{"id":272573,"date":"2026-07-23T21:04:00","date_gmt":"2026-07-23T13:04:00","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=272573"},"modified":"2026-07-22T23:09:37","modified_gmt":"2026-07-22T15:09:37","slug":"%e5%8d%8e%e7%a7%91%e5%a4%a7%e9%bb%84%e4%ba%91%e8%be%89-%e8%a3%b4%e9%9d%9eam%ef%bc%9a%e6%a2%af%e5%ba%a6%e5%85%b1%e4%bb%b7-%e9%9d%9e%e5%85%b1%e4%bb%b7%e5%8a%a8%e6%80%81%e9%94%ae%e7%95%8c%e9%9d%a2","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=272573","title":{"rendered":"\u534e\u79d1\u5927\u9ec4\u4e91\u8f89\/\u88f4\u975eAM\uff1a\u68af\u5ea6\u5171\u4ef7-\u975e\u5171\u4ef7\u52a8\u6001\u952e\u754c\u9762\u81ea\u4fee\u590d\u805a\u5408\u7269\u7535\u89e3\u8d28\u53ca\u5176\u57284.6 V\u7ea7\u9502\u91d1\u5c5e\u7535\u6c60\u4e2d\u7684\u5e94\u7528"},"content":{"rendered":"\n<p><strong>1.\u7814\u7a76\u80cc\u666f<\/strong><strong><\/strong><\/p>\n\n\n\n<p>\u56fa\u6001\u7535\u89e3\u8d28\uff08SSEs\uff09\u662f\u4e0b\u4e00\u4ee3\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u9502\uff08Li\uff09\u7535\u6c60\u7684\u5173\u952e\u7a81\u7834\u6027\u6280\u672f\uff0c\u5176\u4e0e\u9ad8\u538b\u6b63\u6781\u6750\u6599\uff08\u5982LiCoO<sub>2<\/sub>&nbsp;(LCO)\u3001\u5bcc\u954d\u5c42\u72b6LiNi<sub>0.8<\/sub>Co<sub>0.1<\/sub>Mn<sub>0.1<\/sub>O<sub>2<\/sub>&nbsp;(NCM811) \u4ee5\u53ca\u5bcc\u9502\u9530\u57fa\u6c27\u5316\u7269\uff09\u5177\u6709\u4f18\u5f02\u7684\u517c\u5bb9\u6027\u3002\u5c06\u5176\u4e0e\u9ad8\u5bb9\u91cf\u8d1f\u6781\uff08\u5982\u9502\u91d1\u5c5e\u6216\u7845\u78b3\uff08Si-C\uff09\uff09\u76f8\u7ed3\u5408\uff0c\u53ef\u5b9e\u73b0\u8d85\u8fc7500 Wh kg<sup>\u22121<\/sup>\u7684\u7535\u82af\u7ea7\u80fd\u91cf\u5bc6\u5ea6\uff0c\u540c\u65f6\u5177\u5907\u9ad8\u5b89\u5168\u6027\u3002\u7136\u800c\uff0c\u672c\u5f81\u521a\u6027\u7684\u65e0\u673a\u56fa\u6001\u7535\u89e3\u8d28\uff08\u4f8b\u5982\u6c27\u5316\u7269\u548c\u786b\u5316\u7269\u56fa\u6001\u7535\u89e3\u8d28\uff09\u4ee5\u53ca\u67d4\u6027\u805a\u5408\u7269\u7535\u89e3\u8d28\u9762\u4e34\u4e00\u4e2a\u6839\u672c\u6027\u6311\u6218\uff1a\u7535\u6781\u6750\u6599\u5728\uff08\u8131\uff09\u9502\u5316\u8fc7\u7a0b\u4e2d\u4f1a\u53d1\u751f\u663e\u8457\u7684\u4f53\u79ef\u53d8\u5316\u3002\u8fd9\u4f1a\u5728\u7535\u6781-\u7535\u89e3\u8d28\u754c\u9762\u4ea7\u751f\u5de8\u5927\u7684\u5e94\u529b\/\u5e94\u53d8\u96c6\u4e2d\uff0c\u8fdb\u800c\u5728\u56fa\u6001\u7535\u89e3\u8d28\u6216\u754c\u9762\u5c42\u4e2d\u5f15\u53d1\u5fae\u88c2\u7eb9\u548c\u7269\u7406\u5265\u79bb\u3002\u8fd9\u79cd\u529b\u5b66\u9000\u5316\u4f1a\u7834\u574f\u754c\u9762\u79bb\u5b50\u4f20\u8f93\uff0c\u5e76\u5347\u9ad8\u5c40\u90e8\u7535\u6d41\u5bc6\u5ea6\uff0c\u4ece\u800c\u52a0\u901f\u9502\u679d\u6676\u7684\u751f\u957f\uff0c\u5bfc\u81f4\u9ad8\u538b\u9502\u91d1\u5c5e\u7535\u6c60\u5bb9\u91cf\u5feb\u901f\u8870\u51cf\u4e0e\u7535\u6c60\u5931\u6548\u3002<\/p>\n\n\n\n<p><strong>2.\u6210\u679c\u63a0\u5f71<\/strong><strong><\/strong><\/p>\n\n\n\n<p>\u8fd1\u65e5\uff0c\u9ec4\u4e91\u8f89\u3001\u88f4\u975e\u56e2\u961f\u6210\u529f\u5408\u6210\u4e86\u4e00\u79cd\u57fa\u4e8e\u68af\u5ea6\u5171\u4ef7-\u975e\u5171\u4ef7\u52a8\u6001\u952e\u7684\u754c\u9762\u81ea\u4fee\u590d\u805a\u5408\u7269\u7535\u89e3\u8d28\uff08SHPE\uff09\uff0c\u4ee5\u5b9e\u73b0\u56fa\u6001\u9502\u7535\u6c60\u5728\u5168\u5bff\u547d\u671f\u95f4\u7684\u591a\u754c\u9762\u81ea\u4e3b\u4fee\u590d\u3002\u901a\u8fc7\u5206\u5b50\u5de5\u7a0b\uff0c\u5c06\u9ad8\u5f3a\u5ea6\u7684\u787c\u9178\u916f\u952e\u4e0e\u8d85\u5feb\u52a8\u6001\u54cd\u5e94\u7684\u6c22\u952e\u76f8\u7ed3\u5408\uff0c\u5b9e\u73b0\u4e86SSLBs\u754c\u9762\u7f3a\u9677\u7684\u9ad8\u6548\u5ba4\u6e29\u81ea\u4fee\u590d\u3002\u805a\u5408\u7269\u94fe\u4e4b\u95f4\u7684\u5feb\u901f\u52a8\u6001\u4ea4\u6362\u8fdb\u4e00\u6b65\u4fc3\u8fdb\u4e86\u9502\u79bb\u5b50\u7684\u5feb\u901f\u4f20\u5bfc\uff0c\u5ba4\u6e29\uff0825 \u00b0C\uff09\u4e0b\u79bb\u5b50\u7535\u5bfc\u7387\u8fbe\u52301.6 \u00d7 10<sup>\u22123<\/sup>&nbsp;S cm<sup>\u22121<\/sup>\u3002Li|SHPE|Li\u7535\u6c60\u8868\u73b0\u51fa\u8d85\u8fc73000\u5c0f\u65f6\u7684\u7a33\u5b9a\u5faa\u73af\u3002\u5f15\u5165\u8010\u6c27\u5316\u7684\u542b\u787c\u548c\u542b\u6c1f\u5b98\u80fd\u56e2\uff0c\u5c06\u7535\u5316\u5b66\u7a97\u53e3\u62d3\u5bbd\u81f35.2 V\u3002LiFePO<sub>4<\/sub>|SHPE|Li\u548cLiCoO<sub>2<\/sub>\uff08LCO\uff09|SHPE|Li\u7535\u6c60\u5206\u522b\u5b9e\u73b0\u4e86\u8d85\u8fc71000\u6b21\u548c700\u6b21\u5faa\u73af\uff0c\u5373\u4f7f\u5728\u9ad8\u7535\u538b\uff084.6 V\uff09\u3001\u9ad8\u8f7d\u91cf\uff0814 mg cm<sup>\u22122<\/sup>\uff09\u6761\u4ef6\u4e0b\uff0c\u4e5f\u80fd\u7a33\u5b9a\u5de5\u4f5c\u3002\u6700\u7ec8\u5339\u914d\u9ad8\u538bLCO\u6b63\u6781\u53ef\u4ee5\u5b9e\u73b0354 Wh kg<sup>\u22121<\/sup>\u7684\u8f6f\u5305\u7535\u6c60\u7a33\u5b9a\u5faa\u73af200\u6b21\uff0c\u5e76\u987a\u5229\u901a\u8fc7\u9488\u523a\u5b89\u5168\u6d4b\u8bd5\u3002\u672c\u7814\u7a76\u7684\u68af\u5ea6\u8bbe\u8ba1\u7b56\u7565\u4e3a\u5f00\u53d1\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u3001\u957f\u5bff\u547d\u548c\u5b89\u5168\u56fa\u6001\u7535\u6c60\u63d0\u4f9b\u4e86\u4e00\u79cd\u81ea\u4fee\u590d\u6750\u6599\u4f53\u7cfb\u548c\u65b0\u7684\u8bbe\u8ba1\u8303\u5f0f\u3002\u76f8\u5173\u7814\u7a76\u4ee5\u201cInterfacial Self-healing Polymer Electrolytes with Gradient Covalent-Noncovalent Dynamic Bonds for 4.6 V-Class Lithium Metal Batteries\u201d\u4e3a\u9898\u53d1\u8868\u5728\u56fd\u9645\u77e5\u540d\u671f\u520a\u300aAdvanced Materials\u300b\u4e0a\uff0c\u7855\u58eb\u751f\u9ad8\u5f3a\u4e3a\u672c\u6587\u7b2c\u4e00\u4f5c\u8005\u3002<\/p>\n\n\n\n<p><strong>3.\u6838\u5fc3\u521b\u65b0\u70b9<\/strong><strong><\/strong><\/p>\n\n\n\n<p>\u8981\u70b9\u4e00\uff1a\u5206\u5b50\u7ed3\u6784\u8bbe\u8ba1\u5b9e\u73b0\u9ad8\u79bb\u5b50\u7535\u5bfc\u7387<\/p>\n\n\n\n<p>\u901a\u8fc7\u5206\u5b50\u7ed3\u6784\u8bbe\u8ba1\uff0c\u5728\u805a\u5408\u7269\u4e3b\u94fe\u4e2d\u5f15\u5165\u4e86\u9ad8\u952e\u80fd\u7684\u787c\u9178\u916f\u952e\uff08\u52a8\u6001\u5171\u4ef7\u952e\uff09\u548c\u5feb\u901f\u53ef\u9006\u7684\u6c22\u952e\uff08\u975e\u5171\u4ef7\u952e\uff09\u3002\u4e30\u5bcc\u7684\u7fb0\u57fa\u6c27\u3001\u919a\u6c27\u4ee5\u53ca\u52a8\u6001\u787c\u9178\u916f\u952e\u4fc3\u8fdb\u4e86Li\u207a\u7684\u4f20\u8f93\uff0c\u4f7f\u5f97\u572825 \u00b0C\u4e0b\u7684\u5ba4\u6e29\u79bb\u5b50\u7535\u5bfc\u7387\u8fbe\u52301.6 \u00d7 10<sup>\u22123<\/sup>&nbsp;S cm<sup>\u22121<\/sup>\u3002<\/p>\n\n\n\n<p>\u8981\u70b9\u4e8c\uff1a\u68af\u5ea6\u52a8\u6001\u952e\u8bbe\u8ba1\u5b9e\u73b0\u5ba4\u6e29\u81ea\u4fee\u590d<\/p>\n\n\n\n<p>\u4f4e\u952e\u80fd\u7684\u975e\u5171\u4ef7\u952e\u5728\u5ba4\u6e29\u4e0b\u5177\u6709\u8d85\u5feb\u7684\u52a8\u6001\u54cd\u5e94\u7279\u6027\uff0c\u80fd\u591f\u5728\u6570\u79d2\u5185\u5b9e\u73b0\u5bf9\u7eb3\u7c73\u7ea7\u5fae\u88c2\u7eb9\u7684\u521d\u59cb\u4fee\u590d\uff1b\u800c\u9ad8\u952e\u80fd\u7684\u52a8\u6001\u5171\u4ef7\u952e\u5219\u53ef\u6709\u6548\u4fee\u590d\u7535\u6c60\u5faa\u73af\u8fc7\u7a0b\u4e2d\u7d2f\u79ef\u7684\u5fae\u7c73\u7ea7\u5e94\u529b\u635f\u4f24\u3002\u8fd9\u79cd\u68af\u5ea6\u952e\u80fd\u5206\u5e03\u514b\u670d\u4e86\u787c\u9178\u916f\u952e\u5728\u5ba4\u6e29\u4e0b\u81ea\u4fee\u590d\u80fd\u529b\u4e0d\u8db3\u7684\u5e38\u89c1\u95ee\u9898\uff0c\u5b9e\u73b0\u4e86\u5ba4\u6e29\u4e0b\u56fa\u6001\u9502\u91d1\u5c5e\u7535\u6c60\uff08SSLBs\uff09\u754c\u9762\u7f3a\u9677\u7684\u9ad8\u6548\u81ea\u4fee\u590d\u3002<\/p>\n\n\n\n<p>\u8981\u70b9\u4e09\uff1a\u6784\u5efa\u5bcc\u542b\u65e0\u673a\u7ec4\u5206\u7684\u9ad8\u7535\u538b\u7a33\u5b9a\u754c\u9762\u5c42<\/p>\n\n\n\n<p>\u539f\u4f4d\u805a\u5408\u786e\u4fdd\u4e86\u7535\u6781\/\u7535\u89e3\u8d28\u7684\u7d27\u5bc6\u63a5\u89e6\uff0c\u5927\u5e45\u964d\u4f4e\u4e86\u754c\u9762\u7535\u963b\u3002\u542b\u6c1f\u5355\u4f53\u9884\u5148\u5f62\u6210\u4e86\u5bcc\u542bLiF\u7684\u65e0\u673a\u949d\u5316\u5c42\uff0c\u540c\u65f6\u787c\u9178\u916f\u5355\u5143\u751f\u6210\u4e86B-O\u7269\u79cd\u3002\u8fd9\u4e9b\u7ec4\u5206\u65e2\u80fd\u6709\u6548\u6291\u5236\u754c\u9762\u526f\u53cd\u5e94\uff0c\u53c8\u4fdd\u6301\u4e86\u673a\u68b0\u7a33\u5065\u6027\uff0c\u5e76\u5c06\u7535\u5316\u5b66\u7a97\u53e3\u62d3\u5bbd\u81f35.2 V\u3002<\/p>\n\n\n\n<p><strong>4.\u6570\u636e\u6982\u89c8<\/strong><strong><\/strong><\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"650\" height=\"450\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/2382c315a6ba396-18.png\" alt=\"\" class=\"wp-image-272574\"\/><\/figure>\n\n\n\n<p><strong>\u56fe1. \u52a8\u6001SHPE\u7684\u5206\u5b50\u7ed3\u6784\u8bbe\u8ba1\u3002<\/strong>a) IEM PFHE \u548c PCL IEM \u7684\u5316\u5b66\u7ed3\u6784\u3002b) \u4ea4\u8054\u5242 BDB \u7684\u5206\u5b50\u7ed3\u6784\u3002c\u3001d) B F SHPE \u7684\u5206\u5b50\u7ed3\u6784 (c) \u53ca\u5176\u754c\u9762\u81ea\u4fee\u590d\u7684\u5fae\u89c2\u673a\u7406 (d)\u3002e\u3001f) B F SHPE \u4e2d\u52a8\u6001\u787c\u9178\u916f\u952e (e) \u548c\u6c22\u952e (f) \u7684\u793a\u610f\u56fe\u3002g) B F SHPE \u754c\u9762\u81ea\u4fee\u590d\u8fc7\u7a0b\u7684\u793a\u610f\u56fe\u3002h) B F SHPE \u589e\u5f3a LCO||Li \u7535\u6c60\u4e2d\u7535\u6781 \u7535\u89e3\u8d28\u754c\u9762\u7a33\u5b9a\u6027\u7684\u673a\u7406\u3002<strong><\/strong><\/p>\n\n\n\n<p>\u67d4\u6027\u805a\u5df1\u5185\u916f\u901a\u8fc7\u5f02\u6c30\u9178\u916f\u548c\u7f9f\u57fa\u4e4b\u95f4\u7684\u4eb2\u6838\u52a0\u6210\u53cd\u5e94\u5b9e\u73b0\u672b\u7aef\u529f\u80fd\u5316\uff0c\u5c06\u60f0\u6027\u94fe\u6bb5\u8f6c\u5316\u4e3a\u53ef\u805a\u5408\u7684\u70ef\u70c3\u529f\u80fd\u5316\u5355\u4f53\u3002\u5f15\u5165\u5bccF\u7684PFHE\uff0c\u6709\u6548\u5c06PCL\u916f\u57fa\u56e2\u4f18\u8d8a\u7684Li<sup>+<\/sup>\u5bfc\u7535\u6027\u4e0ePFHE\u7684\u7535\u5316\u5b66\u7a97\u53e3\u62d3\u5bbd\u80fd\u529b\u6574\u5408\uff08\u56fea\uff09\u3002\u968f\u540e\uff0cBDB\u88ab\u7528\u4f5c\u52a8\u6001\u4ea4\u8054\u5242\uff08\u56feb\uff09\u3002\u7ebf\u6027\u524d\u9a71\u4f53\u901a\u8fc7\u9ad8\u6548\u7684\u786b\u9187-\u70ef\u70b9\u51fb\u5316\u5b66\u53cd\u5e94\u8fdb\u4e00\u6b65\u4ea4\u8054\u6210\u4e09\u7ef4\u805a\u5408\u7269\u7f51\u7edc\uff08\u56fec\uff09\u3002\u91c7\u7528\u539f\u4f4d\u805a\u5408\u7684\u5408\u6210\u7b56\u7565\uff0c\u4ea7\u751f\u4e86\u9ad8\u6027\u80fd\u805a\u5408\u7269\u7535\u89e3\u8d28\uff0c\u5177\u6709\u826f\u597d\u7684\u81ea\u6108\u5408\u7279\u6027\uff08\u56fed-g\uff09\u3001\u754c\u9762\u517c\u5bb9\u6027\u4ee5\u53ca\u9ad8\u7535\u538b\u7a33\u5b9a\u6027\uff08\u56feh\uff09\u3002<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"600\" height=\"503\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/ce6e2814f207c93-16.png\" alt=\"\" class=\"wp-image-272575\"\/><\/figure>\n\n\n\n<p><strong>\u56fe2. SHPFs\u548cSHPEs\u7684\u7269\u7406\u5316\u5b66\u8868\u5f81\u3002<\/strong>a) B F SHPF\u7684\u5085\u91cc\u53f6\u53d8\u6362\u7ea2\u5916\u5149\u8c31\uff08FTIR\uff09\u3002b) PCL\u3001IEM\u548cB F SHPF\u4e2d\u7fb0\u57fa\u7684FTIR\u5149\u8c31\u3002c) \u5408\u6210\u7684IEM PFHE\u548cBDB\u5728CDCl<sub>3<\/sub>\u4e2d\u76841H\u6838\u78c1\u5171\u632f\uff08NMR\uff09\u8c31\u3002d) SHPFs\u7684X\u5c04\u7ebf\u884d\u5c04\uff08XRD\uff09\u56fe\u8c31\u3002e) SHPFs\u7684\u539f\u5b50\u529b\u663e\u5fae\u955c\uff08AFM\uff09\u56fe\u50cf\u3002f) \u6db2\u6001\u7535\u89e3\u8d28\uff08LE\uff09\u548cSHPEs\u4e2dPF<sub>6<\/sub>\u207b\u7684\u62c9\u66fc\u5149\u8c31\u3002g) \u57fa\u4e8eSHPEs\u7684Li||Li\u5bf9\u79f0\u7535\u6c60\u7684\u5854\u83f2\u5c14\uff08Tafel\uff09\u66f2\u7ebf\u3002h) SHPEs\u7684\u79bb\u5b50\u7535\u5bfc\u7387\u968f\u6e29\u5ea6\u7684\u53d8\u5316\u5173\u7cfb\u3002i) SHPEs\u7684\u7ebf\u6027\u626b\u63cf\u4f0f\u5b89\uff08LSV\uff09\u66f2\u7ebf\u3002j) \u5728Li|SHPEs|Cu\u7535\u6c60\u4e2d\uff0c\u4ee51 mAh cm<sup>\u22122<\/sup>\u7684\u622a\u6b62\u5bb9\u91cf\u8fdb\u884c\u9502\u6c89\u79ef \u5265\u79bb\u6d4b\u8bd5\u7684\u5e73\u5747\u5e93\u4ed1\u6548\u7387\uff08CE<sub>avg<\/sub>\uff09\u3002k) \u626b\u63cf\u7535\u5b50\u663e\u5fae\u955c\uff08SEM\uff09\u56fe\u50cf\uff0c\u5c55\u793a\u4f7f\u7528\u4e0d\u540cSHPEs\u65f6\uff0c\u5728\u94dc\u96c6\u6d41\u4f53\u4e0a\u4ee50.3 mA cm<sup>\u22122<\/sup>\u548c0.3 mA cm<sup>\u22122<\/sup>\u6761\u4ef6\u6c89\u79ef\u7684\u9502\u91d1\u5c5e\u8868\u9762\u5f62\u8c8c\u3002<\/p>\n\n\n\n<p>FT-IR\u548cNMR\u5171\u540c\u8bc1\u5b9e\u4e86\u805a\u5408\u7269\u7684\u6210\u529f\u5408\u6210\u4ee5\u53ca\u787c\u9178\u916f\u952e\u548c\u6c22\u952e\u7684\u5171\u5b58\uff08\u56fea-c\uff09\uff1bXRD\u548cAFM\u8868\u660e\u5408\u6210\u7684\u805a\u5408\u7269\u5177\u6709\u66f4\u4f4e\u7684\u7ed3\u6676\u5ea6\u548c\u66f4\u5149\u6ed1\u7684\u8868\u9762\uff0c\u6709\u5229\u4e8e\u9502\u79bb\u5b50\u4f20\u8f93\u548c\u754c\u9762\u63a5\u89e6\uff08\u56fed\u3001e\uff09\uff1b\u62c9\u66fc\u5149\u8c31\u5206\u6790\u4e86SHPE\u4e2dLi<sup>+<\/sup>\u7684\u6eb6\u5242\u5316\u7ed3\u6784\uff0c\u5728\u6240\u6709\u6837\u54c1\u4e2d\uff0cB-F-SHPE\u8868\u73b0\u51fa\u6700\u9ad8\u7684\u6e38\u79bbPF<sub>6<\/sub><sup>\u2212<\/sup>\uff0c\u8fd9\u5f52\u56e0\u4e8e\u5176\u663e\u8457\u8f83\u4f4e\u7684\u7ed3\u6676\u5ea6\uff0c\u4ee5\u53ca\u9ad8\u6781\u6027\u57fa\u56e2\uff08C=O\u548cC\u2013F\uff09\u548c\u8def\u6613\u65af\u9178\u6027B\u4e2d\u5fc3\u4fc3\u8fdbLiPF<sub>6<\/sub>\u89e3\u79bb\uff08\u56fef\uff09\uff1b\u57fa\u7840\u7535\u5316\u5b66\u6d4b\u8bd5\u8868\u660eB-F-SHPE\u5177\u6709\u6700\u9ad8\u7684\u754c\u9762\u53cd\u5e94\u52a8\u529b\u5b66\uff0c\u79bb\u5b50\u4f20\u8f93\u52a8\u529b\u5b66\u548c\u7535\u5316\u5b66\u7a97\u53e3\uff08\u56feg-i\uff09\uff1bLi||Cu\u534a\u7535\u6c60\u6d4b\u8bd5\u8868\u660eB-F-SHPE\u5177\u6709\u6700\u9ad8\u7684\u5e93\u4f26\u6548\u7387\u4ee5\u53ca\u6700\u5747\u5300\u81f4\u5bc6\u7684\u9502\u6c89\u79ef\uff08\u56fej\u3001k\uff09\u3002<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"650\" height=\"485\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/7f88dbbcaa77a1d-17.png\" alt=\"\" class=\"wp-image-272576\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/7f88dbbcaa77a1d-17.png 650w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/7f88dbbcaa77a1d-17-200x150.png 200w\" sizes=\"(max-width: 650px) 100vw, 650px\" \/><\/figure>\n\n\n\n<p><strong>\u56fe3. Li@SHPEs\u7684\u754c\u9762\u7535\u5316\u5b66\u7a33\u5b9a\u6027\u3002<\/strong>a) Li|SHPEs|Li\u57280.3 mA cm<sup>\u22122<\/sup>\u4e0b\u7684\u5faa\u73af\u6027\u80fd\u3002\u63d2\u56fe\uff1a\u4ee3\u8868\u6027\u7535\u538b\u66f2\u7ebf\u3002b) Li|SHPEs|Li\u7684\u500d\u7387\u6027\u80fd\u3002c e) \u5206\u522b\u4f7f\u7528(c) B SHPE\u3001(d) F SHPE\u548c(e) B F SHPE\u5faa\u73af\u540e\u9502\u91d1\u5c5e\u7684\u626b\u63cf\u7535\u5b50\u663e\u5fae\u955c\uff08SEM\uff09\u56fe\u50cf\u3002f) Li|B F SHPE|Li\u4e2d\u5faa\u73af\u540e\u9502\u8d1f\u6781\u7684\u6a2a\u622a\u9762SEM\u56fe\u50cf\u53ca\u80fd\u8c31\uff08EDS\uff09\u5143\u7d20\u9762\u5206\u5e03\u3002g) Li|B F SHPE|Li\uff08\u4e0a\uff09\u548cLi|F\/B SHPE|Li\uff08\u4e0b\uff09\u4e2dSEI\uff08\u56fa\u4f53\u7535\u89e3\u8d28\u754c\u9762\u819c\uff09\u7684\u793a\u610f\u56fe\u3002h j) \u5728(h) Li|B SHPE|Li\u3001(i) Li|F SHPE|Li\u548c(j) Li|B F SHPE|Li\u4e2d\u5faa\u73af\u540e\u9502\u8d1f\u6781\u7684B 1s\u548cF 1s X\u5c04\u7ebf\u5149\u7535\u5b50\u80fd\u8c31\uff08XPS\uff09\u6df1\u5ea6\u5256\u6790\u6570\u636e\u3002k m) \u5728(k) Li|B SHPE|Li\u3001(l) Li|F SHPE|Li\u548c(m) Li|B F SHPE|Li\u4e2d\u5faa\u73af\u540e\u9502\u8d1f\u6781\u7684\u539f\u5b50\u529b\u663e\u5fae\u955c\uff08AFM\uff09\u8868\u5f81\u7ed3\u679c\u3002<\/p>\n\n\n\n<p>\u57280.3 mA cm<sup>\u22122<\/sup>\u30010.3 mAh cm<sup>\u22122<\/sup>\u6761\u4ef6\u4e0b\uff0cLi|<a>B\u2011F\u2011SHPE<\/a>|Li\u5faa\u73af3100\u5c0f\u65f6\uff08\u56fea\uff09\u3002\u57280.2\u20131.0 mA cm<sup>\u22122<\/sup>\u7535\u6d41\u5bc6\u5ea6\u4e0b\u6d4b\u8bd5\u500d\u7387\u6027\u80fd\uff0cLi|B\u2011F\u2011SHPE|Li\u6781\u5316\u7535\u538b\u66f4\u7a33\u5b9a\uff08\u56feb\uff09\u3002SEM\u68c0\u6d4b\u5230<a>\u4f7f\u7528<\/a>B\u001eF\u001eSHPE\u5faa\u73af\u540e\u9502\u91d1\u5c5e\u5177\u6709\u66f4\u5149\u6ed1\u7684\u8868\u9762\uff08\u56fec-f\uff09\uff1bB\/F\u534f\u540c\u8c03\u63a7\u7684SEI\u53ef\u6291\u5236\u526f\u53cd\u5e94\u548c\u9502\u679d\u6676\uff08\u56feg\uff09\u3002XPS\u6df1\u5ea6\u5256\u6790\u663e\u793a\uff0c\u4f7f\u7528B\u001eF\u001eSHPE\u5faa\u73af\u540e\u7684SEI\u5bcc\u542b\u65e0\u673a\u7ec4\u5206LiF\u548cB-O\u7ec4\u5206\uff1b\u800cB\u2011SHPE\u6216F\u2011SHPE\u7684SEI\u78b3\u4fe1\u53f7\u5f3a\u3001LiF\u5c11\uff0c\u7ed3\u6784\u4e0d\u7a33\u5b9a\uff08\u56feh-j\uff09\uff1bAFM\u8bc1\u5b9e\u5176\u673a\u68b0\u7a33\u5b9a\u6027\u66f4\u4f18\uff08\u56fek-m\uff09\u3002<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"650\" height=\"490\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/4e9a0ba2491dfde-17.png\" alt=\"\" class=\"wp-image-272577\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/4e9a0ba2491dfde-17.png 650w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/4e9a0ba2491dfde-17-200x150.png 200w\" sizes=\"(max-width: 650px) 100vw, 650px\" \/><\/figure>\n\n\n\n<p><strong>\u56fe4. LCO||Li\u7535\u6c60\u7684\u7535\u5316\u5b66\u6027\u80fd\u3002<\/strong>a b) LFP||Li (a) \u548c LCO||Li (b) \u5728 0.5 C \u5145\u7535\/1 C \u653e\u7535\u6761\u4ef6\u4e0b\u7684\u957f\u671f\u5faa\u73af\u6027\u80fd\u3002c\u3001d) \u5728\u622a\u6b62\u7535\u538b\u4e3a 4.5 V \u65f6\uff0cLCO||Li \u7684\u957f\u671f\u5faa\u73af\u7a33\u5b9a\u6027 (c) \u548c\u7535\u538b\u66f2\u7ebf (d)\u3002e) LCO|B F SHPE|Li \u5728\u4e0d\u540c\u500d\u7387\u4e0b\u7684\u7535\u538b\u66f2\u7ebf\u3002f) LCO||Li \u7535\u6c60\u7684\u500d\u7387\u6027\u80fd\u3002g\u3001h) LCO|B F SHPE|Li \u7535\u6c60\u5728\u4e0d\u540c\u622a\u6b62\u7535\u538b\u4e0b\u7684\u957f\u671f\u5faa\u73af\u6027\u80fd (g) \u548c\u7d2f\u8ba1\u80fd\u91cf\uff08\u5bb9\u91cf\uff09(h)\u3002i j) LCO|B F SHPE|Li \u5728\u4e0d\u540c LCO \u8f7d\u91cf (i) \u548c\u4e0d\u540c SHPE \u542b\u91cf (j) \u4e0b\u7684\u5faa\u73af\u6027\u80fd\u3002\u6240\u6709\u7535\u5316\u5b66\u6d4b\u8bd5\u5747\u5728 28 \u00b0C \u4e0b\u8fdb\u884c\u3002<\/p>\n\n\n\n<p>LFP|B-F-SHPE|Li\u57281200\u6b21\u5faa\u73af\u540e\u4fdd\u630181%\u7684\u5bb9\u91cf\uff0cLCO|B-F-SHPE|Li\uff083.0-4.3 V\uff09\u5728750\u6b21\u5faa\u73af\u540e\uff0c\u5bb9\u91cf\u4fdd\u7559\u7387\u4e3a83.3%\uff08\u56fea\u3001b\uff09\uff1b\u5373\u4f7f\u57284.5 V\u7684\u9ad8\u622a\u6b62\u7535\u538b\u4e0b\uff0cLCO|B-F-SHPE|Li\u5728\u5faa\u73af\u7a33\u5b9a\u6027\u4f18\u5f02\uff0c550\u6b21\u5faa\u73af\u540e\u4ecd\u4fdd\u670980.2%\u7684\u5bb9\u91cf\uff1b\u5176\u500d\u7387\u6027\u80fd\u4f18\u5f02\uff080.2\u20134 C\u5bb9\u91cf 110\u2013178 mAh g<sup>\u22121<\/sup>\uff09\uff08\u56fec\u2212f\uff09\u3002\u9ad8\u622a\u6b62\u7535\u538b\u4e0b\uff084.6 V\uff09LCO|B-F-SHPE|Li\u53ef\u5b9e\u73b0\u7a33\u5b9a\u957f\u5faa\u73af\uff08\u56feg\u3001h\uff09\u3002\u9ad8\u8f7d\u91cf\u3001\u9ad8\u56fa\u542b\u91cf\u4e0b\uff0c<a>LCO|B-F-SHPE|Li<\/a>\u7535\u6c60\u4e5f\u8868\u73b0\u51fa\u4f18\u5f02\u7684\u7535\u6c60\u6027\u80fd\uff08\u56fei\u3001j\uff09\u3002<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"650\" height=\"524\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/b14210e1ee30421-16.png\" alt=\"\" class=\"wp-image-272578\"\/><\/figure>\n\n\n\n<p><strong>\u56fe5. \u4f7f\u7528\u4e0d\u540cSHPEs\u5faa\u73af\u540e\u7684LCO\u6b63\u6781\u7684\u5fae\u89c2\u7ed3\u6784\u6f14\u5316\u3002<\/strong>a\u3001b) LCO|SHPEs|Li\u5728\u5145\u7535 (a) \u548c\u653e\u7535 (b) \u8fc7\u7a0b\u4e2d\u4e0d\u540c\u8377\u7535\u72b6\u6001\uff08SOC\uff09\u4e0b\u7684\u539f\u4f4d\u5f1b\u8c6b\u65f6\u95f4\u5206\u5e03\uff08DRT\uff09\u6570\u636e\u3002c) \u5faa\u73af100\u6b21\u540eLCO\u6b63\u6781\u7684\u6a2a\u622a\u9762\u626b\u63cf\u7535\u5b50\u663e\u5fae\u955c\uff08SEM\uff09\u56fe\u50cf\u53ca\u80fd\u8c31\uff08EDS\uff09\u9762\u5206\u5e03\u56fe\u3002d) \u5faa\u73af100\u6b21\u540eLCO\u6b63\u6781\u7684\u9ad8\u5206\u8fa8\u900f\u5c04\u7535\u5b50\u663e\u5fae\u955c\uff08HR-TEM\uff09\u56fe\u50cf\u53ca\u5176\u9762\u5206\u5e03\u56fe\u3002e\u3001f) LCO|B F SHPE|Li\u4e2d\u6b63\u6781\u7535\u89e3\u8d28\u754c\u9762\uff08CEI\uff09\u7684F 1s (e) \u548cB 1s (f) X\u5c04\u7ebf\u5149\u7535\u5b50\u80fd\u8c31\uff08XPS\uff09\u6df1\u5ea6\u5256\u6790\u6570\u636e\u3002g) LCO|B F SHPE|Li\u4e2dCEI\u5185\u7269\u79cd\u788e\u7247\u7684\u98de\u884c\u65f6\u95f4\u4e8c\u6b21\u79bb\u5b50\u8d28\u8c31\uff08TOF SIMS\uff09\u4e09\u7ef4\u91cd\u6784\u3002h) \u5faa\u73af\u540eLCO\u6b63\u6781\u7684\u5f52\u4e00\u5316Co K\u8fb9X\u5c04\u7ebf\u5438\u6536\u8fd1\u8fb9\u7ed3\u6784\uff08XANES\uff09\u8c31\u56fe\u3002i l) LCO|F SHPE|Li\uff08i\u548ck\uff09\u548cLCO|B F SHPE|Li\uff08j\u548cl\uff09\u4e2dCEI\u53caLCO\u5185\u90e8\u7ed3\u6784\u7684HR TEM\u56fe\u50cf\u3002<\/p>\n\n\n\n<p>\u539f\u4f4deis\u6d4b\u8bd5\u8868\u660eLCO|B-F-SHPE|Li\u7535\u6c60\u5728\u5faa\u73af\u8fc7\u7a0b\u4e2d\u5177\u6709\u8f83\u4f4e\u963b\u6297\uff08\u56fea\u3001b\uff09\uff1bSEM\u56fe\u50cf\u548cEDS\u6620\u5c04\u8bc1\u5b9e\u524d\u9a71\u6db2\u6210\u529f\u5728\u9634\u6781\u8868\u9762\u5f62\u6210\u8fde\u7eed\u6e17\u900f\u7684\u79bb\u5b50\u4f20\u5bfc\u8def\u5f84\uff08\u56fec\uff09\uff1bHR-TEM\u7ed3\u679c\u663e\u793aLCO\u9897\u7c92\u4e0a\u8986\u76d6\u7740\u5747\u5300\u4e14\u8584\u7684CEI\u5c42\uff0c\u5bcc\u542bB\u548cF\u5143\u7d20\uff08\u56fed\uff09\uff1bXPS\u548cTOF-SIMS\u7ed3\u679c\u4e5f\u663e\u793a\uff0cCEI\u5c42\u5185LiF\u548cB-O\u7269\u79cd\u7684\u5747\u5300\u5206\u5e03\uff08\u56fee-g\uff09\uff1bCo-K\u8fb9X\u5c04\u7ebf\u5438\u6536\u8fd1\u8fb9\u7ed3\u6784\uff08XANES\uff09\u6d4b\u91cf\u8868\u660eB-F-SHPE\u80fd\u6709\u6548\u6291\u5236\u5faa\u73af\u8fc7\u7a0b\u4e2d\u94b4\u7684\u8fd8\u539f\uff0c\u9632\u6b62\u4f4e\u4ef7\u94b4\u7684\u8fc7\u5ea6\u6eb6\u89e3\uff08\u56feh\uff09\uff1b\u4f7f\u7528B-F-SHPE\u5faa\u73af\u7684LCO\u9897\u7c92\u7684CEI\u539a\u5ea6\u4e3a~5 nm\u660e\u663e\u6bd4F-SHPE\u5f62\u6210\u7684\u539a\u5ea6\u8981\u8584\u5f97\u591a\uff08\u56fei\u3001j\uff09\uff1bHR-TEM\u7ed3\u679c\u8fdb\u4e00\u6b65\u8868\u660e\uff0c\u4f7f\u7528F-SHPE\u5faa\u73af\u540eLCO\u8868\u9762\u53d1\u751f\u4e86\u4e0d\u53ef\u9006\u7684\u76f8\u8f6c\u53d8\uff0c\u4ece\u5c42\u72b6\u7ed3\u6784\u5411\u5ca9\u76d0\u76f8\u6216\u6df7\u5408\u76f8\uff0c\u76f8\u6bd4\u4e4b\u4e0b\uff0c\u4f7f\u7528B-F-SHPE\u5faa\u73af\u7684LCO\u9897\u7c92\u8868\u9762\u7ef4\u6301\u826f\u597d\u5c42\u72b6\u7ed3\u6784\u4e0eLi\u207a\u6269\u6563\u901a\u9053\uff08\u56fek\u3001l\uff09\u3002<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"650\" height=\"485\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/de5bcf7d8eaea98-12.png\" alt=\"\" class=\"wp-image-272579\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/de5bcf7d8eaea98-12.png 650w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/07\/de5bcf7d8eaea98-12-200x150.png 200w\" sizes=\"(max-width: 650px) 100vw, 650px\" \/><\/figure>\n\n\n\n<p><strong>\u56fe6. \u8f6f\u5305\u7535\u6c60\u7684\u7535\u5316\u5b66\u6027\u80fd\u53ca\u754c\u9762\u8868\u5f81\u3002<\/strong>a\u3001b) LCO|SHPEs|Si C (a) \u548c LCO|SHPEs|Li (b) \u8f6f\u5305\u7535\u6c60\u7684\u5faa\u73af\u6027\u80fd\u3002c\u3001d) LCO|B F SHPE|Li \u8f6f\u5305\u7535\u6c60\u5728\u8d85\u8fc750\u6b21\u5faa\u73af\u540e\u7684\u8d85\u58f0\u900f\u5c04\u56fe\u50cf (c) \u53ca\u5bf9\u5e94\u7684\u8d85\u58f0\u6ce2\u66f2\u7ebf (d)\u3002e\u3001f) LCO|F SHPE|Li \u8f6f\u5305\u7535\u6c60\u5728\u8d85\u8fc750\u6b21\u5faa\u73af\u540e\u7684\u8d85\u58f0\u900f\u5c04\u56fe\u50cf (e) \u53ca\u5bf9\u5e94\u7684\u8d85\u58f0\u6ce2\u66f2\u7ebf (f)\u3002g\u3001h) \u5faa\u73af\u540e LCO|B F SHPE|Li (g) \u548c LCO|F SHPE|Li (h) \u8f6f\u5305\u7535\u6c60\u7684\u5149\u5b66\u7167\u7247\u3002i\u3001j) \u8bb0\u5f55 LCO|B F SHPE|Li (i) \u548c LCO|LE|Li (j) \u8f6f\u5305\u7535\u6c60\u9488\u523a\u5b89\u5168\u6d4b\u8bd5\u7684\u7167\u7247\u3002<\/p>\n\n\n\n<p>3 Ah <a>LCO<\/a>|B-F-SHPE|Si\/C\u8f6f\u5305\u7535\u6c60\u57280.2 C\u4e0b\u5faa\u73af400\u6b21\u4fdd\u6301\u7387 80.4%\uff08\u56fea\uff091.2 Ah\u7ea7LCO||Li\u8f6f\u5305\u7535\u6c600.3 C\u500d\u7387\u4e0b\u5faa\u73af200\u6b21\uff08\u56feb\uff09\u3002\u901a\u8fc7\u539f\u4f4d\u8d85\u58f0\u76d1\u6d4b\u6280\u672f\uff08\u4fe1\u53f7\u7279\u5f81\u4e3a\u7ea2\u5f3a\u84dd\u5f31\uff0c\u53cd\u6620\u7535\u6c60\u7ed3\u6784\u4e0e\u754c\u9762\u72b6\u6001\u7684\u53d8\u5316\uff09\u53d1\u73b0\uff0c\u4f7f\u7528B-F-SHPE\u7684\u7535\u6c60\u8868\u73b0\u51fa\u4fe1\u53f7\u5f3a\u5ea6\u9ad8\u4e14\u5206\u5e03\u5747\u5300\u7684\u7279\u70b9\uff0c\u540c\u65f6\u5faa\u73af\u540e\u4ea7\u6c14\u5f88\u5c11\uff0c\u8868\u660e\u5176\u754c\u9762\u66f4\u4e3a\u7a33\u5b9a<a>\uff08\u56fec\u2212h\uff09<\/a>\u3002\u9488\u523a\u5b9e\u9a8c\u8868\u660e\u672c\u5de5\u4f5c\u8bbe\u8ba1\u7684\u56fa\u6001\u7535\u89e3\u8d28\u76f8\u6bd4\u5546\u7528\u7535\u89e3\u6db2\u5177\u6709\u66f4\u4e3a\u4f18\u5f02\u7684\u5b89\u5168\u6027\uff08\u56fei\u3001j\uff09\u3002<\/p>\n\n\n\n<p><strong>5.\u7814\u7a76\u7ed3\u8bba<\/strong><strong><\/strong><\/p>\n\n\n\n<p>\u672c\u7814\u7a76\u6210\u529f\u5408\u6210\u4e86\u57fa\u4e8e\u68af\u5ea6\u5171\u4ef7-\u975e\u5171\u4ef7\u52a8\u6001\u952e\u534f\u540c\u6548\u5e94\u7684SHPE\uff0c\u5b9e\u73b0\u4e86\u56fa\u6001\u9502\u7535\u6c60\uff08SSLBs\uff09\u5168\u670d\u5f79\u5468\u671f\u4e2d\u591a\u754c\u9762\u7684\u81ea\u4e3b\u4fee\u590d\u3002\u5c06\u5177\u6709\u9ad8\u952e\u80fd\u7684\u787c\u9178\u916f\u952e\uff08\u5171\u4ef7\u52a8\u6001\u952e\uff09\u4e0e\u5feb\u901f\u54cd\u5e94\u7684\u6c22\u952e\uff08\u975e\u5171\u4ef7\u52a8\u6001\u952e\uff09\u6574\u5408\u4e8e\u805a\u5408\u7269\u7f51\u7edc\u4e4b\u4e2d\u3002\u5229\u7528\u5176\u5fae\u5c3a\u5ea6\u52a8\u6001\u53ef\u9006\u6027\uff0c\u5728\u6e29\u548c\u6761\u4ef6\u4e0b\uff0830 \u00b0C\uff0c1 h\uff09\u5373\u53ef\u5b9e\u73b0\u754c\u9762\u635f\u4f24\u7684\u9ad8\u6548\u6108\u5408\u3002\u901a\u8fc7\u539f\u4f4d\u805a\u5408\u8fdb\u4e00\u6b65\u589e\u5f3a\u4e86\u7535\u6781-\u7535\u89e3\u8d28\u754c\u9762\u7684\u7d27\u5bc6\u63a5\u89e6\u548c\u81ea\u9002\u5e94\u5339\u914d\u3002\u52a8\u6001\u952e\u7684\u53ef\u9006\u4ea4\u6362\u4fc3\u8fdb\u4e86Li\u207a\u7684\u5feb\u901f\u4f20\u8f93\uff0c\u4f7f\u5ba4\u6e29\uff0825 \u00b0C\uff09\u79bb\u5b50\u7535\u5bfc\u7387\u8fbe\u52301.6 \u00d7 10<sup>\u2212<\/sup><sup>3<\/sup>&nbsp;S cm<sup>\u22121<\/sup>\uff0c\u540c\u65f6\u8010\u6c27\u5316\u7684\u542b\u787c\u548c\u542b\u6c1f\u5b98\u80fd\u56e2\u5c06\u7535\u5316\u5b66\u7a97\u53e3\u62d3\u5bbd\u81f35.2 V\u3002Li|B-F-SHPE|Li\u7535\u6c60\u8868\u73b0\u51fa\u8d85\u8fc73000\u5c0f\u65f6\u7684\u7a33\u5b9a\u5faa\u73af\u3002LFP|SHPE|Li\u548cLCO|SHPE|Li\u7535\u6c60\u5206\u522b\u5b9e\u73b0\u4e86\u8d85\u8fc71000\u6b21\u548c700\u6b21\u7684\u7a33\u5b9a\u5faa\u73af\uff0c\u5bb9\u91cf\u4fdd\u6301\u7387\u5747\u8d85\u8fc780%\uff0c\u540c\u65f6\u5728\u9ad8\u7535\u538b\uff084.6 V\uff09\u548c\u9ad8\u8f7d\u91cf\uff0814 mg cm<sup>\u2212<\/sup><sup>2<\/sup>\uff09\u4e0b\u4e0eLCO\u4f53\u7cfb\u517c\u5bb9\u3002\u7ec4\u88c5\u7684LCO|SHPE|Li\uff081.2 Ah\uff09\u548cLCO|SHPE|Si-C\uff082.5 Ah\uff09\u8f6f\u5305\u7535\u6c60\u5206\u522b\u8868\u73b0\u51fa200\u6b21\u548c400\u6b21\u7684\u957f\u671f\u5faa\u73af\u7a33\u5b9a\u6027\uff0c\u5e76\u987a\u5229\u901a\u8fc7\u9488\u523a\u5b89\u5168\u6d4b\u8bd5\u3002\u672c\u7814\u7a76\u8868\u660e\uff0c\u68af\u5ea6\u8bbe\u8ba1\u7b56\u7565\u4e3a\u5f00\u53d1\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u3001\u957f\u5bff\u547d\u548c\u5b89\u5168\u7684\u56fa\u6001\u7535\u6c60\u63d0\u4f9b\u4e86\u4e00\u79cd\u81ea\u6108\u5408\u754c\u9762\u6750\u6599\u4f53\u7cfb\u53ca\u65b0\u7684\u8bbe\u8ba1\u8303\u5f0f\u3002<\/p>\n\n\n\n<p><strong>\u539f\u6587\u8be6\u60c5<\/strong><strong><\/strong><\/p>\n\n\n\n<p>Qiang Gao, Wenjie Lin, Zhenyu Huang, Yi Zhang, Fenghua Zhang, Kunchi Xie, Danru Huang, Yaqi Liao, Zhengwei Cheng, Yunhui Huang* and Fei Pei* Interfacial Self-Healing Polymer Electrolytes With Gradient Covalent\u2013Noncovalent Dynamic Bonds for 4.6 V-Class Lithium Metal Batteries, 2026, Advanced Materials.<\/p>\n\n\n\n<p><a href=\"https:\/\/doi.org\/10.1002\/adma.74116\">https:\/\/doi.org\/10.1002\/adma.74116<\/a><\/p>\n\n\n\n<p><strong>\u4f5c\u8005\u7b80\u4ecb<\/strong><strong><\/strong><\/p>\n\n\n\n<p>\u88f4\u975e\u7814\u7a76\u5458\uff0c\u695a\u5929\u82f1\u624d\u8ba1\u5212\u9752\u5e74\u62d4\u5c16\u4eba\u624d\uff0c\u534e\u4e2d\u79d1\u6280\u5927\u5b66\u7279\u522b\u8d44\u52a9\u535a\u58eb\u540e(\u9ec4\u4e91\u8f89\u6559\u6388)\u3002\u53a6\u95e8\u5927\u5b66\u535a\u58eb(\u90d1\u5357\u5cf0\u9662\u58eb)\u3002\u957f\u671f\u4ece\u4e8b\u9ad8\u6bd4\u80fd\u56fa\u6001\u9502\u7535\u6c60\u7b49\u65b9\u9762\u7684\u7814\u7a76\u3002\u4e3b\u6301\u56fd\u81ea\u7136\u9762\u4e0a\u9879\u76ee\u3001\u56fd\u81ea\u7136\u9752\u5e74\u57fa\u91d1\u3001\u4e2d\u56fd\u535a\u58eb\u540e\u7279\u522b\u8d44\u52a9\/\u9762\u4e0a\u8d44\u52a9\u7b49\uff0c\u72ec\u7acb\u627f\u62c5\u5e94\u6025\u7ba1\u7406\u90e8\u91cd\u70b9\u5b9e\u9a8c\u5ba4\u5f00\u653e\u8bfe\u9898\u3001\u6d59\u6c5f\u7701\u91cd\u70b9\u5b9e\u9a8c\u5ba4\u5f00\u653e\u8bfe\u9898\u3002\u4ee5\u7b2c\u4e00\/\u901a\u8baf\u4f5c\u8005\u53d1\u8868\u5305\u542bNature\u3001Nat. Commun.(2)\u3001Adv. Mater.(4)\u3001JACS\u3001Natl. Sci. Rev.\u3001Joule\u3001Energy Environ. Sci. (3)\u3001Adv. Energy Mater(3)\u3001Adv. Funct. Mater\u5728\u5185\u7684\u671f\u520a30\u4f59\u7bc7\uff0c\u8c37\u6b4c\u5b66\u672f\u5f15\u75286200\u4f59\u6b21\uff0c\u6388\u6743\/\u516c\u5f00\u53d1\u660e\u4e13\u522920\u9879\u3002\u62c5\u4efb\u56fd\u9645\u671f\u520aScience Bulletin\u3001eScience\u3001Energy Materials\u3001Renewables\u548cCarbon Neutralization\u9752\u5e74\u7f16\u59d4\u3002http:\/\/faculty.hust.edu.cn\/feipei\/zh_CN\/index.htm<\/p>\n\n\n\n<p>\u9ec4\u4e91\u8f89\u6559\u6388\uff0c\u534e\u4e2d\u79d1\u6280\u5927\u5b66\u6559\u6388\/\u535a\u5bfc\uff0c\u56fd\u5bb6\u6770\u9752\u3001\u957f\u6c5f\u5b66\u8005\uff0c\u6821\u5b66\u672f\u59d4\u5458\u4f1a\u526f\u4e3b\u4efb\uff0c\u4e2d\u56fd\u6750\u6599\u7814\u7a76\u5b66\u4f1a\u5e38\u52a1\u7406\u4e8b\uff0cElectrochem. Energy Rev.\u526f\u4e3b\u7f16\u3002\u4e3b\u8981\u7814\u7a76\u65b9\u5411\u4e3a\u4e0b\u4e00\u4ee3\u9ad8\u6bd4\u80fd\u548c\u9ad8\u5b89\u5168\u7535\u6c60\u3001\u7535\u6c60\u5148\u8fdb\u76d1\u6d4b\u6280\u672f\u7b49\u3002\u6240\u7814\u53d1\u7684\u78f7\u9178\u94c1\u9502\u590d\u5408\u6b63\u6781\u6750\u6599\u3001\u7535\u6c60\u8d85\u7ea7\u5feb\u5145\u5173\u952e\u6280\u672f\u3001\u8d85\u58f0\u68c0\u6d4b\u7b49\u4e00\u6279\u6210\u679c\u5df2\u5b9e\u73b0\u5e94\u7528\u3002\u5728Science\u3001Nature\u3001Nat. Mater.\u3001Nat. Sustain.\u3001Nat. Commun.\u3001J. Am. Chem. Soc.\u3001Chem. Soc. Rev\u3001Adv. Mater.\u3001Joule\u7b49\u56fd\u9645\u8457\u540d\u5b66\u672f\u671f\u520a\u4e0a\u53d1\u8868SCI\u8bba\u6587800\u4f59\u7bc7\uff0c\u8bba\u6587\u5f15\u75289.3\u4e07\u4f59\u6b21\uff0cH-\u56e0\u5b50150\uff0c\u83b7\u6559\u80b2\u90e8\u81ea\u7136\u79d1\u5b66\u4e00\u7b49\u5956\u3001\u56fd\u5bb6\u81ea\u7136\u79d1\u5b66\u4e8c\u7b49\u5956\u3001\u6e56\u5317\u7701\u81ea\u7136\u79d1\u5b66\u4e00\u7b49\u5956\u3002<\/p>\n\n\n\n<p>\u9ec4\u4e91\u8f89\u6559\u6388\u8bfe\u9898\u7ec4\u62db\u8058\u805a\u5408\u7269\u56fa\u6001\u9502\u7535\u6c60\u65b9\u5411\u535a\u58eb\u540e\uff0c\u8be6\u60c5\u8054\u7cfb\uff1a<a href=\"mailto:peifei@hust.edu.cn\"><u>peifei@hust.edu.cn<\/u><\/a><\/p>\n\n\n\n<p>\u672c\u6587\u7531\u9ad8\u5f3a\uff08\u534e\u4e2d\u79d1\u6280\u5927\u5b66\u6750\u6599\u79d1\u5b66\u4e0e\u5de5\u7a0b\u5b66\u9662\uff09\u4f9b\u7a3f<\/p>\n","protected":false},"excerpt":{"rendered":"<p>1.\u7814\u7a76\u80cc\u666f \u56fa\u6001\u7535\u89e3\u8d28\uff08SSEs\uff09\u662f\u4e0b\u4e00\u4ee3\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u9502\uff08Li\uff09\u7535\u6c60\u7684\u5173\u952e\u7a81\u7834\u6027\u6280\u672f\uff0c\u5176\u4e0e\u9ad8\u538b\u6b63\u6781\u6750\u6599\uff08\u5982LiCoO2&nbsp;(LCO)\u3001\u5bcc\u954d\u5c42\u72b6LiNi0&#8230;<\/p>\n","protected":false},"author":31345,"featured_media":0,"comment_status":"open","ping_status":"","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[2],"tags":[],"class_list":["post-272573","post","type-post","status-publish","format-standard","hentry","category-keji"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/272573"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/31345"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=272573"}],"version-history":[{"count":1,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/272573\/revisions"}],"predecessor-version":[{"id":272580,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/272573\/revisions\/272580"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=272573"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=272573"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=272573"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}