{"id":269758,"date":"2025-12-06T08:20:00","date_gmt":"2025-12-06T00:20:00","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=269758"},"modified":"2025-12-05T21:24:55","modified_gmt":"2025-12-05T13:24:55","slug":"%e9%93%9d%e9%87%91%e5%b1%9e%e7%94%b5%e6%b1%a0%ef%bc%81%e6%97%b6%e9%9a%94%e5%9b%9b%e5%b9%b4%ef%bc%8c%e5%a4%a9%e6%b4%a5%e5%a4%a7%e5%ad%a6nanoyang%e5%9b%a2%e9%98%9f%e5%86%8d%e5%8f%91nature-sustainability","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=269758","title":{"rendered":"\u94dd\u91d1\u5c5e\u7535\u6c60\uff01\u65f6\u9694\u56db\u5e74\uff0c\u5929\u6d25\u5927\u5b66Nanoyang\u56e2\u961f\u518d\u53d1Nature Sustainability\uff01"},"content":{"rendered":"\n<p>Harvey<\/p>\n\n\n\n<p>\u7b2c\u4e00\u4f5c\u8005\uff1a\u5f20\u6e24\uff0c\u674e\u6cbb\u56fd\uff0c\u97e9\u5927\u91cf\uff0c\u95f5\u5fd7\u96ef<\/p>\n\n\n\n<p>\u901a\u8baf\u4f5c\u8005\uff1a\u6768\u5168\u7ea2\uff0c\u7fc1\u54f2\uff0c\u97e9\u5927\u91cf<\/p>\n\n\n\n<p>\u901a\u8baf\u5355\u4f4d\uff1a\u5929\u6d25\u5927\u5b66<\/p>\n\n\n\n<p>DOI: 10.1038\/s41893-025-01706-6<\/p>\n\n\n\n<p>\u3010\u7814\u7a76\u80cc\u666f\u3011<\/p>\n\n\n\n<p>\u5411\u6e05\u6d01\u80fd\u6e90\u7684\u8f6c\u578b\u8feb\u5207\u9700\u8981\u53d1\u5c55\u9502\u79bb\u5b50\u7535\u6c60\u4e4b\u5916\u7684\u65b0\u578b\u6216\u4e92\u8865\u7535\u6c60\u4f53\u7cfb\u3002\u94dd\u91d1\u5c5e\u7535\u6c60\uff08AMBs\uff09\u51ed\u501f\u94dd\u8d1f\u6781\u8d85\u9ad8\u7684\u7406\u8bba\u6bd4\u5bb9\u91cf\uff082981 mAh g<sup>\u2212<\/sup><sup>1<\/sup>\u30018056 mAh&nbsp;cm<sup>\u2212<\/sup><sup>3<\/sup>\uff09\u3001\u4e30\u5bcc\u7684\u5730\u58f3\u50a8\u91cf\u3001\u4f4e\u6210\u672c\u4ee5\u53ca\u4e09\u7535\u5b50\u8f6c\u79fb\u7279\u6027\uff0c\u5728\u4e0b\u4e00\u4ee3\u50a8\u80fd\u6280\u672f\u4e2d\u5c55\u73b0\u51fa\u5de8\u5927\u6f5c\u529b\u3002\u7136\u800c\uff0c\u5f53\u524d\u94dd\u91d1\u5c5e\u7535\u6c60\u6280\u672f\u4e25\u91cd\u4f9d\u8d56\u4e8e\u80fd\u591f\u6784\u5efa\u9ad8\u9636\u6c2f\u94dd\u9178\u76d0\u9634\u79bb\u5b50\uff08Al<sub>n<\/sub>Cl<sub>3n+1<\/sub><sup>\u2212<\/sup>\uff0cn\u22652\uff09\u7684\u7535\u89e3\u6db2\u4f53\u7cfb\uff08\u5982AlCl<sub>3<\/sub>\/[EMIm]Cl\u79bb\u5b50\u6db2\u4f53\uff09\uff0c\u8fd9\u7c7b\u7535\u89e3\u6db2\u867d\u80fd\u5b9e\u73b0\u94dd\u7684\u53ef\u9006\u6c89\u79ef\/\u6eb6\u89e3\uff0c\u5374\u5b58\u5728\u9ad8\u8150\u8680\u6027\u3001\u9ad8\u6210\u672c\u3001\u9ad8\u7c98\u5ea6\u548c\u52a8\u529b\u5b66\u8fdf\u6ede\u7b49\u95ee\u9898\u3002\u66f4\u4e25\u91cd\u7684\u662f\uff0c\u6b64\u7c7b\u7535\u89e3\u6db2\u7684\u5f3a\u8150\u8680\u6027\u4f1a\u5bfc\u81f4\u7535\u6c60\u91d1\u5c5e\u7ec4\u4ef6\uff08\u5982\u96c6\u6d41\u4f53\u3001\u6781\u8033\u3001\u5bc6\u5c01\u6750\u6599\u7b49\uff09\u5feb\u901f\u52a3\u5316\uff0c\u4e25\u91cd\u963b\u788d\u4e86\u94dd\u91d1\u5c5e\u7535\u6c60\u7684\u5b9e\u7528\u5316\u8fdb\u7a0b\u3002\u56e0\u6b64\uff0c\u5f00\u53d1\u517c\u5177\u4f4e\u8150\u8680\u6027\u3001\u9ad8\u53ef\u9006\u7684\u65b0\u578b\u7535\u89e3\u6db2\u4f53\u7cfb\uff0c\u6210\u4e3a\u94dd\u91d1\u5c5e\u7535\u6c60\u5b9e\u7528\u5316\u7684\u5173\u952e\u7a81\u7834\u53e3\u3002<\/p>\n\n\n\n<p>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/p>\n\n\n\n<p>\u65e5\u524d\uff0c\u5929\u6d25\u5927\u5b66Nanoyang\u56e2\u961f\u5728\u300aNature Sustainability\u300b\u53d1\u8868\u91cd\u8981\u7814\u7a76\u6210\u679c\uff0c\u8be5\u7814\u7a76\u63d0\u51fa\u4e86\u4e00\u79cd\u5168\u65b0\u7684\u201c\u6709\u673a\u53cc\u6c2f\u201d\u7535\u89e3\u6db2\u8bbe\u8ba1\u7b56\u7565\uff0c\u4ee5\u6c2f\u5316\u94dd\/\u6b63\u4e19\u919a\uff08AlCl<sub>3<\/sub>\/DPE\uff09\u6709\u673a\u4f53\u7cfb\u66ff\u4ee3\u4f20\u7edf\u79bb\u5b50\u6db2\u4f53\uff0c\u6709\u6548\u89e3\u51b3\u4e86\u94dd\u91d1\u5c5e\u7535\u6c60\u957f\u671f\u9762\u4e34\u7684\u8150\u8680\u6027\u96be\u9898\uff0c\u4e3a\u5b9e\u73b0\u5b9e\u7528\u5316\u94dd\u91d1\u5c5e\u7535\u6c60\u8fc8\u51fa\u91cd\u8981\u4e00\u6b65\u3002\u901a\u8fc7\u5bf9\u6709\u673a\u6eb6\u5242\u6eb6\u5242\u5316\u80fd\u529b\u7684\u7cbe\u786e\u7b5b\u9009\u4e0e\u8c03\u63a7\uff0c\u6784\u5efa\u4e86\u72ec\u7279\u7684\u201c\u6709\u673a\u53cc\u6c2f\u201d\u6eb6\u5242\u5316\u7ed3\u6784\uff08AlCl<sub>2<\/sub>(DPE)<sub>2<\/sub><sup>+<\/sup>\uff09\uff0c\u4e0d\u4ec5\u663e\u8457\u964d\u4f4e\u4e86\u7535\u89e3\u6db2\u7684\u8150\u8680\u6027\uff0c\u8fd8\u4fdd\u6301\u4e86\u4f18\u5f02\u7684\u94dd\u6c89\u79ef\/\u6eb6\u89e3\u53ef\u9006\u6027\u3002\u5b9e\u9a8c\u8868\u660e\uff0c\u8be5\u7535\u89e3\u6db2\u5bf9\u4e0d\u9508\u94a2\u3001\u94dc\u7b49\u591a\u79cd\u91d1\u5c5e\u96c6\u6d41\u4f53\u8868\u73b0\u51fa\u6781\u4f4e\u7684\u8150\u8680\u901f\u7387\uff0c\u540c\u65f6\u5b9e\u73b0\u94dd\u91d1\u5c5e\u8d1f\u6781\u8d85\u8fc72000\u5c0f\u65f6\u7684\u7a33\u5b9a\u5faa\u73af\u548c\u9ad8\u8fbe99.85%\u7684\u94dd\u6c89\u79ef\/\u6eb6\u89e3\u5e93\u4f26\u6548\u7387\u3002\u57fa\u4e8e\u8be5\u7535\u89e3\u6db2\u7684\u94dd\u91d1\u5c5e\u7535\u6c60\u5c55\u73b0\u51fa\u4f18\u5f02\u7684\u5faa\u73af\u7a33\u5b9a\u6027\uff0c\u53ef\u7a33\u5b9a\u8fd0\u884c300\u6b21\u4ee5\u4e0a\u3002\u8fd9\u4e00\u7a81\u7834\u6027\u8fdb\u5c55\u4e3a\u94dd\u91d1\u5c5e\u7535\u6c60\u7684\u5b9e\u7528\u5316\u94fa\u5e73\u4e86\u9053\u8def\uff0c\u4e5f\u4e3a\u5176\u4ed6\u591a\u4ef7\u91d1\u5c5e\u7535\u6c60\u7535\u89e3\u6db2\u8bbe\u8ba1\u63d0\u4f9b\u4e86\u5168\u65b0\u601d\u8def\u3002\u8be5\u7814\u7a76\u6210\u679c\u4ee5\u201cNon-corrosive organodichloro electrolyte for reversible aluminium metal batteries\u201d\u4e3a\u9898\u4e8e12\u67084\u65e5\u53d1\u8868\u5728Nature&nbsp;Sustainability\uff08DOI: 10.1038\/s41893-025-01706-6\uff09\u4e0a\u3002<\/p>\n\n\n\n<p>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/p>\n\n\n\n<p>\u8981\u70b91&nbsp;\u7535\u89e3\u6db2\u8bbe\u8ba1\u4e0e\u6eb6\u5242\u5316\u7ed3\u6784\u5206\u6790<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"500\" height=\"700\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2025\/12\/2382c315a6ba396-4.png\" alt=\"\" class=\"wp-image-269759\"\/><\/figure>\n\n\n\n<p>\u56fe1 | \u6eb6\u5242\u7b5b\u9009\u4e0e\u7535\u89e3\u6db2\u7ed3\u6784\u89e3\u6790<\/p>\n\n\n\n<p>\u4f5c\u8005\u901a\u8fc7\u6709\u673a\u6eb6\u5242\u5206\u5b50\u9759\u7535\u52bf\u5206\u6790\u4e0e\u94dd\u6c89\u79ef\u52a8\u529b\u5b66\u6d4b\u8bd5\uff0c\u7b5b\u9009\u51fa\u6b63\u4e19\u919a\uff08DPE\uff09\u4f5c\u4e3a\u6700\u4f18\u6eb6\u5242\uff0c\u5176\u5728\u201c\u706b\u5c71\u56fe\u201d\u4e2d\u4f4d\u4e8e\u52a8\u529b\u5b66\u6027\u80fd\u9876\u70b9\uff08\u56fe1a\uff09\uff0c\u8868\u660e\u6eb6\u5242\u7684\u9002\u5ea6\u6eb6\u5242\u5316\u80fd\u529b\u5bf9\u4e8e\u94dd\u7684\u6c89\u79ef\u52a8\u529b\u5b66\u81f3\u5173\u91cd\u8981\u3002\u901a\u8fc7\u6838\u78c1\u3001\u62c9\u66fc\u3001\u8d28\u8c31\u3001\u7406\u8bba\u8ba1\u7b97\u4e0e\u5206\u5b50\u52a8\u529b\u5b66\u6a21\u62df\uff0c\u8bc1\u5b9eAlCl<sub>3<\/sub>\/DPE\u7535\u89e3\u6db2\u4e2d\u7684\u9634\u79bb\u5b50\u4e3b\u8981\u4e3aAlCl<sub>4<\/sub><sup>\u2212<\/sup>\uff0c\u800c\u9633\u79bb\u5b50\u5219\u4e3a\u201c\u6709\u673a\u53cc\u6c2f\u201d\u6eb6\u5242\u5316\u7ed3\u6784\u7684AlCl<sub>2<\/sub>(DPE)<sub>2<\/sub><sup>+<\/sup>\uff0c\u533a\u522b\u4e8e\u4f20\u7edf\u79bb\u5b50\u6db2\u4f53\u548c\u5176\u4ed6\u6709\u673a\u7535\u89e3\u6db2\u3002\u5c3d\u7ba1\u6240\u6709\u6709\u673a\u7535\u89e3\u6db2\u4e2d\u5747\u542b\u6709AlCl<sub>4<\/sub><sup>\u2212<\/sup>\u9634\u79bb\u5b50\uff0c\u4f46\u662f\u4e0d\u540c\u7535\u89e3\u6db2\u4f53\u7cfb\u4e2d\u7684\u9633\u79bb\u5b50\u7269\u79cd\u5374\u4e0d\u5c3d\u76f8\u540c\u3002<strong>\u4f5c\u8005\u53d1\u73b0\u201c\u6709\u673a\u53cc\u6c2f\u201d<\/strong><strong>AlCl<\/strong><strong><sub><strong><sub>2<\/sub><\/strong><\/sub><\/strong><strong>(DPE)<\/strong><strong><sub><strong><sub>2<\/sub><\/strong><\/sub><\/strong><strong><sup><strong><sup>+<\/sup><\/strong><\/sup><\/strong><strong>\u6eb6\u5242\u5316\u7269\u79cd\u7684\u5f62\u6210\u4e0e\u6709\u673a\u6eb6\u5242\u7684\u6eb6\u5242\u5316\u80fd\u529b\u76f4\u63a5\u76f8\u5173<\/strong>\uff0c\u5728\u8f83\u5f3a\u6eb6\u5242\u5316\u80fd\u529b\u7684\u6709\u673a\u6eb6\u5242\u4e2d\uff08\u5982\u78b3\u9178\u4e19\u70ef\u916f(PC)\u3001\u4e59\u8148(ACN)\uff09\uff0c\u7535\u89e3\u6db2\u4e2d\u7684\u9633\u79bb\u5b50\u4ee5<a><\/a>Al(solvent)<sub>6<\/sub><sup>3+<\/sup>\u7684\u5f62\u5f0f\u5b58\u5728\uff0c\u800c\u5f31\u6eb6\u5242\u5316\u80fd\u529b\u7684\u6709\u673a\u6eb6\u5242\u5bf9AlCl<sub>3<\/sub>\u76d0\u7684\u89e3\u79bb\u80fd\u529b\u53c8\u4e0d\u8db3\uff0c\u5bfc\u81f4\u8f83\u4f4e\u7684\u6eb6\u89e3\u5ea6\uff0c<strong>\u53ea\u6709\u5f53\u6709\u673a\u6eb6\u5242\u7684\u6eb6\u5242\u5316\u80fd\u529b\u9002\u4e2d\u65f6\uff0c<\/strong><strong>Cl<\/strong><strong><sup><strong><sup>\u2212<\/sup><\/strong><\/sup><\/strong><strong>\u624d\u4f1a\u4e0e\u6709\u673a\u6eb6\u5242\u5171\u540c\u8fdb\u5165Al<\/strong><strong><sup><strong><sup>3+<\/sup><\/strong><\/sup><\/strong><strong>\u7684\u6eb6\u5242\u5316\u9798\u5c42\uff0c\u5f62\u6210\u201c\u6709\u673a\u53cc\u6c2f\u201d\u6eb6\u5242\u5316\u7ed3\u6784\u7684\u9633\u79bb\u5b50\u7269\u79cd<\/strong>\uff0c\u4ece\u800c\u5b9e\u73b0\u8f83\u5feb\u7684\u94dd\u6c89\u79ef\u52a8\u529b\u5b66\u3002<\/p>\n\n\n\n<p>\u8981\u70b92 \u201c\u6709\u673a\u53cc\u6c2f\u201d\u7684\u8131\u6eb6\u52a8\u529b\u5b66\u5206\u6790<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"500\" height=\"373\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2025\/12\/ce6e2814f207c93-4.png\" alt=\"\" class=\"wp-image-269760\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2025\/12\/ce6e2814f207c93-4.png 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2025\/12\/ce6e2814f207c93-4-200x150.png 200w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/figure>\n\n\n\n<p>\u56fe2 | \u8131\u6eb6\u5242\u5316\u52a8\u529b\u5b66\u673a\u5236<\/p>\n\n\n\n<p>\u6676\u4f53\u8f68\u9053\u54c8\u5bc6\u987f\u5e03\u5c45\uff08COHP\uff09\u5206\u6790\u8868\u660e\uff0cCl<sup>\u2212<\/sup>\u8fdb\u5165Al<sup>3+<\/sup>\u7684\u6eb6\u5242\u5316\u9798\u5c42\u540e\u53ef\u4ee5\u663e\u8457\u5f31\u5316Al\u2013O\u952e\uff0c\u8fdb\u800c\u51cf\u5f31Al<sup>3+<\/sup>\u4e0e\u6eb6\u5242\u4e4b\u95f4\u7684\u76f8\u4e92\u4f5c\u7528\uff0c\u6709\u52a9\u4e8e\u964d\u4f4e\u8131\u6eb6\u5242\u5316\u80fd\u5792\uff08\u56fe2a-b\uff09\u3002\u4f5c\u8005\u8ba4\u4e3a<strong>Cl<\/strong><strong><sup><strong><sup>\u2212<\/sup><\/strong><\/sup><\/strong><strong>\u8fdb\u5165Al<\/strong><strong><sup><strong><sup>3+<\/sup><\/strong><\/sup><\/strong><strong>\u6eb6\u5242\u5316\u9798\u5c42\u540e\u63d0\u5347\u4e86\u6eb6\u5242\u5316\u7269\u79cd\u7684\u6613\u6781\u5316\u80fd\u529b\u3002<\/strong>\u5177\u4f53\u800c\u8a00\uff0c\u6709\u673a\u53cc\u6c2f\u9633\u79bb\u5b50AlCl<sub>2<\/sub>(DPE)<sub>2<\/sub><sup>+<\/sup>\u76f8\u6bd4\u4e8e\u5176\u4ed6Al(solvent)<sub>6<\/sub><sup>3+<\/sup>\u548cAlCl<sub>4<\/sub><sup>\u2212<\/sup>\u4f4e\u6d3b\u6027\u7269\u79cd\u5177\u6709\u66f4\u9ad8\u7684\u5076\u6781\u77e9\uff08\u56fe2c\uff09\uff0c\u8bf4\u660e\u9798\u5c42\u5185\u6b63\u8d1f\u7535\u8377\u4e2d\u5fc3\u7684\u504f\u79fb\u7a0b\u5ea6\u66f4\u5927\uff0c\u8868\u73b0\u51fa\u66f4\u5f3a\u7684\u6613\u6781\u5316\u6027\u8d28\uff0c\u56e0\u6b64\u66f4\u6709\u5229\u4e8e\u5b9e\u73b0\u754c\u9762\u7535\u8377\u5feb\u901f\u8f6c\u79fb\uff0c\u8fdb\u800c\u5b9e\u73b0\u9ad8\u6548\u94dd\u6c89\u79ef\u3002<\/p>\n\n\n\n<p>\u8981\u70b93 &nbsp;\u94dd\u8d1f\u6781\u7684\u7535\u5316\u5b66\u6027\u80fd<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"500\" height=\"702\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2025\/12\/7f88dbbcaa77a1d-4.png\" alt=\"\" class=\"wp-image-269761\"\/><\/figure>\n\n\n\n<p>\u56fe3 \u94dd\u7535\u6781\u5728\u201c\u6709\u673a\u53cc\u6c2f\u201d\u7535\u89e3\u6db2\u4e2d\u7684\u7535\u5316\u5b66\u6027\u80fd<\/p>\n\n\n\n<p>\u5f97\u76ca\u4e8eAlCl<sub>2<\/sub>(DPE)<sub>2<\/sub><sup>+<\/sup>\u9633\u79bb\u5b50\u7684\u9ad8\u5ea6\u6613\u6781\u5316\u6027\u8d28\uff0cAlCl<sub>3<\/sub>\/DPE\u7535\u89e3\u6db2\u57280.2 mA cm<sup>\u22122<\/sup>\u7535\u6d41\u5bc6\u5ea6\u4e0b\u5b9e\u73b0\u4e86\u4f4e\u4e14\u7a33\u5b9a\u7684\u94dd\u6c89\u79ef\u8fc7\u7535\u4f4d~120 mV\uff0c\u5e76\u8868\u73b0\u51fa\u5747\u5300\u81f4\u5bc6\u7684\u94dd\u6c89\u79ef\u884c\u4e3a\uff08\u56fe3a-b\uff09\u3002\u91c7\u7528AlCl<sub>3<\/sub>\/DPE\u7535\u89e3\u6db2\u7684Al\/\/Al\u5bf9\u79f0\u7535\u6c60\u57280.1 mAh cm<sup>\u22122<\/sup>\u4e0b\u5c55\u73b0\u51fa\u8d85\u8fc72000 h\u7684\u957f\u5faa\u73af\u5bff\u547d\uff0c\u6027\u80fd\u8fdc\u4f18\u4e8eAlCl<sub>3<\/sub>\/ACN\u548cAlCl<sub>3<\/sub>\/PC\u4f53\u7cfb\uff08\u56fe3c\uff09\uff0c\u5e76\u80fd\u57282 mA cm<sup>\u22122<\/sup>\u7684\u9ad8\u7535\u6d41\u5bc6\u5ea6\u4e0b\u7a33\u5b9a\u5de5\u4f5c\uff08\u56fe3d\uff09\u3002\u503c\u5f97\u6ce8\u610f\u7684\u662f\uff0c\u91c7\u7528AlCl<sub>3<\/sub>\/DPE\u7535\u89e3\u6db2\u7684Al\/\/Cu\u975e\u5bf9\u79f0\u7535\u6c60\uff0c\u57282 mAh cm<sup>\u22122<\/sup>\u7684\u5927\u9762\u79ef\u5bb9\u91cf\u4e0b\u7a33\u5b9a\u5e93\u4ed1\u6548\u7387\u9ad8\u8fbe~99.85%\uff08\u56fe3e\uff09\u3002\u4e0a\u8ff0\u7ed3\u679c\u8868\u660e\uff0c<strong>\u542b<\/strong><strong>\u201c\u6709\u673a\u53cc\u6c2f\u201d<\/strong><strong>AlCl<\/strong><strong><sub><strong><sub>2<\/sub><\/strong><\/sub><\/strong><strong>(DPE)<\/strong><strong><sub><strong><sub>2<\/sub><\/strong><\/sub><\/strong><strong><sup><strong><sup>+<\/sup><\/strong><\/sup><\/strong><strong>\u9633\u79bb\u5b50\u7684AlCl<\/strong><strong><sub><strong><sub>3<\/sub><\/strong><\/sub><\/strong><strong>\/DPE\u7535\u89e3\u6db2<\/strong><strong>\u6210\u529f<\/strong><strong>\u5b9e\u73b0\u9ad8\u5ea6\u7a33\u5b9a\u4e14\u53ef\u9006\u7684\u94dd\u6c89\u79ef<\/strong><strong>\/\u6eb6\u89e3<\/strong><strong>\u3002<\/strong><strong><\/strong><\/p>\n\n\n\n<p>\u8981\u70b94 \u7535\u89e3\u6db2\u8150\u8680\u6027\u8868\u5f81<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"500\" height=\"523\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2025\/12\/4e9a0ba2491dfde-3.png\" alt=\"\" class=\"wp-image-269762\"\/><\/figure>\n\n\n\n<p>\u56fe4 \u7535\u89e3\u6db2\u8150\u8680\u6027\u8868\u5f81<\/p>\n\n\n\n<p>\u8150\u8680\u6027\u8bc4\u4f30\u5b9e\u9a8c\u663e\u793a\uff0c\u4e0d\u9508\u94a2\u96c6\u6d41\u4f53\u5728\u201c\u6709\u673a\u53cc\u6c2f\u201d\u7535\u89e3\u6db2\u4e2d\u6d78\u6ce190\u5929\u540e\u8868\u9762\u4f9d\u7136\u5149\u4eae\u5982\u65b0\uff0c\u65e0\u660e\u663e\u8150\u8680\u8ff9\u8c61\uff1b\u76f8\u6bd4\u4e4b\u4e0b\uff0c\u4f20\u7edf\u7684\u6c2f\u94dd\u9178\u76d0\u79bb\u5b50\u6db2\u4f53\u5728\u77ed\u77ed2\u5929\u5185\u5c31\u5bfc\u81f4\u4e0d\u9508\u94a2\u4e25\u91cd\u8150\u8680\uff08\u56fe4a-c\uff09\u3002\u7535\u5316\u5b66\u6d4b\u8bd5\u7ed3\u679c\u8868\u660e\uff0c\u4e0d\u9508\u94a2\u5728\u201c\u6709\u673a\u53cc\u6c2f\u201d\u7535\u89e3\u6db2\u4e2d\u7684\u8150\u8680\u7535\u6d41\u5bc6\u5ea6\u4ec5\u4e3a2.8\u00d710<sup>\u2212<\/sup><sup>3<\/sup>&nbsp;mA&nbsp;cm<sup>\u22122<\/sup>\uff0c\u6bd4\u79bb\u5b50\u6db2\u4f53\u4e2d\u4f4e\u4e24\u4e2a\u6570\u91cf\u7ea7\u3002\u5373\u4f7f\u57282 V vs. Al<sup>3+<\/sup>\/Al\u7684\u9ad8\u7535\u4f4d\u4e0b\uff0c\u4e0d\u9508\u94a2\u7535\u6781\u5728AlCl<sub>3<\/sub>\/DPE\u7535\u89e3\u6db2\u4e2d\u4ecd\u8868\u73b0\u51fa\u5353\u8d8a\u7684\u7a33\u5b9a\u6027\u3002\u6709\u673a\u7535\u89e3\u6db2\u663e\u8457\u964d\u4f4e\u7684\u8150\u8680\u6027\u53ef\u80fd\u6e90\u4e8eAlCl<sub>3<\/sub>\u76d0\u7528\u91cf\u7684\u5927\u5e45\u51cf\u5c11\uff0c\u5176AlCl<sub>3<\/sub>\u76d0\u7528\u91cf\u4ec5\u4e3a\u4f20\u7edf\u79bb\u5b50\u6db2\u4f53\u4f53\u7cfb\u7684\u7ea655 wt%\u3002\u6709\u8da3\u7684\u662f\uff0c<strong>\u91c7\u7528\u76f8\u540c<\/strong>AlCl<sub>3<\/sub><strong>\u6d53\u5ea6\u7684\u4e0d\u540c\u7684\u6709\u673a\u7535\u89e3\u6db2\u4e5f\u8868\u73b0\u51fa\u660e\u663e\u7684\u8150\u8680\u6027\u5dee\u5f02<\/strong>\uff0c\u5176\u4e2dAlCl<sub>3<\/sub>\/DPE\u7535\u89e3\u6db2\u5177\u6709\u6700\u4f4e\u7684\u8150\u8680\u6027\u3002\u901a\u8fc7\u6838\u78c1\u7b49\u8868\u5f81\u53d1\u73b0\uff0cAlCl<sub>3<\/sub>\/PC\u548cAlCl<sub>3<\/sub>\/ACN\u7535\u89e3\u6db2\u4e2d\u5b58\u5728\u81ea\u7531Cl<sup>\u2212<\/sup>\u79bb\u5b50\uff0c\u800cAlCl<sub>3<\/sub>\/DPE\u4e2d\u5374\u6ca1\u6709\u81ea\u7531Cl<sup>\u2212<\/sup>\u79bb\u5b50\u5b58\u5728\uff0c\u8fd9\u6e90\u4e8e\u4e0d\u540c\u6eb6\u5242\u7684\u6eb6\u5242\u5316\u80fd\u529b\u5dee\u5f02\u5bfc\u81f4\u7684\u7535\u89e3\u6db2\u6eb6\u5242\u5316\u7ed3\u6784\u5dee\u5f02\u3002\u5177\u4f53\u800c\u8a00\uff0c\u5177\u6709\u5f3a\u6eb6\u5242\u5316\u80fd\u529b\u7684PC\u3001ACN\u6eb6\u5242\uff0c\u5728\u6eb6\u5242\u5316\u8fc7\u7a0b\u4e2d\u5bf9Cl<sup>\u2212<\/sup>\u7684\u7ade\u4e89\u6027\u6700\u5f3a\uff0c\u5265\u593a\u4e86Al<sub>2<\/sub>Cl<sub>6<\/sub>\u76d0\u5468\u56f4\u7684Cl<sup>\u2212<\/sup>\uff0c\u5bfc\u81f4\u66f4\u591a\u7684\u81ea\u7531Cl<sup>\u2212<\/sup>\u79bb\u5b50\u5b58\u5728\u3002\u76f8\u6bd4\u4e4b\u4e0b\uff0c\u5177\u6709\u9002\u5b9c\u6eb6\u5242\u5316\u80fd\u529b\u7684DPE\u5206\u5b50\u5728\u8bf1\u5bfcAl<sub>2<\/sub>Cl<sub>6<\/sub>\u76d0\u4e0d\u5bf9\u79f0\u88c2\u5206\u8fc7\u7a0b\u4e2d\u540c\u65f6\u5f62\u6210\u4e86\u201c\u6709\u673a\u53cc\u6c2f\u201dAlCl<sub>2<\/sub>(DPE)<sub>2<\/sub><sup>+<\/sup>\u9633\u79bb\u5b50\u548cAlCl<sub>4<\/sub><sup>\u2212<\/sup>\u9634\u79bb\u5b50\uff0c\u4ece\u800c<strong>\u5c06\u6240\u6709\u8150\u8680\u6027\u7684Cl<\/strong><strong><sup><strong><sup>\u2212<\/sup><\/strong><\/sup><\/strong><strong>\u79bb\u5b50\u201c\u9650\u57df\u201d\u4e8eAl<\/strong><strong><sup><strong><sup>3+<\/sup><\/strong><\/sup><\/strong><strong>\u5468\u56f4\uff0c\u6700\u7ec8\u6784\u5efa\u4e86\u65e0\u8150\u8680\u6709\u673a\u7535\u89e3\u6db2\u3002<\/strong><\/p>\n\n\n\n<p>\u8981\u70b95 &nbsp;Al\/\/Mo<sub>6<\/sub>S<sub>8<\/sub>\u5168\u7535\u6c60\u7535\u5316\u5b66\u6027\u80fd<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"500\" height=\"577\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2025\/12\/b14210e1ee30421-2.png\" alt=\"\" class=\"wp-image-269763\"\/><\/figure>\n\n\n\n<p>\u56fe5 | \u5168\u7535\u6c60\u6027\u80fd<a>\u4e0e\u50a8\u80fd\u673a\u5236<\/a><\/p>\n\n\n\n<p>\u6700\u540e\uff0c\u4f5c\u8005\u91c7\u7528Mo<sub>6<\/sub>S<sub>8<\/sub>\u6b63\u6781\u4e0eAl\u8d1f\u6781\u5339\u914d\u7ec4\u88c5\u4e86\u5168\u7535\u6c60\u539f\u578b\u5668\u4ef6\uff0c\u4ee5\u63a2\u7a76AlCl<sub>3<\/sub>\/DPE\u7535\u89e3\u6db2\u4e0e\u6b63\u6781\u7684\u517c\u5bb9\u6027\u548c\u5728\u5168\u7535\u6c60\u4e2d\u7684\u9002\u7528\u6027\u3002\u5f97\u76ca\u4e8e\u5176\u72ec\u7279\u7684\u6613\u8131\u6eb6AlCl<sub>2<\/sub>(DPE)<sub>2<\/sub><sup>+<\/sup>\u9633\u79bb\u5b50\uff0c\u91c7\u7528AlCl<sub>3<\/sub>\/DPE\u7535\u89e3\u6db2Mo<sub>6<\/sub>S<sub>8<\/sub>\/\/Al\u5168\u7535\u6c60\u663e\u793a\u51fa\u6700\u9ad8\u7684\u6bd4\u5bb9\u91cf\u548c\u6700\u5c0f\u7684\u7535\u538b\u4e4b\u540e\uff08\u56fe5a\uff09\u3002<sup>27<\/sup>Al\u8c31\u56fa\u4f53\u6838\u78c1\u8bc1\u5b9e\u4e86Al<sup>3+<\/sup>\u5728Mo<sub>6<\/sub>S<sub>8<\/sub>\u4e2d\u7684\u53ef\u9006\u5d4c\u5165\/\u8131\u51fa\uff08\u56fe5b\uff09\uff0c\u5e76\u5b9e\u73b0\u7a33\u5b9a\u5faa\u73af\uff0c300\u6b21\u5faa\u73af\u540e\u5bb9\u91cf\u4fdd\u6301\u7387\u7ea6\u4e3a75%\uff08\u56fe5c\uff09\uff0c\u8868\u660e\u8be5\u7535\u89e3\u6db2\u4e0eAl\u8d1f\u6781\u548c\u6b63\u6781\u5747\u5177\u6709\u51fa\u8272\u7684\u517c\u5bb9\u6027\u3002<\/p>\n\n\n\n<p>\u603b\u7ed3\u4e0e\u5c55\u671b<\/p>\n\n\n\n<p>\u8be5\u7814\u7a76\u7a81\u7834\u4f20\u7edf\u201c\u552f\u9634\u79bb\u5b50\u201d\u6d3b\u6027\u7269\u79cd\u7684\u7535\u89e3\u6db2\u8bbe\u8ba1\u6846\u67b6\uff0c\u63d0\u51fa\u4e86\u201c\u6709\u673a\u53cc\u6c2f\u201d\u9633\u79bb\u5b50AlCl<sub>2<\/sub>(DPE)<sub>2<\/sub><sup>+<\/sup>\u4e3a\u6d3b\u6027\u79bb\u5b50\u7684\u7535\u89e3\u6db2\u8bbe\u8ba1\u65b0\u601d\u8def\uff0c\u8fd9\u79cd\u5355\u4ef7\u7684\u9633\u79bb\u5b50\u6eb6\u5242\u5316\u7ed3\u6784\u5177\u6709\u9ad8\u5ea6\u6613\u6781\u5316\u7279\u6027\uff0c\u4e0d\u4ec5\u6709\u5229\u4e8e\u8131\u6eb6\u5242\u8fc7\u7a0b\uff0c\u8fd8\u80fd\u6709\u6548\u675f\u7f1a\u8150\u8680\u6027\u6e38\u79bbCl<sup>\u2212<\/sup>\u79bb\u5b50\uff0c\u6709\u6548\u89e3\u51b3\u4f20\u7edf\u9634\u79bb\u5b50\u7269\u79cd\u7535\u89e3\u6db2\u7684\u5f3a\u8150\u8680\u6027\u96be\u9898\u3002\u6b64\u5916\uff0c\u6709\u673a\u53cc\u6c2f\u7535\u89e3\u6db2\u540c\u65f6\u89e3\u51b3\u4e86\u4f20\u7edf\u9634\u79bb\u5b50\u7535\u89e3\u6db2\u5728\u4f20\u8d28\u4e0e\u53cd\u5e94\u52a8\u529b\u5b66\u4e4b\u95f4\u7684\u56fa\u6709\u77db\u76fe\uff1a\u4f9d\u8d56Al<sub>2<\/sub>Cl<sub>7<\/sub><sup>\u2212<\/sup>\u8fd8\u539f\u6c89\u79ef\u4e0eAlCl<sub>4<\/sub><sup>\u2212<\/sup>\u5d4c\u5165\u6b63\u6781\u7684\u9634\u79bb\u5b50\u53cd\u5e94\u8def\u5f84\uff0c\u800c\u975e\u542bAl\u9633\u79bb\u5b50\u53c2\u4e0e\u7684\u7535\u5316\u5b66\u8fc7\u7a0b\u3002\u8be5\u673a\u5236\u5bfc\u81f4\u6bcf\u8f6c\u79fb3\u4e2a\u7535\u5b50\u9700\u6d88\u80178\u4e2a\u94dd\u539f\u5b50\uff0c\u4e25\u91cd\u9650\u5236\u4e86\u5b9e\u9645\u80fd\u91cf\u5bc6\u5ea6\uff08\u56fe5d\uff09\uff1b\u540c\u65f6\uff0c\u5e26\u8d1f\u7535\u7684\u7535\u6d3b\u6027\u7269\u8d28\u8fc1\u79fb\u65b9\u5411\u4e0e\u7535\u573a\u65b9\u5411\u76f8\u6096\uff0c\u52a0\u5267\u6d53\u5dee\u6781\u5316\u3002\u8be5\u7814\u7a76\u63d0\u51fa\u7684\u201c\u6709\u673a\u53cc\u6c2f\u201d\u9633\u79bb\u5b50AlCl<sub>2<\/sub>(DPE)<sub>2<\/sub><sup>+<\/sup>\u4f5c\u4e3a\u8f7d\u6d41\u5b50\u663e\u8457\u63d0\u9ad8\u4e86\u94dd\u79bb\u5b50\u8131\u6eb6\u5242\u5316\u6548\u7387\uff08<strong>\u6bcf\u94dd\u539f\u5b50\u53ef\u5229\u7528\u7535\u5b50\u6570\u4ece0.375\u4e2a\u5927\u5e45\u63d0\u5347\u4e09\u500d\u81f31.5\u4e2a<\/strong>\uff09\uff0c\u540c\u65f6\u7531\u4e8e\u5176\u8fc1\u79fb\u65b9\u5411\u4e0e\u7535\u573a\u65b9\u5411\u4e00\u81f4\uff0c\u786e\u4fdd\u4e86\u6d3b\u6027\u9633\u79bb\u5b50\u7684\u5feb\u901f\u9ad8\u6548\u8865\u5145\uff0c\u63d0\u5347\u4e86\u4f20\u8d28\u52a8\u529b\u5b66\uff08\u56fe5e\uff09\u3002\u8be5\u5de5\u4f5c\u4e0d\u4ec5\u63d0\u4f9b\u4e86\u4e00\u79cd\u65b0\u578b\u7535\u89e3\u6db2\u914d\u65b9\uff0c\u66f4\u5f00\u521b\u4e86\u57fa\u4e8e\u9633\u79bb\u5b50\u6d3b\u6027\u7269\u79cd\u7684\u94dd\u6c89\u79ef\/\u6eb6\u89e3\u5168\u65b0\u7535\u5316\u5b66\u8def\u5f84\uff0c\u4e3a\u89e3\u51b3\u94dd\u91d1\u5c5e\u7535\u6c60\u4e43\u81f3\u5176\u4ed6\u591a\u4ef7\u91d1\u5c5e\u7535\u6c60\u4e2d\u7684\u8150\u8680\u3001\u52a8\u529b\u5b66\u7f13\u6162\u3001\u4f20\u8d28\u53d7\u963b\u7b49\u5171\u6027\u96be\u9898\u63d0\u4f9b\u4e86\u65b0\u7684\u601d\u8def\u3002<\/p>\n\n\n\n<p><strong>\u3010\u56e2\u961f\u4ecb\u7ecd\u3011<\/strong><\/p>\n\n\n\n<p><strong>\u6768\u5168\u7ea2<\/strong>\uff0c\u5929\u6d25\u5927\u5b66\u5316\u5de5\u5b66\u9662\u5317\u6d0b\u8bb2\u5e2d\u6559\u6388\uff0c\u535a\u58eb\u751f\u5bfc\u5e08\u3002\u7b2c\u5341\u56db\u5c4a\u5168\u56fd\u653f\u534f\u59d4\u5458\uff0c\u4e2d\u56fd\u5316\u5de5\u5b66\u4f1a\u4f1a\u58eb\uff0c\u56fd\u5bb6\u6770\u9752\u3001\u957f\u6c5f\u5b66\u8005\u3001\u4e07\u4eba\u9886\u519b\uff0c\u56fd\u5bb6\u91cd\u70b9\u7814\u53d1\u8ba1\u5212\u9996\u5e2d\u79d1\u5b66\u5bb6\u3001\u5929\u6d25\u5e02\u5148\u8fdb\u78b3\u4e0e\u7535\u5316\u5b66\u50a8\u80fd\u91cd\u70b9\u5b9e\u9a8c\u5ba4\u4e3b\u4efb\u3001\u79d1\u777f\u552f\u5b89\u5168\u7403\u9ad8\u88ab\u5f15\u79d1\u5b66\u5bb6\u3002\u957f\u671f\u4ece\u4e8b\u78b3\u529f\u80fd\u6750\u6599\u3001\u5148\u8fdb\u7535\u6c60\u3001\u50a8\u80fd\u6280\u672f\u548c\u53cc\u78b3\u6218\u7565\u7814\u7a76\uff0c\u5f15\u9886\u4e86\u81f4\u5bc6\u50a8\u80fd\u3001\u9502\u786b\u50ac\u5316\u3001\u7b5b\u5206\u50a8\u80fd\u7b49\u7814\u7a76\u65b9\u5411\u3002\u53d1\u8868SCI\u8bba\u6587400\u4f59\u7bc7\uff0c\u4ed6\u4eba\u5f15\u752860,000\u4f59\u6b21\uff0cH\u56e0\u5b50128\u3002\u6388\u6743\u4e2d\u56fd\u548c\u56fd\u9645\u53d1\u660e\u4e13\u522960\u4f59\u4ef6\u3002\u83b7\u56fd\u5bb6\u6280\u672f\u53d1\u660e\u4e8c\u7b49\u5956\u3001\u5929\u6d25\u5e02\u81ea\u7136\u79d1\u5b66\u4e00\u7b49\u5956\uff08\u4e24\u9879\uff09\u7b49\u5956\u9879\u3002\u62c5\u4efb\u300aEnergy Storage Materials\u300b\u7b493\u4efd\u671f\u520a\u526f\u4e3b\u7f16\uff0c\u300aAdvanced Energy Materials\u300b\u3001\u300aNational Science Review\u300b\u7b4910\u4f59\u4efd\u520a\u7269\u7f16\u8f91\u7ec4\u6210\u5458\u6216\u7f16\u59d4\u3002<\/p>\n\n\n\n<p><strong>\u7fc1\u54f2<\/strong>\uff0c\u5929\u6d25\u5927\u5b66\u5316\u5de5\u5b66\u9662\uff0c\u83c1\u82f1\u6559\u6388\uff0c\u535a\u58eb\u751f\u5bfc\u5e08\uff0c\u5165\u9009\u56fd\u5bb6\u9ad8\u5c42\u6b21\u6d77\u5916\u9752\u5e74\u4eba\u624d\u8ba1\u5212\u3002\u4e3b\u8981\u4ece\u4e8b\u950c\u79bb\u5b50\u7535\u6c60\u3001\u7535\u50ac\u5316\u4e8c\u6c27\u5316\u78b3\u8fd8\u539f\u7b49\u7535\u5316\u5b66\u5de5\u7a0b\u5e94\u7528\u65b9\u5411\uff0c\u805a\u7126\u5176\u4e2d\u7535\u5316\u5b66\u754c\u9762\u7684\u8fc7\u7a0b\u5f3a\u5316\u7814\u7a76\uff0c\u5305\u62ec\u754c\u9762\u7684\u52a8\u6001\u6f14\u53d8\u673a\u5236\u3001\u5b9a\u5236\u5316\u8bbe\u8ba1\u4ee5\u53ca\u539f\u4f4d\u6784\u7b51\u3002\u5728Nat Sustain, Nat Commun, J Am Chem Soc, Angew Chem Int Ed, Adv Mater, Energy Environ Sci\u7b49\u56fd\u9645\u6743\u5a01\u5b66\u672f\u671f\u520a\u53d1\u8868SCI\u4e00\u533a\u8bba\u658750\u4f59\u7bc7\uff0c\u88ab\u4ed6\u5f159600\u4f59\u6b21\uff0c\u6388\u6743\u53d1\u660e\u4e13\u52297\u4ef6\uff0c\u53c2\u4e0e\u5236\u5b9a\u6c34\u7cfb\u91d1\u5c5e\u79bb\u5b50\u7535\u6c60\u56e2\u4f53\u6807\u51c62\u9879\uff1b\u83b72024\u5e74\u5929\u6d25\u5e02\u81ea\u7136\u79d1\u5b66\u4e00\u7b49\u59561\u9879\uff08\u6392\u540d\u7b2c\u4e09\uff09\u30012024\u5e74\u4e2d\u56fd\u9752\u5e74\u79d1\u6280\u5956\u5929\u6d25\u5e02\u63d0\u540d\uff1b\u4e3b\u6301\u56fd\u5bb6\u91cd\u70b9\u7814\u53d1\u8ba1\u5212\u8bfe\u9898\u3001\u56fd\u5bb6\u81ea\u7136\u79d1\u5b66\u57fa\u91d1\u9762\u4e0a\u9879\u76ee\u3001\u5929\u6d25\u5e02\u81ea\u7136\u57fa\u91d1\u9762\u4e0a\u9879\u76ee\u7b49\u591a\u9879\u7701\/\u90e8\u7ea7\u9879\u76ee\uff1b\u4efbJournal of Electrochemistry\uff08\u7535\u5316\u5b66\uff09\u3001Renewables\u3001Materials Reports Energy\u3001Green Carbon\u7b49\u671f\u520a\u9752\u5e74\u7f16\u59d4\u3002<\/p>\n\n\n\n<p><strong>\u97e9\u5927\u91cf<\/strong>\uff0c\u5929\u6d25\u5927\u5b66\u5316\u5de5\u5b66\u9662\u526f\u7814\u7a76\u5458\uff0c\u535a\u58eb\u751f\u5bfc\u5e08\uff0c\u5165\u9009\u56fd\u5bb6\u7ea7\u9752\u5e74\u4eba\u624d\u652f\u6301\u8ba1\u5212\u3002\u4e3b\u8981\u4ece\u4e8b\u6c34\u7cfb\u548c\u591a\u4ef7\u91d1\u5c5e\u7535\u6c60\u76f8\u5173\u7814\u7a76\uff0c\u4ee5\u7b2c\u4e00\/\u901a\u8baf\uff08\u542b\u5171\u540c\uff09\u4f5c\u8005\u5728Nat. Sustain.\u3001Nat. Commun.\u3001Adv. Mater.\u3001Angew. Chem. Int. Ed.\u3001Energy Environ. Sci.\u3001Adv. Energy Mater.\u3001Chem\u3001Energy Storage Mater.\u7b49\u9ad8\u6c34\u5e73\u671f\u520a\u53d1\u8868\u8bba\u658720\u4f59\u7bc7\uff0c\u88ab\u5f154300\u4f59\u6b21\uff1b\u83b7\u5929\u6d25\u5e02\u81ea\u7136\u79d1\u5b66\u4e00\u7b49\u5956\u3001Nano Research Energy\u5b66\u672f\u65b0\u661f\u91d1\u5956\u7b49\u8363\u8a89\uff1b\u4e3b\u6301\u56fd\u5bb6\u81ea\u7136\u79d1\u5b66\u57fa\u91d1\u9762\u4e0a\u548c\u9752\u5e74\u9879\u76ee\u3001\u56fd\u5bb6\u91cd\u70b9\u7814\u53d1\u8ba1\u5212\u5b50\u8bfe\u9898\u3001\u4e2d\u56fd\u535a\u58eb\u540e\u79d1\u5b66\u57fa\u91d1\u7279\u522b\u8d44\u52a9\u9879\u76ee\u548c\u9762\u4e0a\u9879\u76ee\u3001\u5929\u6d25\u5e02\u81ea\u7136\u79d1\u5b66\u57fa\u91d1\u7b49\u591a\u9879\u57fa\u91d1\uff1b\u62c5\u4efbeScience\u3001Energy Materials and Devices\u3001Nano-Micro Letters\u3001Carbon Neutralization\u7b49\u591a\u4efd\u671f\u520a\u9752\u5e74\u7f16\u59d4\u3002<\/p>\n\n\n\n<p>\u539f\u6587\u94fe\u63a5\uff1a<\/p>\n\n\n\n<p><a href=\"https:\/\/www.nature.com\/articles\/s41893-025-01706-6\">https:\/\/www.nature.com\/articles\/s41893-025-01706-6<\/a><\/p>\n\n\n\n<p>NanoYang\u8bfe\u9898\u7ec4\u7f51\u7ad9\uff1a<\/p>\n\n\n\n<p><a href=\"http:\/\/nanoyang.tju.edu.cn\/\"><u>http:\/\/nanoyang.tju.edu.cn\/<\/u><\/a><\/p>\n\n\n\n<p><strong>\u3010\u56e2\u961f\u62db\u8058\u3011<\/strong><\/p>\n\n\n\n<p>\u56e2\u961f\u5e38\u5e74\u62db\u6536\u4ee5\u4e0b\u4e13\u4e1a\u80cc\u666f\u7684\u7855\u58eb\u3001\u535a\u58eb\u7814\u7a76\u751f\uff0c\u4ee5\u53ca\u535a\u58eb\u540e\uff1a\u5316\u5b66\uff08\u6709\u673a\u3001\u9ad8\u5206\u5b50\u3001\u7269\u7406\u5316\u5b66\u3001\u5206\u6790\u5316\u5b66\uff09\u3001\u7535\u5316\u5b66\u3001\u6750\u6599\u5b66\u3001\u5316\u5de5\u3001\u7269\u7406\u3001\u50ac\u5316\u548c\u8868\u754c\u9762\u5316\u5b66\u7b49\uff0c\u5177\u6709\u7535\u5316\u5b66\u3001\u7406\u8bba\u8ba1\u7b97\u3001\u540c\u6b65\u8f90\u5c04\u6216\u5176\u4ed6\u539f\u4f4d\u7535\u5316\u5b66\u8868\u5f81\u7ecf\u9a8c\u8005\u4f18\u5148\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>Harvey \u7b2c\u4e00\u4f5c\u8005\uff1a\u5f20\u6e24\uff0c\u674e\u6cbb\u56fd\uff0c\u97e9\u5927\u91cf\uff0c\u95f5\u5fd7\u96ef \u901a\u8baf\u4f5c\u8005\uff1a\u6768\u5168\u7ea2\uff0c\u7fc1\u54f2\uff0c\u97e9\u5927\u91cf \u901a\u8baf\u5355\u4f4d\uff1a\u5929\u6d25\u5927\u5b66 DOI: 10.1038\/s41893-025-017&#8230;<\/p>\n","protected":false},"author":31345,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[2],"tags":[],"class_list":["post-269758","post","type-post","status-publish","format-standard","hentry","category-keji"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/269758"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/31345"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=269758"}],"version-history":[{"count":1,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/269758\/revisions"}],"predecessor-version":[{"id":269764,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/269758\/revisions\/269764"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=269758"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=269758"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=269758"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}