{"id":272448,"date":"2026-07-14T07:52:46","date_gmt":"2026-07-13T23:52:46","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=272448"},"modified":"2026-07-14T07:52:46","modified_gmt":"2026-07-13T23:52:46","slug":"%e4%b8%9c%e5%8d%8e%e5%a4%a7%e5%ad%a6%e5%86%af%e8%ae%ad%e8%be%be%e8%af%be%e9%a2%98%e7%bb%84%e3%80%8anature-chemical-engineering%e3%80%8b%ef%bc%9a%e6%b5%81%e4%bd%93%e5%a4%b1%e7%a8%b3%e9%a9%b1%e5%8a%a8","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=272448","title":{"rendered":"\u4e1c\u534e\u5927\u5b66\u51af\u8bad\u8fbe\u8bfe\u9898\u7ec4\u300aNature Chemical Engineering\u300b\uff1a\u6d41\u4f53\u5931\u7a33\u9a71\u52a8\u754c\u9762\u805a\u5408\u819c\u7ed3\u6784\u6f14\u5316\u7684\u754c\u9762\u6d41\u53d8\u673a\u5236"},"content":{"rendered":"\n<p>\u5bcc\u5170\u514b\u6797\u65e9\u572818\u4e16\u7eaa\u5c31\u53d1\u73b0\uff0c\u4e00\u5c0f\u52fa\u6a44\u6984\u6cb9\u53ef\u4ee5\u8fc5\u901f\u94fa\u5c55\u5728\u6c60\u5858\u6c34\u9762\u4e0a\uff0c\u5f62\u6210\u63a5\u8fd1\u5355\u5206\u5b50\u5c42\u539a\u5ea6\u7684\u6cb9\u819c\uff0c\u5e76\u4f7f\u539f\u672c\u8d77\u4f0f\u7684\u6c34\u9762\u53d8\u5f97\u5e73\u9759\u3002\u53cd\u5e38\u7684\u662f\uff0c\u6cb9\u819c\u964d\u4f4e\u754c\u9762\u5f20\u529b\u672c\u5e94\u4f7f\u6c34\u9762\u66f4\u6613\u5f62\u53d8\uff0c\u5374\u53cd\u800c\u4f7f\u8868\u9762\u6ce2\u8fc5\u901f\u8870\u51cf\u3002\u8fd9\u8868\u660e\uff0c\u5404\u5411\u540c\u6027\u7684\u754c\u9762\u5f20\u529b\u4e0d\u8db3\u4ee5\u523b\u753b\u590d\u6742\u754c\u9762\u7684\u52a8\u6001\u54cd\u5e94\u3002\u5f53\u8868\u9762\u6d3b\u6027\u5206\u5b50\u3001\u805a\u5408\u7269\u6216\u9897\u7c92\u5728\u754c\u9762\u5bcc\u96c6\u540e\uff0c\u5f62\u53d8\u4f1a\u5f15\u8d77\u754c\u9762\u7ec4\u6210\u53d8\u5316\u548c\u5fae\u7ed3\u6784\u91cd\u6392\uff0c\u8fdb\u800c\u4ea7\u751f\u989d\u5916\u5e94\u529b\u4e0e\u9ecf\u6027\u8017\u6563\u3002\u9762\u79ef\u53d8\u5316\u5f15\u8d77\u7684\u754c\u9762\u6d53\u5ea6\u548c\u5f20\u529b\u6539\u53d8\uff0c\u8868\u73b0\u4e3aGibbs\u754c\u9762\u5f39\u6027\uff1b\u5206\u5b50\u4ea4\u6362\u548c\u5fae\u7ed3\u6784\u677e\u5f1b\u5219\u4f1a\u5e26\u6765\u968f\u65f6\u95f4\u6f14\u5316\u7684\u9ecf\u6027\u8017\u6563\u3002Boussinesq\u6700\u65e9\u5173\u4e8e\u8868\u9762\u9ecf\u6027\u7684\u601d\u60f3\uff0c\u4ee5\u53ca\u540e\u6765\u7684Boussinesq\u2013Scriven\u6a21\u578b\uff0c\u5c06\u754c\u9762\u9ecf\u6027\u7eb3\u5165\u6d41\u4f53\u529b\u5b66\u63cf\u8ff0\u3002\u754c\u9762\u7684\u8fd9\u79cd\u52a8\u6001\u529b\u5b66\u54cd\u5e94\u4e0d\u4ec5\u5173\u7cfb\u5230\u6ce1\u6cab\u548c\u4e73\u6db2\u7684\u7a33\u5b9a\uff0c\u4e5f\u4f1a\u6539\u53d8\u754c\u9762\u4f20\u8d28\u4ee5\u53ca\u80ba\u6ce1\u7b49\u751f\u7269\u6d41\u4f53\u754c\u9762\u7684\u8fd0\u52a8\u3002<strong>\u8fd1\u5e74\u6765\uff0c\u754c\u9762\u9ecf\u5f39\u6027\u88ab\u7528\u4e8e\u7406\u89e3\u5404\u79cd\u6d41\u4f53\u5931\u7a33\u8fc7\u7a0b\uff0c\u5305\u62ec\u9ecf\u6027\u6db2\u67f1\u65ad\u88c2\u3001\u6db2\u6ef4\u5939\u65ad\u4ee5\u53ca\u9ecf\u6027\u6307\u8fdb\u7684\u5c16\u7aef\u5206\u88c2\uff0c\u8868\u660e\u754c\u9762\u81ea\u8eab\u7684\u6062\u590d\u4e0e\u8017\u6563\u80fd\u591f\u6539\u53d8\u5931\u7a33\u7684\u589e\u957f\u548c\u5c3a\u5ea6\u9009\u62e9\u3002<\/strong><\/p>\n\n\n\n<p>\u901a\u8fc7\u6c34\u6cb9\u754c\u9762\u805a\u5408\uff08IP\uff09\u5236\u5907\u7684\u8584\u5c42\u590d\u5408\u805a\u9170\u80fa\uff08PA\uff09\u819c\uff0c\u662f\u73b0\u4ee3\u53cd\u6e17\u900f\u548c\u7eb3\u6ee4\u8fc7\u7a0b\u4e2d\u7684\u6838\u5fc3\u6750\u6599\u3002\u7136\u800c\uff0c\u5176\u53d1\u5c55\u957f\u671f\u53d7\u5230\u6e17\u900f\u6027\u4e0e\u9009\u62e9\u6027\u6743\u8861\u7684\u9650\u5236\uff0c\u800c\u8fd9\u4e00\u74f6\u9888\u4e0ePA\u9009\u62e9\u5c42\u590d\u6742\u4e14\u96be\u4ee5\u8c03\u63a7\u7684\u5f62\u6210\u8fc7\u7a0b\u5bc6\u5207\u76f8\u5173\u3002\u5728IP\u8fc7\u7a0b\u4e2d\uff0c\u6c34\u76f8\u4e2d\u7684\u80fa\u5355\u4f53\u8de8\u8d8a\u754c\u9762\u8fdb\u5165\u6cb9\u76f8\uff0c\u5e76\u4e0e\u9170\u6c2f\u5355\u4f53\u53cd\u5e94\u751f\u6210PA\u8584\u5c42\u3002\u5355\u4f53\u4f20\u8d28\u3001\u5316\u5b66\u53cd\u5e94\u548c\u754c\u9762\u6d41\u52a8\u9ad8\u5ea6\u8026\u5408\uff0c\u5e76\u8fdb\u4e00\u6b65\u5851\u9020\u819c\u8868\u9762\u7684\u8936\u76b1\u3001\u810a\u72b6\u548c\u7a7a\u8154\u7ed3\u6784\uff0c\u6700\u7ec8\u5f71\u54cd\u6709\u6548\u4f20\u8d28\u9762\u79ef\u3001\u9009\u62e9\u5c42\u7ed3\u6784\u548c\u5206\u79bb\u6027\u80fd\u3002\u8fd9\u8bf4\u660e\uff0cIP\u4e2d\u7684\u6c34\u6cb9\u754c\u9762\u53ef\u80fd\u5e76\u975e\u56fa\u5b9a\u4e0d\u52a8\u7684\u5149\u6ed1\u5e73\u9762\uff0c\u800c\u662f\u5728\u8fd9\u8fc7\u7a0b\u4e2d\u7ecf\u5386\u52a8\u6001\u7684\u6269\u5f20\u548c\u8d77\u4f0f\uff08<strong>\u56fe<\/strong><strong>1a<\/strong>\uff09\u3002\u5bf9\u4e8e\u8fd9\u6837\u4e00\u4e2a\u52a8\u6001\u7684\u754c\u9762\uff0c\u968f\u5f62\u53d8\uff08\u5982\u9762\u79ef\u6269\u5f20\uff09\u4ea7\u751f\u7684\u6062\u590d\u4e0e\u8017\u6563\u662f\u5176\u5185\u5728\u7684\u529b\u5b66\u5c5e\u6027\uff0c\u754c\u9762\u9ecf\u5f39\u6027\u56e0\u6b64\u4e0d\u53ef\u5ffd\u7565\uff08<strong>\u56fe<\/strong><strong>1b<\/strong>\uff09\u3002<\/p>\n\n\n\n<p>\u8981\u5398\u6e05\u754c\u9762\u6d41\u53d8\u5bf9PA\u819c\u7ed3\u6784\u5f62\u6210\u7684\u4f5c\u7528\u673a\u5236\uff0c\u5173\u952e\u5728\u4e8e\u5efa\u7acb\u4e00\u4e2a\u80fd\u591f\u8fde\u7eed\u8c03\u8282\u754c\u9762\u9ecf\u5f39\u6027\uff0c\u540c\u65f6\u4fdd\u6301\u9759\u6001\u754c\u9762\u5f20\u529b\u548c\u754c\u9762\u57fa\u672c\u5316\u5b66\u5c5e\u6027\u4e0d\u53d8\u7684\u5e73\u53f0\u3002\u867d\u7136\u8868\u9762\u6d3b\u6027\u5206\u5b50\u3001\u805a\u5408\u7269\u6216\u9897\u7c92\u7b49\u754c\u9762\u6539\u6027\u5242\u5df2\u88ab\u5e7f\u6cdb\u7528\u4e8e\u8c03\u8282\u819c\u7ed3\u6784\u5e76\u6539\u5584\u5206\u79bb\u6027\u80fd\uff0c\u4f46\u73b0\u6709\u7814\u7a76\u4e3b\u8981\u5173\u6ce8\u754c\u9762\u5f20\u529b\u548c\u5355\u4f53\u5206\u914d\u7b49\u5e73\u8861\u6216\u5e73\u5747\u7269\u7406\u91cf\uff0c\u754c\u9762\u5728\u5f62\u53d8\u4e2d\u7684\u52a8\u6001\u5e94\u529b\u54cd\u5e94\u88ab\u957f\u671f\u5ffd\u7565\u3002<\/p>\n\n\n\n<p>\u57fa\u4e8e\u8fd9\u4e00\u8ba4\u8bc6\uff0c<strong>\u4e1c\u534e\u5927\u5b66<\/strong><strong>\u5148\u8fdb\u7ea4\u7ef4\u6750\u6599\u5168\u56fd\u91cd\u70b9\u5b9e\u9a8c\u5ba4\u3001\u5148\u8fdb\u4f4e\u7ef4\u6750\u6599\u4e2d\u5fc3<\/strong><strong>\u51af\u8bad\u8fbe<\/strong><strong>\u8bfe\u9898\u7ec4<\/strong>\u63ed\u793a\u4e86\u754c\u9762\u9ecf\u5f39\u6027\u63a7\u5236\u754c\u9762\u805a\u5408\u6d41\u4f53\u5931\u7a33\u4e0e\u819c\u7ed3\u6784\u6f14\u5316\u7684\u6838\u5fc3\u673a\u5236\u3002\u7814\u7a76\u56e2\u961f\u5229\u7528\u5149\u53cd\u5e94\u6027\u4e24\u4eb2\u5206\u5b50\u5728\u6c34\u6cb9\u754c\u9762\u5f62\u6210\u5355\u5206\u5b50\u5c42\uff0c\u5e76\u901a\u8fc7\u7cbe\u786e\u53ef\u63a7\u7684\u7d2b\u5916\u5149\u7167\u8c03\u8282\u5176\u754c\u9762\u5806\u79ef\u72b6\u6001\u548c\u754c\u9762\u6d41\u53d8\u54cd\u5e94\uff08<strong>\u56fe1c<\/strong>\uff09\u3002\u5728\u4fdd\u6301\u9759\u6001\u754c\u9762\u5f20\u529b\u7b49\u7269\u7406\u91cf\u4e0d\u53d8\u7684\u60c5\u51b5\u4e0b\uff0c\u5efa\u7acb\u4e86\u4e00\u4e2a\u53ef\u8fde\u7eed\u8c03\u8282\u754c\u9762\u6d41\u53d8\u72b6\u6001\u7684\u7814\u7a76\u5e73\u53f0\u3002\u7814\u7a76\u8868\u660e\uff0c\u754c\u9762\u9ecf\u5ea6\u80fd\u591f\u663e\u8457\u5f71\u54cd\u754c\u9762\u4e0d\u7a33\u5b9a\u6027\u7684\u963b\u5c3c\u8fc7\u7a0b\uff0c\u5e76\u51b3\u5b9a\u819c\u8868\u9762\u7a7a\u5fc3\u810a\u72b6\u7ed3\u6784\u7684\u7279\u5f81\u5c3a\u5ea6\uff08<strong>\u56fe1d<\/strong>\uff09\u3002\u7531\u6b64\u5236\u5907\u7684\u805a\u9170\u80fa\u819c\u5448\u73b0\u51fa\u5927\u9762\u79ef\u5747\u4e00\u7684\u7a7a\u5fc3\u8936\u76b1\u5f62\u8c8c\uff0c\u5e76\u4e14\u8fd9\u4e9b\u7ed3\u6784\u5177\u6709\u660e\u786e\u3001\u53ef\u91cf\u5316\u7684\u7279\u5f81\u5c3a\u5ea6\uff08<strong>\u56fe<\/strong><strong>1e<\/strong>\uff09\u3002\u57fa\u4e8e\u8fd9\u4e00\u673a\u5236\u5236\u5907\u7684\u805a\u9170\u80fa\u7eb3\u6ee4\u819c\u5177\u6709\u5b8f\u89c2\u5747\u4e00\u7684\u7a7a\u5fc3\u810a\u72b6\u7ed3\u6784\uff0c\u5b9e\u73b0\u4e86\u9ad8\u8fbe44.15 LMH\/bar\u7684\u6c34\u6e17\u900f\u7387\u548c99.82%\u7684Na<sub>2<\/sub>SO<sub>4<\/sub>\u622a\u7559\u7387\uff0c\u5e76\u8fdb\u4e00\u6b65\u5728\u819c\u7ec4\u4ef6\u5c3a\u5ea6\u4e0a\u9a8c\u8bc1\u4e86\u8be5\u7b56\u7565\u7684\u53ef\u653e\u5927\u6027\u3002<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"700\" height=\"487\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/2382c315a6ba396-5.png\" alt=\"\" class=\"wp-image-272449\"\/><\/figure>\n\n\n\n<p><strong>\u56fe1\uff5c\u754c\u9762\u6d41\u53d8\u8c03\u63a7\u754c\u9762\u805a\u5408\u4e2d\u7684\u6d41\u4f53<\/strong><strong>\u5931\u7a33<\/strong><strong>\u53ca<\/strong><strong>\u5927\u9762\u79ef\u89c4\u5219\u7684PA<\/strong><strong>\u819c\u5f62\u8c8c<\/strong><strong><\/strong><\/p>\n\n\n\n<p><strong>\u56fe<\/strong><strong>2<\/strong>\u7cfb\u7edf\u5c55\u793a\u4e86\u57fa\u4e8e\u754c\u9762\u6d41\u53d8\u8c03\u63a7\u540ePA\u819c\u5f62\u8c8c\u5177\u6709\u7279\u5f81\u5c3a\u5bf8\u53ef\u8c03\u6027\u548c\u53ef\u91cf\u5316\u6027\u3002\u4ee5\u4e24\u6027\u79bb\u5b50\u578bMAC\u4f53\u7cfb\u4e3a\u4f8b\uff0c\u7ecf\u8fc7\u4e0d\u540c\u7d2b\u5916\u5149\u5f3a\u9884\u5904\u7406\u540e\uff0cIP-MAC<em><sub><em><sub>I<\/sub><\/em><\/sub><\/em>\u819c\u5747\u5f62\u6210\u7531\u76c6\u5730\u533a\u57df\u548c\u6761\u5e26\u72b6\u810a\u7ed3\u6784\u7ec4\u6210\u7684\u5747\u4e00\u8868\u9762\u7eb9\u7406\u3002\u968f\u7740\u7d2b\u5916\u5149\u5f3a\u589e\u52a0\uff0c\u810a\u72b6\u7ed3\u6784\u7684\u95f4\u8ddd\u9010\u6e10\u51cf\u5c0f\u3001\u5bc6\u5ea6\u9010\u6e10\u5347\u9ad8\uff0c\u800c\u5f62\u8c8c\u7684\u6574\u4f53\u89c4\u5219\u6027\u4ecd\u5f97\u4ee5\u4fdd\u6301\uff08<strong>\u56fe2<\/strong><strong>a\uff09<\/strong>\u3002\u4f20\u7edfIP\u819c\u4ee5\u53ca\u672a\u5f15\u5165\u4e24\u4eb2\u5206\u5b50\u5355\u5c42\u7684\u7d2b\u5916\u5904\u7406\u819c\u5747\u4e0d\u5f62\u6210\u7c7b\u4f3c\u89c4\u5219\u7ed3\u6784\uff0c\u8bf4\u660e\u8be5\u5f62\u8c8c\u4e0d\u662f\u7531\u4e8e\u7d2b\u5916\u5149\u7167\u4ea7\u751f\u7684\u3002\u622a\u9762TEM\u548c\u819c\u53cd\u9762SEM\u8fdb\u4e00\u6b65\u8bc1\u660e\uff0c\u8fd9\u4e9b\u810a\u72b6\u7ed3\u6784\u5177\u6709\u7a7a\u5fc3\u5185\u90e8\uff0c\u800c\u9009\u62e9\u5c42\u539a\u5ea6\u57fa\u672c\u4fdd\u6301\u5728\u7ea630 nm\uff08<strong>\u56fe2<\/strong><strong>b, c, d<\/strong>\uff09\u3002AFM\u8fdb\u4e00\u6b65\u8868\u660e\uff0c\u8fd9\u4e9b\u8868\u9762\u56fe\u6848\u5177\u6709\u7ea6400 nm\u7684\u663e\u8457\u810a\u9ad8\uff1b\u8868\u9762\u79ef\u6269\u5f20\u6bd4<em>\u03c6<\/em>\u968f\u7d2b\u5916\u5149\u5f3a\u5347\u9ad8\u800c\u6301\u7eed\u589e\u52a0\uff0c\u8bf4\u660e\u5f62\u8c8c\u8c03\u63a7\u540c\u65f6\u5e26\u6765\u4e86\u6709\u6548\u4f20\u8d28\u9762\u79ef\u7684\u63d0\u5347\uff08<strong>\u56fe2<\/strong><strong>e, f<\/strong>\uff09\u3002\u4e8c\u7ef4FFT\u5206\u6790\u8fdb\u4e00\u6b65\u5c06\u8fd9\u79cd\u8868\u9762\u5f62\u8c8c\u8f6c\u5316\u4e3a\u53ef\u5b9a\u91cf\u6bd4\u8f83\u7684\u7ed3\u6784\u53c2\u6570\u3002\u867d\u7136\u810a\u72b6\u7ed3\u6784\u5e76\u975e\u4e25\u683c\u5468\u671f\u6392\u5217\uff0c\u4f46\u5012\u6613\u7a7a\u95f4\u4e2d\u51fa\u73b0\u6e05\u6670\u7279\u5f81\u5cf0\uff0c\u8868\u660e\u5176\u5177\u6709\u660e\u786e\u7684\u4f18\u9009\u95f4\u8ddd\uff08<strong>\u56fe2<\/strong><strong>g<\/strong>\uff09\u3002\u56e0\u6b64\uff0c\u7279\u5f81\u957f\u5ea6\u5c3a\u5ea6<em>d<\/em>\u53ef\u4ee5\u7528\u4e8e\u63cf\u8ff0\u754c\u9762\u4e0d\u7a33\u5b9a\u6027\u88ab\u56fa\u5316\u540e\u5f62\u6210\u7684\u819c\u8868\u9762\u7ed3\u6784\u5c3a\u5ea6\u3002\u968f\u7740\u7d2b\u5916\u5149\u5f3a\u5347\u9ad8\uff0c<em>d<\/em>\u5355\u8c03\u51cf\u5c0f\uff0c\u800c1\/<em>d<\/em>\u00b2\u8868\u5f81\u7684\u810a\u5bc6\u5ea6\u540c\u6b65\u589e\u52a0\uff1b\u8fd9\u4e00\u8d8b\u52bf\u5728MAC\u3001MTAB\u548cMUSS\u4e09\u79cd\u4e0d\u540c\u5934\u57fa\u5316\u5b66\u7ed3\u6784\u7684\u4e24\u4eb2\u5206\u5b50\u4f53\u7cfb\u4e2d\u5747\u53ef\u89c2\u5bdf\u5230\uff0c\u8bf4\u660e\u8be5\u8c03\u63a7\u89c4\u5f8b\u5177\u6709\u8de8\u4f53\u7cfb\u7684\u4e00\u81f4\u6027\uff08<strong>\u56fe2<\/strong><strong>h, i, j, k<\/strong>\uff09\u3002<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"600\" height=\"519\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/ce6e2814f207c93-4.png\" alt=\"\" class=\"wp-image-272450\"\/><\/figure>\n\n\n\n<p><strong>\u56fe2\uff5c<\/strong><strong>\u7cbe\u786e<\/strong><strong>\u8c03\u63a7\u754c\u9762\u6d41\u53d8\u5b9e\u73b0PA\u819c\u7a7a\u810a\u72b6\u7ed3\u6784\u7684\u8fde\u7eed\u6f14\u5316<\/strong><\/p>\n\n\n\n<p>\u5229\u7528\u540c\u6b65\u8f90\u5c04X-\u5c04\u7ebf\u53cd\u5c04\u7387\u8868\u5f81\u7d2b\u5916\u5149\u7167\u540eMAC\u754c\u9762\u5c42\u7684\u7ed3\u6784\u53d8\u5316\uff08<strong>\u56fe<\/strong><strong>3a<\/strong>\uff09\u3002\u968f\u7740\u5149\u5f3a\u589e\u52a0\uff0cKiessig \u6761\u7eb9\u95f4\u8ddd\u589e\u5927\u3001\u632f\u5e45\u51cf\u5f31\uff0c\u8bf4\u660e\u754c\u9762\u5c42\u8f7b\u5fae\u53d8\u8584\uff0c\u540c\u65f6\u7ed3\u6784\u5747\u4e00\u6027\u548c\u76f8\u5e72\u6027\u4e0b\u964d\u3002\u7ed3\u5408 NMR \u548c GPC \u7ed3\u679c\u53ef\u77e5\uff0c\u7d2b\u5916\u5149\u53ea\u662f\u8bf1\u5bfc\u5c11\u91cf\u5206\u5b50\u4f4e\u805a\u5316\uff0c\u4f7f\u5355\u4f53\u4e0e\u4f4e\u805a\u7269\u5171\u5b58\u4e8e\u754c\u9762\uff0c\u5e76\u6270\u4e71\u539f\u6709\u7684\u4e8c\u7ef4\u5206\u5b50\u5806\u79ef\u3002\u503c\u5f97\u6ce8\u610f\u7684\u662f\uff0c\u8fd9\u4e00\u7ed3\u6784\u6f14\u5316\u5e76\u672a\u663e\u8457\u6539\u53d8\u9759\u6001\u754c\u9762\u5f20\u529b\uff0c\u4e0d\u540c\u5149\u7167\u6761\u4ef6\u4e0b\u7684\u6b63\u5df1\u70f7\/\u6c34\u754c\u9762\u5f20\u529b\u59cb\u7ec8\u7ef4\u6301\u5728\u7ea6 6 mN m\u207b\u00b9\uff08<strong>\u56fe3b<\/strong>\uff09\u3002\u7814\u7a76\u56e2\u961f\u8fdb\u4e00\u6b65\u91c7\u7528\u632f\u8361\u6ed1\u969c\u6cd5\u5bf9\u754c\u9762\u5c42\u7684\u754c\u9762\u6d41\u53d8\u6027\u8d28\u8fdb\u884c\u8868\u5f81\uff08<strong>\u56fe3c<\/strong>\uff09\u3002\u5728\u5c0f\u632f\u5e45\u7b80\u8c10\u9762\u79ef\u632f\u8361\u4e0b\uff0c\u5f20\u529b\u54cd\u5e94\u8868\u73b0\u51fa\u4e0d\u540c\u7684\u5e45\u503c\u548c\u76f8\u4f4d\u6ede\u540e\uff0c\u53cd\u6620\u4e86\u754c\u9762\u50a8\u5b58\u548c\u8017\u6563\u5f62\u53d8\u80fd\u91cf\u7684\u80fd\u529b\uff0c\u7531\u6b64\u5f97\u5230\u8868\u89c2\u590d\u5408\u6a21\u91cf\u548c\u754c\u9762\u9ecf\u5ea6\uff08<strong>\u56fe3d<\/strong>\uff09\u3002\u5b9e\u9a8c\u7ed3\u679c\u663e\u793a\uff0cMAC\u3001MUSS \u548c MTAB \u4e09\u79cd\u4f53\u7cfb\u7684\u590d\u5408\u754c\u9762\u6a21\u91cf\u3001\u754c\u9762\u9ecf\u5ea6\u5747\u968f\u7d2b\u5916\u5149\u5f3a\u589e\u52a0\u800c\u663e\u8457\u964d\u4f4e\uff0c\u5e76\u5728\u9ad8\u5149\u5f3a\u4e0b\u9010\u6e10\u8d8b\u4e8e\u5e73\u53f0\uff08<strong>\u56fe3e<\/strong>\uff09\u3002\u66f4\u91cd\u8981\u7684\u662f\uff0c\u4e09\u79cd\u4f53\u7cfb\u7684\u8868\u89c2\u754c\u9762\u9ecf\u5ea6\u5747\u9075\u5faa\u7531\u4e8c\u7ef4\u5149\u805a\u5408\u52a8\u529b\u5b66\u548c\u754c\u9762\u7ed3\u6784\u76f8\u5e72\u6027\u5171\u540c\u51b3\u5b9a\u7684\u6807\u5ea6\u5173\u7cfb\uff0c\u7edf\u4e00\u63cf\u8ff0\u4e86\u4f4e\u5149\u5f3a\u4e0b\u7684\u5feb\u901f\u4e0b\u964d\u548c\u9ad8\u5149\u5f3a\u4e0b\u7684\u5e73\u53f0\u5316\u8d8b\u52bf\u3002\u5206\u5b50\u52a8\u529b\u5b66\u6a21\u62df\u8fdb\u4e00\u6b65\u89e3\u91ca\u4e86\u754c\u9762\u6d41\u53d8\u53ef\u63a7\u7684\u5206\u5b50\u673a\u5236\u3002\u5c11\u91cf\u4f4e\u805a\u7269\u4f1a\u7834\u574f\u539f\u672c\u8f83\u4e3a\u534f\u540c\u7684\u5806\u79ef\uff0c\u5e76\u63d0\u9ad8\u754c\u9762\u5206\u5b50\u7684\u6a2a\u5411\u8fc1\u79fb\u80fd\u529b\uff08<strong>\u56fe3f, g, h<\/strong>\uff09\u3002\u7531\u6b64\u4ea7\u751f\u7684\u7f3a\u9677\u72b6\u5f02\u8d28\u7ed3\u6784\u964d\u4f4e\u4e86\u754c\u9762\u5c42\u7684\u7ed3\u6784\u76f8\u5e72\u6027\uff0c\u589e\u52a0\u4e86\u53ef\u4f9b\u5206\u5b50\u91cd\u65b0\u6392\u5217\u7684\u81ea\u7531\u7a7a\u95f4\uff08<strong>\u56fe3i<\/strong>\uff09\u3002<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"550\" height=\"570\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/7f88dbbcaa77a1d-4.png\" alt=\"\" class=\"wp-image-272451\"\/><\/figure>\n\n\n\n<p><strong>\u56fe3\uff5c<\/strong><strong>\u754c\u9762\u5fae\u7ed3\u6784\u6f14\u5316\u8c03\u63a7\u6c34\u6cb9\u754c\u9762\u6d41\u53d8\u5e76\u63a7\u5236PA\u819c\u5f62\u8c8c\u7279\u5f81\u5c3a\u5ea6<\/strong><strong><\/strong><\/p>\n\n\n\n<p>\u4e3a\u660e\u786e\u810a\u72b6\u7ed3\u6784\u7684\u5f62\u6210\u673a\u5236\uff0c\u7814\u7a76\u56e2\u961f\u9996\u5148\u6392\u9664\u4e86\u51e0\u79cd\u53ef\u80fd\u7684\u5931\u7a33\u6765\u6e90\u3002\u622a\u9762TEM\u548c\u819c\u53cd\u9762SEM\u663e\u793a\uff0c\u810a\u72b6\u7ed3\u6784\u5177\u6709\u660e\u663e\u7684\u7a7a\u5fc3\u5185\u90e8\uff0c\u800cPA\u9009\u62e9\u5c42\u539a\u5ea6\u59cb\u7ec8\u4fdd\u6301\u5728\u7ea630 nm\u3002\u8fd9\u79cd\u5f62\u8c8c\u66f4\u7b26\u5408\u539a\u5ea6\u76f8\u5bf9\u5747\u4e00\u7684\u805a\u9170\u80fa\u8584\u5c42\u968f\u754c\u9762\u8d77\u4f0f\u968f\u540e\u56fa\u5316\u7684\u8fc7\u7a0b\uff0c\u800c\u4e0d\u652f\u6301Turing\u578b\u53cd\u5e94\u6269\u6563\u673a\u5236\u3002\u82e5\u7531&nbsp;spinodal \u76f8\u5206\u79bb\u4e3b\u5bfc\uff0c\u9009\u62e9\u5c42\u5185\u90e8\u5e94\u51fa\u73b0\u805a\u5408\u7269\u5bc6\u5ea6\u5206\u5316\uff0c\u5176\u7279\u5f81\u5c3a\u5ea6\u7531\u76f8\u5206\u79bb\u70ed\u529b\u5b66\u548c\u52a8\u529b\u5b66\u63a7\u5236\uff0c\u8fd9\u4e0e\u672c\u6587\u89c2\u5bdf\u5230\u7684\u539a\u5ea6\u5747\u4e00\u3001\u5185\u90e8\u4e2d\u7a7a\u7684\u810a\u72b6\u7ed3\u6784\u4e0d\u7b26\u3002\u4e0e\u6b64\u540c\u65f6\uff0cRayleigh\u6570\u8fdc\u5c0f\u4e8e1\uff0c\u8868\u660e Rayleigh\u2013Taylor \u4e0d\u7a33\u5b9a\u6027\u548c\u53cc\u6269\u6563\u8fc7\u7a0b\u5728\u5f53\u524d\u6761\u4ef6\u4e0b\u4e5f\u96be\u4ee5\u53d1\u6325\u4e3b\u5bfc\u4f5c\u7528\u3002\u5728\u6b64\u57fa\u7840\u4e0a\uff0c\u7814\u7a76\u56e2\u961f\u5c06\u5f62\u8c8c\u5f62\u6210\u5f52\u56e0\u4e8e\u4f20\u8d28\u8bf1\u5bfc\u7684\u9a6c\u5170\u6208\u5c3c\u5931\u7a33\u3002\u901a\u8fc7\u539f\u4f4d\u6d4b\u8bd5\u52a8\u6001\u754c\u9762\u5f20\u529b\u663e\u793a\uff0cPIP \u8de8\u8d8a\u6c34\u6cb9\u754c\u9762\u8fdb\u5165\u6b63\u5df1\u70f7\u76f8\u65f6\uff0c\u4f1a\u4e0d\u65ad\u964d\u4f4e\u754c\u9762\u5f20\u529b\uff0c\u8868\u660e\u754c\u9762\u5f20\u529b\u5bf9\u754c\u9762PIP\u6d53\u5ea6\u9ad8\u5ea6\u654f\u611f\uff0c\u5e76\u6ee1\u8db3 \u2202\u03b3\/\u2202c&lt;0\u3002\u56e0\u6b64\uff0c\u5373\u4f7f\u5fae\u5c0f\u7684\u6d53\u5ea6\u8d77\u4f0f\uff0c\u4e5f\u4f1a\u8f6c\u5316\u4e3a\u6cbf\u754c\u9762\u7684\u5f20\u529b\u68af\u5ea6\uff0c\u5e76\u4ea7\u751f\u9a6c\u5170\u6208\u5c3c\u5e94\u529b\u3002\u6839\u636e Sternling\u548cScriven \u7b49\u5bf9\u4f20\u8d28\u8bf1\u5bfc\u754c\u9762\u6e4d\u52a8\u7684\u7ecf\u5178\u5206\u6790\uff0c\u8fd9\u7c7b\u5f20\u529b\u68af\u5ea6\u80fd\u591f\u653e\u5927\u539f\u6709\u6270\u52a8\uff0c\u4f7f\u6c34\u6cb9\u754c\u9762\u8fdb\u5165\u6d41\u4f53\u5931\u7a33\u72b6\u6001\u3002<\/p>\n\n\n\n<p>\u503c\u5f97\u6ce8\u610f\u7684\u662f\uff0c\u5149\u8f90\u5c04\u5bf9PIP\u5206\u914d\u3001\u9759\u6001\u754c\u9762\u5f20\u529b\u968f\u7d2b\u5916\u5149\u5f3a\u5ea6\u57fa\u672c\u4fdd\u6301\u4e0d\u53d8\uff0c\u8bf4\u660e\u5931\u7a33\u9a71\u52a8\u529b\u5e76\u672a\u663e\u8457\u6539\u53d8\u3002\u819c\u5f62\u8c8c\u5c3a\u5ea6\u7684\u7cfb\u7edf\u53d8\u5316\u66f4\u53ef\u80fd\u6765\u81ea\u754c\u9762\u6d41\u53d8\u963b\u5c3c\u7684\u8c03\u8282\u3002\u5bf9\u4e8e\u5bcc\u96c6MAC\u3001MTAB\u6216MUSS\u7684\u6c34\u6cb9\u754c\u9762\uff0c\u6d4b\u5f97\u7684\u8868\u89c2\u754c\u9762\u9ecf\u5ea6\u4f4d\u4e8e1\u201340 mPa\u00b7s\u00b7m\u8303\u56f4\u5185\uff0c\u5e76\u53ef\u4ee5\u901a\u8fc7\u7d2b\u5916\u5149\u8f90\u5c04\u7cbe\u786e\u53ef\u63a7\u3002\u76f8\u6bd4\u4e4b\u4e0b\uff0c\u6c34\u76f8\u548c\u6b63\u5df1\u70f7\u7684\u4f53\u76f8\u9ecf\u5ea6\u5206\u522b\u7ea6\u4e3a1\u548c0.3 mPa\u00b7s\u3002\u8003\u8651\u5230\u672c\u4f53\u7cfb\u7684\u754c\u9762\u9ecf\u5ea6\u3001\u4f53\u76f8\u9ecf\u5ea6\u548c\u5fae\u7c73\u7ea7\u5c3a\u5ea6\uff0c\u6240\u5f97<strong>Boussinesq<\/strong><strong>\u6570\u8fdc\u8fdc\u5927\u4e8e<\/strong><strong>1<\/strong><strong>\uff0c\u8bf4\u660e\u754c\u9762\u9ecf\u6027\u8017\u6563\u5360\u636e\u4e3b\u5bfc<\/strong>\u3002<strong>\u56fe<\/strong><strong>3j<\/strong>\u8fdb\u4e00\u6b65\u5efa\u7acb\u4e86\u754c\u9762\u6d41\u53d8\u72b6\u6001\u4e0ePA\u819c\u8868\u9762\u7ed3\u6784\u5c3a\u5ea6\u4e4b\u95f4\u7684\u76f4\u63a5\u5173\u8054\u3002\u5f53\u4ee5\u754c\u9762\u9ecf\u5ea6\u4e3a\u6a2a\u5750\u6807\u91cd\u65b0\u5206\u6790\u7ed3\u6784\u7279\u5f81\u957f\u5ea6<em>d<\/em>\u7684\u53d8\u5316\u65f6\uff0c\u4e09\u79cd\u4f53\u7cfb\u7684\u6570\u636e\u6536\u655b\u5230\u540c\u4e00\u5355\u8c03\u8d8b\u52bf\u3002\u8be5\u7ed3\u679c\u8868\u660e\uff0c\u754c\u9762\u5931\u7a33\u7ed3\u6784\u7684\u7279\u5f81\u5c3a\u5ea6\u4e3b\u8981\u7531\u754c\u9762\u6d41\u53d8\u72b6\u6001\u51b3\u5b9a\uff0c\u800c\u4e0d\u662f\u7531\u7279\u5b9a\u4e24\u4eb2\u5206\u5b50\u7684\u5316\u5b66\u6027\u8d28\u51b3\u5b9a\u3002<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"700\" height=\"446\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/4e9a0ba2491dfde-4.png\" alt=\"\" class=\"wp-image-272452\"\/><\/figure>\n\n\n\n<p><strong>\u56fe4\uff5c<\/strong><strong>PA<\/strong><strong>\u819c\u7684\u7eb3\u6ee4\u6027\u80fd<\/strong><strong>\u53ca\u7ec4\u4ef6\u5316\u5e94\u7528<\/strong><strong><\/strong><\/p>\n\n\n\n<p>\u5728\u660e\u786e\u754c\u9762\u6d41\u53d8\u5bf9\u819c\u5f62\u8c8c\u7684\u8c03\u63a7\u4f5c\u7528\u540e\uff0c\u7814\u7a76\u56e2\u961f\u8fdb\u4e00\u6b65\u8bc4\u4f30\u4e86PA\u819c\u7684\u7eb3\u6ee4\u6027\u80fd\u3002\u89c4\u5219\u7a7a\u5fc3\u810a\u72b6\u7ed3\u6784\u663e\u8457\u63d0\u5347\u4e86\u819c\u7684\u6709\u6548\u4f20\u8d28\u9762\u79ef\uff0c\u540c\u65f6\u4fdd\u6301\u8f83\u8584\u9009\u62e9\u5c42\u3002\u4ee3\u8868\u6027IP-MAC<sub>10<\/sub>\u819c\u7684\u6c34\u6e17\u900f\u7387\u8fbe\u523044.15 \u00b1 1.21 L m\u207b\u00b2 h\u207b\u00b9 bar\u207b\u00b9\uff0c\u5e76\u4fdd\u630199.82 \u00b1 0.08%\u7684Na<sub>2<\/sub>SO<sub>4<\/sub>\u622a\u7559\u7387\uff0c\u5728\u6c34\u6e17\u900f\u7387\u4e0e\u9009\u62e9\u6027\u4e4b\u95f4\u8868\u73b0\u51fa\u5177\u6709\u7ade\u4e89\u529b\u7684\u5e73\u8861\u3002\u810a\u72b6\u7ed3\u6784\u5e76\u975e\u8d8a\u5bc6\u8d8a\u597d\uff0c\u8fc7\u5ea6\u62e5\u6324\u4f1a\u9020\u6210\u5c40\u90e8\u63a5\u89e6\u548c\u6709\u6548\u9762\u79ef\u635f\u5931\u3002\u9ad8\u9009\u62e9\u6027\u6765\u81ea\u819c\u7ed3\u6784\u4e0e\u754c\u9762\u5316\u5b66\u7684\u5171\u540c\u4f5c\u7528\u3002\u53d7\u63a7\u5931\u7a33\u5f62\u6210\u4e86\u66f4\u81f4\u5bc6\u3001\u7f3a\u9677\u66f4\u5c11\u7684PA\u7f51\u7edc\uff0cIP-MAC<sub>10<\/sub>\u819c\u7684\u5e73\u5747\u6709\u6548\u5b54\u534a\u5f84\u7531\u5e38\u89c4\u819c\u7684\u7ea60.29 nm \u964d\u81f30.26 nm\uff0c\u540c\u65f6\u810a\u72b6\u7ed3\u6784\u589e\u52a0\u4e86\u819c\u8868\u9762\u7fa7\u9178\u57fa\u56e2\u7684\u66b4\u9732\u9762\u79ef\uff0c\u5f3a\u5316\u4e86\u5bf9\u4e8c\u4ef7\u9634\u79bb\u5b50\u7684Donnan\u6392\u65a5\u3002\u5728\u6df7\u76d0\u4f53\u7cfb\u4e2d\uff0c\u8be5\u819c\u4ecd\u4fdd\u6301\u8d85\u8fc799.5%\u7684Na<sub>2<\/sub>SO<sub>4<\/sub>\u622a\u7559\u7387\uff0c\u5e76\u5141\u8bb8\u63a5\u8fd180%\u7684NaCl\u901a\u8fc7\uff0cNaCl\/Na<sub>2<\/sub>SO<sub>4<\/sub>\u9009\u62e9\u6027\u56e0\u5b50\u6700\u9ad8\u8fbe\u5230439\u3002\u8be5\u7b56\u7565\u8fd8\u5c55\u73b0\u51fa\u826f\u597d\u7684\u653e\u5927\u6f5c\u529b\uff0c\u56e2\u961f\u6210\u529f\u5236\u5907\u4e860.64 m \u00d7 0.32 m\u7684\u5927\u9762\u79ef\u819c\u7247\uff0c\u5e76\u7ec4\u88c5\u6210\u6709\u6548\u819c\u9762\u79ef\u4e3a0.54 m<sup>2<\/sup>\u7684\u5377\u5f0f\u7ec4\u4ef6\u3002\u4e03\u4e2a\u819c\u7ec4\u4ef6\u5747\u8868\u73b0\u51fa\u7a33\u5b9a\u4e14\u53ef\u91cd\u590d\u7684\u6c34\u901a\u91cf\u548cNa<sub>2<\/sub>SO<sub>4<\/sub>\u622a\u7559\u6027\u80fd\uff0c\u8bf4\u660e\u7d2b\u5916\u8c03\u63a7\u754c\u9762\u6d41\u53d8\u53ef\u4e0e\u73b0\u6709\u5377\u5bf9\u5377\u5236\u819c\u5de5\u827a\u8854\u63a5\uff0c\u4e3a\u7ec4\u4ef6\u5316\u5e94\u7528\u63d0\u4f9b\u4e86\u53ef\u884c\u8def\u5f84\u3002<\/p>\n\n\n\n<p>\u76f8\u5173\u7814\u7a76\u6210\u679c\u4ee5\u201cInterfacial rheology for physics-based structuring of polyamide desalination membranes\u201d\u4e3a\u9898\u53d1\u8868\u5728<strong><em><strong><em>Nature Chemical Engineering<\/em><\/strong><\/em><\/strong><em>&nbsp;<\/em>(2026, DOI:&nbsp;10.1038\/s44286-026-00419-7)\u4e0a\uff0c<strong>\u4e1c\u534e\u5927\u5b66\u5148\u8fdb\u7ea4\u7ef4\u6750\u6599\u5168\u56fd\u91cd\u70b9\u5b9e\u9a8c\u5ba4\u3001\u5148\u8fdb\u4f4e\u7ef4\u6750\u6599\u4e2d\u5fc3\u4e3a\u7b2c\u4e00\u5355\u4f4d<\/strong>\uff0c<strong>\u51af\u8bad\u8fbe<\/strong>\u7814\u7a76\u5458\u4e3a\u672c\u6587\u7684\u901a\u8baf\u4f5c\u8005\uff0c\u4e2d\u56fd\u79d1\u6280\u5927\u5b66<strong>\u5415\u5174\u9716<\/strong>\u6559\u6388\u3001\u7f8e\u56fd\u83b1\u65af\u5927\u5b66<strong>Elimelech<\/strong>\u6559\u6388\u4e3a\u5171\u540c\u901a\u8baf\u4f5c\u8005\u3002\u4e1c\u534e\u5927\u5b66\u535a\u58eb\u751f<strong>\u6c64\u6e05\u6668<\/strong>\u4e3a\u672c\u6587\u7b2c\u4e00\u4f5c\u8005\u3002\u4e1c\u534e\u5927\u5b66\u4fe1\u606f\u4e0e\u667a\u80fd\u79d1\u5b66\u5b66\u9662<strong>\u5e38\u59d7<\/strong>\u6559\u6388\u3001\u65e5\u672c\u4e5d\u5dde\u5927\u5b66<strong>\u8d75\u677e\u5ddd<\/strong>\u526f\u6559\u6388\u3001\u65e5\u672c\u4e1c\u5317\u5927\u5b66<strong>\u5f20\u4ea6\u5468<\/strong>\u526f\u6559\u6388\u4e5f\u505a\u51fa\u91cd\u8981\u8d21\u732e\u3002\u8be5\u5de5\u4f5c\u5f97\u5230\u4e86\u56fd\u5bb6\u81ea\u7136\u79d1\u5b66\u57fa\u91d1\u3001\u4e2d\u592e\u9ad8\u6821\u57fa\u672c\u4e1a\u52a1\u8d39\u548c\u4e0a\u6d77\u5e02\u81ea\u7136\u79d1\u5b66\u57fa\u91d1\u9879\u76ee\u7684\u8d44\u52a9\u3002\u611f\u8c22\u4e0a\u6d77\u540c\u6b65\u8f90\u5c04\u5149\u6e90BL02U2\u8868\u9762\u884d\u5c04\u5149\u675f\u7ebf\u7ad9\u4e3a\u672c\u6587X-\u5c04\u7ebf\u53cd\u5c04\u7387\u6d4b\u8bd5\u63d0\u4f9b\u7684\u5927\u529b\u652f\u6301\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u5bcc\u5170\u514b\u6797\u65e9\u572818\u4e16\u7eaa\u5c31\u53d1\u73b0\uff0c\u4e00\u5c0f\u52fa\u6a44\u6984\u6cb9\u53ef\u4ee5\u8fc5\u901f\u94fa\u5c55\u5728\u6c60\u5858\u6c34\u9762\u4e0a\uff0c\u5f62\u6210\u63a5\u8fd1\u5355\u5206\u5b50\u5c42\u539a\u5ea6\u7684\u6cb9\u819c\uff0c\u5e76\u4f7f\u539f\u672c\u8d77\u4f0f\u7684\u6c34\u9762\u53d8\u5f97\u5e73\u9759\u3002\u53cd\u5e38\u7684\u662f\uff0c\u6cb9\u819c\u964d\u4f4e\u754c\u9762\u5f20\u529b\u672c\u5e94\u4f7f\u6c34\u9762\u66f4&#8230;<\/p>\n","protected":false},"author":31345,"featured_media":0,"comment_status":"open","ping_status":"","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[2],"tags":[],"class_list":["post-272448","post","type-post","status-publish","format-standard","hentry","category-keji"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/272448"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/31345"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=272448"}],"version-history":[{"count":1,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/272448\/revisions"}],"predecessor-version":[{"id":272453,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/272448\/revisions\/272453"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=272448"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=272448"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=272448"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}