{"id":272502,"date":"2026-07-18T09:09:00","date_gmt":"2026-07-18T01:09:00","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=272502"},"modified":"2026-07-17T21:30:23","modified_gmt":"2026-07-17T13:30:23","slug":"%e5%a4%aa%e5%8e%9f%e7%90%86%e5%b7%a5-%e5%8c%97%e4%ba%ac%e7%90%86%e5%b7%a5-%e9%bd%90%e9%b2%81%e5%b7%a5%e4%b8%9aafm%ef%bc%9a%e5%86%85%e7%bd%ae%e6%b0%a2%e6%ba%a2%e6%b5%81%e6%95%88%e5%ba%94%e9%ab%98","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=272502","title":{"rendered":"\u592a\u539f\u7406\u5de5\/\u5317\u4eac\u7406\u5de5\/\u9f50\u9c81\u5de5\u4e1aAFM\uff1a\u5185\u7f6e\u6c22\u6ea2\u6d41\u6548\u5e94\u9ad8\u6548\u78b1\u6027\u7535\u89e3\u6c34"},"content":{"rendered":"\n<p><\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"700\" height=\"403\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/2382c315a6ba396-11.png\" alt=\"\" class=\"wp-image-272515\"\/><\/figure>\n\n\n\n<p><\/p>\n\n\n\n<p>\u7b2c\u4e00\u4f5c\u8005\uff1a\u674e\u94a6\u3001\u5170\u5efa\u5b8f<\/p>\n\n\n\n<p>\u901a\u8baf\u4f5c\u8005\uff1a\u987e\u5c11\u6960\u3001\u5468\u5bb6\u4e1c\u3001\u738b\u7f8e\u73b2<\/p>\n\n\n\n<p>\u901a\u8baf\u5355\u4f4d\uff1a\u592a\u539f\u7406\u5de5\u5927\u5b66\u3001\u5317\u4eac\u7406\u5de5\u5927\u5b66\u3001\u9f50\u9c81\u5de5\u4e1a\u5927\u5b66<\/p>\n\n\n\n<p>\u8bba\u6587DOI\uff1ahttps:\/\/doi.org\/10.1002\/adfm.77151<\/p>\n\n\n\n<p><strong>\u3010\u5168\u6587\u901f\u89c8\u3011<\/strong><\/p>\n\n\n\n<p>\u78b1\u6027\u9634\u79bb\u5b50\u4ea4\u6362\u819c\u6c34\u7535\u89e3\uff08AEMWE\uff09\u88ab\u89c6\u4e3a\u5177\u6709\u5e94\u7528\u524d\u666f\u7684\u7eff\u6c22\u5236\u5907\u6280\u672f\u4e4b\u4e00\u3002\u7136\u800c\uff0c\u78b1\u6027\u7535\u89e3\u8d28\u4e2d\u6790\u6c22\u53cd\u5e94\uff08HER\uff09\u52a8\u529b\u5b66\u7f13\u6162\uff0c\u4e3b\u8981\u53d7\u9650\u4e8e\u989d\u5916\u7684\u6c34\u79bb\u89e3\u80fd\u5792\u3002\u73b0\u6709\u7814\u7a76\u8868\u660e\uff0c\u5f15\u5165\u4eb2\u6c27\u4f4d\u70b9\u53ef\u4fc3\u8fdbOH\u5438\u9644\uff0c\u52a0\u901fH\u751f\u6210\uff1b\u4f46\u968f\u540eH*\u5728\u6d3b\u6027\u4f4d\u70b9\u4e0a\u7684\u5438\u9644\u4e0e\u8131\u9644\u884c\u4e3a\u5f80\u5f80\u96be\u4ee5\u517c\u987e\uff0c\u6210\u4e3a\u9650\u5236\u50ac\u5316\u6548\u7387\u7684\u5173\u952e\u56e0\u7d20\u4e4b\u4e00\u3002\u6c22\u6ea2\u6d41\u6548\u5e94\u88ab\u8bc1\u5b9e\u53ef\u5728\u4e00\u5b9a\u7a0b\u5ea6\u4e0a\u5e73\u8861H*\u7684\u5438\u9644\u4e0e\u8131\u9644\u8fc7\u7a0b\u3002\u4f46\u5728\u4f20\u7edf\u8d1f\u8f7d\u578b\u50ac\u5316\u5242\u4e2d\uff0c\u6c22\u6ea2\u6d41\u901a\u5e38\u9700\u8981\u514b\u670d\u8f83\u957f\u7684\u8fc1\u79fb\u8def\u5f84\u53ca\u91d1\u5c5e-\u8f7d\u4f53\u754c\u9762\u7684\u989d\u5916\u963b\u529b\uff0c\u5bfc\u81f4\u6574\u4f53\u53cd\u5e94\u901f\u7387\u53d7\u9650\u3002\u5982\u4f55\u7f29\u77ed\u6c22\u8fc1\u79fb\u8def\u5f84\u3001\u964d\u4f4e\u754c\u9762\u8fc1\u79fb\u52bf\u5792\uff0c\u6210\u4e3a\u63d0\u5347\u78b1\u6027HER\u50ac\u5316\u6548\u7387\u7684\u91cd\u8981\u79d1\u5b66\u95ee\u9898\u3002<\/p>\n\n\n\n<p>\u57fa\u4e8e\u4e0a\u8ff0\u80cc\u666f\uff0c\u592a\u539f\u7406\u5de5\u5927\u5b66\u738b\u7f8e\u73b2\u8054\u5408\u5317\u4eac\u7406\u5de5\u5927\u5b66\u5468\u5bb6\u4e1c\u548c\u9f50\u9c81\u5de5\u4e1a\u5927\u5b66\u987e\u5c11\u6960\u63d0\u51fa\u5229\u7528\u9650\u57df-\u70ed\u89e3\u7b56\u7565\uff0c\u5728Mo<sub>2<\/sub>C\u8f7d\u4f53\u4e2d\u6784\u5efa\u94c2\u539f\u5b50\u5c9b\u7ed3\u6784\uff0c\u5efa\u7acb\u4e86\u4e00\u6761\u201c\u65e0\u754c\u9762\u201d\u8d85\u77ed\u6c22\u6ea2\u6d41\u901a\u9053\u3002\u5b9e\u9a8c\u8868\u5f81\u4e0e\u5bc6\u5ea6\u6cdb\u51fd\u7406\u8bba\u8ba1\u7b97\u5171\u540c\u63ed\u793a\uff0c\u539f\u5b50\u5c9b\u5185\u4e0d\u540c\u914d\u4f4d\u73af\u5883\u7684\u94c2\u539f\u5b50\uff08Pt<sub>1<\/sub>\u3001Pt<sub>2<\/sub>\u3001Pt<sub>3<\/sub>\uff09\u5206\u522b\u627f\u62c5H*\u5feb\u901f\u5438\u9644\u3001\u70ed\u4e2d\u6027\u8fc1\u79fb\u53caH<sub>2<\/sub>\u9ad8\u6548\u8131\u9644\u7684\u9636\u68af\u5f0f\u529f\u80fd\uff0c\u4ece\u800c\u5c06\u6c22\u6ea2\u6d41\u8def\u5f84\u4ece\u4f20\u7edf\u8d1f\u8f7d\u578b\u50ac\u5316\u5242\u7684\u8de8\u754c\u9762\u957f\u7a0b\u8fc1\u79fb\u7f29\u77ed\u4e3a\u539f\u5b50\u5c3a\u5ea6\u5185\u7684\u8fde\u7eed\u8fc7\u7a0b\u3002<\/p>\n\n\n\n<p><strong>\u3010\u7814\u7a76\u5de5\u4f5c<\/strong><strong>\u4eae\u70b9<\/strong><strong>\u3011<\/strong><\/p>\n\n\n\n<p>\u672c\u7814\u7a76\u5728Mo<sub>2<\/sub>C\u8f7d\u4f53\u4e2d\u6784\u5efa\u4e86\u94c2\u539f\u5b50\u5c9b\u8fd9\u4e00\u4ecb\u4e8e\u5355\u539f\u5b50\u4e0e\u7eb3\u7c73\u56e2\u7c07\u4e4b\u95f4\u7684\u65b0\u578b\u539f\u5b50\u7ea7\u7ed3\u6784\u3002\u901a\u8fc7\u9650\u57df-\u70ed\u89e3\u7b56\u7565\uff0c\u5b9e\u73b0\u4e86\u94c2\u539f\u5b50\u5728Mo<sub>2<\/sub>C\u6676\u683c\u5185\u8fde\u7eed\u53d6\u4ee3Mo\u4f4d\u70b9\uff0c\u5f62\u6210\u7531\u94c2\u539f\u5b50\u7ec4\u6210\u7684\u539f\u5b50\u5c9b\u3002\u8be5\u7ed3\u6784\u7684\u5173\u952e\u521b\u65b0\u5728\u4e8e\uff1a\u539f\u5b50\u5c9b\u5185\u4e0d\u540c\u914d\u4f4d\u73af\u5883\u7684\u94c2\u539f\u5b50\uff08Pt<sub>1<\/sub>\u3001Pt<sub>2<\/sub>\u3001Pt<sub>3<\/sub>\uff09\u56e0\u4e0eMo<sub>2<\/sub>C\u8f7d\u4f53\u7535\u5b50\u76f8\u4e92\u4f5c\u7528\u5f3a\u5ea6\u7684\u5dee\u5f02\uff0c\u81ea\u53d1\u5f62\u6210\u591a\u529f\u80fd\u4e00\u4f53\u5316\u6d3b\u6027\u4e2d\u5fc3\uff0c\u5728\u540c\u4e00\u7eb3\u7c73\u5c3a\u5ea6\u5355\u5143\u5185\u96c6\u6210\u4e86H*\u5438\u9644\u3001\u8fc1\u79fb\u548c\u8131\u9644\u4e09\u79cd\u4e92\u8865\u529f\u80fd\u3002\u8fd9\u4e0e\u4f20\u7edf\u50ac\u5316\u5242\u4e2d\u9700\u501f\u52a9\u91d1\u5c5e-\u8f7d\u4f53\u754c\u9762\u6216\u4e0d\u540c\u7ec4\u5206\u95f4\u534f\u540c\u5de5\u4f5c\u7684\u6a21\u5f0f\u6709\u672c\u8d28\u533a\u522b\u3002<\/p>\n\n\n\n<p>\u672c\u7814\u7a76\u7684\u6838\u5fc3\u79d1\u5b66\u8d21\u732e\u5728\u4e8e\uff0c\u901a\u8fc7\u539f\u5b50\u5c9b\u7ed3\u6784\u5728\u5355\u7ec4\u5206\u50ac\u5316\u4f53\u7cfb\u5185\u90e8\u5b9e\u73b0\u4e86\u7c7b\u4f3c\u5355\u76f8\u50ac\u5316\u5242\u7684\u539f\u5b50\u7ea7\u6c22\u6ea2\u6d41\u6548\u5e94\u3002\u8be5\u8bbe\u8ba1\u4ece\u6839\u672c\u4e0a\u89c4\u907f\u4e86\u4f20\u7edf\u8d1f\u8f7d\u578b\u50ac\u5316\u5242\u4e2d\u6c22\u7269\u79cd\u8de8\u8fc7\u91d1\u5c5e-\u8f7d\u4f53\u754c\u9762\u6240\u9700\u514b\u670d\u7684\u989d\u5916\u80fd\u5792\u53ca\u957f\u7a0b\u6269\u6563\u8def\u5f84\u3002\u5b9e\u9a8c\u65b9\u9762\uff0c\u6c22\/\u6c18\u52a8\u529b\u5b66\u540c\u4f4d\u7d20\u6548\u5e94\uff08KIE\uff09\u5b9a\u91cf\u5bf9\u6bd4\u8868\u660e\uff0cPt<sub>ai<\/sub>@Mo<sub>2<\/sub>C@PC\u7684KIE\u503c\u663e\u8457\u9ad8\u4e8ePt<sub>sa<\/sub>@Mo<sub>2<\/sub>C@PC\uff0c\u8bf4\u660e\u5728\u5355\u539f\u5b50\u4f53\u7cfb\u4e2d\u6c22\u8fc1\u79fb\u662f\u9650\u5236\u6574\u4f53\u53cd\u5e94\u901f\u7387\u7684\u4e3b\u8981\u52a8\u529b\u5b66\u74f6\u9888\uff0c\u800c\u539f\u5b50\u5c9b\u7ed3\u6784\u7684\u5f15\u5165\u4f7f\u8be5\u6b65\u9aa4\u7684\u52a8\u529b\u5b66\u969c\u788d\u5f97\u5230\u663e\u8457\u7f13\u89e3\u3002\u7406\u8bba\u8ba1\u7b97\u5219\u8fdb\u4e00\u6b65\u63ed\u793a\u4e86\u4e24\u7c7b\u50ac\u5316\u5242\u5728\u6c22\u8fc1\u79fb\u8def\u5f84\u4e0a\u7684\u672c\u8d28\u5dee\u5f02\uff1a\u5bf9\u4e8ePt<sub>ai<\/sub>@Mo<sub>2<\/sub>C@PC\uff0cH\u4eceMo\u4f4d\u70b9\u89e3\u79bb\u6c34\u540e\uff0c\u4f9d\u6b21\u7ecfPt<sub>1<\/sub>\uff08\u5f3a\u5438\u9644\uff0c\u0394G = -0.33 eV\uff09\u2192 Pt<sub>2<\/sub>\uff08\u70ed\u4e2d\u6027\uff0c\u0394G = -0.11&nbsp;eV\uff09\u2192 Pt<sub>3<\/sub>\uff08\u5f31\u5438\u9644\uff0c\u0394G = -0.03 eV\uff09\u5b8c\u6210\u9636\u68af\u5f0f\u6ea2\u6d41\uff0c\u51b3\u901f\u6b65\u80fd\u5792\u4ec5\u4e3a0.27 eV\uff1b\u76f8\u6bd4\u4e4b\u4e0b\uff0cPt<sub>sa<\/sub>@Mo<sub>2<\/sub>C@PC\u4e2d\u5b64\u7acbPt\u4f4d\u70b9\u7f3a\u4e4f\u76f8\u90bb\u539f\u5b50\u7684\u534f\u540c\u63a5\u529b\uff0cH\u9700\u76f4\u63a5\u4ece\u5f3a\u5438\u9644\u4f4d\u70b9\u8131\u9644\u6216\u7ecf\u7531\u8f7d\u4f53\u8868\u9762\u957f\u7a0b\u8fc1\u79fb\uff0c\u76f8\u5e94\u80fd\u5792\u9ad8\u8fbe0.33 eV\u3002\u4e0a\u8ff0\u5b9e\u9a8c\u4e0e\u7406\u8bba\u5bf9\u6bd4\u5171\u540c\u8bc1\u5b9e\uff0c\u539f\u5b50\u5c9b\u7ed3\u6784\u901a\u8fc7\u63d0\u4f9b\u8fde\u7eed\u7684\u5438\u9644\u80fd\u7ea7\u68af\u5ea6\u548c\u8d85\u77ed\u8fc1\u79fb\u8def\u5f84\uff0c\u6709\u6548\u964d\u4f4e\u4e86\u6c22\u6ea2\u6d41\u8fc7\u7a0b\u4e2d\u7684\u80fd\u91cf\u969c\u788d<\/p>\n\n\n\n<p><strong>\u3010<\/strong><strong>\u6570\u636e\u6982\u89c8<\/strong><strong>\u3011<\/strong><\/p>\n\n\n\n<p><strong>\u8981\u70b91\uff1aPt\u539f\u5b50\u5c9b\u50ac\u5316\u5242\uff08Pt<\/strong><strong><sub><strong><sub>ai<\/sub><\/strong><\/sub><\/strong><strong>@Mo<\/strong><strong><sub><strong><sub>2<\/sub><\/strong><\/sub><\/strong><strong>C@PC\uff09\u7684\u5408\u6210\u8def\u5f84\u53ca\u7ed3\u6784\u7279\u5f81\uff1a <\/strong><strong><\/strong><\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"550\" height=\"615\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/ce6e2814f207c93-9.png\" alt=\"\" class=\"wp-image-272516\"\/><\/figure>\n\n\n\n<p>\u56fe1\u3001Pt<sub>ai<\/sub>@Mo<sub>2<\/sub>C@PC \u548c Pt<sub>sa<\/sub>@Mo<sub>2<\/sub>C@PC \u7684\u5408\u6210\u793a\u610f\u56fe\u3002 (b,c) Pt<sub>ai<\/sub>@Mo<sub>2<\/sub>C@PC \u7684 HADDF-STEM \u56fe\u50cf\u3002 (d) \u6cbf (c) \u4e2d\u7684\u7eff\u8272\u77e9\u5f62\u622a\u53d6\u7684\u4e09\u7ef4 (3D) \u8868\u9762\u5f3a\u5ea6\u5256\u9762\u3002 (e,f) Pt<sub>sa<\/sub>@Mo<sub>2<\/sub>C@PC \u7684 HADDF-STEM \u56fe\u50cf\u3002 (g) Pt<sub>ai<\/sub>@Mo<sub>2<\/sub>C@PC\u3001Pt<sub>sa<\/sub>@Mo<sub>2<\/sub>C@PC\u3001Mo<sub>2<\/sub>C\/PC \u548c Pt<sub>np<\/sub>@PC \u7684 XRD \u56fe\u3002 Pt<sub>ai<\/sub>@Mo<sub>2<\/sub>C@PC \u548c Pt<sub>sa<\/sub>@Mo<sub>2<\/sub>C@PC \u7684\u793a\u610f\u56fe\u5982\u56fe 1c\u3001f \u6240\u793a\uff1bPt\u539f\u5b50\u5c9b\u7528\u9ec4\u8272\u6846\u6807\u8bb0\uff0c\u800c\u5b64\u7acb\u7684 Pt \u5355\u539f\u5b50\u7528\u7ea2\u8272\u5706\u5708\u7a81\u51fa\u663e\u793a\u3002<\/p>\n\n\n\n<p>\u56fe1 \u4ece\u5408\u6210-\u5f62\u8c8c-\u6676\u76f8\u4e09\u4e2a\u5c42\u9762\uff0c\u8bc1\u5b9e\u4e86Pt<sub>ai<\/sub>@Mo<sub>2<\/sub>C@PC\u4e2d\u94c2\u539f\u5b50\u5c9b\u7684\u6210\u529f\u6784\u5efa\uff0c\u5e76\u63ed\u793a\u4e86\u5176\u4e0e\u5355\u539f\u5b50\u50ac\u5316\u5242\u5728\u7ed3\u6784\u4e0a\u7684\u672c\u8d28\u5dee\u5f02\u2014\u2014\u5373\u539f\u5b50\u5c9b\u5185Pt-Pt\u76f8\u90bb\u539f\u5b50\u53ca\u76f8\u5e94\u7684\u6676\u683c\u5e94\u53d8\u6548\u5e94\uff0c\u4e3a\u540e\u7eed\u63a2\u7a76\u5176\u591a\u529f\u80fd\u6d3b\u6027\u4e2d\u5fc3\u53ca\u6c22\u6ea2\u6d41\u673a\u5236\u63d0\u4f9b\u4e86\u7ed3\u6784\u57fa\u7840\u3002<\/p>\n\n\n\n<p><strong>\u8981\u70b92\uff1a<\/strong><strong>\u914d\u4f4d\u4fe1\u606f\u7b49\u7684\u8868\u5f81<\/strong><strong><\/strong><\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"700\" height=\"380\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/7f88dbbcaa77a1d-10.png\" alt=\"\" class=\"wp-image-272517\"\/><\/figure>\n\n\n\n<p>\u56fe2 (a) Pt<sub>ai<\/sub>@Mo<sub>2<\/sub>C@PC\u3001Pt<sub>sa<\/sub>@Mo<sub>2<\/sub>C@PC \u548c Mo<sub>2<\/sub>C\/PC \u7684 Mo 3<em>d<\/em>&nbsp;\u7684 XPS \u8c31\u3002 (b) Pt<sub>ai<\/sub>@Mo<sub>2<\/sub>C@PC \u548c Pt<sub>sa<\/sub>@Mo<sub>2<\/sub>C@PC \u7684 Pt 4<em>f<\/em>&nbsp;\u7684 XPS \u8c31\u3002 (c,d) Pt L3 \u8fb9\u7f18\u7684 XANES \u5149\u8c31\u548c FT-EXAFS \u5149\u8c31\u3002 (e,f) Pt<sub>ai<\/sub>@Mo<sub>2<\/sub>C@PC \u548c Pt<sub>sa<\/sub>@Mo<sub>2<\/sub>C@PC \u89e3\u5438\u8fc7\u7a0b\u540e\u5438\u9644\u7684 CO \u7684 CO-IR \u5149\u8c31<\/p>\n\n\n\n<p>\u56fe2\u4e2dXPS\u663e\u793aMo\u5411Pt\u53d1\u751f\u7535\u5b50\u8f6c\u79fb\uff0c\u4e14\u539f\u5b50\u5c9b\u5185Pt\u7684\u7ed3\u5408\u80fd\u9ad8\u4e8e\u5355\u539f\u5b50\u4f53\u7cfb\uff0c\u5f52\u56e0\u4e8e\u7535\u5b50\u5728\u591a\u4e2aPt\u539f\u5b50\u95f4\u7684\u79bb\u57df\u5316\u6548\u5e94\u3002EXAFS\u5b9a\u91cf\u62df\u5408\u5f97\u51faPt<sub>ai<\/sub>\u4e2dPt\u2013Pt\u914d\u4f4d\u6570\u4e3a5.1\u3001Pt\u2013Mo\u914d\u4f4d\u6570\u4e3a8.1\uff0c\u786e\u8ba4Pt\u53d6\u4ee3Mo\u6676\u683c\u4f4d\u70b9\u5f62\u6210\u539f\u5b50\u5c9b\u3002CO\u7ea2\u5916\u4ece\u5206\u5b50\u63a2\u9488\u5c42\u9762\u6392\u9664\u4e86\u91d1\u5c5e\u6001Pt\u9897\u7c92\u7684\u5b58\u5728\u3002<\/p>\n\n\n\n<p><strong>\u8981\u70b93\uff1aHER\u6027\u80fd\u6d4b\u8bd5:<\/strong><strong><\/strong><\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"600\" height=\"485\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/4e9a0ba2491dfde-10.png\" alt=\"\" class=\"wp-image-272518\"\/><\/figure>\n\n\n\n<p>\u56fe3 Pt<sub>ai<\/sub>@Mo<sub>2<\/sub>C@PC\u7684\u50ac\u5316\u6027\u80fd<\/p>\n\n\n\n<p>\u56fe3\u663e\u793aPt<sub>ai<\/sub>@Mo<sub>2<\/sub>C@PC\u5728\u78b1\u6027HER\u4e2d\u8fc7\u7535\u4f4d\uff08\u03b7<sub>10<\/sub>=11.8 mV\uff0c\u03b7<sub>100<\/sub>=52.9 mV\uff09\u3001Tafel\u659c\u7387\uff0828.13 mV dec<sup>-1<\/sup>\uff09\u53ca\u8d28\u91cf\u6d3b\u6027\uff083.13 A mg&nbsp;Pt<sup>-1<\/sup>\uff09\u5747\u663e\u8457\u4f18\u4e8ePt<sub>sa<\/sub>@Mo<sub>2<\/sub>C@PC\u53ca\u5546\u7528Pt\/C\u3002AEMWE\u5668\u4ef6\u57281.0 A cm<sup>-2<\/sup>\u5de5\u4e1a\u7ea7\u7535\u6d41\u5bc6\u5ea6\u4e0b\u4ec5\u97001.77 V\uff0c\u7a33\u5b9a\u8fd0\u884c200\u5c0f\u65f6\u65e0\u8870\u51cf\uff0c\u7efc\u5408\u6027\u80fd\u5728\u5df2\u62a5\u9053\u7684AEMWE\u9634\u6781\u50ac\u5316\u5242\u4e2d\u5904\u4e8e\u9886\u5148\u5730\u4f4d\uff0c\u9a8c\u8bc1\u4e86\u539f\u5b50\u5c9b\u7ed3\u6784\u5728\u5b9e\u9645\u5668\u4ef6\u4e2d\u7684\u53ef\u884c\u6027\u4e0e\u7a33\u5b9a\u6027\u3002<\/p>\n\n\n\n<p><strong>\u8981\u70b94\uff1a<\/strong><strong>\u5185\u7f6e\u6c22\u6ea2\u6d41\u9a8c\u8bc1<\/strong><strong><\/strong><\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"750\" height=\"390\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/b14210e1ee30421-9.png\" alt=\"\" class=\"wp-image-272519\"\/><\/figure>\n\n\n\n<p>\u56fe4 \u6c22\u6ea2\u6d41\u7684\u89c1\u89e3<\/p>\n\n\n\n<p>\u56fe4\u6c22\/\u6c18\u52a8\u529b\u5b66\u540c\u4f4d\u7d20\u6548\u5e94\uff08KIE\uff09\u663e\u793aPt<sub>ai<\/sub>\u7684KIE\u503c\u663e\u8457\u9ad8\u4e8ePt<sub>sa<\/sub>\uff0c\u5b9a\u91cf\u8868\u660e\u539f\u5b50\u5c9b\u7ed3\u6784\u4f7f\u6c22\u8fc1\u79fb\u6b65\u9aa4\u7684\u52a8\u529b\u5b66\u969c\u788d\u5f97\u5230\u663e\u8457\u7f13\u89e3\uff0c\u800c\u5355\u539f\u5b50\u4f53\u7cfb\u4e2d\u6c22\u8fc1\u79fb\u662f\u9650\u5236\u6574\u4f53\u53cd\u5e94\u901f\u7387\u7684\u74f6\u9888\u3002CO\u5265\u79bb\u4e0ePt\u4e2d\u6bd2\u5b9e\u9a8c\u8fdb\u4e00\u6b65\u786e\u8ba4Pt\u4e3a\u6d3b\u6027\u4e2d\u5fc3\uff0c\u539f\u4f4d\u5149\u8c31\u672a\u68c0\u6d4b\u5230OH\u79ef\u7d2f\uff0c\u95f4\u63a5\u652f\u6301\u539f\u5b50\u5c9b\u4fc3\u8fdbH\u5feb\u901f\u8f6c\u79fb\u3001\u907f\u514d\u6d3b\u6027\u4f4d\u70b9\u88abOH*\u6bd2\u5316\u7684\u673a\u5236\u3002<\/p>\n\n\n\n<p><strong>\u8981\u70b95\uff1a<\/strong><strong>\u5185\u7f6e<\/strong><strong>H<\/strong><strong>\u6ea2\u6d41<\/strong><strong>\u673a\u5236\uff1a<\/strong><\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"550\" height=\"539\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/de5bcf7d8eaea98-8.png\" alt=\"\" class=\"wp-image-272520\"\/><\/figure>\n\n\n\n<p>\u56fe5 \u7406\u8bba\u8ba1\u7b97\u63a2\u8ba8H\u6ea2\u51fa\u7f13\u51b2\u673a\u5236<\/p>\n\n\n\n<p>\u56fe5\u7406\u8bba\u8ba1\u7b97\u9a8c\u8bc1\u539f\u5b50\u5c9b\u5185\u4e0d\u540c\u914d\u4f4d\u73af\u5883\u7684\u94c2\u539f\u5b50\uff08Pt<sub>1<\/sub>\u3001Pt<sub>2<\/sub>\u3001Pt<sub>3<\/sub>\uff09\u5206\u522b\u627f\u62c5H*\u5feb\u901f\u5438\u9644\u3001\u70ed\u4e2d\u6027\u8fc1\u79fb\u53caH<sub>2<\/sub>\u9ad8\u6548\u8131\u9644\u7684\u9636\u68af\u5f0f\u529f\u80fd\u3002<\/p>\n\n\n\n<p><strong>05 <\/strong><strong>\u603b\u7ed3\u4e0e\u5c55\u671b<\/strong><strong><\/strong><\/p>\n\n\n\n<p>\u672c\u7814\u7a76\u901a\u8fc7\u5728Mo<sub>2<\/sub>C\u8f7d\u4f53\u4e2d\u6784\u5efa\u94c2\u539f\u5b50\u5c9b\u7ed3\u6784\uff0c\u5b9e\u73b0\u4e86\u50ac\u5316\u5242\u5185\u90e8\u591a\u529f\u80fd\u6d3b\u6027\u4e2d\u5fc3\u7684\u96c6\u6210\uff0c\u5efa\u7acb\u4e86\u4e00\u6761\u5185\u7f6e\u8d85\u77ed\u6c22\u6ea2\u6d41\u901a\u9053\u3002\u5b9e\u9a8c\u4e0e\u7406\u8bba\u8ba1\u7b97\u5171\u540c\u8868\u660e\uff0c\u8be5\u8bbe\u8ba1\u6709\u6548\u964d\u4f4e\u4e86\u6c22\u8fc1\u79fb\u8fc7\u7a0b\u4e2d\u7684\u80fd\u5792\uff0c\u663e\u8457\u63d0\u5347\u4e86\u78b1\u6027HER\u52a8\u529b\u5b66\u6027\u80fd\u3002\u8be5\u5de5\u4f5c\u4e3a\u8d1f\u8f7d\u578b\u50ac\u5316\u5242\u4e2d\u6c22\u6ea2\u6d41\u6548\u5e94\u7684\u8c03\u63a7\u63d0\u4f9b\u4e86\u53ef\u53c2\u8003\u7684\u8bbe\u8ba1\u601d\u8def\uff0c\u5bf9\u78b1\u6027\u6c34\u7535\u89e3\u5236\u6c22\u6280\u672f\u7684\u8fdb\u4e00\u6b65\u53d1\u5c55\u5177\u6709\u4e00\u5b9a\u501f\u9274\u610f\u4e49\u3002<\/p>\n\n\n\n<p><strong>\u3010<\/strong><strong>\u6587\u732e\u4fe1\u606f<\/strong><strong>\u3011<\/strong><\/p>\n\n\n\n<p>Qin Li, Jianhong Lan, Xuguang Liu, Longyi Fu, Yadi Guan, Shaonan Gu, Jiadong Zhou, Meiling Wang, Advanced Functional Materials, 2026, DOI: https:\/\/doi.org\/10.1002\/adfm.77151.<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u7b2c\u4e00\u4f5c\u8005\uff1a\u674e\u94a6\u3001\u5170\u5efa\u5b8f \u901a\u8baf\u4f5c\u8005\uff1a\u987e\u5c11\u6960\u3001\u5468\u5bb6\u4e1c\u3001\u738b\u7f8e\u73b2 \u901a\u8baf\u5355\u4f4d\uff1a\u592a\u539f\u7406\u5de5\u5927\u5b66\u3001\u5317\u4eac\u7406\u5de5\u5927\u5b66\u3001\u9f50\u9c81\u5de5\u4e1a\u5927\u5b66 \u8bba\u6587DOI\uff1ahttps:\/\/doi.org\/10&#8230;.<\/p>\n","protected":false},"author":31345,"featured_media":0,"comment_status":"open","ping_status":"","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[2],"tags":[],"class_list":["post-272502","post","type-post","status-publish","format-standard","hentry","category-keji"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/272502"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/31345"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=272502"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/272502\/revisions"}],"predecessor-version":[{"id":272521,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/272502\/revisions\/272521"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=272502"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=272502"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=272502"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}