{"id":31411,"date":"2016-08-05T14:01:36","date_gmt":"2016-08-05T06:01:36","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=31411"},"modified":"2016-08-05T15:41:48","modified_gmt":"2016-08-05T07:41:48","slug":"%e9%a1%b6%e5%88%8a%e5%8a%a8%e6%80%81-prlprb%e8%ae%a1%e7%ae%97%e6%9d%90%e6%96%99%e5%ad%a6%e6%9c%af%e8%bf%9b%e5%b1%95%e6%b1%87%e6%80%bb%e3%80%90%e7%ac%ac8%e6%9c%9f%e3%80%91","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=31411","title":{"rendered":"\u9876\u520a\u52a8\u6001 | PRL\/PRB\u8ba1\u7b97\u6750\u6599\u5b66\u672f\u8fdb\u5c55\u6c47\u603b\u3010\u7b2c8\u671f\u3011"},"content":{"rendered":"<p><strong>1\u3001PRB\uff1a\u78f7\u70ef\u7eb3\u7c73\u5e26\u7684\u6fc0\u5b50\u8c31\u548c\u5149\u8c31<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-31422\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/1-7.jpg\" alt=\"1\" width=\"500\" height=\"287\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/1-7.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/1-7-300x172.jpg 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p style=\"text-align: center;\"><strong>\u56fe2 4-zPNR\u5bf9\u6cbfzz\u65b9\u5411\u504f\u632f\u5149\u7684\u5149\u5438\u6536<\/strong><\/p>\n<p>\u81ea\u4ece\u78f7\u70ef\u8bde\u751f\u4ee5\u6765\uff0c\u7279\u522b\u662f2014\u5e74\u6210\u529f\u5229\u7528\u9ed1\u78f7\u5265\u79bb\u5f97\u5230\u78f7\u70ef\u4e4b\u540e\uff0c\u5148\u8fdb\u4e8c\u7ef4\uff082D\uff09\u6676\u4f53\u6750\u6599\u4e2d\u7684\u8fd9\u4e00\u6210\u5458\u4ee5\u5176\u72ec\u7279\u7684\u6027\u80fd\u5438\u5f15\u4e86\u5f88\u591a\u7684\u5173\u6ce8\u3002\u78f7\u70ef\u6709\u223c1.4 eV\u7684\u76f4\u63a5\u5e26\u9699\u3001\u9ad8\u8f7d\u6d41\u5b50\u8fc1\u79fb\u7387\u4ee5\u53ca\u7528\u4e8e\u573a\u6548\u5e94\u6676\u4f53\u7ba1\u7684\u9ad8\u5f00\u5173\u6bd4\u3002\u4e8b\u5b9e\u4e0a\uff0c\u78f7\u70ef\u6210\u4e3a\u4e00\u4e2a\u7279\u6b8a2D\u7cfb\u7edf\u7684\u539f\u56e0\u662f\u5176\u5177\u6709\u9ad8\u5ea6\u7684\u5404\u5411\u5f02\u6027\u3002<\/p>\n<p>\u4f0a\u6717\u57fa\u7840\u79d1\u5b66\u7814\u7a76\u6240\uff08IPM\uff09\u7684Reza Asgari\uff08\u901a\u8baf\u4f5c\u8005\uff09\u548cZahra Nourbakhsh\uff08\u901a\u8baf\u4f5c\u8005\uff09\u5728\u591a\u4f53\u4ece\u5934\u7b97\u8ba1\u7b97\u7684\u57fa\u7840\u4e0a\uff0c\u5229\u7528\u5355\u8109\u51b2G0W0\u65b9\u6cd5\u548cBethe Salpeter\u65b9\u7a0b\uff0c\u5bf9\u78f7\u70ef\u7eb3\u7c73\u5e26\uff08PNRs\uff09\u7684\u952f\u9f7f\u578b\u548c\u6276\u624b\u6905\u578b\u8fd9\u4e24\u4e2a\u5178\u578b\u65b9\u5411\u8fdb\u884c\u4e86\u7814\u7a76\u3002\u7814\u7a76\u5c0f\u7ec4\u8ba1\u7b97\u4e86\u4e0d\u540c\u5c3a\u5bf8\u7684PNRs\u7684\u7535\u5b50\u7ed3\u6784\u3001\u5149\u5438\u6536\u3001\u7535\u5b50\u7a7a\u7a74\uff08\u6fc0\u5b50\uff09\u7ed3\u5408\u80fd\u3001\u6fc0\u5b50\u4ea4\u6362\u5288\u88c2\u4ee5\u53ca\u6fc0\u5b50\u6ce2\u51fd\u6570\u3002\u5355\u91cd\u6001\u6fc0\u5b50\u548c\u4e09\u91cd\u6001\u6fc0\u5b50\u4e4b\u95f4\u5178\u578b\u7684\u5f3a\u5288\u88c2\u4f7f\u5f97PNRs\u6709\u671b\u7528\u4e8e\u5149\u7535\u5668\u4ef6\u4e2d\u3002\u91cf\u5b50\u9650\u57df\u5728\u4e24\u79cdPNRs\u4e2d\u90fd\u5b58\u5728\uff0c\u5176\u4e2d\u5728zPNRs\u7cfb\u7edf\u66f4\u52a0\u5f3a\u70c8\uff0c\u5176\u884c\u4e3a\u7c7b\u4f3c\u4e8e\u51c6\u96f6\u7ef4\u7cfb\u7edf\u3002\u7814\u7a76\u8868\u660e\u591a\u4f53\u76f8\u4e92\u4f5c\u7528\u5bf9PNR\u7684\u5149\u5438\u6536\u5149\u8c31\u6709\u7740\u91cd\u8981\u5f71\u54cd\uff0c\u800c\u4e14\u662f\u4e0d\u80fd\u5ffd\u89c6\u7684\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"http:\/\/journals.aps.org\/prb\/abstract\/10.1103\/PhysRevB.94.035437\" target=\"_blank\">Excitons and optical spectra of phosphorene nanoribbons <\/a>\uff08Phys. Rev. B\uff0c2016\uff0cDOI: 10.1103\/PhysRevB.94.035437\uff09<\/p>\n<p><strong>2\u3001PRB\uff1a\u77f3\u58a8\u70ef\u4e0a\u7684\u952f\u9f7f\u5f62\u77f3\u58a8\u7eb3\u7c73\u5e26\u7684\u534a\u91d1\u5c5e\u72c4\u62c9\u514b\u9525<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-31423\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/2-7.jpg\" alt=\"2\" width=\"600\" height=\"319\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/2-7.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/2-7-300x160.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p style=\"text-align: center;\"><strong>\u56fe2 K\u70b9\u9644\u8fd1\u7684\u7535\u5b50\u80fd\u5e26\u7ed3\u6784<\/strong><\/p>\n<p>\u77f3\u58a8\u70ef\u7684\u53d1\u73b0\u6fc0\u53d1\u4e86\u57fa\u4e8e\u77f3\u58a8\u70ef\u7684\u7eb3\u7c73\u7ed3\u6784\u548c\u5b83\u4eec\u7684\u884d\u751f\u7269\u6d53\u539a\u7684\u7684\u7814\u7a76\u5174\u8da3\uff0c\u5982\u8303\u5fb7\u534e\u529b\uff08vdW\uff09\u5f02\u8d28\u7ed3\u6784\u3002\u77f3\u58a8\u70ef\u4e2d\u7684\u4e00\u4e2a\u6709\u8da3\u7684\u7279\u70b9\u662f\u771f\u5b9e\u81ea\u65cb\u548c\u8d5d\u81ea\u65cb\u7684\u7ed3\u5408\uff0c\u8fd9\u4f7f\u5f97\u5728\u8fd9\u4e00\u72ec\u7279\u7684\u4e24\u7ef4\u7cfb\u7edf\u4e2d\u4ea7\u751f\u4e86\u4e30\u5bcc\u7269\u7406\u73b0\u8c61\uff0c\u4f8b\u5982\u53cd\u5e38\u91cf\u5b50\u970d\u5c14\u6548\u5e94\u3002<\/p>\n<p>\u9274\u4e8e\u72ec\u7acb\u7684\u952f\u9f7f\u578b\u77f3\u58a8\u70ef\u7eb3\u7c73\u5e26\u662f\u53cd\u94c1\u78c1\u534a\u5bfc\u4f53\uff0c\u7f8e\u56fd\u5a01\u65af\u5eb7\u8f9b\u5927\u5b66\u7684M. X. Chen\uff08\u901a\u8baf\u4f5c\u8005\uff09\u7b49\u4eba\u901a\u8fc7\u7b2c\u4e00\u6027\u539f\u7406\u4e0e\u7d27\u675f\u7f1a\u8ba1\u7b97\u5f97\u5230\uff0c\u5728\u77f3\u58a8\u70ef\u4e0a\u7684\u952f\u9f7f\u578b\u77f3\u58a8\u70ef\u7eb3\u7c73\u5e26\u7531\u4e8e\u81ea\u65cb\u548c\u8d5d\u81ea\u65cb\u5bf9\u79f0\u6027\u7834\u7f3a\u5bfc\u81f4\u5176\u4e3a\u534a\u91d1\u5c5e\u3002\u7279\u522b\u5730\uff0c\u534a\u91d1\u5c5e\u72c4\u62c9\u514b\u9525\u4f53\u662f\u5728\u8d39\u7c73\u80fd\u7ea7\u9644\u8fd1\u7684K\uff08K&#8217;\uff09\u70b9\u4e0a\u5f62\u6210\u7684\u3002\u76ee\u524d\u7684\u7ed3\u679c\u8868\u660e\uff0c\u5728\u952f\u9f7f\u578b\u77f3\u58a8\u7eb3\u7c73\u5e26\u4e2d\u72ec\u7279\u7684\u81ea\u65cb\u548c\u8d5d\u81ea\u65cb\u7684\u7ed3\u5408\u53ef\u4ee5\u88ab\u7528\u4e8e\u64cd\u7eb5\u77f3\u58a8\u70ef\u7684\u7535\u5b50\u7279\u6027\uff0c\u5e76\u4e14\u53ef\u80fd\u5bf9\u6709\u6f5c\u529b\u7684\u77f3\u58a8\u70ef\u7eb3\u7c73\u7535\u5b50\u5668\u4ef6\u4ea7\u751f\u5b9e\u9645\u5f71\u54cd\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5:\u00a0<a href=\"http:\/\/journals.aps.org\/prb\/abstract\/10.1103\/PhysRevB.94.035433\" target=\"_blank\">Half-metallic Dirac cone in zigzag graphene nanoribbons on graphene<\/a> \uff08Phys. Rev. B\uff0c2016\uff0cDOI: 10.1103\/PhysRevB.94.035433\uff09<\/p>\n<p><strong>3\u3001PRB\uff1a\u5939\u5c42\u77f3\u58a8\u70ef\u4e2d\u7684\u975e\u5e38\u89c4\u91cf\u5316\u8fb9\u7f18\u8fd0\u8f93<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-31424\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/3-8.jpg\" alt=\"3\" width=\"500\" height=\"277\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/3-8.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/3-8-300x166.jpg 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p style=\"text-align: center;\"><strong>\u56fe3 G\/i-Ta\/SiC\u7684\u4fef\u89c6\u56fe\u4e0e\u4fa7\u89c6\u56fe<\/strong><\/p>\n<p>\u4eba\u4eec\u666e\u904d\u8ba4\u4e3a\uff0c\u8fb9\u7f18\u8026\u5408\u7834\u574f\u4e86\u91cf\u5b50\u81ea\u65cb\u970d\u5c14\u6548\u5e94\uff08QSH\uff09\uff0c\u8fd8\u4f7f\u72c4\u62c9\u514b\u70b9\u51fa\u73b0\u7f3a\u53e3\u3002<\/p>\n<p>\u5229\u7528\u7b2c\u4e00\u6027\u539f\u7406\u8ba1\u7b97\uff0c\u56fd\u5bb6\u7eb3\u7c73\u79d1\u5b66\u4e2d\u5fc3\u674e\u5143\u660c\uff08\u901a\u8baf\u4f5c\u8005\uff09\u7814\u7a76\u53d1\u73b0\uff1aTa\u63d2\u5c42\u5916\u5ef6\u77f3\u58a8\u70efSiC\u662f\u5229\u7528\u7b2c\u4e00\u6027\u539f\u7406\u8ba1\u7b97\u7684\u7cfb\u7edf\uff0c\u91cf\u5316\u8fb9\u7f18\u8f93\u8fd0\u575a\u6301Ta\u5d4c\u5165\u5916\u5ef6\u77f3\u58a8\u70ef\u7684SiC\uff080001\uff09\u4e0a\u5b58\u5728\u8fb9\u7f18\u8026\u5408\uff0c\u5b83\u662f\u4e00\u4e2a81 meV\u5de8\u5927\u7535\u52bf\u5dee\u7684QSH\u7edd\u7f18\u4f53\u3002\u5728\u8fd9\u79cd\u60c5\u51b5\u4e0b\uff0c\u5b83\u4eec\u7531\u7279\u6709\u7684\u5177\u6709\u4e0d\u540c\u7684\u8d39\u7c73\u901f\u5ea6\u7684\u72c4\u62c9\u514b\u9525\u6784\u6210\uff0c\u4f46\u53ea\u6709\u4e00\u4e2a\u4fdd\u6301\u8fb9\u7f18\u72b6\u6001\u7684\u529f\u80fd\u3002\u6211\u4eec\u628a\u8fd9\u6837\u7684\u8f68\u9053\u4f9d\u8d56\u6027\u51cf\u5f31\u7684\u53cd\u5e38\u8fb9\u7f18\u72b6\u6001\u5f52\u56e0\u4e8e\u4f53\u79ef\uff0c\u4f53\u79ef\u7684\u9650\u5236\u4f7f\u5f97\u8fb9\u7f18\u8026\u5408\u53ea\u80fd\u5141\u8bb8\u4e00\u7ec4\u8fb9\u7f18\u72b6\u6001\uff0c\u800c\u4e0d\u662f\u4e24\u4e2a\u3002\u6587\u7ae0\u4e2d\u4e0e\u5e38\u89c4\u7814\u7a76\u7684QSH\u7684\u5173\u952e\u533a\u522b\u5728\u4e8eG\/i-Ta\/SiC\u4e2d\u663e\u8457\u7684\u62c9\u4ec0\u5df4\u5206\u88c2\uff0c\u5bfc\u81f4\u8fb9\u7f18\u6001\u660e\u663e\u8870\u9000\u3002\u7edd\u7f18\u5b50\u662fG \/ I-TA \/\u78b3\u5316\u7845\u7684\u663e\u8457\u62c9\u4ec0\u5df4\u5206\u88c2\uff0c\u8fd9\u5bfc\u81f4\u8fb9\u7f18\u72b6\u6001\u7684\u4e0d\u540c\u8870\u51cf\u957f\u5ea6\u6210\u6279\u91cf\u3002\u56e0\u6b64\uff0c\u968f\u7740G\/i-Ta\/SiC\u8272\u5e26\u5bbd\u5ea6\u51cf\u5c11\uff0c\u4f9d\u6b21\u51fa\u73b0\u4e09\u4e2a\u76f8\u6001\uff0c\u5373\uff081\uff09 QSH\u65f6\u95f4\u53cd\u6f14\u5bf9\u79f0\u6027\u4fdd\u62a4\u6001\uff082\uff09\u4e92\u52a8\u91cf\u5316\u8fb9\u7f18\u4f20\u8f93\u72b6\u6001\uff0c\uff083\uff09\u7410\u788e\u7edd\u7f18\u4f53\u72b6\u6001\u3002\u5728\u9636\u6bb5\uff082\uff09\u4e2d\uff0c\u540c\u65f6\u5b58\u5728\u4f53\u79ef\u548c\u8fb9\u7f18\u72c4\u62c9\u514b\u8d39\u7c73\u5b50\uff0c\u8fd9\u662f\u56e0\u4e3a\u8fb9\u7f18\u8026\u5408\u53ea\u6709\u4e00\u7ec4\u8fb9\u7f18\u6001\u3002\u8fd9\u4e9b\u7814\u7a76\u7ed3\u679c\u5bf9\u4e8e\u66f4\u52a0\u6df1\u523b\u7684\u7406\u89e3\u62d3\u6251\u76f8\u53d8\u548c\u62d3\u6251\u4fdd\u62a4\u91cf\u5316\u8fd0\u8f93\u6709\u7740\u5f88\u5927\u7684\u7406\u8bba\u610f\u4e49\u548c\u4ef7\u503c\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"http:\/\/journals.aps.org\/prb\/abstract\/10.1103\/PhysRevB.94.035147\" target=\"_blank\">Unconventional quantized edge transport in the presence of interedge coupling in intercalated graphene<\/a>\uff08Phys. Rev. B\uff0c2016\uff0cDOI: 10.1103\/PhysRevB.94.035147\uff09<\/p>\n<p><strong>4\u3001PRB\uff1aIV\u65cf\u5355\u786b\u65cf\u5316\u7269\u7684\u6781\u5316\u548c\u8c37\u503c\u5f00\u5173<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-31425\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/4-6.jpg\" alt=\"4\" width=\"500\" height=\"262\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/4-6.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/4-6-300x157.jpg 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p style=\"text-align: left;\"><strong>\u56fe4 \u00a0\u5747\u5300\u7535\u573a\u8fc7\u6e21\u70b9\u4e2d\u7684\u5355\u5c42SnS\u53ef\u89c6\u5316\u7ed3\u6784\uff08\u6ce8\uff1a\u8936\u76b1\u548c\u7535\u5076\u6781\u53d6\u5411\uff08\u7ea2\u8272\u7bad\u5934\uff09\u53ef\u4ee5\u4ece\u6b63x\uff08b\uff09\u81f3\u5207\u6362\u4efb\u8d1fx\uff08a\uff09\u6216\u6b63\u7684y\uff08C\uff09\uff0c\u8fd9\u53d6\u51b3\u4e8e\u6240\u5e94\u7528\u7684\u7535\u573a\u65b9\u5411\uff09<\/strong><\/p>\n<p>IV\u65cf\u5355\u786b\u5316\u7269\u662f\u4e8c\u7ef4\u76b1\u8936\u6750\u6599\u5bb6\u65cf\u4e2d\u7684\u4e00\u5458\uff0c\u5177\u6709\u7531\u6781\u6027\u5c42\u7684\u6784\u6210\u7684\u659c\u65b9\u6676\u7cfb\u7ed3\u6784\u3002\u901a\u8fc7\u7b2c\u4e00\u6027\u539f\u7406\u8ba1\u7b97\u663e\u793a\u5355\u5c42\u7684SnS\u548cGESE\u7684\u591a\u7a33\u6001\uff0c\u4e24\u539f\u6750\u6599\u8936\u76b1\u7684\u65b9\u5411\u53ef\u7531\u62c9\u4f38\u5e94\u529b\u6216\u65bd\u52a0\u7535\u573a\u6539\u53d8\u3002\u6b64\u5916\uff0c\u52bf\u573a\u4e2d\u4e24\u4e2a\u4e0d\u7b49\u7684\u4f4e\u8c37\u7531\u8936\u76b1\u7684\u65b9\u5411\u51b3\u5b9a\uff0c\u53ef\u4f7f\u7528\u76f4\u7ebf\u504f\u632f\u5149\u9009\u62e9\u6027\u6fc0\u53d1\uff0c\u8fd9\u4e3a\u786e\u5b9a\u504f\u632f\u65b9\u5411\u63d0\u4f9b\u4e86\u989d\u5916\u7684\u5de5\u5177<\/p>\n<p>\u6700\u8fd1\uff0c\u6ce2\u58eb\u987f\u5927\u5b66David K. Campbell\uff08\u901a\u8baf\u4f5c\u8005\uff09\u548c\u65b0\u52a0\u5761\u56fd\u7acb\u5927\u5b66Harold S. Park\uff08\u901a\u8baf\u4f5c\u8005\uff09\u7b49\u4eba\u5206\u6790IV\u65cf\u5355\u786b\u5316\u7269\u5355\u5c42\u7684\u7a33\u5b9a\u6027\uff0c\u5355\u786b\u65cf\u5316\u7269MX\uff08M = Ge\u3001Sn\uff0cX = S\u3001Se\uff09\uff0c\u4ee5SnS\u7684\u548cGeSe\u4f5c\u4e3a\u539f\u578b\u3002\u5728\u4e00\u5b9a\u73af\u5883\u6761\u4ef6\u4e0b\uff0cSnS\u548cGeSe\u7ed3\u6676\u4e3aPnma\u7a7a\u95f4\u7fa4\u659c\u65b9\u6676\u7cfb\u7ed3\u6784\u3002 \u6e29\u5ea6\u4e3a878 K\u65f6\uff0cSnS\u7684\u7ecf\u8fc7\u4e8c\u9636\u4f4d\u79fb\u76f8\u8fc7\u6e21\u5230\u03b2-SnS\u76f8\uff0c\u5bf9\u79f0\u6027\u53d8\u4e3aCmcm\u3002\u5bf9\u4e8eGeSe\uff0c\u5e76\u672a\u53d1\u73b0\u8fd9\u6837\u7684\u76f8\u53d8\u8fc7\u7a0b\u3002\u76f8\u53cd\uff0c\u5728924K\uff0cGeSe\u8f6c\u53d8\u6210\u5728\u5ca9\u76d0\u76f8\uff08\u7a7a\u95f4\u7fa4Fm3m\uff09\u3002\u6b64\u9636\u6bb5\u4e5f\u901a\u8fc7\u5916\u529b\u4f7f\u4e4b\u7a33\u5b9a\u3002\u7814\u7a76\u7ed3\u679c\u8868\u660e\uff0cSnS\u7684\u548cGeSe\u5355\u5c42\u53ef\u80fd\u89c2\u5bdf\u5230\u7684\u94c1\u7535\u6027\u548c\u591a\u7a33\u5b9a\u6027\uff0c\u5728\u4fe1\u606f\u5b58\u50a8\u65b9\u9762\u6709\u6f5c\u5728\u5e94\u7528\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"http:\/\/journals.aps.org\/prb\/abstract\/10.1103\/PhysRevB.94.035304\" target=\"_blank\">Polarization and valley switching in monolayer group-IV monochalcogenides<\/a>\uff08Phys. Rev. B\uff0c2016\uff0cDOI: 10.1103\/PhysRevB.94.035304\uff09<\/p>\n<p><strong>5\u3001PRB\uff1a\u975e\u6676\u6c27\u5316\u7269\u4e2d\u6df1\u7535\u5b50\u7a7a\u7a74\u5bf9\u7684\u6781\u5316\u548c\u975e\u6781\u5316\u7814\u7a76<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-31426\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/5-5.jpg\" alt=\"5\" width=\"500\" height=\"600\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/5-5.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/5-5-250x300.jpg 250w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p style=\"text-align: center;\"><strong>\u56fe5 \u7531\u4e8e\u5c40\u57df\u5316\u548c\u989d\u5916\u7535\u5b50\u9020\u6210\u7684Hf\u548cO\u79bb\u5b50\u5178\u578b\u7684\u81ea\u65cb\u5bc6\u5ea6\u5206\u5e03\u548c\u4f4d\u79fb\uff08\u5355\u4f4d\u4e3a\u00c5\uff09<\/strong><\/p>\n<p>\u975e\u6676\u03b1-HfO2\u662f\u4e00\u79cd\u5e94\u7528\u5e7f\u6cdb\u7684\u9ad8\u4ecb\u7535\u5e38\u6570\u7edd\u7f18\u4f53\u7684\u539f\u578b\u3002<\/p>\n<p>\u8fd1\u65e5\uff0c\u65e5\u672c\u4e1c\u5317\u5927\u5b66\u7684Moloud Kaviani\uff08\u901a\u8baf\u4f5c\u8005\uff09\u3001\u82f1\u56fd\u4f26\u6566\u5927\u5b66\u7684Alexander Shluger\uff08\u901a\u8baf\u4f5c\u8005\uff09\u3001\u6bd4\u5229\u65f6\u9c81\u6c76\u5927\u5b66Valery V. Afanas&#8217;ev\uff08\u901a\u8baf\u4f5c\u8005\uff09\u4ee5\u53ca\u65e5\u672c\u4e1c\u5317\u5927\u5b66\u548c\u82f1\u56fd\u4f26\u6566\u5927\u5b66Alexander L. Shluger\uff08\u901a\u8baf\u4f5c\u8005\uff09\u4f7f\u7528\u4ece\u5934\u8ba1\u7b97\u6cd5\uff0c\u6210\u529f\u53d1\u73b0\u591a\u4f59\u7684\u7535\u5b50\u548c\u7a7a\u7a74\u80fd\u591f\u4ee5\u4e00\u79cd\u6bd4\u5355\u659c\u6676\u76f8\u66f4\u6df1\u7684\u80fd\u91cf\u6781\u5316\u6001\u9677\u5165\u03b1-HfO2\u4e2d\u3002\u7535\u5b50\u7a7a\u7a74\u5bf9\u5b9a\u4f4d\u4e8e\u524d\u8eaf\u4f53\uff0c\u6bd4\u5982\u7ec6\u957f\u7684Hf-O\u952e\u6216\u8005\u8c03\u8282\u540e\u7684Hf\u548cO\u539f\u5b50\uff0c\u540c\u65f6\uff0c\u6781\u5316\u5b50\u88ab\u65e0\u5b9a\u5f62\u5c40\u57df\u7f51\u7edc\u653e\u5927\u3002\u5355\u7535\u5b50\u6781\u5316\u4f7f\u5f97\u7981\u5e26\u5bbd\u5ea6\u7ea6\u4e3a2ev\uff0c\u4f4e\u4e8e\u5bfc\u5e26\u5e95\u7684\u5e73\u5747\u7684\u9677\u9631\u80fd1eV\u3002\u800c\u5728\u540c\u6837\u7684\u8bbe\u7f6e\u4e0b\uff0c\u53cc\u7535\u5b50\u53ef\u4ee5\u5f62\u6210\u751a\u81f3\u66f4\u6df1\u7684\u975e\u6781\u5316\u6001\u3002\u7a7a\u7a74\u53ef\u4ee5\u4f7f\u5f97O\u79bb\u5b50\u7684\u5e73\u5747\u9677\u9631\u80fd\u4e3a1.4eV\u3002\u8fd9\u4e9b\u5c31\u4f7f\u5f97\u7814\u7a76\u4eba\u5458\u901a\u8fc7\u8bc1\u5b9e\u6df1\u5ea6\u6781\u5316\u6001\u662f\u56fa\u6709\u7684\u540c\u65f6\u4e0d\u518d\u8981\u6c42\u4efb\u4f55\u952e\u7684\u65ad\u88c2\u6765\u5f62\u6210\u524d\u9a71\u4f53\u4f4d\uff0c\u5c31\u8fd9\u6837\u4ece\u800c\u7406\u89e3\u4e86\u975e\u6676\u6c27\u5316\u7269\u4e2d\u7684\u7535\u8377\u4fd8\u83b7\u673a\u5236\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"http:\/\/journals.aps.org\/prb\/abstract\/10.1103\/PhysRevB.94.020103\" target=\"_blank\">Deep electron and hole polarons and bipolarons in amorphous oxide<\/a> \uff08Phys. Rev. B\uff0c2016\uff0cDOI:10.1103\/PhysRevB.94.020103\uff09<\/p>\n<p><strong>6\u3001PRL\uff1a\u81ea\u7ec4\u7ec7\u751f\u957f\u3001\u7ed3\u6784\u548c\u5355\u539f\u5b50\u94fe\u7684\u78c1\u6027\u8fc7\u6e21\u91d1\u5c5e\u6c27\u5316\u7269<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-31427\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/6-6.jpg\" alt=\"6\" width=\"500\" height=\"500\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/6-6.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/6-6-150x150.jpg 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/6-6-300x300.jpg 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p><strong>\u56fe6 \u5177\u67093&#215;1\u5468\u671f\u6027\u7ed3\u6784\u7684CoO2\u5728\u94f1\uff08100\uff09\u6676\u9762\u4e0a\uff08a\uff09LEED\u5206\u6790\uff1b\uff08b\uff09\u5927\u5c3a\u5ea6\u4e0b\u5176STM\u56fe\uff1b\uff08c\uff09\u539f\u5b50\u7ea7STM\u56fe\uff0c\u5176\u4e2d\u7684\u63d2\u56fe\u662fDFT\u6cd5\u5206\u6790\u7ed3\u679c\uff1b\uff08d\uff09\u5927\u5c3a\u5ea6\u4e0b\u7684STM\u56fe<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c\u5fb7\u56fd\u57c3\u5c14\u6717\u6839-\u7ebd\u4f26\u5821\u5927\u5b66\u7684Pascal Ferstl\uff08\u901a\u8baf\u4f5c\u8005\uff09\u548c\u5965\u5730\u5229\u7ef4\u4e5f\u7eb3\u6280\u672f\u5927\u5b66\u7684Florian Mittendorfer\uff08\u901a\u8baf\u4f5c\u8005\uff09\u7b49\u4eba\u5408\u4f5c\uff0c\u5bf9\u5177\u67093&#215;1\u5468\u671f\u6027\u53d8\u5316\u7684\u5355\u539f\u5b50\u8fc7\u6e21\u91d1\u5c5e\u6c27\u5316\u7269\u94fe\u7684\u81ea\u7ec4\u7ec7\u751f\u957f\u673a\u5236\u4ee5\u53ca\u4e0d\u5bfb\u5e38\u7684MO2\u7c7b\uff08M\u8868\u793aNi\u3001Co\u3001Fe\u3001Mn\uff09\u91d1\u5c5e\u6c27\u5316\u7269\u8fdb\u884c\u4e86\u62a5\u9053\u3002\u4ed6\u4eec\u5229\u7528\u5b9a\u91cf\u4f4e\u80fd\u7535\u5b50\u884d\u5c04\uff08LEED\uff09\u3001\u626b\u63cf\u96a7\u9053\u663e\u5fae\u955c\uff08STM\uff09\u4ee5\u53ca\u5bc6\u5ea6\u6cdb\u51fd\u7406\u8bba\uff08DFT\uff09\u51e0\u79cd\u8ba1\u7b97\u5206\u6790\u65b9\u6cd5\u5206\u6790\u4e86\u8fd9\u4e9b\u6c27\u5316\u7269\u7684\u7ed3\u6784\u548c\u78c1\u5b66\u6027\u80fd\u3002LEED\u7684\u5206\u6790\u7ed3\u679c\u63ed\u793a\u4e00\u4e2a\u4ee4\u4eba\u7740\u8ff7\u7684\u539f\u5b50\u7ed3\u6784\uff0c\u5176\u4e2d\u7684\u8fc7\u6e21\u91d1\u5c5e\u539f\u5b50\u4f4d\u4e8e\u5931\u884c\u7ed3\u6784\u8868\u9762\u5e76\u4e14\u4ec5\u901a\u8fc7\u6c27\u539f\u5b50\u4e0e\u57fa\u5e95\u6210\u5bf9\u3002\u8fd9\u79cd\u7ed3\u6784\u8fdb\u4e00\u6b65\u5229\u7528\u504f\u5dee\u5c0f\u4e8e1.7 pm\u7684\u7ed3\u6784\u53c2\u6570DFT\u6cd5\u8fdb\u884c\u4e86\u786e\u8ba4\u3002\u5176\u4e2d\uff0cDFT\u6cd5\u9884\u6d4bNiO2\u94fe\u65e0\u78c1\u6027\uff0cCoO2\u94fe\u5177\u6709\u94c1\u78c1\u6027\uff0c\u800cFeO2\u548cMnO2\u5747\u4e3a\u53cd\u94c1\u78c1\u6027\u3002\u6240\u6709\u7684\u7ed3\u6784\u8868\u660e\u53ea\u6709\u5f31\u94c1\u78c1\u6027\u7684\u94fe\u95f4\u80fd\u591f\u6210\u5bf9\u3002\u8fdb\u4e00\u6b65\u6765\u8bf4\uff0c\u4ed6\u4eec\u8bc1\u5b9e\u4e86Co\u548cFe\u6216\u8005\u4e0eNi\u7684\u4e8c\u5143\u5408\u91d1\u6c27\u5316\u94fe\u5728\u94f1\u57fa\u5e95\uff08100\uff09\u6676\u9762\u65b9\u5411\u7684\u751f\u957f\uff0c\u8fd9\u4e00\u6210\u679c\u7684\u53d1\u73b0\uff0c\u53ef\u4ee5\u4f7f\u5f97\u4ed6\u4eec\u80fd\u591f\u751f\u4ea7\u51fa\u7531\u4e8e\u975e\u78c1\u6027\u6216\u8005\u53cd\u94c1\u78c1\u6027\u800c\u5177\u6709\u4e0d\u540c\u957f\u5ea6\u7684\u826f\u597d\u63a7\u5236\u6027\u7684\u94c1\u78c1\u6027\u94fe\u6574\u4f53\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"http:\/\/journals.aps.org\/prl\/abstract\/10.1103\/PhysRevLett.117.046101\" target=\"_blank\">Self-Organized Growth, Structure, and Magnetism of Monatomic Transition-Metal Oxide Chains <\/a>\uff08Phys. Rev. Lett. \uff0c2016 DOI: 10.1103\/PhysRevLett.117.046101\uff09<\/p>\n<p><strong>7\u3001PRB\uff1aScF3\u4e2d\u7684\u53cd\u5e38\u70ed\u5bfc\u7387\u4e0e\u8d1f\u70ed\u81a8\u80c0\u7684\u6291\u5236<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-31428\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/7-6.jpg\" alt=\"7\" width=\"500\" height=\"364\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/7-6.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/7-6-300x218.jpg 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p><strong>\u56fe7 \u5de6\u56fe\u4e3a\u572815\u00d715\u00d715\u7684\u6676\u683c\u4e2d\uff0c\u58f0\u5b50\u5bff\u547d\u7684\u80fd\u91cf\u51fd\u6570\uff1b\u53f3\u56fe\u4e3a\u63d2\u5165\u4e0e\u4e0d\u540c\u6e29\u5ea6\u76f8\u5bf9\u5e94\u7684\u7b2c\u4e00\u3001\u7b2c\u4e8c\u529b\u5e38\u6570\u8ba1\u7b97\u5f97\u5230\u7684\u70ed\u5bfc\u7387<\/strong><\/p>\n<p>\u5bf9\u4e8e\u83b7\u5f97\u5728\u7ed9\u5b9a\u6e29\u5ea6\u8303\u56f4\u5185\u65e0\u4f53\u79ef\u53d8\u5316\u7684\u6750\u6599\uff0c\u56fa\u4f53\u4e2d\u7531\u975e\u8c10\u6027\u5f15\u8d77\u7684\u8d1f\u70ed\u81a8\u80c0\u7cfb\u6570\uff08NTE\uff09\u662f\u81f3\u5173\u91cd\u8981\u7684\u3002\u56e0\u6b64\u901a\u8fc7\u4ece\u5934\u8ba1\u7b97\u6cd5\u627e\u5230\u5177\u6709\u8fd9\u79cd\u884c\u4e3a\u7684\u6750\u6599\u662f\u4e00\u4e2a\u91cd\u8981\u7684\u95ee\u9898\u3002\u6700\u8fd1\uff0cScF3\u7684\u53d1\u73b0\u5438\u5f15\u4e86\u4f17\u591a\u7684\u5173\u6ce8\uff0c\u8fd9\u79cd\u9499\u949b\u77ff\u7ed3\u6784\u6c1f\u5316\u7269\u7684NTE\u8fbe\u5230\u4e861100K\u3002\u4f46\u662f\u5230\u76ee\u524d\u4e3a\u6b62\uff0c\u8fd8\u5f88\u5c11\u6709\u5de5\u4f5c\u901a\u8fc7\u8ba1\u7b97\u6765\u7406\u89e3\u548c\u91cd\u73b0\u8fd9\u79cd\u8d1f\u70ed\u81a8\u80c0\u7684\u884c\u4e3a\u3002\u800c\u4e14\uff0c\u76ee\u524d\u4e5f\u6ca1\u6709\u6587\u732e\u62a5\u9053ScF3\u70ed\u5bfc\u7387\u7684\u8ba1\u7b97\u548c\u6d4b\u91cf\u65b9\u5f0f\u3002<\/p>\n<p>\u6cd5\u56fdCEA LITEN\u5b9e\u9a8c\u5ba4Ambroise van Roekeghem\uff08\u901a\u8baf\u4f5c\u8005\uff09\u7b49\u4eba\u901a\u8fc7\u4ece\u5934\u8ba1\u7b97\u6cd5\uff0c\u83b7\u5f97\u9499\u949b\u77ff\u578bScF3\u7684\u9ad8\u6548\u6e29\u5ea6\u58f0\u5b50\u8c31\uff0c\u6e05\u6670\u5730\u63cf\u8ff0\u4e86\u8fd9\u79cd\u5316\u5408\u7269\u4ee5\u53ca\u8d1f\u70ed\u81a8\u80c0\u6291\u5236\u7684\u884c\u4e3a\u3002\u57fa\u4e8e\u8fd9\u4e2a\u7ed3\u679c\uff0c\u9884\u6d4b\u4e86\u70ed\u5bfc\u7387\u53cd\u5e38\u7684\u6e29\u5ea6\u4f9d\u8d56\u6027\uff0c\u5e76\u5c06\u6b64\u4f5c\u4e3a\u9499\u949b\u77ff\u7c7b\u5316\u5408\u7269\u7684\u666e\u904d\u7279\u5f81\u3002\u6700\u540e\uff0c\u5c55\u793a\u4e86\u9ad8\u6e29\u4e0b\u8d1f\u70ed\u81a8\u80c0\u7684\u6291\u5236\u5728\u51c6\u8c10\u8fd1\u4f3c\u7684\u8303\u56f4\u4e4b\u5916\uff0c\u5e76\u4ece\u683c\u5f8b\u4e43\u68ee\uff08Gr\u00fcneisen\uff09\u53c2\u6570\u65b9\u9762\u8ba8\u8bba\u4e86\u8fd9\u4e2a\u73b0\u8c61\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"http:\/\/journals.aps.org\/prb\/abstract\/10.1103\/PhysRevB.94.020303\" target=\"_blank\">Anomalous thermal conductivity and suppression of negative thermal expansion in ScF3. <\/a>\uff08Phys. Rev. B\uff0c2016\uff0cDOI: 10.1103\/PhysRevB.94.020303\uff09<\/p>\n<p>\u672c\u671f\u6587\u732e\u6c47\u603b\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u8ba1\u7b97\u6750\u6599\u7ec4carbon\u3001\u5929\u884c\u5065\u3001\u674e\u4ea6\u56de\u548c\u5f90\u53cc\u7389\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u7f16\u8f91\u6574\u7406\u3002<\/p>\n<p><strong>\u6b22\u8fce\u8bd5\u7528\u6750\u6599\u4eba\u4ee3\u7406\u7684\u5929\u6cb32\u53f7\u8d85\u7ea7\u8ba1\u7b97\u673a<\/strong>\uff1b\u53c2\u4e0e\u8ba1\u7b97\u6750\u6599\u8bdd\u9898\u8ba8\u8bba\uff0c\u8bf7\u52a0\u5165\u6750\u6599\u4eba\u8ba1\u7b97\u6750\u6599\u7fa4\uff08562663183\uff09\uff1b\u53c2\u4e0e\u8ba1\u7b97\u6750\u6599\u6587\u732e\u89e3\u8bfb\u548c\u6587\u732e\u6c47\u603b\u53ca\u8ba1\u7b97\u6750\u6599\u77e5\u8bc6\u79d1\u666e\u7b49\uff0c\u8bf7\u52a0\u5165\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u8ba1\u7b97\u6750\u6599\u7ec4\uff08<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\">\u62a5\u540d\u8bf7\u6233\u6211<\/a>\uff09\u6216\u8005\u8054\u7cfb\uff1a\u7075\u5bf8\uff08418703364\uff09\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>1\u3001PRB\uff1a\u78f7\u70ef\u7eb3\u7c73\u5e26\u7684\u6fc0\u5b50\u8c31\u548c\u5149\u8c31 \u56fe2 4-zPNR\u5bf9\u6cbfzz\u65b9\u5411\u504f\u632f\u5149\u7684\u5149\u5438\u6536 \u81ea\u4ece\u78f7\u70ef\u8bde\u751f\u4ee5\u6765\uff0c\u7279\u522b\u662f2014\u5e74\u6210\u529f\u5229\u7528\u9ed1\u78f7\u5265\u79bb\u5f97\u5230\u78f7\u70ef\u4e4b\u540e\uff0c\u5148\u8fdb\u4e8c\u7ef4\uff082&#8230;<\/p>\n","protected":false},"author":372,"featured_media":31428,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[67],"tags":[97],"class_list":["post-31411","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-zhoubao","tag-computation"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/31411"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/372"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=31411"}],"version-history":[{"count":8,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/31411\/revisions"}],"predecessor-version":[{"id":31455,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/31411\/revisions\/31455"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/31428"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=31411"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=31411"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=31411"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}