{"id":273443,"date":"2026-11-06T09:12:00","date_gmt":"2026-11-06T01:12:00","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=273443"},"modified":"2026-11-05T22:35:56","modified_gmt":"2026-11-05T14:35:56","slug":"%e8%a5%bf%e5%ae%89%e5%bb%ba%e5%a4%a7%e4%ba%91%e6%96%af%e5%ae%81%e6%95%99%e6%8e%88advanced-functional-materials%ef%bc%9a%e6%9c%89%e6%9c%ba%e9%85%8d%e4%bd%93%e5%8a%9f%e8%83%bd%e5%8c%96-con2-c-n2ni","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=273443","title":{"rendered":"\u897f\u5b89\u5efa\u5927\u4e91\u65af\u5b81\u6559\u6388Advanced Functional Materials\uff1a\u6709\u673a\u914d\u4f53\u529f\u80fd\u5316 CoN2-C-N2Ni \u53cc\u539f\u5b50\u5b9a\u5411\u8c03\u63a7\u6790\u6c22\u4e0e\u7898\u8fd8\u539f\u4e2d\u7684\u8d28\u5b50\u548c\u975e\u8d28\u5b50\u8f6c\u79fb"},"content":{"rendered":"\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"700\" height=\"346\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/11\/2382c315a6ba396-1.png\" alt=\"\" class=\"wp-image-273444\"\/><\/figure>\n\n\n\n<p><strong>\u3010\u6587\u7ae0\u4fe1\u606f\u3011<\/strong><strong><\/strong><\/p>\n\n\n\n<p>\u6709\u673a\u914d\u4f53\u529f\u80fd\u5316 CoN<sub>2<\/sub>-C-N<sub>2<\/sub>Ni \u53cc\u539f\u5b50\u5b9a\u5411\u8c03\u63a7\u6790\u6c22\u4e0e\u7898\u8fd8\u539f\u4e2d\u7684\u8d28\u5b50\u548c\u975e\u8d28\u5b50\u8f6c\u79fb<\/p>\n\n\n\n<p>\u7b2c\u4e00\u4f5c\u8005\uff1a\u51af\u67d4\u3001\u5b59\u68a6\u9f99<\/p>\n\n\n\n<p>\u901a\u8baf\u4f5c\u8005\uff1a\u4e91\u65af\u5b81*<\/p>\n\n\n\n<p>\u4f5c\u8005\u5355\u4f4d\uff1a\u897f\u5b89\u5efa\u7b51\u79d1\u6280\u5927\u5b66\u3001\u4e2d\u56fd\u79d1\u5b66\u9662\u5316\u5b66\u7814\u7a76\u6240<\/p>\n\n\n\n<p><strong>\u3010\u7814\u7a76\u80cc\u666f\u3011<a><\/a><\/strong><strong><\/strong><\/p>\n\n\n\n<p>\u53cd\u5e94\u4e2d\u95f4\u4f53\u7684\u6301\u7eed\u4f9b\u7ed9\u3001\u754c\u9762\u5bcc\u96c6\u4e0e\u53ca\u65f6\u91ca\u653e\uff0c\u662f\u5f71\u54cd\u591a\u7535\u5b50\u50ac\u5316\u53cd\u5e94\u901f\u7387\u548c\u7a33\u5b9a\u6027\u7684\u5173\u952e\u56e0\u7d20\u3002\u5bf9\u4e8e\u6790\u6c22\u53cd\u5e94\uff08HER\uff09\u548c\u4e09\u7898\u5316\u7269\u8fd8\u539f\u53cd\u5e94\uff08IRR\uff09\u800c\u8a00\uff0c\u9664\u4e86\u6d3b\u6027\u4f4d\u70b9\u672c\u8eab\u7684\u5438\/\u8131\u9644\u80fd\u529b\uff0c\u754c\u9762\u4e2d\u95f4\u4f53\u7684\u8fc1\u79fb\u8def\u5f84\u53ca\u5c40\u90e8\u6d53\u5ea6\u540c\u6837\u51b3\u5b9a\u4e86\u53cd\u5e94\u52a8\u529b\u5b66\u3002\u4e2d\u95f4\u4f53\u4f9b\u7ed9\u4e0d\u8db3\u5c06\u9650\u5236\u53cd\u5e94\u901f\u7387\uff0c\u800c\u5c40\u90e8\u8fc7\u91cf\u79ef\u7d2f\u5219\u53ef\u80fd\u9020\u6210\u6d3b\u6027\u4f4d\u70b9\u5835\u585e\u548c\u754c\u9762\u4f20\u8f93\u53d7\u963b\u3002<\/p>\n\n\n\n<p>\u53cc\u539f\u5b50\u50ac\u5316\u5242\u80fd\u591f\u5229\u7528\u76f8\u90bb\u91d1\u5c5e\u4f4d\u70b9\u4e4b\u95f4\u7684\u534f\u540c\u4f5c\u7528\u8c03\u8282\u53cd\u5e94\u8fc7\u7a0b\uff0c\u4f46\u5df2\u6709\u7814\u7a76\u591a\u805a\u7126\u4e8e\u91d1\u5c5e\u914d\u4f4d\u7ed3\u6784\u3001\u7535\u5b50\u6001\u53ca\u5438\u9644\u80fd\u7684\u4f18\u5316\uff0c\u5bf9\u4e2d\u95f4\u4f53\u5982\u4f55\u6301\u7eed\u5230\u8fbe\u6d3b\u6027\u4f4d\u70b9\u3001\u5982\u4f55\u907f\u514d\u5c40\u90e8\u8fc7\u5ea6\u79ef\u7d2f\u7684\u5173\u6ce8\u76f8\u5bf9\u6709\u9650\u3002<a>HER\u6d89\u53ca\u6790\u6c22\u76f8\u5173\u7684\u8d28\u5b50\u578b\u4e2d\u95f4\u4f53\uff1bIRR\u6d89\u53ca\u7898\u8fd8\u539f\u76f8\u5173\u7684\u975e\u8d28\u5b50\u578b\u4e2d\u95f4\u4f53\uff0c\u4e24\u7c7b\u53cd\u5e94\u5bf9\u754c\u9762\u7269\u79cd\u4f20\u8f93\u7684\u9700\u6c42\u4e0d\u540c<\/a>\u3002\u56e0\u6b64\uff0c\u5728\u540c\u4e00\u50ac\u5316\u4f53\u7cfb\u4e2d\uff0c\u6784\u7b51\u517c\u5177\u8d28\u5b50\u4e0e\u975e\u8d28\u5b50\u578b\u4e2d\u95f4\u4f53\u8c03\u63a7\u80fd\u529b\u7684\u4f20\u8f93\u901a\u9053\uff0c\u4ecd\u5177\u6709\u6311\u6218\u6027\u3002<\/p>\n\n\n\n<p>\u5747\u82ef\u4e09\u7532\u9178\uff08Trimesic acid, TMA\uff09\u4e2d\u7684-COOH\/-COO<sup>\u2013<\/sup>\u57fa\u56e2\u53ef\u901a\u8fc7\u53ef\u9006\u7684\u8d28\u5b50\u5316\/\u53bb\u8d28\u5b50\u5316\u8fc7\u7a0b\u53c2\u4e0e\u6c22\u76f8\u5173\u7269\u79cd\u4f20\u9012\uff0c\u5176\u82b3\u9999\u9aa8\u67b6\u53ca\u6781\u6027\u7fa7\u9178\u76d0\u73af\u5883\u6709\u671b\u8c03\u8282\u7898\u76f8\u5173\u7269\u79cd\u7684\u754c\u9762\u5206\u5e03\u3002\u5c06\u8fd9\u79cd\u6709\u673a\u914d\u4f53\u4e0e\u53cc\u539f\u5b50\u4f4d\u70b9\u76f8\u7ed3\u5408\uff0c\u4e3a\u540c\u65f6\u4f18\u5316\u6d3b\u6027\u4e2d\u5fc3\u4e0e\u4e2d\u95f4\u4f53\u4f20\u8f93\u63d0\u4f9b\u4e86\u65b0\u7684\u754c\u9762\u5de5\u7a0b\u601d\u8def\u3002<\/p>\n\n\n\n<p><strong>\u3010\u6587\u7ae0\u7b80\u4ecb\u3011<\/strong><strong><\/strong><\/p>\n\n\n\n<p><a><\/a>\u8fd1\u65e5\uff0c<strong>\u897f\u5b89\u5efa\u7b51\u79d1\u6280\u5927\u5b66\u4e91\u65af\u5b81\u6559\u6388\u56e2\u961f<\/strong>\u5728\u56fd\u9645\u77e5\u540d\u671f\u520a<strong><em><strong><em>Advanced Functional Materials<\/em><\/strong><\/em><\/strong>\u4e0a\u53d1\u8868\u4e86\u9898\u4e3a<strong>\u201cOrganic Ligand-Functionalized CoN<\/strong><strong><sub><strong><sub>2<\/sub><\/strong><\/sub><\/strong><strong>-C-N<\/strong><strong><sub><strong><sub>2<\/sub><\/strong><\/sub><\/strong><strong>Ni Dual-Atom for Tailored Proton and Non-Proton Transfer in Hydrogen Evolution and Triiodide Reduction<\/strong>\u201d\u7684\u7814\u7a76\u8bba\u6587\u3002<a>\u8be5\u7814\u7a76\u4ee5Ti<\/a><sub>3<\/sub>C<sub>2<\/sub>T<sub>X<\/sub><sub>&nbsp;<\/sub>MXene\u4e3a\u8f7d\u4f53\uff0c\u6784\u7b51CoN<sub>2<\/sub>-C-N<sub>2<\/sub>Ni\u53cc\u539f\u5b50\u6d3b\u6027\u4e2d\u5fc3\uff0c\u5e76\u901a\u8fc7TMA\u914d\u4f53\u529f\u80fd\u5316\u5f62\u6210\u6709\u673a-\u65e0\u673a\u8026\u5408\u754c\u9762\u3002TMA\u7684\u82b3\u9999\u03c0-\u03c0\u5806\u79ef\u7ed3\u6784\u4e0e-COOH\/-COO<sup>&#8211;<\/sup>\u57fa\u56e2\u534f\u540c\u4f5c\u7528\uff0c\u5728\u4fdd\u7559Co\/Ni\u53cc\u539f\u5b50\u914d\u4f4d\u7ed3\u6784\u7684\u540c\u65f6\uff0c\u6269\u5927MXene\u5c42\u95f4\u7a7a\u95f4\uff0c\u4fc3\u8fdb\u8d28\u5b50\u578bH<sup>*<\/sup>\u4e0e\u975e\u8d28\u5b50\u578bI<sup>*<\/sup>\u4e2d\u95f4\u4f53\u6301\u7eed\u5411\u6d3b\u6027\u4f4d\u70b9\u4f20\u8f93\u5e76\u51cf\u8f7b\u5176\u5c40\u90e8\u8fc7\u5ea6\u79ef\u7d2f\u3002<a>TMA-CoNi<\/a><sub>DA<\/sub>-MXene\u4f5c\u4e3aIRR\u57fa\u592a\u9633\u80fd\u7535\u6c60\u5bf9\u7535\u6781\uff0c\u5149\u7535\u8f6c\u6362\u6548\u7387\u8fbe8.62%\uff1b \u7528\u4e8e\u78b1\u6027HER\u9634\u6781\uff0c\u572810 mA&nbsp;cm<sup>-2<\/sup>\u4e0b\u4ec5\u970071 mV\u8fc7\u7535\u4f4d\u3002\u539f\u4f4d\u62c9\u66fc\u3001\u539f\u4f4d\u7ea2\u5916\u548c\u7406\u8bba\u8ba1\u7b97\u8fdb\u4e00\u6b65\u63ed\u793a\u4e86\u4e24\u7c7b\u4e2d\u95f4\u4f53\u7684\u5dee\u5f02\u5316\u754c\u9762\u4f20\u8f93\u673a\u5236\u3002<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"700\" height=\"387\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/11\/ce6e2814f207c93-1.png\" alt=\"\" class=\"wp-image-273445\"\/><\/figure>\n\n\n\n<p><strong>\u3010\u672c\u6587\u8981\u70b9\u3011<\/strong><\/p>\n\n\n\n<p><a><\/a><strong>\u8981\u70b9\u4e00\uff1a<a>TMA\u529f\u80fd\u5316<\/a><\/strong><strong>Mxene\u8d1f\u8f7d<\/strong><strong>Co<\/strong><strong>\/<\/strong><strong>Ni\u53cc\u539f\u5b50\u6784\u7b51\u6709\u673a-\u65e0\u673a\u754c\u9762\u8fde\u7eed\u4f20\u8f93\u901a\u9053<\/strong><strong><\/strong><\/p>\n\n\n\n<p><a><\/a>\u9996\u5148\u901a\u8fc7\u9009\u62e9\u6027\u523b\u8680\u5236\u5907Ti<sub>3<\/sub>C<sub>2<\/sub>T<sub>x<\/sub><sub>&nbsp;<\/sub>MXene\uff0c\u518d\u4ee5\u4e09\u805a\u6c30\u80fa\u4e3a\u6c2e\u6e90\u548c\u914d\u4f4d\u951a\u5b9a\u70b9\u5f15\u5165Co\/Ni\u53cc\u539f\u5b50\uff0c\u968f\u540e\u5229\u7528TMA\u4fee\u9970\u83b7\u5f97<strong>TMA-CoNi<\/strong><strong><sub><strong><sub>DA<\/sub><\/strong><\/sub><\/strong><strong>-MXene<\/strong>\uff08\u56fe1a\uff09\u3002SEM\u4e0eTEM\u663e\u793a\uff0c\u4fee\u9970\u540e\u6750\u6599\u4ecd\u4fdd\u6301MXene\u5c42\u72b6\u7ed3\u6784\uff1b\u540c\u65f6\u5c42\u95f4\u5448\u73b0\u66f4\u5f00\u653e\u7684\u5f62\u8c8c\u3002HAADF-STEM\u89c2\u5bdf\u5230\u76f8\u90bb\u539f\u5b50\u7ea7\u4eae\u70b9\uff0c\u5e73\u5747\u95f4\u8ddd\u7ea62.93 \u00c5\uff0cEDS\u8868\u660eCo\u3001Ni\u7b49\u5143\u7d20\u5206\u5e03\u5747\u5300\uff08\u56fe1b-e\uff09\u3002XRD\u4e2d\uff08002\uff09\u884d\u5c04\u5cf0\u5411\u4f4e\u89d2\u5ea6\u79fb\u52a8\uff0c\u8868\u660e\u5c42\u95f4\u8ddd\u6269\u5927\uff0c\u7ea627\u00b0\u5904\u7684\u65b0\u884d\u5c04\u5cf0\u5f52\u56e0\u4e8e\u82b3\u9999TMA\u7684\u03c0\u2013\u03c0\u5806\u79ef\uff08\u56fe1f\uff09\u3002FT-IR\u57281705\u30011560\u548c1395 cm<sup>-1<\/sup>\u5904\u5448\u73b0\u7fa7\u57fa\u76f8\u5173\u632f\u52a8\uff0c\u5e76\u57281278 cm<sup>-1<\/sup>\u5904\u51fa\u73b0Ti-O-C\u5438\u6536\u4fe1\u53f7\uff0c\u8bc1\u5b9eTMA\u901a\u8fc7\u542b\u6c27\u57fa\u56e2\u4e0e\u8f7d\u4f53\u7ed3\u5408\uff08\u56fe1g\uff09\u3002\u8fd9\u4e9b\u7ed3\u679c\u8868\u660e\uff0cTMA\u529f\u80fd\u5316\u62d3\u5c55\u4e86\u754c\u9762\u4f20\u8f93\u7a7a\u95f4\uff0c\u4e14\u672a\u660e\u663e\u7834\u574fMXene\u7684\u4e3b\u4f53\u7ed3\u6784\u3002<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"700\" height=\"785\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/11\/7f88dbbcaa77a1d-1.png\" alt=\"\" class=\"wp-image-273446\"\/><\/figure>\n\n\n\n<p>\u56fe1. a) <a><\/a>TMA-CoNi<sub>DA<\/sub>-MXene\u7684\u5408\u6210\u8fc7\u7a0b\u793a\u610f\u56fe\u3002b) TMA-CoNi<sub>DA<\/sub>-Mxene\u7684SEM\u53ca\u5c40\u90e8\u653e\u5927\u56fe\u3002c) <a><\/a>TMA-CoNi<sub>DA<\/sub>-MXene\u7684HRTEM\u56fe\u3002d) \u56fec\u5bf9\u5e94\u533a\u57df\u7684IFFT\u56fe\u50cf\u3002e) TMA-CoNi<sub>DA<\/sub>-MXene\u7684HAADF-STEM\u3001\u76f8\u90bbCo\/Ni\u4f4d\u70b9\u5f3a\u5ea6\u5206\u5e03\u53caEDS\u5143\u7d20\u6620\u5c04\u56fe\u3002f)&nbsp;<a>MXene<\/a>, CoNi<sub>DA<\/sub>-MXene\u4e0eTMA-CoNi<sub>DA<\/sub>-MXene\u7684XRD\u8c31\u56fe\u3002(g) \u5404\u6837\u54c1\u7684FT-IR\u5149\u8c31\u3002<\/p>\n\n\n\n<p><strong>\u8981\u70b9\u4e8c\uff1a\u89e3\u6790CoN<\/strong><strong><sub><strong><sub>2<\/sub><\/strong><\/sub><\/strong><strong>&#8211;<\/strong><strong>C<\/strong><strong>&#8211;<\/strong><strong>N<\/strong><strong><sub><strong><sub>2<\/sub><\/strong><\/sub><\/strong><strong>Ni\u914d\u4f4d\u7ed3\u6784\u53caTMA<\/strong><strong>\/<\/strong><strong>\u8f7d\u4f53\u754c\u9762\u8026\u5408<\/strong><strong><\/strong><\/p>\n\n\n\n<p><a><\/a>XPS\u8c31\u56fe\u663e\u793a\uff0cTMA\u5904\u7406\u540eTi\u76f8\u5173\u7ec4\u5206\u7ed3\u5408\u80fd\u53d1\u751f\u53d8\u5316\uff0c\u7ed3\u5408FT-IR\uff0c\u8fdb\u4e00\u6b65\u8bc1\u5b9e\u7fa7\u57fa\u4e3b\u8981\u4e0eMXene\u4e2d\u7684Ti\u4f4d\u70b9\u53d1\u751f\u754c\u9762\u8026\u5408\uff08\u56fe2a-c\uff09\u3002Co\u3001Ni\u7684\u5149\u7535\u5b50\u80fd\u8c31\u548cK\u8fb9XANES\u5728TMA\u529f\u80fd\u5316\u524d\u540e\u53d8\u5316\u8f83\u5c0f\uff0c\u8868\u660e\u53cc\u539f\u5b50\u4e2d\u5fc3\u7684\u7535\u5b50\u73af\u5883\u603b\u4f53\u4fdd\u6301\u7a33\u5b9a\u3002Co\u4e0eNi\u7684\u5085\u91cc\u53f6\u53d8\u6362EXAFS\u5747\u5448\u73b0\u4ee5M-N\/C\u4e3a\u4e3b\u7684\u8fd1\u90bb\u914d\u4f4d\u4fe1\u53f7\uff0c\u5e76\u5728\u8f83\u9ad8\u914d\u4f4d\u58f3\u5c42\u51fa\u73b0\u8f83\u5f31\u7684Co-Ni\/Ni-Co\u76f8\u5173\u7279\u5f81\uff1b\u62df\u5408\u7ed3\u679c\u8fdb\u4e00\u6b65\u8868\u660e\u5176\u5c40\u57df\u7ed3\u6784\u4e3aCo-N<sub>2<\/sub>C\u4e0eNi-N<sub>2<\/sub>C\uff08\u56fe2d-i\uff09\u3002\u7ed3\u5408\u5c0f\u6ce2\u53d8\u6362\u5206\u6790\uff08\u56fe2j-m\uff09\uff0c\u53ef\u77e5\u76f8\u90bbCo\u3001Ni\u901a\u8fc7\u5171\u4eab\u78b3\u6865\u5f62\u6210CoN<sub>2<\/sub>-C-N<sub>2<\/sub>Ni\u53cc\u539f\u5b50\u6784\u578b\uff0c\u4e14TMA\u5f15\u5165\u540e\u8be5\u7ed3\u6784\u672a\u88ab\u7834\u574f\u3002ICP-MS\u6d4b\u5f97\u6837\u54c1\u4e2dCo\u548cNi\u542b\u91cf\u5206\u522b\u4e3a2.08 wt%\u548c1.98 wt%\uff0c\u8fdb\u4e00\u6b65\u8bf4\u660e\u4e24\u79cd\u91d1\u5c5e\u7684\u5f15\u5165\u6bd4\u4f8b\u63a5\u8fd11:1\u3002<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"700\" height=\"757\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/11\/4e9a0ba2491dfde-1.png\" alt=\"\" class=\"wp-image-273447\"\/><\/figure>\n\n\n\n<p>\u56fe2. <a><\/a>MXene\uff0c<a><\/a>CoNi<sub>DA<\/sub>-MXene\u4e0eTMA-CoNi<sub>DA<\/sub>-MXene\u7684&nbsp;a) Ti 2p\uff0cb) C 1s\uff0cc) O 1s\u9ad8\u5206\u8fa8XPS\u8c31\u56fe\u3002<a><\/a>CoNi<sub>DA<\/sub>-MXene\u4e0eTMA-CoNi<sub>DA<\/sub>-MXene\u7684d) Co K-edge\u8c31\uff0ce) \u5085\u91cc\u53f6\u53d8\u6362EXAFS\u8c31\uff0cf) <a>R\u7a7a\u95f4<\/a>\u62df\u5408\u56fe\u8c31\u3002<a><\/a>CoNi<sub>DA<\/sub>-MXene\u4e0eTMA-CoNi<sub>DA<\/sub>-MXene\u7684g) Ni K<a><\/a>-edge\u8c31\uff0ch) R\u7a7a\u95f4\u53cai) \u62df\u5408\u56fe\u8c31\u3002j-m) TMA-CoNi<sub>DA<\/sub>-MXene\u4e0eCoNi<sub>DA<\/sub>-MXene\u7684Co\u3001Ni EXAFS\u5c0f\u6ce2\u53d8\u6362\u3002<\/p>\n\n\n\n<p><strong>\u8981\u70b9\u4e09\uff1a<\/strong><strong>TMA\u529f\u80fd\u5316<\/strong><strong>\u4e2d\u95f4\u4f53\u4f20\u8f93<\/strong><strong>\u901a\u9053\u9ad8\u6548\u50ac\u5316<\/strong><strong>IRR\u548cHER<\/strong><strong><\/strong><\/p>\n\n\n\n<p><a><\/a><a><\/a><a>TMA-CoNi<\/a><sub>DA<\/sub>-MXene\u5728IRR\u5668\u4ef6\u4e2d\u7684\u5149\u7535\u8f6c\u6362\u6548\u7387\u8fbe8.62%\uff0c\u9ad8\u4e8e\u53c2\u7167\u7ec4\u7684CoNi<sub>DA<\/sub>-MXene\u3001MXene\u548cPt<a>\uff08\u56fe3a\uff09<\/a>\u3002CV\u6c27\u5316-\u8fd8\u539f\u5cf0\u95f4\u8ddd\u7f29\u5c0f\u81f30.49 V\uff0c\u4ea4\u6362\u7535\u6d41\u5bc6\u5ea6\u4e3a3.47 mA\u00b7cm<sup>-2<\/sup>\uff0c\u8868\u660e\u4e09\u7898\u5316\u7269\u8fd8\u539f\u52a8\u529b\u5b66\u52a0\u5feb\uff08\u56fe3b-d\uff09\u3002EIS\u663e\u793a\uff0cTMA-CoNi<sub>DA<\/sub>-MXene\u7684\u754c\u9762\u7535\u8377\u8f6c\u79fb\u7535\u963b\u4ec5\u4e3a1.07 \u03a9\u00b7cm<sup>2<\/sup>\u300250\u5708\u8fde\u7eedCV\u4e0e\u5149\u5f00\u5173\u6d4b\u8bd5\u4e5f\u8868\u73b0\u51fa\u8f83\u7a33\u5b9a\u7684\u54cd\u5e94\uff08\u56fe3e-i\uff09\u3002\u4e0a\u8ff0\u7ed3\u679c\u8868\u660e\uff0cTMA\u754c\u9762\u8c03\u63a7\u4fc3\u8fdb\u4e86\u975e\u8d28\u5b50\u578b\u76f8\u5173\u7269\u79cd\u7684\u4f20\u8f93\u53caI<sub>3<\/sub><sup>&#8211;<\/sup>\/I<sup>&#8211;<\/sup>\u7684\u9ad8\u6548\u8f6c\u5316\u3002<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"700\" height=\"584\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/11\/b14210e1ee30421-1.png\" alt=\"\" class=\"wp-image-273448\"\/><\/figure>\n\n\n\n<p>\u56fe3. a) \u4e0d\u540c\u5bf9\u7535\u6781\u5668\u4ef6\u7684J-V\u66f2\u7ebf\u3002<a><\/a><a>MXene<\/a>\uff0cCoNi<sub>DA<\/sub>-MXene\u4e0e<a><\/a>TMA-CoNi<sub>DA<\/sub>-MXene\u7684b) Tafel\u66f2\u7ebf\uff0cc) CV\uff0cd) \u5cf0\u503c\u7535\u6d41\u4e0e\u626b\u63cf\u901f\u7387\u5173\u7cfb\u56fe\u53cae) Nyquist\u56fe\u3002TMA-CoNi<sub>DA<\/sub>-MXene\u7684f) 50\u5708CV\u5faa\u73af\u4e0eg) \u6c27\u5316\/\u8fd8\u539f\u5cf0\u503c\u7535\u6d41\u53d8\u5316\u3002MXene\uff0cCoNi<sub>DA<\/sub>-MXene\u4e0e<a><\/a>TMA-CoNi<sub>DA<\/sub>-MXene\u7684h) \u5149\u5f00\u5173\u54cd\u5e94\u53cai) \u5149\u7535\u6d41\u7a33\u5b9a\u6027\u3002<\/p>\n\n\n\n<p><a><\/a>\u5728\u78b1\u6027HER\u4e2d\uff0cTMA-CoNi<sub>DA<\/sub>-MXene\u8fbe\u523010 mA\u00b7cm<sup>-2<\/sup>\u7684\u8fc7\u7535\u4f4d\u4ec5\u4e3a71 mV\u3002Tafel\u659c\u7387\u7531\u672a\u529f\u80fd\u5316\u768495 mV\u00b7dec<sup>-1<\/sup>\u964d\u4f4e\u81f358 mV\u00b7dec<sup>-1<\/sup>\uff0c\u8868\u660e\u53cd\u5e94\u52a8\u529b\u5b66\u5f97\u5230\u6539\u5584\uff08\u56fe4a-c\uff09\u3002\u5176C<sub>dl<\/sub>\u8fbe5.15 mF\u00b7cm<sup>-2<\/sup>\uff0c\u4f30\u7b97\u7535\u5316\u5b66\u6d3b\u6027\u9762\u79ef\u7ea6103 cm<sup>2<\/sup>\uff0c\u7535\u8377\u8f6c\u79fb\u7535\u963b\u4ec55.96 \u03a9\u3002\u6b64\u5916\uff0c1000\u5708\u6781\u5316\u5faa\u73af\u540eLSV\u53d8\u5316\u8f83\u5c0f\uff0c30 h\u6052\u7535\u6d41\u6d4b\u8bd5\u4e5f\u8868\u73b0\u51fa\u826f\u597d\u7684\u957f\u671f\u7a33\u5b9a\u6027\uff08\u56fe4d-h\uff09\u3002<a>\u8fd9<\/a>\u8868\u660eTMA\u4e0d\u4ec5\u63d0\u9ad8\u4e86\u6d3b\u6027\u4f4d\u70b9\u7684\u5229\u7528\u7387\uff0c\u8fd8\u6709\u52a9\u4e8e\u6539\u5584\u754c\u9762\u8d28\u5b50\u578bH<sup>*<\/sup>\u7684\u6301\u7eed\u4f20\u9012\u3002<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"700\" height=\"584\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/11\/de5bcf7d8eaea98-1.png\" alt=\"\" class=\"wp-image-273449\"\/><\/figure>\n\n\n\n<p>\u56fe4. \u5404\u79cd\u50ac\u5316\u5242\u7684a) LSV\u6781\u5316\u66f2\u7ebf\u548cb) Tafel\u659c\u7387\u3002TMA-CoNi<sub>DA<\/sub>-MXene\u5728c) \u4e0d\u540c\u8fc7\u7535\u4f4d\u533a\u95f4\u7684Tafel\u5bf9\u6bd4\u3002Ni Foam\uff0c<a><\/a>MXene\uff0c<a><\/a>CoNi<sub>DA<\/sub>-MXene\u4e0eTMA-CoNi<sub>DA<\/sub>-MXene\u7684d) C<sub>dl<\/sub>\u503c\uff0ce) ECSA\uff0cf) Nyquist\u56fe\u3002MXene\uff0cCoNi<sub>DA<\/sub>-MXene\u4e0eTMA-CoNi<sub>DA<\/sub>-MXene\u7684g) 1000\u5708\u5faa\u73af\u524d\u540eLSV\u66f2\u7ebf\u53cah) \u6052\u7535\u6d41\u7a33\u5b9a\u6027\u3002<\/p>\n\n\n\n<p><a><\/a><strong>\u8981\u70b9\u56db\uff1a\u539f\u4f4d\u5149\u8c31\u4e0e\u7406\u8bba\u8ba1\u7b97\u63ed\u793a<\/strong><strong>\u975e\u8d28\u5b50\u548c\u8d28\u5b50\u578b<\/strong><strong>\u4e2d\u95f4\u4f53\u7684\u5dee\u5f02\u5316\u4f20\u8f93\u673a\u5236<\/strong><strong><\/strong><\/p>\n\n\n\n<p><a><\/a>\u7814\u7a76\u91c7\u7528\u539f\u4f4d\u62c9\u66fc\u8ffd\u8e2aIRR\u8fc7\u7a0b\u4e2d\u7684\u975e\u8d28\u5b50\u578bI<sup>*<\/sup>\u7684\u6f14\u5316\u3002\u968f\u7535\u4f4d\u8d1f\u79fb\uff0cCoNi<sub>DA<\/sub>-MXene\u7684\u754c\u9762I<sub>3<\/sub><sup>&#8211;<\/sup>\u4fe1\u53f7\u5148\u5347\u540e\u964d\uff0c\u57280.1 V\u9644\u8fd1\u8fbe\u5230\u6700\u5f3a<a><\/a>\uff0c\u8868\u660e\u975e\u8d28\u5b50\u578bI<sup>*<\/sup>\u5728\u6d3b\u6027\u4f4d\u70b9\u9644\u8fd1\u8fc7\u5ea6\u79ef\u7d2f\uff08\u56fe5a\uff09\u3002TMA\u529f\u80fd\u5316\u540e\uff0cI<sub>3<\/sub><sup>&#8211;<\/sup>\u4fe1\u53f7\u968f\u7535\u4f4d\u6301\u7eed\u964d\u4f4e\uff0cCo\/Ni-I\u4fe1\u53f7\u6e05\u6670\u53ef\u8fa8\uff0c\u8868\u660e\u5176\u66f4\u6709\u5229\u4e8e\u7f13\u51b2\u548c\u8f6c\u79fb\u975e\u8d28\u5b50\u578bI<sup>*<\/sup>\uff08\u56fe5b-c\uff09\u3002\u539f\u4f4d\u7ea2\u5916\u8fdb\u4e00\u6b65\u663e\u793a\uff0cTMA-CoNi<sub>DA<\/sub>-MXene\u5728HER\u4e2d\u5177\u6709\u66f4\u5f3a\u7684\u754c\u9762\u6c34\u4f38\u7f29\u548c\u5f2f\u66f2\u632f\u52a8\u4fe1\u53f7\u3002\u5206\u5cf0\u5206\u6790\u8868\u660e\uff0c\u672a\u4fee\u9970\u6837\u54c1\u7684\u754c\u9762\u6c34\u4e2d\u81ea\u7531\u6c34\u5360\u6bd4\u7ea660%\uff0c\u800cTMA\u529f\u80fd\u5316\u6837\u54c1\u4e2d\u56db\u914d\u4f4d\u6c22\u952e\u6c34\uff084-HB H<sub>2<\/sub>O\uff09\u5360\u6bd4\u8d85\u8fc770%\uff0c\u8868\u660eTMA\u6709\u5229\u4e8e\u91cd\u6784\u8fde\u7eed\u7684\u754c\u9762\u6c22\u952e\u7f51\u7edc\uff0c\u4e3a\u8d28\u5b50\u578bH<sup>*<\/sup>\u4f20\u9012\u63d0\u4f9b\u66f4\u9002\u5b9c\u7684\u5fae\u73af\u5883\uff08\u56fe5d-i\uff09\u3002<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"700\" height=\"770\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/11\/aa3023e0288002c.png\" alt=\"\" class=\"wp-image-273450\"\/><\/figure>\n\n\n\n<p>\u56fe5. a)&nbsp;<a><\/a><a><\/a><a>CoNi<\/a><sub>DA<\/sub>-MXene\u4e0eb) <a>TMA-<\/a>CoNi<sub>DA<\/sub>-MXene\u7684IRR\u539f\u4f4d\u62c9\u66fc\u5149\u8c31\u53cac) I<sub>3<\/sub><sup>&#8211;<\/sup>\u5cf0\u5f3a\u5ea6\u53d8\u5316\u3002d) <a><\/a>CoNi<sub>DA<\/sub>-MXene\u4e0ee) <a>TMA-<\/a>CoNi<sub>DA<\/sub>-MXene\u7684HER\u539f\u4f4d\u7ea2\u5916\u8c31\u3002f)&nbsp;CoNi<sub>DA<\/sub>-MXene\u4e0eg) TMA-CoNi<sub>DA<\/sub>-MXene\u7684\u754c\u9762\u6c34\u7ec4\u5206\u62df\u5408\u53cah) \u4e0d\u540c\u7535\u4f4d\u4e0b\u754c\u9762\u6c34\u7684\u6bd4\u4f8b\u3002i) TMA\u4fc3\u8fdb\u975e\u8d28\u5b50\u578b\u7898\u4e0e\u8d28\u5b50\u578b\u6c22\u76f8\u5173\u4e2d\u95f4\u4f53\u4f20\u8f93\u7684\u793a\u610f\u56fe\u3002<\/p>\n\n\n\n<p><a><\/a>\u7406\u8bba\u8ba1\u7b97\u8fdb\u4e00\u6b65\u89e3\u6790\u4e86TMA\u529f\u80fd\u5316\u754c\u9762\u4e0a\u7684\u4e2d\u95f4\u4f53\u8fc1\u79fb\u4e0e\u80fd\u91cf\u53d8\u5316\u3002\u5728IRR\u4e2d\uff0cI<sup>*<\/sup>\u5438\u9644\u81ea\u7531\u80fd\u7531CoNi<sub>DA<\/sub>-MXene\u7684-2.48 eV\u8c03\u6574\u4e3aTMA-CoNi<sub>DA<\/sub>-MXene\u7684-2.27 eV\uff0c\u8868\u660e\u4fee\u9970\u540e\u8fc7\u5f3a\u7684I<sup>*<\/sup>\u7ed3\u5408\u5f97\u5230\u7f13\u548c\uff0c\u6709\u5229\u4e8e\u540e\u7eed\u8f6c\u5316\u53ca\u8131\u9644\u3002\u5728HER\u4e2d\uff0cTMA\u529f\u80fd\u5316\u754c\u9762\u6709\u52a9\u4e8e\u7ef4\u6301\u6c34\u5206\u5b50\u5438\u9644\u53ca\u89e3\u79bb\u4e2d\u95f4\u4f53\u7684\u7a33\u5b9a\uff08\u56fe6\uff09\u3002<\/p>\n\n\n\n<figure class=\"wp-block-image size-full\"><img loading=\"lazy\" decoding=\"async\" width=\"700\" height=\"391\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2026\/11\/e2f457ec632c1f6.png\" alt=\"\" class=\"wp-image-273451\"\/><\/figure>\n\n\n\n<p>\u56fe6. a) \u975e\u8d28\u5b50\u578b\u7898\u548cb) \u8d28\u5b50\u578b\u6c22\u4e2d\u95f4\u4f53\u5728TMA-CoNi<sub>DA<\/sub>-MXene\u4e0a\u7684\u8fc1\u79fb\u8def\u5f84\u3002CoNi<sub>DA<\/sub>-MXene\u4e0eTMA-CoNi<sub>DA<\/sub>-MXene\u7684c) IRR\u81ea\u7531\u80fd\u53cad) HER\u81ea\u7531\u80fd\u3002<\/p>\n\n\n\n<p><a><\/a>\u603b\u4e4b\uff0c\u672c\u7814\u7a76\u63d0\u51fa\u4e86\u4e00\u79cd\u6709\u673a\u914d\u4f53\u529f\u80fd\u5316Co\/Ni\u53cc\u539f\u5b50\u50ac\u5316\u754c\u9762\u7684\u65b0\u7b56\u7565\uff0c\u5c06\u4f20\u7edf\u6d3b\u6027\u4f4d\u70b9\u8c03\u63a7\u62d3\u5c55\u81f3\u53cd\u5e94\u4e2d\u95f4\u4f53\u7684\u6301\u7eed\u4f20\u8f93\u4e0e\u5c40\u90e8\u6d53\u5ea6\u7ba1\u7406\u3002\u901a\u8fc7\u5728MXene\u4e0a\u6784\u7b51\u7a33\u5b9a\u7684CoN<sub>2<\/sub>-C-N<sub>2<\/sub>Ni\u53cc\u539f\u5b50\u4e2d\u5fc3\uff0c\u5f15\u5165\u517c\u5177\u82b3\u9999\u03c0\u5171\u8f6d\u9aa8\u67b6\u4e0e-COOH\/-COO<sup>&#8211;<\/sup>\u5b98\u80fd\u56e2\u7684TMA\uff0c\u5b9e\u73b0\u4e86\u5c42\u95f4\u7ed3\u6784\u5f00\u653e\u3001\u6d3b\u6027\u4f4d\u70b9\u5229\u7528\u7387\u6539\u5584\u4e0e\u754c\u9762\u4e2d\u95f4\u4f53\u4f20\u8f93\u8c03\u63a7\u7684\u534f\u540c\u3002\u5728IRR\u4e2d\uff0c\u82b3\u9999\u03c0\u5171\u8f6d\u9aa8\u67b6\u4e0e\u6781\u6027\u7fa7\u57fa\u5171\u540c\u8c03\u8282\u975e\u8d28\u5b50\u578bI<sup>*<\/sup>\u7684\u5c40\u90e8\u5206\u5e03\u3001\u4fc3\u8fdb\u5176\u5411\u53cc\u539f\u5b50\u4f4d\u70b9\u8fc1\u79fb\uff1b\u5728\u78b1\u6027HER\u4e2d\uff0c\u7fa7\u57fa\u7684\u53ef\u9006\u8d28\u5b50\u5316\/\u53bb\u8d28\u5b50\u5316\u8fc7\u7a0b\u4e0e\u6709\u5e8f\u6c22\u952e\u7f51\u7edc\u5171\u540c\u4fc3\u8fdb\u975e\u8d28\u5b50\u578bH<sup>*<\/sup>\u7684\u8fde\u7eed\u8f6c\u79fb\uff0c<a><\/a>\u4ece\u800c\u5b9e\u73b0\u540c\u4e00\u754c\u9762\u5bf9\u8d28\u5b50\u578bH\u4e0e\u975e\u8d28\u5b50\u578bI\u4e24\u7c7b\u4e2d\u95f4\u4f53\u4f20\u8f93\u8fc7\u7a0b\u7684\u540c\u6b65\u8c03\u63a7\u3002\u8be5\u5de5\u4f5c\u4e3a\u9762\u5411\u4e0d\u540c\u53cd\u5e94\u4e2d\u95f4\u4f53\u8bbe\u8ba1\u6709\u673a\u2013\u65e0\u673a\u534f\u540c\u754c\u9762\u4ee5\u53ca\u6784\u7b51\u9ad8\u6027\u80fd\u53cc\u539f\u5b50\u50ac\u5316\u5242\u63d0\u4f9b\u4e86\u65b0\u7684\u7814\u7a76\u601d\u8def\u3002<\/p>\n\n\n\n<p><strong>\u3010\u6587\u7ae0\u94fe\u63a5\u3011<\/strong><strong><\/strong><\/p>\n\n\n\n<p><strong>Organic Ligand-Functionalized CoN<\/strong><strong><sub><strong><sub>2<\/sub><\/strong><\/sub><\/strong><strong>-C-N<\/strong><strong><sub><strong><sub>2<\/sub><\/strong><\/sub><\/strong><strong>Ni Dual-Atom for Tailored Proton and Non-Proton Transfer in Hydrogen Evolution and Triiodide Reduction<\/strong><\/p>\n\n\n\n<p>Rou Feng, Menglong Sun, Zechang Liu, Tianxiang Yang, Jiaoe Dang, Zhiguo Wang, Haijiang Yang, Weidong Tian, Sining Yun*<\/p>\n\n\n\n<p>Advanced Functional Materials<\/p>\n\n\n\n<p><a href=\"https:\/\/doi.org\/10.1002\/adfm.79186\">https:\/\/doi.org\/10.1002\/adfm.79186<\/a><\/p>\n\n\n\n<p><a href=\"https:\/\/advanced.onlinelibrary.wiley.com\/doi\/10.1002\/adfm.79186\">https:\/\/advanced.onlinelibrary.wiley.com\/doi\/10.1002\/adfm.79186<\/a><\/p>\n\n\n\n<p><strong>\u3010\u901a\u8baf\u4f5c\u8005\u7b80\u4ecb\u3011<\/strong><strong><\/strong><\/p>\n\n\n\n<p>\u4e91\u65af\u5b81\uff0c\u897f\u5b89\u5efa\u7b51\u79d1\u6280\u5927\u5b66\uff0c\u4e8c\u7ea7\u6559\u6388\uff0c\u535a\u58eb\u751f\u5bfc\u5e08\uff0c\u9655\u897f\u7701\u4e2d\u9752\u5e74\u79d1\u6280\u521b\u65b0\u9886\u519b\u4eba\u624d\uff0c\u9655\u897f\u7701\u201c\u7279\u652f\u8ba1\u5212\u201d\u79d1\u6280\u521b\u65b0\u9886\u519b\u4eba\u624d\uff0c\u9655\u897f\u7701\u91cd\u70b9\u79d1\u6280\u521b\u65b0\u56e2\u961f\u5e26\u5934\u4eba\uff0c\u9655\u897f\u7701\u9ad8\u7b49\u5b66\u6821\u5b66\u79d1\u521b\u65b0\u57fa\u5730\u8d1f\u8d23\u4eba\u3002\u8fde\u7eed8\u5e74\u5165\u9009\u201c\u5168\u7403\u524d2%\u9876\u5c16\u79d1\u5b66\u5bb6\u699c\u5355\uff08World&#8217;s Top 2% Scientists\uff09\u201d\uff0c\u5165\u9009\u201c\u7ec8\u8eab\u79d1\u5b66\u5f71\u54cd\u529b\u6392\u884c\u699c\u201d\u548c\u201c\u79d1\u5b66\u5f71\u54cd\u529b\u6392\u884c\u699c\u201d\u3002\u535a\u58eb\u6bd5\u4e1a\u4e8e\u897f\u5b89\u4ea4\u901a\u5927\u5b66\uff0c\u6b64\u540e\u5206\u522b\u5728\u97e9\u56fd\u5ef6\u4e16\u5927\u5b66\u3001\u7f8e\u56fd\u65af\u5766\u798f\u5927\u5b66\u3001\u7f8e\u56fd\u52a0\u5dde\u5927\u5b66\u3001\u7f8e\u56fd\u52b3\u4f26\u65af\u4f2f\u514b\u5229\u56fd\u5bb6\u5b9e\u9a8c\u5ba4\u3001\u82f1\u56fd\u91cc\u4e01\u5927\u5b66\u3001\u745e\u58eb\u6d1b\u6851\u8054\u90a6\u7406\u5de5\u5b66\u9662\u7b49\u8bbf\u95ee\u3001\u4ea4\u6d41\u4e0e\u5b66\u4e60\u3002\u76ee\u524d\u4e3b\u8981\u4ece\u4e8b\u65b0\u80fd\u6e90\u6750\u6599\u9ad8\u6548\u548c\u8d44\u6e90\u5316\u5229\u7528\u7814\u7a76\uff0c\u5982\u65b0\u4e00\u4ee3\u592a\u9633\u7535\u6c60\u3001\u71c3\u6599\u7535\u6c60\u3001\u8d85\u7ea7\u7535\u5bb9\u5668\u3001\u751f\u7269\u50ac\u5316\u3001\u5236\u6c22\u3001\u591a\u80fd\u4e92\u8865\u7b49\u3002\u4e3b\u6301\u79d1\u6280\u90e8\u91cd\u70b9\u7814\u53d1\u8ba1\u5212\uff08\u6c22\u80fd\u4e13\u9879\uff09\u3001\u79d1\u6280\u90e8\u5341\u4e8c\u4e94\u79d1\u6280\u652f\u6491\u8ba1\u5212\u3001\u4eba\u793e\u90e8\u91cd\u70b9\u3001\u57fa\u91d1\u59d4NSFC\u9762\u4e0a\u3001\u9655\u897f\u7701\u91cd\u70b9\u7814\u53d1\u8ba1\u5212\u3001\u9655\u897f\u7701\u56fd\u9645\u5408\u4f5c\u91cd\u70b9\u7b4920\u4f59\u9879\u79d1\u7814\u8bfe\u9898\u3002\u5728Chem Sov Rev, Prog Polym Sci, Energy Environ Sci, Electrochem Energy Rev, Adv Mater, Adv Energy Mater, Adv Funct Mater, Adv Powder Mater, ACS Energy Lett, Appl Catal B-Environ, Nano Energy, Angew Chem Int Edit, Renew Sust Energy Rev, J Mater Chem A, Chem Eng J, Small, Materials Today\u7cfb\u5217\u7b49\u56fd\u9645\u671f\u520a\u53d1\u8868\u8bba\u6587270\u4f59\u7bc7\uff08IF&gt;10\u7684\u8bba\u6587100\u4f59\u7bc7\uff09\uff0cH-\u56e0\u5b5071\uff0c\u5148\u540e\u670927\u7bc7\u8bba\u6587\u5165\u9009ESI\u70ed\u70b9\/\u9ad8\u88ab\u5f15\u8bba\u6587\uff1b\u4e3b\u7f16\/\u53c2\u7f16\u4e2d\u3001\u82f1\u6587\u4e13\u8457\/\u6559\u675013\u90e8\uff1b\u62e5\u670930\u9879\u56fd\u5bb6\u6388\u6743\u4e13\u5229\u6280\u672f\u30022016\u5e74\u83b7\u201cWiley\u6750\u6599\u5b66\u9ad8\u5cf0\u8bba\u575b-\u897f\u5b89\u201dHighly-cited Author Award\u30022017\u5e74\u83b7\u4e2d\u56fd\u56fd\u9645\u5149\u4f0f\u5927\u4f1aBest Presentation Award\u5956\u30022017-2023\u5e74\uff0c\u5148\u540e\u83b7\u9655\u897f\u7701\u79d1\u5b66\u6280\u672f\u8fdb\u6b65\u5956\u4e00\u7b49\u5956\u3001\u9655\u897f\u7701\u79d1\u5b66\u6280\u672f\u5956\u4e8c\u7b49\u5956\u3001\u9655\u897f\u9ad8\u7b49\u5b66\u6821\u79d1\u5b66\u6280\u672f\u7814\u7a76\u4f18\u79c0\u6210\u679c\u5956\u7279\u7b49\u5956\u3001\u9655\u897f\u9ad8\u7b49\u5b66\u6821\u79d1\u5b66\u6280\u672f\u5956\u4e00\u7b49\u5956\u3001\u5185\u8499\u53e4\u81ea\u6cbb\u533a\u79d1\u6280\u8fdb\u6b65\u4e8c\u7b49\u5956\u7b49\u3002\u5148\u540e\u62c5\u4efb\u56fd\u9645\u671f\u520aInternational Journal of Hydrogen Energy\u548cRenewable &amp; Sustainable Energy Reviews\u5ba2\u5ea7\u7f16\u8f91\uff08Guest Editor\u56fd\u9645\u671f\u520a\uff09\u3002\u76ee\u524d\u62c5\u4efbInternational Journal of Green Energy, Oxford Open Energy\u7b49\u7f16\u59d4\uff1b\u62c5\u4efbESCI\u56fd\u9645\u671f\u520aEnergy Materials\uff08\u5f71\u54cd\u56e0\u5b5011.8\uff09\u526f\u4e3b\u7f16\uff1b170\u4f59\u79cd\u4e3b\u8981\u56fd\u9645SCI\u5b66\u672f\u671f\u520a\u7684\u7279\u9080\u5ba1\u7a3f\u548c\u4ef2\u88c1\u4e13\u5bb6\u3002<\/p>\n\n\n\n<p>\u66f4\u591a\u8be6\u60c5\uff0c\u8bf7\u8bbf\u95ee\u5bfc\u5e08\u4e3b\u9875\u548c\u8bfe\u9898\u7ec4\u4e3b\u9875<\/p>\n\n\n\n<p><a href=\"https:\/\/xajzkj.teacher.360eol.com\/teacherBasic\/preview?teacherId=21532\">https:\/\/xajzkj.teacher.360eol.com\/teacherBasic\/preview?teacherId=21532<\/a><\/p>\n\n\n\n<p><a href=\"https:\/\/www.x-mol.com\/groups\/Sining_Yun\">https:\/\/www.x-mol.com\/groups\/Sining_Yun<\/a><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u6587\u7ae0\u4fe1\u606f\u3011 \u6709\u673a\u914d\u4f53\u529f\u80fd\u5316 CoN2-C-N2Ni \u53cc\u539f\u5b50\u5b9a\u5411\u8c03\u63a7\u6790\u6c22\u4e0e\u7898\u8fd8\u539f\u4e2d\u7684\u8d28\u5b50\u548c\u975e\u8d28\u5b50\u8f6c\u79fb \u7b2c\u4e00\u4f5c\u8005\uff1a\u51af\u67d4\u3001\u5b59\u68a6\u9f99 \u901a\u8baf\u4f5c\u8005\uff1a\u4e91\u65af\u5b81* \u4f5c\u8005\u5355\u4f4d\uff1a\u897f\u5b89&#8230;<\/p>\n","protected":false},"author":31345,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[2],"tags":[],"class_list":["post-273443","post","type-post","status-publish","format-standard","hentry","category-keji"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/273443"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/31345"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=273443"}],"version-history":[{"count":1,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/273443\/revisions"}],"predecessor-version":[{"id":273452,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/273443\/revisions\/273452"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=273443"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=273443"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=273443"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}