{"id":273118,"date":"2026-09-14T09:18:00","date_gmt":"2026-09-14T01:18:00","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=273118"},"modified":"2026-09-13T23:27:17","modified_gmt":"2026-09-13T15:27:17","slug":"%e8%8e%86%e7%94%b0%e5%ad%a6%e9%99%a2%e6%98%93%e6%98%8e%e6%9d%b0%e6%95%99%e6%8e%88-%e5%93%88%e5%b0%94%e6%bb%a8%e5%b7%a5%e4%b8%9a%e5%a4%a7%e5%ad%a6%e5%bc%a0%e5%98%89%e6%81%92%e6%95%99%e6%8e%88cej-znse","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=273118","title":{"rendered":"\u8386\u7530\u5b66\u9662\u6613\u660e\u6770\u6559\u6388\/\u54c8\u5c14\u6ee8\u5de5\u4e1a\u5927\u5b66\u5f20\u5609\u6052\u6559\u6388CEJ: ZnSe\/V2O5\u5f02\u8d28\u7ed3\u754c\u9762\u7535\u8377\u91cd\u5206\u5e03\u6784\u7b51\u9ad8\u6027\u80fd\u5bbd\u6e29\u533a\u950c\u001e\u7a7a\u6c14\u7535\u6c60"},"content":{"rendered":"\n<ul class=\"wp-block-list\">\n<li>\u5bfc\u8bfb<\/li>\n<\/ul>\n\n\n\n<p>\u950c\u7a7a\u6c14\u7535\u6c60\u51ed\u501f\u5176\u9ad8\u7406\u8bba\u80fd\u91cf\u5bc6\u5ea6\u3001\u4f4e\u539f\u6599\u6210\u672c\u3001\u826f\u597d\u5b89\u5168\u6027\u4e0e\u73af\u5883\u53cb\u597d\u6027\uff0c\u5728\u5927\u89c4\u6a21\u50a8\u80fd\u3001\u7279\u79cd\u7535\u6e90\u53ca\u67d4\u6027\u7535\u5b50\u8bbe\u5907\u7b49\u9886\u57df\u5177\u6709\u5e7f\u9614\u5e94\u7528\u524d\u666f\u3002\u7136\u800c\uff0c\u4f20\u7edf\u6c34\u7cfb\u7535\u89e3\u6db2\u4f53\u7cfb\u5728\u5bbd\u6e29\u533a\u6761\u4ef6\u4e0b\u5b58\u5728\u4e25\u91cd\u6027\u80fd\u74f6\u9888\uff1a\u4f4e\u6e29\u4e0b\u79bb\u5b50\u7535\u5bfc\u7387\u9aa4\u964d\u3001\u6c27\u53cd\u5e94\u52a8\u529b\u5b66\u8fdf\u7f13\uff1b\u9ad8\u6e29\u4e0b\u950c\u8d1f\u6781\u8150\u8680\u52a0\u5267\u3001\u50ac\u5316\u5242\u5feb\u901f\u5931\u6d3b\uff0c\u4e25\u91cd\u5236\u7ea6\u4e86\u5176\u5728\u6781\u7aef\u6e29\u5ea6\u573a\u666f\u4e2d\u7684\u5e94\u7528\u3002\u8fc7\u6e21\u91d1\u5c5e\u5316\u5408\u7269\u5982\u5c42\u72b6V\u2082O\u2085\u548cZnSe\u867d\u5404\u5177\u50ac\u5316\u6f5c\u529b\uff0c\u4f46\u53d7\u9650\u4e8e\u5bfc\u7535\u6027\u5dee\u3001\u7a33\u5b9a\u6027\u4e0d\u8db3\u6216\u53cd\u5e94\u52a8\u529b\u5b66\u4e0d\u7406\u60f3\u7b49\u95ee\u9898\u3002\u754c\u9762\u5de5\u7a0b\u6784\u5efa\u5f02\u8d28\u7ed3\u53ef\u8bf1\u5bfc\u7535\u8377\u91cd\u5206\u5e03\u4e0e\u5185\u5efa\u7535\u573a\uff0c\u6709\u671b\u52a0\u901f\u79bb\u5b50\u8fc1\u79fb\u3001\u4f18\u5316\u4e2d\u95f4\u4f53\u5438\u9644\u80fd\u5e76\u63d0\u5347\u50ac\u5316\u7a33\u5b9a\u6027\uff1b\u540c\u65f6\uff0c\u591a\u5143\u7d20\u63ba\u6742\u78b3\u8f7d\u4f53\u53ef\u8fdb\u4e00\u6b65\u534f\u540c\u589e\u5f3a\u5bfc\u7535\u6027\u4e0e\u6d3b\u6027\u4f4d\u70b9\u5206\u6563\u6027\u3002\u7136\u800c\uff0c\u76ee\u524d\u9488\u5bf9V\u2082O\u2085\/ZnSe\u6c27\u5316\u7269-\u7852\u5316\u7269\u5f02\u8d28\u7ed3\u5728\u5bbd\u6e29\u533a\u950c\u7a7a\u6c14\u7535\u6c60\u4e2d\u7684\u7535\u8377\u91cd\u5206\u5e03\u673a\u5236\u53ca\u5176\u5bf9\u50ac\u5316\u6027\u80fd\u5f71\u54cd\u7684\u7814\u7a76\u5c1a\u5c5e\u7a7a\u767d\uff0c\u4e9f\u9700\u7cfb\u7edf\u63a2\u7d22\u3002<\/p>\n\n\n\n<ul class=\"wp-block-list\">\n<li>\u6210\u679c\u63a0\u5f71<\/li>\n<\/ul>\n\n\n\n<h1 class=\"wp-block-heading\">\u8fd1\u65e5\uff0c\u8386\u7530\u5b66\u9662\u6613\u660e\u6770\u6559\u6388\u8054\u5408\u54c8\u5c14\u6ee8\u5de5\u4e1a\u5927\u5b66\u5f20\u5609\u6052\u6559\u6388\u5c06\u79bb\u5b50\u6db2\u4f53\u4f5c\u4e3a\u591a\u5143\u7d20\u63ba\u6742\u5242\u5f15\u5165Zn-V-MOFs\uff0c\u7ecf\u7852\u5316\u5408\u6210ZnSe-V\u2082O\u2085\u5f02\u8d28\u7ed3\u5e76\u5305\u88f9\u4e8eN\u3001P\u63ba\u6742\u78b3\u4e2d\uff08ZnSe-V\u2082O\u2085\/NPC\uff09\u6765\u5236\u5907\u9ad8\u6027\u80fd\u5bbd\u6e29\u533a\u950c\u7a7a\u6c14\u7535\u6c60\u3002\u8be5\u6837\u54c1\u5177\u6709\u4ee5\u4e0b\u4f18\u70b9\uff1a\uff081\uff09\u5f02\u8d28\u7ed3\u754c\u9762\u7535\u8377\u91cd\u5206\u5e03\u5f62\u6210\u5185\u5efa\u7535\u573a\uff0c\u534f\u540c\u591a\u5143\u7d20\uff08N\u3001P\u7b49\uff09\u63ba\u6742\u8c03\u63a7\u78b3\u6750\u6599\u7535\u5b50\u7ed3\u6784\uff0c\u6539\u5584\u7535\u5b50\u4f20\u8f93\u73af\u5883\uff0c\u4f7f\u6d3b\u6027\u4f4d\u70b9\u5747\u5300\u5206\u6563\u4e14\u5229\u7528\u7387\u663e\u8457\u63d0\u5347\uff1b\uff082\uff09\u591a\u5143\u7d20\u63ba\u6742\u78b3\u7684\u9ad8\u5bfc\u7535\u6027\u5f25\u8865\u4e86V\u2082O\u2085\u5bfc\u7535\u6027\u5dee\u7684\u7f3a\u9677\uff0c\u52a0\u901f\u754c\u9762\u7535\u8377\u8f6c\u79fb\u3001\u964d\u4f4e\u4f20\u8f93\u963b\u529b\uff0c\u540c\u65f6\u8bf1\u5bfc\u989d\u5916\u6d3b\u6027\u4e2d\u5fc3\uff0c\u534f\u540c\u5f02\u8d28\u7ed3\u5f3a\u5316\u50ac\u5316\u6d3b\u6027\u5e76\u63d0\u5347\u754c\u9762\u76f8\u5bb9\u6027\uff1b\uff083\uff09V\u2082O\u2085\/ZnSe\u7684\u754c\u9762\u534f\u540c\u6548\u5e94\u7ed3\u5408\u63ba\u6742\u78b3\u7684\u7a33\u5b9a\u6027\u8c03\u63a7\uff0c\u4f18\u5316\u4e86ORR\/OER\u4e2d\u95f4\u4f53\uff08OOH\u3001O\u3001*OH\uff09\u7684\u5438\u9644-\u8131\u9644\u81ea\u7531\u80fd\uff0c\u4f7f\u50ac\u5316\u5242\u5728\u5bbd\u6e29\u533a\u5185\u4fdd\u6301\u4f18\u5f02\u52a8\u529b\u5b66\u7279\u6027\u3002\u8be5\u7814\u7a76\u4e3a\u5bbd\u6e29\u533a\u67d4\u6027\u950c\u7a7a\u6c14\u7535\u6c60\u7535\u6781\u6750\u6599\u8bbe\u8ba1\u63d0\u4f9b\u4e86\u91cd\u8981\u542f\u793a\uff0c\u5176\u4e2dZnSe\/V\u2082O\u2085\u5f02\u8d28\u7ed3\u7535\u8377\u91cd\u5206\u5e03\u5f15\u53d1\u7684\u4f18\u5316\u673a\u7406\uff0c\u53ef\u62d3\u5c55\u5e94\u7528\u4e8e\u5176\u4ed6\u6c27\u5316\u7269\/\u7852\u5316\u7269\u5f02\u8d28\u7ed3\u4f53\u7cfb\uff0c\u52a9\u529b\u950c\u7a7a\u6c14\u7535\u6c60\u5728\u6781\u7aef\u6e29\u5ea6\u6761\u4ef6\u4e0b\u7684\u5b9e\u7528\u5316\u63a8\u5e7f\u3002<\/h1>\n\n\n\n<h2 class=\"wp-block-heading\">\u8be5\u6210\u679c\u4ee5\u8386\u7530\u5b66\u9662\u4e3a\u7b2c\u4e00\u5355\u4f4d\u4ee5\u9898\u76ee\u201cInterfacial charge redistribution at ZnSe\/V<sub>2<\/sub>O<sub>5<\/sub>&nbsp;heterojunction encapsulated in N, P-doped carbon enables high-performance wide-temperature Zn-air batteries\u201d\u5728\u56fd\u9645\u9876\u7ea7\u5316\u5b66\u5de5\u7a0b\u7814\u7a76\u671f\u520aChemical Engineering Journal\uff08\u4e2d\u79d1\u9662\u4e00\u533a\uff09\u4e0a\u53d1\u8868\uff0c\u5f71\u54cd\u56e0\u5b50\u4e3a12.8\u3002<\/h2>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"600\" height=\"247\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/09\/2382c315a6ba396-7.png\" alt=\"\" class=\"wp-image-273119\"\/><\/figure>\n\n\n\n<p>\u4e09\u3001\u6838\u5fc3\u521b\u65b0\u70b9<\/p>\n\n\n\n<p>\u672c\u7814\u7a76\u9488\u5bf9\u67d4\u6027\u950c\u7a7a\u6c14\u7535\u6c60\u96be\u4ee5\u9002\u5e94\u5bbd\u6e29\u533a\u6781\u7aef\u73af\u5883\u7684\u5173\u952e\u74f6\u9888\uff0c\u9762\u5411\u53ef\u7a7f\u6234\u4e0e\u67d4\u6027\u50a8\u80fd\u5b9e\u9645\u5e94\u7528\u9700\u6c42\uff0c\u9488\u5bf9\u5355\u4e00 V\u2082O\u2085\u7535\u5bfc\u7387\u4f4e\u3001\u78b1\u6027\u7a33\u5b9a\u6027\u5dee\u4ee5\u53ca ZnSe \u672c\u5f81 ORR\/OER \u53cd\u5e94\u52a8\u529b\u5b66\u4e0d\u8db3\u7684\u6750\u6599\u7f3a\u9677\uff0c\u6784\u5efa ZnSe\u001eV\u2082O\u2085\u6c27\u5316\u7269\u001e\u7852\u5316\u7269\u5f02\u8d28\u7ed3\uff0c\u4f9d\u6258\u5f02\u8d28\u754c\u9762\u7535\u8377\u91cd\u5206\u5e03\u8bf1\u53d1\u7684\u5185\u5efa\u7535\u573a\u8c03\u63a7\u79bb\u5b50\u8f93\u8fd0\u884c\u4e3a\u4e0e\u6c27\u4e2d\u95f4\u4f53\u5438\u9644\u80fd\uff0c\u6539\u5584\u5bbd\u6e29\u533a\u50ac\u5316\u52a8\u529b\u5b66\u4e0e\u5faa\u73af\u7a33\u5b9a\u6027\uff1b\u8fdb\u4e00\u6b65\u5f15\u5165\u591a\u5143\u7d20\u63ba\u6742\u78b3\u8f7d\u4f53\u5b9e\u73b0\u534f\u540c\u6539\u6027\uff0c\u5229\u7528\u63ba\u6742\u78b3\u4f18\u5f02\u7684\u5bfc\u7535\u7f51\u7edc\u3001\u591a\u5b54\u7ed3\u6784\u4e0e\u7535\u5b50\u8c03\u63a7\u6548\u5e94\u5f25\u8865\u5355\u4e00\u5f02\u8d28\u7ed3\u5728\u9ad8\u7535\u6d41\u53ca\u6781\u7aef\u6e29\u5ea6\u4e0b\u7684\u7ed3\u6784\u7a33\u5b9a\u6027\u77ed\u677f\uff0c\u7cfb\u7edf\u63a2\u7a76\u8be5\u5f02\u8d28\u7ed3\u590d\u5408\u6750\u6599\u7684\u754c\u9762\u4f5c\u7528\u673a\u5236\u53ca\u5176\u5bf9\u5bbd\u6e29\u533a\u67d4\u6027\u950c\u7a7a\u6c14\u7535\u6c60\u7535\u5316\u5b66\u6027\u80fd\u7684\u8c03\u63a7\u89c4\u5f8b\uff0c\u4e3a\u6781\u7aef\u6e29\u5ea6\u6761\u4ef6\u4e0b\u67d4\u6027\u950c\u7a7a\u6c14\u7535\u6c60\u9ad8\u6027\u80fd\u7535\u50ac\u5316\u5242\u7684\u8bbe\u8ba1\u4e0e\u5b9e\u7528\u5316\u5f00\u53d1\u63d0\u4f9b\u65b0\u7684\u601d\u8def\u4e0e\u5b9e\u9a8c\u4f9d\u636e\u3002<\/p>\n\n\n\n<p>\u56db\u3001\u6570\u636e\u6982\u89c8<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"550\" height=\"635\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/09\/ce6e2814f207c93-7.png\" alt=\"\" class=\"wp-image-273120\"\/><\/figure>\n\n\n\n<p><strong>Fig<\/strong><strong>.<\/strong><strong>&nbsp;1.<\/strong>&nbsp;(a)&nbsp;The illustration of the preparation process of ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC. (b)&nbsp;SEM&nbsp;and (c)&nbsp;TEM&nbsp;images of Zn-V-ILs-MOF.&nbsp;(d)&nbsp;SEM&nbsp;and (e)&nbsp;TEM&nbsp;images of&nbsp;ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC.&nbsp;(f)&nbsp;The mapping of ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC. (g)&nbsp;HRTEM image, (l)&nbsp;inverse FFT lattice image, (m)&nbsp;lattice spacing, and SAED diffraction pattern of ZnSe&nbsp;and V<sub>2<\/sub>O<sub>5<\/sub><sub>&nbsp;<\/sub>in ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC. (k, l) GPA analysis of ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC. (m)&nbsp;The water contact angles of ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC, ZnSe\/NPC, and V<sub>2<\/sub>O<sub>5<\/sub>\/NPC.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"550\" height=\"493\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/09\/7f88dbbcaa77a1d-7.png\" alt=\"\" class=\"wp-image-273121\"\/><\/figure>\n\n\n\n<p><strong>Fig<\/strong><strong>.<\/strong><strong>&nbsp;2.<\/strong>&nbsp;(a) X-ray diffraction (XRD) patterns of ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC. The (b) specific surface area and (c) Pore size distribution of ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC. XPS peaks of (d) Zn 2<em>p, <\/em>(e) V&nbsp;2<em>p<\/em>,<em>&nbsp;<\/em>(f)<em>&nbsp;<\/em>Se<em>&nbsp;<\/em>3<em>d<\/em>&nbsp;and (g) O&nbsp;1<em>s<\/em><em>&nbsp;<\/em>for ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC. (h) Schematic diagram of synchrotron radiation. (i)&nbsp;XANES spectra and (j)&nbsp;the corresponding FT EXAFS data&nbsp;at Zn&nbsp;K-edge for Zn&nbsp;foil, ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC, and ZnSe\/NPC. WT EXAFS plots at the Zn&nbsp;K-edge for (k) ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC&nbsp;and&nbsp;(l)&nbsp;ZnSe\/NPC.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"550\" height=\"467\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/09\/4e9a0ba2491dfde-7.png\" alt=\"\" class=\"wp-image-273122\"\/><\/figure>\n\n\n\n<p><strong>Fig<\/strong><strong>.<\/strong><strong>&nbsp;<\/strong><strong>3<\/strong><strong>.<\/strong><strong>&nbsp;<\/strong>(a) Schematic diagram of the OER principle and testing. (b)&nbsp;Polarization curves in OER of ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC, RuO<sub>2<\/sub>, ZnSe\/NPC, and V<sub>2<\/sub>O<sub>5<\/sub>\/NPC. (c) Tafel plots derived from the panel.&nbsp;(d) Comparison of overpotentials and Tafel slopes.&nbsp;(e) The EIS of ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC, RuO<sub>2<\/sub>&nbsp;ZnSe\/NPC, and V<sub>2<\/sub>O<sub>5<\/sub>\/NPC.<sub>&nbsp;<\/sub>(f)&nbsp;CV curves&nbsp;and&nbsp;(g)&nbsp;relative electrochemically active surface area.&nbsp;(h)&nbsp;Amount of gas measured and calculated&nbsp;of the ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC.&nbsp;(i)&nbsp;Polarization curves of before and after 1000th LSV tests and (j)&nbsp;the chronoamperometric stabilities&nbsp;of of the ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC. (k)&nbsp;Spectra, (l)&nbsp;contour plots, and (m)&nbsp;3D mapping plots of in-situ infrared spectroscopy testing.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"550\" height=\"555\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/09\/b14210e1ee30421-7.png\" alt=\"\" class=\"wp-image-273123\"\/><\/figure>\n\n\n\n<p><strong>Fig<\/strong><strong>.<\/strong><strong>&nbsp;<\/strong><strong>4<\/strong><strong>.<\/strong><strong>&nbsp;<\/strong>(a) Schematic diagram of the ORR principle and testing. (b)&nbsp;Polarization curves in ORR of ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC, Pt\/C, ZnSe\/NPC, and V<sub>2<\/sub>O<sub>5<\/sub>\/NPC&nbsp;in 0.1 M KOH (rotating speed:1600 rpm). (c) Tafel plots derived from the panel.&nbsp;(d) Comparison of overpotentials and Tafel slopes.&nbsp;(e) LSV curves at different rotating speeds and (f) the corresponding Koutecky-Levich plots at different potentials.&nbsp;(g) The EIS of ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC, Pt\/C, ZnSe\/NPC, and V<sub>2<\/sub>O<sub>5<\/sub>\/NPC.<sub>&nbsp;<\/sub>(h) Polarization curves&nbsp;before and after 1000th LSVs tests. (i) The chronoamperometric stabilities of the ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC&nbsp;in ORR. (j) SEM image after cycles. (k)&nbsp;Spectra, (l)&nbsp;contour plots, and (m)&nbsp;3D mapping plots of in-situ infrared spectroscopy testing. (n) The overall polarization curves&nbsp;of catalysts within the ORR and OER potential window&nbsp;and the specific value.&nbsp;(o) Comparison of OER and ORR bifunctional activities in this work with representative electrocatalysts in references.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"550\" height=\"523\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/09\/de5bcf7d8eaea98-5.png\" alt=\"\" class=\"wp-image-273124\"\/><\/figure>\n\n\n\n<p><strong>Fig<\/strong><strong>.<\/strong><strong>&nbsp;<\/strong><strong>5<\/strong><strong>.<\/strong><strong>&nbsp;<\/strong>(a) Side views of ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>, ZnSe, and V<sub>2<\/sub>O<sub>5<\/sub>.<sub>&nbsp;<\/sub>(b) Electron density difference images of ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>. Total density of states (TDOS) and <em>d<\/em>-bond centre data for (c) ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>, (d) ZnSe, and (e) V<sub>2<\/sub>O<sub>5<\/sub>. The ICOHP of V-O in (f)&nbsp;ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>&nbsp;and (g) V<sub>2<\/sub>O<sub>5<\/sub>.<sub>&nbsp;<\/sub>The ICOHP of V-OH<sup>&#8211;<\/sup>&nbsp;in (h)&nbsp;ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>&nbsp;and (i) V<sub>2<\/sub>O<sub>5<\/sub>. The free energy diagram for the elementary reduction steps in (j) OER and (k) ORR.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"550\" height=\"571\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/09\/aa3023e0288002c-5.png\" alt=\"\" class=\"wp-image-273125\"\/><\/figure>\n\n\n\n<p><strong>Fig<\/strong><strong>.<\/strong><strong>&nbsp;<\/strong><strong>6<\/strong><strong>.<\/strong><strong>&nbsp;<\/strong>(a)&nbsp;Schematic diagram of accessories for a Zn-air battery. (b)&nbsp;Schematic of testing for a Zn-air battery.&nbsp;(c) Open circuit potential curves (inset: Schematic diagram of application), (d) discharge rate performance, (e) discharge capacity, (f)&nbsp;polarization and power density curves&nbsp;of ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC&nbsp;and Pt\/C+RuO<sub>2<\/sub>. (g)&nbsp;Comparison to recent Zn-air battery power densities.&nbsp;(h)&nbsp;Galvanostatic discharge-charge cycling curves of&nbsp;ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC&nbsp;and Pt\/C+RuO<sub>2<\/sub>. (i)&nbsp;Setup diagram, (j)&nbsp;spectra, and (k)&nbsp;contour map of in-situ Raman testing. (l)&nbsp;Setup diagram, (m)&nbsp;spectra, and (n)&nbsp;contour map of in-situ XRD&nbsp;testing.<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"550\" height=\"538\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/09\/e2f457ec632c1f6-3.png\" alt=\"\" class=\"wp-image-273126\"\/><\/figure>\n\n\n\n<p><strong>Fig<\/strong><strong>.<\/strong><strong>&nbsp;<\/strong><strong>7<\/strong><strong>.<\/strong><strong>&nbsp;<\/strong>(a) Diagram of the freestanding air cathode. (b)&nbsp;Schematic of a flexible Zn-air battery for a wide temperature range. (c) Open circuit potential curves, (d)&nbsp;Discharge polarization and power density curves , (e) discharge rate performance, (f) specific capacity,&nbsp;and (g)&nbsp;galvanostatic discharge-charge cycling curves of ZnSe-V<sub>2<\/sub>O<sub>5<\/sub>\/NPC&nbsp;at different temperatures. (h) Charge-discharge under different bending states at 5 mA cm<sup>-2<\/sup>. (i, j) Image of charging by tandem devices.<\/p>\n\n\n\n<p>\u4e94\u3001\u6210\u679c\u542f\u793a<\/p>\n\n\n\n<p>\u4e0a\u8ff0\u7814\u7a76\u7ed3\u679c\u8868\u660e\uff0c\u901a\u8fc7\u6784\u5efa\u6c27\u5316\u7269\u001e\u7852\u5316\u7269\u5f02\u8d28\u7ed3\u5e76\u8026\u5408\u591a\u5143\u7d20\u63ba\u6742\u78b3\u8f7d\u4f53\u7684\u534f\u540c\u6539\u6027\u7b56\u7565\uff0c\u662f\u7a81\u7834\u67d4\u6027\u950c\u7a7a\u6c14\u7535\u6c60\u5bbd\u6e29\u533a\u6027\u80fd\u77ed\u677f\u7684\u6709\u6548\u9014\u5f84\u3002\u5f02\u8d28\u754c\u9762\u8bf1\u5bfc\u7684\u7535\u8377\u91cd\u5206\u5e03\u6548\u5e94\u80fd\u591f\u6784\u7b51\u5185\u5efa\u7535\u573a\uff0c\u4f18\u5316\u79bb\u5b50\u8fc1\u79fb\u884c\u4e3a\u4e0e\u6c27\u53cd\u5e94\u4e2d\u95f4\u4f53\u5438\u9644\u81ea\u7531\u80fd\uff0c\u517c\u987e\u4f4e\u6e29\u79bb\u5b50\u4f20\u8f93\u8fdf\u6ede\u4e0e\u9ad8\u6e29\u754c\u9762\u5931\u7a33\u95ee\u9898\uff0c\u540c\u6b65\u63d0\u5347 ORR\/OER \u53cc\u529f\u80fd\u50ac\u5316\u6d3b\u6027\uff1b\u800c\u591a\u5143\u7d20\u63ba\u6742\u78b3\u4e0d\u4ec5\u53ef\u4ee5\u642d\u5efa\u9ad8\u6548\u5bfc\u7535\u7f51\u7edc\u3001\u63d0\u4f9b\u4e30\u5bcc\u5b54\u9053\uff0c\u8fd8\u53ef\u8fdb\u4e00\u6b65\u8c03\u63a7\u7535\u5b50\u7ed3\u6784\u3001\u5f3a\u5316\u754c\u9762\u76f8\u5bb9\u6027\uff0c\u7f13\u89e3\u9ad8\u7535\u6d41\u5bc6\u5ea6\u4e0e\u6781\u7aef\u6e29\u5ea6\u4e0b\u6d3b\u6027\u7269\u8d28\u56e2\u805a\u3001\u4f53\u79ef\u81a8\u80c0\u4e0e\u7ec4\u5206\u6d41\u5931\u73b0\u8c61\uff0c\u5f25\u8865\u4ec5\u4f9d\u9760\u5f02\u8d28\u7ed3\u6539\u6027\u5e26\u6765\u7684\u7ed3\u6784\u7a33\u5b9a\u6027\u4e0d\u8db3\u3002\u8be5\u5de5\u4f5c\u63ed\u793a\u4e86 V\u2082O\u2085\/ZnSe \u5f02\u8d28\u7ed3\u7684\u754c\u9762\u4f5c\u7528\u673a\u5236\uff0c\u4e3a\u8fc7\u6e21\u91d1\u5c5e\u6c27\u5316\u7269\u001e\u7852\u5316\u7269\u57fa\u5bbd\u6e29\u533a\u53cc\u529f\u80fd\u7535\u50ac\u5316\u5242\u7684\u7406\u6027\u8bbe\u8ba1\u63d0\u4f9b\u7406\u8bba\u53c2\u8003\uff0c\u540c\u65f6\u4e5f\u4e3a\u9762\u5411\u53ef\u7a7f\u6234\u7535\u5b50\u3001\u6781\u7aef\u573a\u666f\u50a8\u80fd\u5e94\u7528\u7684\u67d4\u6027\u950c\u7a7a\u6c14\u7535\u6c60\u7535\u6781\u6750\u6599\u5f00\u53d1\u63d0\u4f9b\u53ef\u884c\u7684\u5b9e\u9a8c\u601d\u8def\u3002<strong><\/strong><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u950c\u7a7a\u6c14\u7535\u6c60\u51ed\u501f\u5176\u9ad8\u7406\u8bba\u80fd\u91cf\u5bc6\u5ea6\u3001\u4f4e\u539f\u6599\u6210\u672c\u3001\u826f\u597d\u5b89\u5168\u6027\u4e0e\u73af\u5883\u53cb\u597d\u6027\uff0c\u5728\u5927\u89c4\u6a21\u50a8\u80fd\u3001\u7279\u79cd\u7535\u6e90\u53ca\u67d4\u6027\u7535\u5b50\u8bbe\u5907\u7b49\u9886\u57df\u5177\u6709\u5e7f\u9614\u5e94\u7528\u524d\u666f\u3002\u7136\u800c\uff0c\u4f20\u7edf\u6c34\u7cfb\u7535\u89e3\u6db2\u4f53\u7cfb\u5728\u5bbd\u6e29\u533a&#8230;<\/p>\n","protected":false},"author":31345,"featured_media":0,"comment_status":"open","ping_status":"","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[2],"tags":[],"class_list":["post-273118","post","type-post","status-publish","format-standard","hentry","category-keji"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/273118"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/31345"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=273118"}],"version-history":[{"count":1,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/273118\/revisions"}],"predecessor-version":[{"id":273127,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/273118\/revisions\/273127"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=273118"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=273118"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=273118"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}