9ad8\u5bfc\u70edCu\/C\u590d\u5408\u6750\u6599\u7684\u5236\u5907\u63d0\u4f9b\u4e86\u4e00\u79cd\u4f4e\u6210\u672c\u65b9\u6848\u3002<\/p>\n\n\n\n<p>\u76f8\u5173\u5de5\u4f5c\u4ee5\u201cIn-situ construction of <a>Cu\/Cr<\/a><sub>3<\/sub>C<sub>2<\/sub>&nbsp;(ZrC)&nbsp;\/C heterogeneous interfaces&nbsp;in high thermal conductivity Cu\/Carbon fibers&nbsp;composites via&nbsp;turbulence-shock homogeneous casting\u201d\u4e3a\u9898\u53d1\u8868\u5728\u56fd\u9645\u8457\u540d\u671f\u520a\u300aCarbon\u300b\u4e0a\u3002<\/p>\n\n\n\n<p>\u8bba\u6587\u94fe\u63a5\uff1a<a href=\"https:\/\/doi.org\/10.1016\/j.carbon.2025.120654\"><u>https:\/\/doi.org\/10.1016\/j.carbon.2025.120654<\/u><\/a><\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"1153\" height=\"802\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2025\/07\/\u56fe\u72471-5.png\" alt=\"\" class=\"wp-image-267601\"\/><\/figure>\n\n\n\n<p>\u5177\u4f53\u5185\u5bb9<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"1271\" height=\"1219\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2025\/07\/\u56fe\u72472-5.png\" alt=\"\" class=\"wp-image-267615\"\/><\/figure>\n\n\n\n<p>\u56fe1 \u6570\u636e\u9a71\u52a8\u5143\u7d20\u7b5b\u9009\u7b56\u7565<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"710\" height=\"748\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2025\/07\/\u56fe\u72473-5.png\" alt=\"\" class=\"wp-image-267616\"\/><\/figure>\n\n\n\n<p>\u56fe2\uff08a\uff09CFs\u7684SEM\u5f62\u8c8c\uff1b\uff08b\uff09CFs\u7684\u62c9\u66fc\u5149\u8c31\u56fe\uff1b\uff08c\uff09CFs\u7684XRD\u56fe\uff1b\uff08d\uff09\u6e4d\u6d41\u51b2\u51fb\u5747\u8d28\u94f8\u9020\u7684\u5236\u5907\u8fc7\u7a0b\u53ca\u673a\u7406\u793a\u610f\u56fe\uff1b\uff08e\uff0cf\uff09Pure Cu\/18-CFs\u548cCu-Zr\/18-CFs\u590d\u5408\u6750\u6599\u5728\u8f6c\u901f\u4e3a800 rpm\u7684SEM\u5f62\u8c8c\uff1b\uff08g-j\uff09Cu-Cr-Zr\/18-CFs\u590d\u5408\u6750\u6599\u5728\u4e0d\u540c\u8f6c\u901f\u4e0b\u7684SEM\u5f62\u8c8c<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"700\" height=\"775\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2025\/07\/\u56fe\u72474-2.png\" alt=\"\" class=\"wp-image-267609\"\/><\/figure>\n\n\n\n<p>\u56fe3\uff08a\uff0cb\uff0cd\uff0ce\uff09BSE\u56fe\u50cf\uff1b\uff08c\uff0cf\uff09SE\u56fe\u50cf\u53ca\u76f8\u5e94\u7684\u5143\u7d20\u9762\u5206\u5e03\u56fe\uff1b Cu-Cr-Zr\/18-CFs\u590d\u5408\u6750\u6599CFs\u7684\uff08g\uff093D X\u5c04\u7ebfmicro-CT\u5206\u5e03\u56fe\u50cf\uff0c\uff08h-j\uff09\u5e73\u9762X\u5c04\u7ebfmicro-CT\u56fe\u50cf\u4ee5\u53ca\u5b54\u9699\u5206\u5e03\uff0c\uff08k\uff09\u5b54\u5f84\u5c3a\u5bf8\u7edf\u8ba1\u56fe\uff1b\uff08l\uff09\u4e0d\u540cCu\/CFs\u590d\u5408\u6750\u6599\u7684\u76f8\u5bf9\u5bc6\u5ea6\u67f1\u72b6\u56fe<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"954\" height=\"711\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2025\/07\/\u56fe\u72475-2.png\" alt=\"\" class=\"wp-image-267610\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2025\/07\/\u56fe\u72475-2.png 954w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2025\/07\/\u56fe\u72475-2-200x150.png 200w\" sizes=\"(max-width: 954px) 100vw, 954px\" \/><\/figure>\n\n\n\n<p>\u56fe4 <a>Cu-Cr\/18-CFs\u590d\u5408\u6750\u6599\u4e2d\u8403\u53d6CFs\u7684\uff08a\uff09SEM\u56fe\u50cf<\/a>\uff0c\uff08b-d\uff09\u76f8\u5e94\u7684\u5143\u7d20\u9762\u5206\u5e03\u56fe\uff0c\uff08e\uff09XRD\u56fe\u50cf\uff1b Cu-Cr-Zr\/18-CFs\u590d\u5408\u6750\u6599\u4e2d\u8403\u53d6CFs\u7684\uff08f\uff09SEM\u56fe\u50cf\uff0c\uff08g-i\uff09\u76f8\u5e94\u7684\u5143\u7d20\u9762\u5206\u5e03\u56fe\uff0c\uff08j\uff09XRD\u56fe\uff1b\uff08k\uff0cl\uff09Cu-Cr-Zr\/18-CFs\u590d\u5408\u6750\u6599\u7ecf\u8fc7\u6df1\u8150\u8680\u5904\u7406\u540e\u7684SEM\u6574\u4f53\u5f62\u8c8c\u53ca\u76f8\u5e94\u7684\u5143\u7d20\u9762\u5206\u5e03\u56fe\uff1b\uff08m-p\uff09Cu-Cr-Zr\/18-CFs\u590d\u5408\u6750\u6599\u7ecf\u8fc7\u6df1\u8150\u8680\u5904\u7406\u540eCFs\u7684SEM\u5f62\u8c8c<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"1271\" height=\"1097\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2025\/07\/\u56fe\u72476-1.png\" alt=\"\" class=\"wp-image-267611\"\/><\/figure>\n\n\n\n<p>\u56fe5 \u4e0d\u540c\u72b6\u6001CFs\u7684XPS\u7ed3\u679c\uff1a\uff08a-c\uff09\u539f\u6599CFs\uff1b\uff08d-f\uff09Cu-Cr\/18-CFs\u590d\u5408\u6750\u6599\u4e2d\u8403\u53d6\u7684CFs\uff1bCu-Cr-Zr\/18-CFs\u590d\u5408\u6750\u6599\u4e2d\u8403\u53d6\u7684CFs<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"663\" height=\"776\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2025\/07\/\u56fe\u72477-1.png\" alt=\"\" class=\"wp-image-267612\"\/><\/figure>\n\n\n\n<p>\u56fe6 Cu-Cr-Zr\/18-CFs\u590d\u5408\u6750\u6599\u7684TEM\u56fe\u50cf\uff1a\uff08a\uff09BF\u56fe\u548c\u76f8\u5e94\u7684\u5143\u7d20\u9762\u5206\u5e03\u56fe\uff1b\uff08b\uff0cc\uff09\u5404\u5143\u7d20\u7684\u7ebf\u5206\u5e03\u56fe\uff1b\uff08d-g\uff0cj\uff0cm\uff09<a>HRTEM\u56fe\u50cf<\/a>\u548c\u76f8\u5e94\u7684FFT\u56fe\uff1b\uff08h\uff0ci\uff09HAADF\u56fe\u548c\u76f8\u5e94\u7684\u5143\u7d20\u9762\u5206\u5e03\u56fe\uff1b\uff08k\uff0cm\uff09HRTEM\u56fe\u50cf<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"1271\" height=\"753\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2025\/07\/\u56fe\u72478.png\" alt=\"\" class=\"wp-image-267613\"\/><\/figure>\n\n\n\n<p>\u56fe7 \uff08a\uff0cb\uff09Cu\/CFs\u590d\u5408\u6750\u6599\u5728\u5e73\u9762\u5185\u548c\u5782\u76f4\u5e73\u9762\u65b9\u5411\u7684\u70ed\u6269\u6563\u7cfb\u6570\u548cTC\uff1b<a>\uff08c\uff0925-200\u2103\u8303\u56f4\u5185\u4e0d\u540cCu\/CFs\u590d\u5408\u6750\u6599\u5728\u5e73\u9762\u5185\u65b9\u5411\u957f\u5ea6\u53d8\u5316\u7387\u968f\u6e29\u5ea6\u7684\u53d8\u5316\uff1b\uff08d\uff0925-200<\/a>\u2103\u5404Cu\/CFs\u590d\u5408\u6750\u6599\u5728\u5e73\u9762\u5185\u548c\u5782\u76f4\u5e73\u9762\u65b9\u5411\u7684CTE\uff1b\uff08e-h\uff09\u7eafCu\u3001Cu-Cr\/18-CFs\u590d\u5408\u6750\u6599\u548cCu-Cr-Zr\/18-CFs\u590d\u5408\u6750\u6599\u5728\u52a0\u70ed\u548c\u51b7\u5374\u8fc7\u7a0b\u4e2d\u7684\u7ea2\u5916\u70ed\u6210\u50cf\u56fe\uff1b\uff08i\uff09Cu\/CFs\u590d\u5408\u6750\u6599\u7684\u5f2f\u66f2\u5e94\u529b-\u5e94\u53d8\u66f2\u7ebf\uff0c\uff08j\uff09FS\u7684\u67f1\u72b6\u56fe\uff1b\uff08k-m\uff09Cu-Cr-Zr\/18-CFs\u590d\u5408\u6750\u6599\u7684\u5f2f\u66f2\u65ad\u53e3SEM\u56fe\u50cf<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"1120\" height=\"926\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2025\/07\/\u56fe\u72479.png\" alt=\"\" class=\"wp-image-267617\"\/><\/figure>\n\n\n\n<p>\u56fe8 \u672c\u7814\u7a76\u4e2dCu-Cr-Zr\/CFs\u590d\u5408\u6750\u6599\u4e0e\u4e4b\u524d\u6587\u732e\u62a5\u9053\u4e2d\u7684\u9ad8\u5bfc\u70edCu\u57fa\u590d\u5408\u6750\u6599\u7684\u6027\u80fd\u6bd4\u8f83<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"1271\" height=\"821\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2025\/07\/\u56fe\u724710.png\" alt=\"\" class=\"wp-image-267614\"\/><\/figure>\n\n\n\n<p>\u56fe9\uff08a\uff09\u6e4d\u6d41\u51b2\u51fb\u5747\u8d28\u94f8\u9020\u5236\u5907Cu\/CFs\u590d\u5408\u6750\u6599 3D CF\u7f51\u7edc\u5f62\u6210\u673a\u5236\u793a\u610f\u56fe\uff1b\uff08b\uff09\u6539\u8fdbAgari\u5bfc\u70ed\u6a21\u578b\u7684\u673a\u7406\u793a\u610f\u56fe\uff1b\uff08b\uff09\u5e76\u8054\u6a21\u578b\u3001EMPT\u6a21\u578b\u3001\u6539\u8fdb\u7684Agari\u6a21\u578bTC\u8ba1\u7b97\u7ed3\u679c\u4ee5\u53ca\u5b9e\u9a8c\u7ed3\u679c\u7684\u6bd4\u8f83<\/p>\n\n\n\n<p>5.\u603b\u7ed3<\/p>\n\n\n\n<p>\u672c\u7814\u7a76\u5728\u975e\u63a5\u89e6\u5f0f\u6405\u62cc\u88c5\u7f6e\u7684\u57fa\u7840\u4e0a\uff0c\u5f00\u53d1\u4e86\u4e00\u79cd\u6e4d\u6d41\u51b2\u51fb\u5747\u8d28\u94f8\u9020\u7684\u65b0\u65b9\u6cd5\uff0c\u5e76\u7ed3\u5408\u6570\u636e\u9a71\u52a8\u5143\u7d20\u7b5b\u9009\u7b56\u7565\u6210\u529f\u5236\u5907\u4e86\u5177\u67093D\u8fde\u901aCF\u7f51\u7edc\u7684<a>Cu-Cr-Zr\/CFs\u590d\u5408\u6750\u6599<\/a>\u3002\u901a\u8fc7\u5728\u7194\u4f53\u4e2d\u5236\u9020\u5f3a\u70c8\u7684\u6e4d\u6d41\u4f7fCFs\u5206\u6563\u5747\u5300\u5e76\u4e0e\u6539\u6027\u5143\u7d20\u53d1\u751f\u5145\u5206\u7684\u539f\u4f4d\u754c\u9762\u53cd\u5e94\uff0c\u6210\u529f\u5b9e\u73b0\u4e86CFs\u5728\u4f4e\u542b\u91cf\uff0812-30 vol%\uff09\u4e0b\u7684\u81ea\u8fde\u63a5\u3002\u5f97\u5230\u7684Cu-Cr-Zr\/CFs\u590d\u5408\u6750\u6599\u5177\u6709\u4f18\u5f02\u7684\u70ed\u5b66\u6027\u80fd\u548c\u529b\u5b66\u6027\u80fd\u3002\u5176\u4e2dCu-Cr-Zr\/18-CFs\u590d\u5408\u6750\u6599\u5728CFs\u542b\u91cf\u4ec5\u4e3a<a>18 vol%\u7684\u60c5\u51b5\u4e0b\uff0c\u5e73\u9762\u5185\u548c\u5782\u76f4\u5e73\u9762\u65b9\u5411\u7684TC\u5206\u522b\u8fbe\u5230562 W m<\/a><sup>-1<\/sup>&nbsp;K<sup>-1<\/sup>\u548c547 W m<sup>-1<\/sup>&nbsp;K<sup>-1<\/sup>\uff0c\u540c\u65f6FS\u8fbe\u5230247 MPa\u3002\u9ad8\u901f\u6e4d\u6d41\u5bf9\u4f20\u8d28\u6548\u7387\u7684\u63d0\u5347\u4f7fCFs\u4e0eCr\u548cZr\u539f\u5b50\u5728\u7194\u4f53\u5185\u53d1\u751f\u5145\u5206\u7684\u539f\u4f4d\u754c\u9762\u53cd\u5e94\u3002\u5f62\u6210\u7684Cu\/Cr<sub>3<\/sub>C<sub>2 <\/sub>(ZrC) \/CF\u5f02\u8d28\u754c\u9762\u8fc7\u6e21\u5c42\u6781\u5927\u6539\u5584\u4e86\u754c\u9762\u7ed3\u5408\uff0c\u6709\u5229\u4e8eCu-Cr-Zr\/CFs\u590d\u5408\u6750\u6599\u7efc\u5408\u6027\u80fd\u7684\u63d0\u5347\u3002Zr\u5143\u7d20\u7684\u6dfb\u52a0\u63d0\u5347\u4e86CFs\u5728Cu\u7194\u4f53\u4e2d\u7684\u5206\u6563\u6027\uff0c\u4f7f\u5f97\u539f\u4f4d\u754c\u9762\u53cd\u5e94\u8fc7\u7a0b\u66f4\u52a0\u5145\u5206\uff0c\u56e0\u6b64\u4f7fCu-Cr-Zr\/CFs\u590d\u5408\u6750\u6599\u76f8\u6bd4\u4e8eCu-Cr\/18-CFs\u590d\u5408\u6750\u6599\u5177\u6709\u66f4\u4f18\u5f02\u7684\u6027\u80fd\u3002\u7194\u4f53\u5728\u8d85\u91cd\u529b\u4f5c\u7528\u4e0b\u7684\u5747\u5300\u51dd\u56fa\u4fc3\u8fdb\u4e86Cu-Cr-Zr\/CFs\u590d\u5408\u6750\u6599\u8fde\u901aCF\u7f51\u7edc\u7684\u5f62\u6210\u3002\u9ad8\u6548\u4e92\u8fdeCF\u5bfc\u70ed\u7f51\u7edc\u4f7f\u5f97\u70ed\u91cf\u4f18\u5148\u5728\u5176\u5185\u90e8\u4f20\u9012\uff0c\u4ece\u800c\u63d0\u5347\u4e86Cu-Cr-Zr\/CFs\u590d\u5408\u6750\u6599\u7684\u5bfc\u70ed\u6027\u80fd\u3002\u5efa\u7acb\u4e86\u6539\u8fdb\u7684Agari\u6a21\u578b\u5bf9Cu-Cr-Zr\/CFs\u590d\u5408\u6750\u6599\u7684TC\u8fdb\u884c\u4e86\u5206\u6790\u3002\u7ed3\u679c\u8868\u660e\uff0c\u76f8\u5bf9\u4e8e\u5e76\u8054\u6a21\u578b\u548cEMPT\u6a21\u578b\uff0c\u6539\u8fdb\u7684Agari\u6a21\u578b\u4e0e\u5b9e\u9a8c\u7ed3\u679c\u80fd\u591f\u66f4\u597d\u7684\u543b\u5408\u3002\u8fd9\u4e3b\u8981\u662f\u7531\u4e8e\u5176\u8003\u8651\u4e86\u7531CF\u5bfc\u70ed\u94fe\u5f62\u6210\u7684\u7f51\u7edc\u4ee5\u53ca\u754c\u9762\u70ed\u963b\u5bf9TC\u7684\u5f71\u54cd\uff0c\u800c\u5e76\u8054\u6a21\u578b\u548cEMPT\u6a21\u578b\u672a\u8003\u8651\u5176\u5bf9TC\u7684\u5f71\u54cd\u3002\u6e4d\u6d41\u51b2\u51fb\u5747\u8d28\u94f8\u9020\u7684\u5f00\u53d1\u4e3a\u4f4e\u6210\u672c\u9ad8\u6027\u80fdCu\u57fa\u590d\u5408\u6750\u6599\u7684\u5236\u5907\u5f00\u8f9f\u4e86\u5168\u65b0\u7684\u9014\u5f84\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u7814\u7a76\u5185\u5bb9\u7b80\u4ecb: \u7531\u4e8eCu\u548cC\u5bc6\u5ea6\u5dee\u5927\u4e14\u754c\u9762\u4e0d\u6da6\u6e7f\uff0c\u901a\u8fc7\u4f20\u7edf\u7684\u7194\u94f8\u65b9\u5f0f\u5f88\u96be\u5728Cu\u57fa\u4f53\u4e2d\u5747\u5300\u5206\u6563\u78b3\u586b\u6599\u3002\u8fd1\u671f\uff0c\u4e2d\u5357\u5927\u5b66\u9f9a\u6df1\u6559\u6388\u56e2\u961f\u5728\u975e\u63a5\u89e6\u5f0f\u6405\u62cc\u88c5\u7f6e\u7684\u57fa\u7840\u4e0a\uff0c\u5f00\u53d1\u4e86&#8230;<\/p>\n","protected":false},"author":31345,"featured_media":0,"comment_status":"open","ping_status":"","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[2],"tags":[],"class_list":["post-267600","post","type-post","status-publish","format-standard","hentry","category-keji"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/267600"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/31345"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=267600"}],"version-history":[{"count":3,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/267600\/revisions"}],"predecessor-version":[{"id":267621,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/267600\/revisions\/267621"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=267600"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=267600"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=267600"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}