{"id":270445,"date":"2026-01-23T09:44:48","date_gmt":"2026-01-23T01:44:48","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=270445"},"modified":"2026-01-23T09:45:12","modified_gmt":"2026-01-23T01:45:12","slug":"%e4%b8%ad%e7%a7%91%e9%99%a2%e7%89%a9%e7%90%86%e6%89%80%e9%99%a2%e5%a3%ab%e5%9b%a2%e9%98%9f%e6%9c%80%e6%96%b0science","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=270445","title":{"rendered":"\u4e2d\u79d1\u9662\u7269\u7406\u6240\u9662\u58eb\u56e2\u961f\u6700\u65b0Science"},"content":{"rendered":"\n<h2 class=\"wp-block-heading\"><strong>\u4e00\u3001\u3010\u79d1\u5b66\u80cc\u666f\u3011<\/strong><\/h2>\n\n\n\n<p>\u5728\u94c1\u7535\u4f53\u7eb3\u7c73\u7535\u5b50\u5b66\u9886\u57df\uff0c\u5e26\u7535\u7574\u58c1\uff08CDWs\uff09\u4f5c\u4e3a\u5177\u6709\u72ec\u7279\u7535\u3001\u78c1\u529f\u80fd\u7684\u4e8c\u7ef4\u6216\u51c6\u4e8c\u7ef4\u62d3\u6251\u7f3a\u9677\uff0c\u662f\u201c\u58c1\u5373\u5668\u4ef6\u201d\u7406\u5ff5\u7684\u6838\u5fc3\u6d3b\u6027\u5355\u5143\uff0c\u5728\u975e\u6613\u5931\u6027\u5b58\u50a8\u548c\u903b\u8f91\u5668\u4ef6\u4e2d\u5177\u6709\u91cd\u8981\u5e94\u7528\u6f5c\u529b\u3002\u7136\u800c\uff0c\u4f20\u7edf\u94c1\u7535\u4f53\u591a\u4e3a\u4e09\u7ef4\u6676\u4f53\u7ed3\u6784\uff0c\u5bfc\u81f4\u7574\u58c1\u96be\u4ee5\u7a81\u7834\u4e8c\u7ef4\u7ef4\u5ea6\u9650\u5236\uff0c\u5236\u7ea6\u4e86\u5668\u4ef6\u96c6\u6210\u5bc6\u5ea6\u7684\u8fdb\u4e00\u6b65\u63d0\u5347\u3002\u6c1f\u77f3\u578b\u94c1\u7535\u4f53\uff08\u5982ZrO<sub>2<\/sub>\uff09\u867d\u5177\u5907\u4ea4\u66ff\u6392\u5217\u7684\u4e8c\u7ef4\u6781\u6027\u5c42\u4e0e\u975e\u6781\u6027\u95f4\u9694\u5c42\u72ec\u7279\u7ed3\u6784\uff0c\u76f8\u90bb\u6781\u6027\u4e9a\u80de\u95f4\u76f8\u4e92\u4f5c\u7528\u6781\u5f31\uff0c\u4e3a\u5b9e\u73b0\u7574\u58c1\u7684\u4e00\u7ef4\u9650\u57df\u63d0\u4f9b\u4e86\u6f5c\u5728\u4f53\u7cfb\uff0c\u4f46\u6b64\u524d\u4e00\u7ef4\u5e26\u7535\u7574\u58c1\u7684\u5b58\u5728\u7f3a\u4e4f\u5b9e\u9a8c\u8bc1\u5b9e\uff0c\u4e14\u7406\u8bba\u9884\u6d4b\u5176\u56e0\u6781\u9ad8\u7684\u675f\u7f1a\u6781\u5316\u7535\u8377\u5bc6\u5ea6\u6613\u53d1\u751f\u80fd\u91cf\u4e0d\u7a33\u5b9a\uff0c\u4f20\u7edf\u4f9d\u8d56\u81ea\u7531\u7535\u5b50\u6216\u7a7a\u7a74\u7684\u7535\u8377\u7b5b\u9009\u673a\u5236\u4e5f\u65e0\u6cd5\u9002\u914d\u5176\u539f\u5b50\u5c3a\u5ea6\u539a\u5ea6\u7684\u9700\u6c42\u3002<\/p>\n\n\n\n<p>\u540c\u65f6\uff0c\u5373\u4fbf\u5047\u8bbe\u4e00\u7ef4\u5e26\u7535\u7574\u58c1\u53ef\u7a33\u5b9a\u5b58\u5728\uff0c\u5176\u4e0e\u94c1\u7535\u4f53\u5173\u952e\u7269\u7406\u8fc7\u7a0b\uff08\u5982\u6781\u5316\u7ffb\u8f6c\u3001\u79bb\u5b50\u8f93\u8fd0\uff09\u7684\u5fae\u89c2\u8026\u5408\u5173\u7cfb\u4ecd\u4e0d\u660e\u786e\uff0c\u4e14\u7531\u4e8e\u7ed3\u6784\u5c3a\u5ea6\u6781\u5c0f\uff0c\u7f3a\u4e4f\u8d85\u9ad8\u5206\u8fa8\u7387\u6280\u672f\u5b9e\u73b0\u5bf9\u5176\u7ed3\u6784\u7279\u5f81\u3001\u7a33\u5b9a\u673a\u5236\u53ca\u52a8\u6001\u884c\u4e3a\u7684\u76f4\u63a5\u89c2\u6d4b\u4e0e\u9a8c\u8bc1\uff0c\u8fd9\u4e9b\u96be\u9898\u90fd\u6210\u4e3a\u5236\u7ea6\u94c1\u7535\u4f53\u5668\u4ef6\u5411\u66f4\u9ad8\u5bc6\u5ea6\u3001\u66f4\u4f18\u6027\u80fd\u53d1\u5c55\u7684\u5173\u952e\u74f6\u9888\u3002<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"1045\" height=\"477\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/01\/0.jpg\" alt=\"\" class=\"wp-image-270446\" \/><\/figure>\n\n\n\n<h2 class=\"wp-block-heading\"><strong>\u4e8c\u3001\u3010\u521b\u65b0\u6210\u679c\u3011<\/strong><\/h2>\n\n\n\n<p>\u4e3a\u89e3\u51b3\u4f20\u7edf\u94c1\u7535\u4f53\u4e2dCDWs\u591a\u4e3a\u4e8c\u7ef4\u7ed3\u6784\u3001\u5668\u4ef6\u96c6\u6210\u5bc6\u5ea6\u53d7\u9650\uff0c\u4e14\u4e00\u7ef4CDWs\u56e0\u7535\u8377\u8865\u507f\u96be\u9898\u7406\u8bba\u4e0a\u96be\u4ee5\u7a33\u5b9a\u5b58\u5728\u7684\u6838\u5fc3\u95ee\u9898\uff0c\u4e2d\u56fd\u79d1\u5b66\u9662\u7269\u7406\u7814\u7a76\u6240<strong>\u845b\u741b\u7814\u7a76\u5458<\/strong>\uff0c<strong>\u91d1\u594e\u5a1f\u9662\u58eb<\/strong>\u548c<strong>\u5f20\u5e86\u534e\u526f\u7814\u7a76<\/strong>\u5458\u4ee5\u5177\u6709\u4ea4\u66ff\u6781\u6027\/\u975e\u6781\u6027\u4e9a\u80de\u7ed3\u6784\u7684\u6c1f\u77f3\u578b\u94c1\u7535\u4f53ZrO\u2082\u4e3a\u7814\u7a76\u4f53\u7cfb\uff0c\u901a\u8fc7\u8109\u51b2\u6fc0\u5149\u6c89\u79ef\u6cd5\u5236\u59075 nm\u539a\u81ea\u652f\u6491\u8584\u819c\uff0c\u5e76\u7ed3\u5408\u8d85\u9ad8\u5206\u8fa8\u7387\u591a\u5c42\u7535\u5b50\u53e0\u5c42\u6210\u50cf\u3001\u96c6\u6210\u5dee\u5206\u76f8\u886c\u626b\u63cf\u900f\u5c04\u7535\u955c\u7b49\u8868\u5f81\u6280\u672f\u4e0e\u539f\u4f4d\u7535\u573a\u64cd\u63a7\u624b\u6bb5\uff0c\u9996\u6b21\u89c2\u6d4b\u5230180\u00b0\u5934\u5bf9\u5934\u548c\u5c3e\u5bf9\u5c3e\u4e24\u79cd\u4e00\u7ef4CDWs\uff0c\u5176\u5bbd\u5ea6\u548c\u539a\u5ea6\u5747\u8fbe\u5230\u539f\u5b50\u5c3a\u5ea6\uff08&lt;2.7 \u00c5\uff09\uff0c\u6253\u7834\u4e86\u7574\u58c1\u5fc5\u4e3a\u4e8c\u7ef4\u7684\u56fa\u6709\u8ba4\u77e5\u3002\u63ed\u793a\u4e86\u72ec\u7279\u7684\u81ea\u5e73\u8861\u6c27\u5360\u4f4d\u7535\u8377\u7b5b\u9009\u673a\u5236\uff0c\u4f7f\u4e00\u7ef4CDWs\u7a33\u5b9a\u5b58\u5728\u3002\u5b9e\u73b0\u4e86\u7535\u573a\u9a71\u52a8\u4e0b\u4e00\u7ef4CDWs\u7684\u521b\u5efa\u3001\u8fd0\u52a8\u4e0e\u64e6\u9664\uff0c\u660e\u786e\u4e86\u6781\u5316\u7ffb\u8f6c\u4e0e\u6c27\u79bb\u5b50\u8de8\u57df\u8f93\u8fd0\u7684\u5fae\u89c2\u8026\u5408\u5173\u7cfb\uff0c\u4e14\u6240\u5236\u5907\u5f02\u8d28\u7ed3\u6784\u5728\u5ba4\u6e29\u4e0b\u5c55\u73b0\u51fa\u4f18\u4e8e\u4f20\u7edf\u56fa\u4f53\u6c27\u5316\u7269\u7535\u89e3\u8d28\u7684\u6c27\u79bb\u5b50\u5bfc\u7535\u6027\uff0c\u4e3a\u4e0b\u4e00\u4ee3\u8d85\u9ad8\u5bc6\u5ea6\u7eb3\u7c73\u7535\u5b50\u5668\u4ef6\u63d0\u4f9b\u4e86\u57fa\u7840\u3002\u8be5\u6210\u679c\u4ee5\u201cObservation of one-dimensional, charged domain walls in ferroelectric ZrO<sub>2<\/sub>\u201d\u4e3a\u9898\u53d1\u8868\u5728\u56fd\u9645\u5b66\u672f\u671f\u520a\u300aScience\u300b\u3002<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"1181\" height=\"685\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/01\/1-2.jpg\" alt=\"\" class=\"wp-image-270448\" \/><\/figure>\n\n\n\n<p>\u56fe1. \u4e00\u7ef4\u7574\u58c1\u7684\u6982\u5ff5\u4e0e\u5b9e\u73b0\u793a\u610f\u56fe\u3002<a>\u00a9 2026 AAAS<\/a><\/p>\n\n\n\n<figure class=\"wp-block-image size-full is-resized\"><img loading=\"lazy\" decoding=\"async\" width=\"1068\" height=\"974\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/01\/2-2.jpg\" alt=\"\" class=\"wp-image-270450\" style=\"width:840px;height:auto\" \/><\/figure>\n\n\n\n<p>\u56fe2. \u4e00\u7ef4\u5e26\u7535\u7574\u58c1\u3002\u00a9 2026 AAAS<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"1269\" height=\"606\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/01\/3-2.jpg\" alt=\"\" class=\"wp-image-270451\" \/><\/figure>\n\n\n\n<p>\u56fe3. \u6c27\u5316\u9506\u4e2d\u4e00\u7ef4H-H\u5e26\u7535\u7574\u58c1\u7684\u8fd0\u52a8\u7279\u6027\u3002\u00a9 2026 AAAS<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"1269\" height=\"699\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/01\/4-2.png\" alt=\"\" class=\"wp-image-270454\" \/><\/figure>\n\n\n\n<p>\u56fe4. \u6c1f\u77f3\u578b\u94c1\u7535\u4f53\u4e2d\u5e26\u7535\u7574\u58c1\u8fd0\u52a8\u4e0e\u6c27\u8f93\u8fd0\u7684\u8026\u5408\u7279\u6027\u3002\u00a9 2026 AAAS<\/p>\n\n\n\n<h2 class=\"wp-block-heading\"><strong>\u4e09\u3001\u3010\u79d1\u5b66\u542f\u8fea\u3011<\/strong><\/h2>\n\n\n\n<p>\u8fd9\u9879\u5de5\u4f5c\u4ee5\u6c1f\u77f3\u578b\u94c1\u7535\u4f53ZrO<sub>2<\/sub>\u4e3a\u7814\u7a76\u4f53\u7cfb\uff0c\u9996\u6b21\u89c2\u6d4b\u5230\u88ab\u9650\u57df\u4e8e\u51762D\u6781\u6027\u5c42\u5185\u3001\u5bbd\u5ea6\u548c\u539a\u5ea6\u5747\u4e3a\u539f\u5b50\u5c3a\u5ea6\uff08&lt;2.7 \u00c5\uff09\u7684180\u00b0\u5934\u5bf9\u5934\uff08H-H\uff09\u548c\u5c3e\u5bf9\u5c3e\uff08T-T\uff09\u4e00\u7ef4\u5e26\u7535\u7574\u58c1\uff0c\u63ed\u793a\u4e86\u5176\u901a\u8fc7\u81ea\u5e73\u8861\u6c27\u5360\u4f4d\u8865\u507f\u675f\u7f1a\u7535\u8377\u7684\u72ec\u7279\u7a33\u5b9a\u673a\u5236\uff0c\u5b9e\u73b0\u4e86\u7535\u573a\u9a71\u52a8\u4e0b\u4e00\u7ef4\u5e26\u7535\u7574\u58c1\u7684\u521b\u5efa\u3001\u8fd0\u52a8\u4e0e\u64e6\u9664\uff0c\u660e\u786e\u4e86\u6781\u5316\u7ffb\u8f6c\u4e0e\u6c27\u79bb\u5b50\u8de8\u57df\u8f93\u8fd0\u7684\u5fae\u89c2\u8026\u5408\u5173\u7cfb\uff0c\u4e14\u6240\u5236\u5907\u7684HZO\/LSMO\/STO\u7b49\u5f02\u8d28\u7ed3\u6784\u5728\u5ba4\u6e29\u4e0b\u5c55\u73b0\u51fa\u4f18\u4e8e\u4f20\u7edf\u56fa\u4f53\u6c27\u5316\u7269\u7535\u89e3\u8d28\u7684\u6c27\u79bb\u5b50\u5bfc\u7535\u6027\uff0c\u4e3a\u4e0b\u4e00\u4ee3\u8d85\u9ad8\u5bc6\u5ea6\u7eb3\u7c73\u7535\u5b50\u5668\u4ef6\u7684\u7814\u53d1\u63d0\u4f9b\u4e86\u57fa\u7840\uff0c\u62d3\u5c55\u4e86\u4f4e\u7ef4\u62d3\u6251\u7f3a\u9677\u5728\u6750\u6599\u79d1\u5b66\u9886\u57df\u7684\u7814\u7a76\u4e0e\u5e94\u7528\u8fb9\u754c\u3002<\/p>\n\n\n\n<p>\u539f\u6587\u4fe1\u606f\uff1aHai Zhong et al. ,Observation of one-dimensional, charged domain walls in ferroelectric ZrO<sub>2<\/sub>. Science 391, 407-411 (2026).<\/p>\n\n\n\n<p><a href=\"https:\/\/www.science.org\/doi\/10.1126\/science.aeb7280\">https:\/\/www.science.org\/doi\/10.1126\/science.aeb7280<\/a><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u4e00\u3001\u3010\u79d1\u5b66\u80cc\u666f\u3011 \u5728\u94c1\u7535\u4f53\u7eb3\u7c73\u7535\u5b50\u5b66\u9886\u57df\uff0c\u5e26\u7535\u7574\u58c1\uff08CDWs\uff09\u4f5c\u4e3a\u5177\u6709\u72ec\u7279\u7535\u3001\u78c1\u529f\u80fd\u7684\u4e8c\u7ef4\u6216\u51c6\u4e8c\u7ef4\u62d3\u6251\u7f3a\u9677\uff0c\u662f\u201c\u58c1\u5373\u5668\u4ef6\u201d\u7406\u5ff5\u7684\u6838\u5fc3\u6d3b\u6027\u5355\u5143\uff0c\u5728\u975e\u6613\u5931\u6027\u5b58\u50a8\u548c\u903b&#8230;<\/p>\n","protected":false},"author":186431,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[2],"tags":[],"class_list":["post-270445","post","type-post","status-publish","format-standard","hentry","category-keji"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/270445"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/186431"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=270445"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/270445\/revisions"}],"predecessor-version":[{"id":270455,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/270445\/revisions\/270455"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=270445"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=270445"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=270445"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}