{"id":273278,"date":"2026-10-10T08:38:00","date_gmt":"2026-10-10T00:38:00","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=273278"},"modified":"2026-10-09T23:45:16","modified_gmt":"2026-10-09T15:45:16","slug":"%e8%be%bd%e7%a7%91%e5%a4%a7%e8%b5%b5%e5%8d%93%e3%80%81%e7%8e%8b%e6%b0%b8%e9%a3%9e%e6%b7%b1%e8%81%8c%e5%a4%a7%e6%9e%97%e6%b5%a9%e7%84%b6-advanced-energy-materials%ef%bc%9a%e7%b4%a7%e5%87%91%e5%9e%8b","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=273278","title":{"rendered":"\u8fbd\u79d1\u5927\u8d75\u5353\u3001\u738b\u6c38\u98de&#038;\u6df1\u804c\u5927\u6797\u6d69\u7136 Advanced Energy Materials\uff1a\u7d27\u51d1\u578b\u591a\u529f\u80fd\u9633\u79bb\u5b50\u8c03\u63a71D\/3D\u5f02\u8d28\u754c\u9762\uff0c\u5b9e\u73b0\u9ad8\u6548\u7a33\u5b9a\u5012\u7f6e\u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60"},"content":{"rendered":"\n<p><strong>\u3010<\/strong><strong>\u6587\u7ae0\u4fe1\u606f<\/strong><strong>\u3011<\/strong><\/p>\n\n\n\n<p>\u7d27\u51d1\u578b\u591a\u529f\u80fd\u9633\u79bb\u5b50\u8c03\u63a71D\/3D\u5f02\u8d28\u754c\u9762\u7528\u4e8e\u9ad8\u6548\u5012\u7f6e\u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60<\/p>\n\n\n\n<p>\u7b2c\u4e00\u4f5c\u8005\uff1a\u66f9\u7eee\uff0c\u97e9\u6c38\u78ca\uff08\u5171\u540c\u4e00\u4f5c\uff09<\/p>\n\n\n\n<p>\u901a\u8baf\u4f5c\u8005\uff1a\u8d75\u5353*\uff0c\u738b\u6c38\u98de*\uff0c\u6797\u6d69\u7136*<\/p>\n\n\n\n<p>\u5355\u4f4d\uff1a\u6df1\u5733\u804c\u4e1a\u6280\u672f\u5927\u5b66\u970d\u592b\u66fc\u5148\u8fdb\u6750\u6599\u7814\u7a76\u9662\uff1b\u8fbd\u5b81\u79d1\u6280\u5927\u5b66\u6750\u6599\u4e0e\u51b6\u91d1\u5b66\u9662<\/p>\n\n\n\n<p><strong>\u6587\u7ae0\u662f\u5426\u4e00\u7a3f\u591a\u6295\uff1a\u662f\u221a \/ \u5426<\/strong><strong><\/strong><\/p>\n\n\n\n<p><strong>\u3010<\/strong><strong>\u7814\u7a76\u80cc\u666f<\/strong><strong>\u3011<\/strong><\/p>\n\n\n\n<p>\u91d1\u5c5e\u5364\u5316\u7269\u9499\u949b\u77ff\u51ed\u501f\u4f18\u5f02\u7684\u5149\u7535\u6027\u80fd\u3001\u4f4e\u6210\u672c\u6eb6\u6db2\u53ef\u52a0\u5de5\u6027\uff0c\u6210\u4e3a\u4e0b\u4e00\u4ee3\u5149\u4f0f\u6280\u672f\u7684\u7814\u7a76\u70ed\u70b9\uff0c\u5176\u5355\u7ed3\u5668\u4ef6\u5149\u7535\u8f6c\u6362\u6548\u7387\uff08PCE\uff09\u5df2\u7a81\u783427.3%\uff0c\u8d8b\u8fd1\u5546\u4e1a\u5316\u8981\u6c42\u3002\u7136\u800c\uff0c\u9499\u949b\u77ff\u8584\u819c\u5185\u90e8\u7ec4\u5206\u65e0\u5e8f\u3001\u754c\u9762\u7f3a\u9677\u7e41\u591a\uff0c\u975e\u8f90\u5c04\u590d\u5408\u4e25\u91cd\u5236\u7ea6\u4e86\u5668\u4ef6\u6548\u7387\u4e0e\u957f\u671f\u8fd0\u884c\u7a33\u5b9a\u6027\u7684\u540c\u6b65\u63d0\u5347\u3002\u754c\u9762\u5de5\u7a0b\u88ab\u8bc1\u660e\u662f\u6784\u5efa\u9ad8\u6548\u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60\u7684\u6709\u6548\u7b56\u7565\u4e4b\u4e00\uff1a\u901a\u8fc7\u5f15\u5165\u6709\u673a\u5c0f\u5206\u5b50\u3001\u79bb\u5b50\u6db2\u4f53\u6216\u529f\u80fd\u6dfb\u52a0\u5242\uff0c\u53ef\u5728\u4e09\u7ef4\uff083D\uff09\u9499\u949b\u77ff\u8868\u9762\u539f\u4f4d\u5f62\u6210\u4f4e\u7ef4\uff08LD\uff09\u9499\u949b\u77ff\u76f8\uff0c\u6784\u7b511D\/3D\u62162D\/3D\u5f02\u8d28\u754c\u9762\uff0c\u4ece\u800c\u6291\u5236\u975e\u8f90\u5c04\u590d\u5408\u3001\u4f18\u5316\u80fd\u7ea7\u6392\u5217\u5e76\u63d0\u5347\u73af\u5883\u7a33\u5b9a\u6027\u3002<\/p>\n\n\n\n<p>\u7136\u800c\uff0c\u4f20\u7edf\u4f4e\u7ef4\u754c\u9762\u4fee\u9970\u5206\u5b50\u9762\u4e34\u8bf8\u591a\u6311\u6218\uff1a\u4e00\u65b9\u9762\uff0c\u7531\u4e8e2D\u4e0e3D\u9499\u949b\u77ff\u5f62\u6210\u80fd\u76f8\u8fd1\uff0c\u53cd\u5e94\u8fc7\u7a0b\u4e2d\u5bb9\u6613\u540c\u65f6\u751f\u6210\u7ade\u4e89\u6027LD\u76f8\uff0c\u5bfc\u81f4\u754c\u9762\u7ed3\u6784\u4e0d\u5747\u4e00\u3001\u96be\u4ee5\u7cbe\u786e\u63a7\u5236\uff1b\u53e6\u4e00\u65b9\u9762\uff0c\u5e38\u7528\u6709\u673a\u80fa\u76d0\u901a\u5e38\u4ec5\u5177\u5907\u5355\u4e00\u7684Lewis\u9178\u6216Lewis\u78b1\u529f\u80fd\uff0c\u96be\u4ee5\u5b9e\u73b0\u5bf9\u591a\u79cd\u7f3a\u9677\u6001\u7684\u534f\u540c\u949d\u5316\u3002\u56e0\u6b64\uff0c\u5f00\u53d1\u7ed3\u6784\u7d27\u51d1\u3001\u529f\u80fd\u591a\u5143\u7684\u65b0\u578b\u754c\u9762\u4fee\u9970\u5206\u5b50\uff0c\u5b9e\u73b0\u5bf9\u4f4e\u7ef4\u76f8\u751f\u957f\u3001\u7f3a\u9677\u5316\u5b66\u548c\u80fd\u7ea7\u6392\u5217\u7684\u540c\u6b65\u8c03\u63a7\uff0c\u662f\u5f53\u524d\u5012\u7f6e\u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60\u9886\u57df\u4e9f\u5f85\u89e3\u51b3\u7684\u5173\u952e\u95ee\u9898\u3002<\/p>\n\n\n\n<p><strong>\u3010<\/strong><strong>\u6587\u7ae0\u7b80\u4ecb<\/strong><strong>\u3011<\/strong><\/p>\n\n\n\n<p>\u8fd1\u65e5\uff0c\u8fbd\u5b81\u79d1\u6280\u5927\u5b66\u8d75\u5353\u526f\u6559\u6388\u3001\u738b\u6c38\u98de\u526f\u6559\u6388\u8054\u5408\u6df1\u5733\u804c\u4e1a\u6280\u672f\u5927\u5b66\u970d\u592b\u66fc\u5148\u8fdb\u6750\u6599\u7814\u7a76\u9662\u6797\u6d69\u7136\u526f\u6559\u6388\uff0c\u5728\u56fd\u9645\u80fd\u6e90\u9886\u57df\u9876\u7ea7\u671f\u520aAdvanced Energy Materials\u4e0a\u53d1\u8868\u9898\u4e3a&#8221;Compact Multifunctional Cation Regulating 1D\/3D Heterointerface for High-Performance Inverted Perovskite Solar Cells&#8221;\u7684\u7814\u7a76\u8bba\u6587\u3002\u8be5\u5de5\u4f5c\u8bbe\u8ba1\u5f00\u53d1\u4e86\u4e00\u79cd\u591a\u529f\u80fd\u77ed\u94fe\u6709\u673a\u76d0\u2014\u20144,5-\u4e8c\u6c22\u54aa\u5511-2-\u80bc\u6c22\u6eb4\u9178\u76d0\uff08HyImBr\uff09\uff0c\u7528\u4e8e\u57283D\u9499\u949b\u77ff\u8868\u9762\u539f\u4f4d\u6784\u7b51\u7ed3\u6784\u81f4\u5bc6\u7684\u4e00\u7ef4\/\u4e09\u7ef4\uff081D\/3D\uff09\u5f02\u8d28\u754c\u9762\u3002<\/p>\n\n\n\n<p>HyImBr\u5206\u5b50\u7ed3\u5408\u4e86\u54aa\u5511\u5549\u73af\u4e0e\u80bc\u57fa\u56e2\uff0c\u51ed\u501f\u5176\u7d27\u51d1\u7684\u5206\u5b50\u7ed3\u6784\uff0c\u80fd\u591f\u540c\u65f6\u5b9e\u73b0\u591a\u91cd\u754c\u9762\u8c03\u63a7\uff1a\u4e30\u5bcc\u7684\u6c22\u952e\u4f9b\u4f53\/\u53d7\u4f53\u4f4d\u70b9\u4e0e\u9499\u949b\u77ffA\u4f4d\u9633\u79bb\u5b50\u3001\u672a\u914d\u4f4dPb\u00b2\u207a\u5f62\u6210\u591a\u9f7f\u76f8\u4e92\u4f5c\u7528\uff0c\u5f15\u5bfc\u4f4e\u7ef4\u76f8\u9009\u62e9\u6027\u7ec4\u88c5\u4e3a\u7a33\u5b9a\u76841D\u9499\u949b\u77ff\u7ed3\u6784\uff1b\u5176Lewis\u78b1\u4f4d\u70b9\u53ef\u949d\u5316\u591a\u79cd\u754c\u9762\u7f3a\u9677\uff0c\u5927\u5e45\u964d\u4f4e\u7f3a\u9677\u6001\u5bc6\u5ea6\uff1b\u80bc\u57fa\u56e2\u5f15\u5165\u7684\u8fd8\u539f\u6027\u529f\u80fd\u53ef\u51cf\u8f7b\u6c27\u5316\u7269\u79cd\u79ef\u7d2f\uff0c\u6291\u5236\u6c27\u5316\u8bf1\u5bfc\u964d\u89e3\uff1b\u540c\u65f6\u754c\u9762\u91cd\u6784\u6709\u6548\u91ca\u653e\u4e86\u8584\u819c\u5c40\u90e8\u62c9\u4f38\u5e94\u529b\uff0c\u5e76\u4f18\u5316\u4e86\u754c\u9762\u80fd\u7ea7\u6392\u5e03\uff0c\u4fc3\u8fdb\u7535\u5b50\u9ad8\u6548\u63d0\u53d6\u3002\u57fa\u4e8eHyImBr\u754c\u9762\u4fee\u9970\u7684\u5012\u7f6e\u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60\uff0cPCE\u8fbe\u523026.11%\uff0c\u663e\u8457\u4f18\u4e8e\u5bf9\u7167\u7ec4\u768423.51%\uff1b\u5728\u672a\u5c01\u88c5\u6761\u4ef6\u4e0b\u7ecf1100 h\u5b58\u50a8\u540e\u4ecd\u7ef4\u630192.16%\u7684\u521d\u59cb\u6548\u7387\u3002<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"700\" height=\"281\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/10\/2382c315a6ba396.png\" alt=\"\" class=\"wp-image-273279\"\/><\/figure>\n\n\n\n<p><strong>\u56fe1. HyImBr\u5206\u5b50\u7ed3\u6784\u53ca\u5176\u5728\u9499\u949b\u77ff\u8868\u9762\u6784\u7b51\u81f4\u5bc61D\/3D\u5f02\u8d28\u754c\u9762\u7684\u591a\u91cd\u529f\u80fd\u793a\u610f\u56fe<\/strong><strong><\/strong><\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"600\" height=\"563\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/10\/ce6e2814f207c93.png\" alt=\"\" class=\"wp-image-273280\"\/><\/figure>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"660\" height=\"475\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/10\/7f88dbbcaa77a1d.png\" alt=\"\" class=\"wp-image-273281\"\/><\/figure>\n\n\n\n<p><strong>\u3010<\/strong><strong>\u672c\u6587\u8981\u70b9<\/strong><strong>\u3011<\/strong><\/p>\n\n\n\n<p><strong>\u8981\u70b9\u4e00\uff1a\u81f4\u5bc61D\/3D\u5f02\u8d28\u754c\u9762\u7684\u539f\u4f4d\u6784\u7b51\u4e0e\u7ed3\u6784\u8868\u5f81<\/strong><strong><\/strong><\/p>\n\n\n\n<p>\u4e0d\u540c\u4e8e\u4f20\u7edf\u4ee5\u7a7a\u95f4\u4f4d\u963b\u6216\u5355\u4e00\u7f3a\u9677\u76f8\u4e92\u4f5c\u7528\u4e3a\u4e3b\u7684LD\u4fee\u9970\u5206\u5b50\uff0cHyImBr\u88ab\u8bbe\u8ba1\u4e3a\u591a\u529f\u80fd\u9633\u79bb\u5b50\uff1a\u5176\u54aa\u5511\u5549\u73af\u4e0e\u80bc\u57fa\u56e2\u53ef\u540c\u65f6\u63d0\u4f9b\u4e30\u5bcc\u7684\u6c22\u952e\u4f9b\u4f53\/\u53d7\u4f53\u548cLewis\u9178-\u78b1\u4f4d\u70b9\uff0c\u5f15\u5bfc\u5f62\u6210\u4e92\u8fde\u7684\u6c22\u952e\u7f51\u7edc\u800c\u975e\u79bb\u6563\u7684\u4f4e\u7ef4\u76f8\u3002SEM\u8868\u5f81\u663e\u793a\uff0c\u7ecf0.25 mg mL\u207b\u00b9 HyImBr\u4fee\u9970\u540e\uff0c\u9499\u949b\u77ff\u8584\u819c\u8868\u9762\u5f62\u6210\u81f4\u5bc6\u3001\u7eb3\u7c73\u9488\u72b6\u6676\u7c07\u5747\u5300\u5206\u5e03\u7684\u91cd\u6784\u5c42\uff0c\u6676\u7c92\u5c3a\u5bf8\u4ece528 nm\u589e\u5927\u81f3\u7ea6710 nm\uff1bAFM\u6d4b\u5f97\u8868\u9762\u7c97\u7cd9\u5ea6\uff08RMS\uff09\u753122 nm\u964d\u81f320 nm\u3002GIWAXS\u5206\u6790\u8bc1\u5b9e\uff0cHyImBr\u5904\u7406\u540ePbI\u2082\u7279\u5f81\u884d\u5c04\u5cf0\u663e\u8457\u51cf\u5f31\uff0c\u5e76\u51fa\u73b0\u65b01D\u76f8\u884d\u5c04\u5cf0\uff1b\u6df1\u5ea6\u5256\u6790\u8868\u660e\u8be51D\u76f8\u4e3b\u8981\u96c6\u4e2d\u4e8e\u9499\u949b\u77ff\u8868\u9762\u533a\u57df\uff0c\u800c\u975e\u4ec5\u5b58\u5728\u4e8e\u8584\u819c\u8868\u5c42\u3002<\/p>\n\n\n\n<p><strong>\u8981\u70b9\u4e8c\uff1a\u591a\u5c3a\u5ea6\u7f3a\u9677\u949d\u5316\u4e0e\u975e\u8f90\u5c04\u590d\u5408\u6291\u5236<\/strong><strong><\/strong><\/p>\n\n\n\n<p>XPS\u7ed3\u679c\u663e\u793aHyImBr\u4fee\u9970\u540ePb 4f\u3001I 3d\u548cN 1s\u5cf0\u5747\u5411\u9ad8\u7ed3\u5408\u80fd\u65b9\u5411\u79fb\u52a8\uff0c\u8868\u660e\u754c\u9762\u76f8\u4e92\u4f5c\u7528\u589e\u5f3a\uff1bFTIR\u8bc1\u5b9eN\u2013H\u952e\u548cC=N\u952e\u53d1\u751f\u7ea2\u79fb\u4e0e\u5bbd\u5316\uff0c\u63ed\u793a\u4e86HyImBr\u4e0eFA\u207a\/MA\u207a\u4e4b\u95f4\u7684\u6c22\u952e\u4f5c\u7528\u4ee5\u53ca\u4e0e\u672a\u914d\u4f4dPb\u00b2\u207a\u7684\u914d\u4f4d\u4f5c\u7528\u3002\u7a33\u6001\/\u65f6\u95f4\u5206\u8fa8\u5149\u81f4\u53d1\u5149\uff08PL\/TRPL\uff09\u8868\u660e\uff0cHyImBr\u4fee\u9970\u8584\u819c\u7684PL\u5f3a\u5ea6\u663e\u8457\u589e\u5f3a\uff0cTRPL\u8f7d\u6d41\u5b50\u5bff\u547d\u4ece127 ns\u5ef6\u957f\u81f3524 ns\uff1b\u5728PCBM\/C\u2086\u2080\u7535\u5b50\u4f20\u8f93\u5c42\u5668\u4ef6\u4e2d\uff0cPLQY\u4ece0.35%\u63d0\u5347\u81f31.22%\uff0c\u51c6\u8d39\u7c73\u80fd\u7ea7\u5206\u88c2\uff08QFLS\uff09\u4ece146 meV\u63d0\u5347\u81f3214 meV\u3002\u7a7a\u95f4\u7535\u8377\u9650\u5236\u7535\u6d41\uff08SCLC\uff09\u6d4b\u8bd5\u8ba1\u7b97\u5f97\u9677\u9631\u6001\u5bc6\u5ea6\u4ece6.11\u00d710\u00b9\u2075 cm\u207b\u00b3\u964d\u81f35.54\u00d710\u00b9\u2075 cm\u207b\u00b3\u3002DFT\u8ba1\u7b97\u8fdb\u4e00\u6b65\u8868\u660e\uff0cHyImBr\u5728V_Pb\u3001V_I\u3001I_Pb\u548cPb_I\u7b49\u5178\u578b\u7f3a\u9677\u8868\u9762\u5747\u8868\u73b0\u51fa\u8f83\u5f3a\u7684\u5438\u9644\u80fd\uff08\u22121.47 \uff5e \u22122.78 eV\uff09\uff0c\u53ef\u663e\u8457\u964d\u4f4e\u7f3a\u9677\u6001\u5728\u5e26\u9699\u4e2d\u7684\u5f15\u5165\uff0c\u6291\u5236Shockley-Read-Hall\u975e\u8f90\u5c04\u590d\u5408\u3002<\/p>\n\n\n\n<p><strong>\u8981\u70b9\u4e09\uff1a\u80fd\u7ea7\u4f18\u5316\u4e0e\u7535\u8377\u63d0\u53d6\u589e\u5f3a<\/strong><strong><\/strong><\/p>\n\n\n\n<p>Kelvin\u63a2\u9488\u529b\u663e\u5fae\u955c\uff08KPFM\uff09\u6d4b\u5f97\u5bf9\u7167\u7ec4\u4e0eHyImBr\u4fee\u9970\u7ec4\u7684\u8868\u9762\u63a5\u89e6\u7535\u4f4d\u5dee\u5206\u522b\u4e3a453 mV\u548c286 mV\uff0c\u8868\u660e\u4fee\u9970\u540e\u8868\u9762\u7535\u52bf\u5206\u5e03\u66f4\u5747\u5300\u3002\u7d2b\u5916\u5149\u7535\u5b50\u80fd\u8c31\uff08UPS\uff09\u663e\u793a\uff0cHyImBr\u4fee\u9970\u540e\u529f\u51fd\u6570\u75314.55&nbsp;eV\u964d\u81f34.36 eV\uff0c\u5bfc\u5e26\u6700\u5c0f\u503c\uff08CBM\uff09\u7531\u22123.99 eV\u964d\u81f3\u22124.26 eV\uff0c\u4ef7\u5e26\u6700\u5927\u503c\uff08VBM\uff09\u7531\u22125.55 eV\u964d\u81f3\u22125.82 eV\uff0c\u5f62\u6210\u4e86\u6709\u5229\u4e8e\u7535\u5b50\u63d0\u53d6\u3001\u7a7a\u7a74\u963b\u6321\u7684\u80fd\u5e26\u5f2f\u66f2\u3002DFT\u7535\u8377\u5bc6\u5ea6\u5dee\u5206\u5206\u6790\u8868\u660e\uff0cC\u2086\u2080\u5728HyImBr\u4fee\u9970\u8868\u9762\u7684\u7535\u8377\u8f6c\u79fb\u91cf\u4ece0.084 e\u663e\u8457\u964d\u81f3\u22120.003 e\uff0c\u8868\u660e\u754c\u9762\u7535\u5b50\u63d0\u53d6\u901a\u9053\u66f4\u4f18\uff0c\u7535\u8377\u590d\u5408\u88ab\u6709\u6548\u6291\u5236\u3002\u7535\u5316\u5b66\u963b\u6297\u8c31\uff08EIS\uff09\u663e\u793a\u590d\u5408\u7535\u963b\u4ece543 \u03a9\u5927\u5e45\u63d0\u5347\u81f33810 \u03a9\uff1bMott-Schottky\u5206\u6790\u5185\u5efa\u7535\u52bf\u4ece0.91 V\u63d0\u5347\u81f31.02 V\uff0c\u4e0e\u5f00\u8def\u7535\u538b\u63d0\u5347\u4e00\u81f4\u3002<\/p>\n\n\n\n<p><strong>\u8981\u70b9\u56db\uff1a\u5668\u4ef6\u5149\u4f0f\u6027\u80fd\u4e0e\u8fd0\u884c\u7a33\u5b9a\u6027<\/strong><strong><\/strong><\/p>\n\n\n\n<p>\u57fa\u4e8eITO\/PADCB\/\u9499\u949b\u77ff(HyImBr)\/PCBM\/C\u2086\u2080\/bathocuproine(BCP)\/Ag\u7ed3\u6784\u7684\u5668\u4ef6\uff0c\u5bf9\u7167\u7ec4PCE\u4e3a23.51%\uff08Voc=1.11 V\uff0cJsc=25.91 mA cm\u207b\u00b2\uff0cFF=81.0%\uff09\uff0c\u800cHyImBr\u4fee\u9970\u7684\u5668\u4ef6PCE\u8fbe\u523026.11%\uff08Voc=1.18 V\uff0cJsc=25.91 mA cm\u207b\u00b2\uff0cFF=85.27%\uff09\uff0c\u5f00\u8def\u7535\u538b\u548c\u586b\u5145\u56e0\u5b50\u540c\u6b65\u63d0\u5347\u3002EQE\u79ef\u5206\u7535\u6d41\u4e0eJsc\u4e00\u81f4\uff0c50 nm\u6ce2\u957f\u5904\u7684\u9ad8\u54cd\u5e94\u53ca600\u2013760 nm\u8303\u56f4EQE\u7684\u589e\u5f3a\u8bc1\u5b9e\u4e86\u5149\u6355\u83b7\u548c\u754c\u9762\u7535\u8377\u63d0\u53d6\u7684\u534f\u540c\u6539\u5584\u3002\u7a33\u5b9a\u6027\u65b9\u9762\uff1a\u672a\u5c01\u88c5\u5668\u4ef6\u572825\u00b0C\u300130% RH\u4e0b\u5b58\u50a81100 h\u540e\u4fdd\u630192.16%\u521d\u59cb\u6548\u7387\uff08\u5bf9\u7167\u7ec4\u4ec572%\uff09\uff1bISOS-L-2\u6761\u4ef6\uff0865\u00b0C\u8fde\u7eed\u5149\u7167\uff0c\u5c01\u88c5\uff09\u4e0b533 h\u540e\u4fdd\u630183.5%\uff08\u5bf9\u7167\u7ec4\u7ea6150 h\u5373\u8870\u51cf\u81f350%\u4ee5\u4e0b\uff09\uff1b80\u00b0C\u6c2e\u6c14\u6c1b\u56f4\u4e0b880 h\u540e\u4fdd\u630186%\uff08\u5bf9\u7167\u7ec4408 h\u540e\u964d\u81f360%\uff09\u3002\u6c34\u63a5\u89e6\u89d2\u4ece48\u00b0\u63d0\u5347\u81f358\u00b0\uff0c\u6297\u6c27\u5316\u6d4b\u8bd5\uff08O\u2083\u66b4\u973210\u5929\uff09\u8868\u660eHyImBr\u5904\u7406\u8584\u819c\u964d\u89e3\u663e\u8457\u51cf\u7f13\uff0c1H NMR\u8bc1\u5b9e\u80bc\u57fa\u56e2\u5bf9I\u2082\u6c27\u5316\u7269\u79cd\u7684\u8fd8\u539f\u4f5c\u7528\uff0c\u5171\u540c\u4fc3\u6210\u4e86\u4f18\u5f02\u7684\u8fd0\u884c\u7a33\u5b9a\u6027\u3002<\/p>\n\n\n\n<p><strong>\u3010<\/strong><strong>\u6587\u7ae0<\/strong><strong>\u94fe<\/strong><strong>\u63a5<\/strong><strong>\u3011<\/strong><\/p>\n\n\n\n<p>Compact Multifunctional Cation Regulating 1D\/3D Heterointerface for High-Performance Inverted Perovskite Solar Cells<\/p>\n\n\n\n<p><a href=\"https:\/\/doi.org\/10.1002\/aenm.202507160\">https:\/\/doi.org\/10.1002\/aenm.202507160<\/a><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u6587\u7ae0\u4fe1\u606f\u3011 \u7d27\u51d1\u578b\u591a\u529f\u80fd\u9633\u79bb\u5b50\u8c03\u63a71D\/3D\u5f02\u8d28\u754c\u9762\u7528\u4e8e\u9ad8\u6548\u5012\u7f6e\u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60 \u7b2c\u4e00\u4f5c\u8005\uff1a\u66f9\u7eee\uff0c\u97e9\u6c38\u78ca\uff08\u5171\u540c\u4e00\u4f5c\uff09 \u901a\u8baf\u4f5c\u8005\uff1a\u8d75\u5353*\uff0c\u738b\u6c38\u98de*\uff0c\u6797\u6d69\u7136* \u5355&#8230;<\/p>\n","protected":false},"author":31345,"featured_media":0,"comment_status":"open","ping_status":"","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[2],"tags":[],"class_list":["post-273278","post","type-post","status-publish","format-standard","hentry","category-keji"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/273278"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/31345"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=273278"}],"version-history":[{"count":1,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/273278\/revisions"}],"predecessor-version":[{"id":273282,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/273278\/revisions\/273282"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=273278"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=273278"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=273278"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}