{"id":44147,"date":"2016-10-04T06:30:45","date_gmt":"2016-10-03T22:30:45","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=44147"},"modified":"2017-03-18T21:25:50","modified_gmt":"2017-03-18T13:25:50","slug":"adv-funct-mater-%ef%bc%9a%e8%bf%98%e5%8e%9f%e5%9e%8b%e6%9f%93%e6%96%99%e7%9f%b3%e5%a2%a8%e7%83%af%e5%a4%8d%e5%90%88%e6%9d%90%e6%96%99%e5%8f%af%e7%94%a8%e4%bd%9c%e9%ab%98%e8%83%bd%e9%87%8f%e9%94%82","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=44147","title":{"rendered":"Adv. Funct. Mater. \uff1a\u8fd8\u539f\u578b\u67d3\u6599\/\u77f3\u58a8\u70ef\u590d\u5408\u6750\u6599\u53ef\u7528\u4f5c\u9ad8\u80fd\u91cf\u9502\u79bb\u5b50\u7535\u6c60\u7684\u6709\u673a\u6b63\u6781\u6750\u6599"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u50a8\u80fd\u662f\u5f53\u4eca21\u4e16\u7eaa\u6700\u91cd\u8981\u7684\u8bdd\u9898\u4e4b\u4e00\u3002\u81ea20\u4e16\u7eaa90\u5e74\u4ee3\u9502\u79bb\u5b50\u7535\u6c60\u8bde\u751f\u4ee5\u6765\uff0c\u5b83\u5df2\u7ecf\u5728\u4fbf\u643a\u5f0f\u7535\u5b50\u4ea7\u54c1\u9886\u57df\u5360\u636e\u4e86\u4e3b\u8981\u5e02\u573a\uff0c\u6210\u4e3a\u4e86\u6700\u6709\u6f5c\u529b\u7684\u50a8\u80fd\u65b9\u5f0f\u3002\u7136\u800c\uff0c\u9502\u79bb\u5b50\u7535\u6c60\u7684\u53d1\u5c55\u5e76\u4e0d\u80fd\u8ddf\u968f\u65f6\u4ee3\u7684\u811a\u6b65\u6ee1\u8db3\u65e5\u76ca\u589e\u957f\u7684\u80fd\u91cf\u9700\u6c42\uff0c\u5c24\u5176\u662f\u5bf9\u65b0\u5174\u7684\u7535\u52a8\u6c7d\u8f66\u548c\u667a\u80fd\u7535\u7f51\u7684\u53d1\u5c55\u3002\u8fdb\u4e00\u6b65\u63d0\u9ad8\u9502\u79bb\u5b50\u7535\u6c60\u80fd\u91cf\u5b58\u50a8\u80fd\u529b\u7684\u5173\u952e\u5728\u4e8e\u7535\u6781\u6750\u6599\u6bd4\u5bb9\u91cf\u7684\u63d0\u5347\u3002\u4e8b\u5b9e\u4e0a\uff0c\u4f20\u7edf\u65e0\u673a\u5d4c\u5c42\u6b63\u6781\u6750\u6599\u901a\u5e38\u53d1\u751f\u4e00\u7535\u5b50\u53cd\u5e94\uff0c\u4f7f\u5176\u5b9e\u9645\u5bb9\u91cf\u88ab\u9650\u5236\u5728200 mAhg<sup>-1<\/sup>\uff0c\u4f7f\u9502\u79bb\u5b50\u7535\u6c60\u6027\u80fd\u7684\u7814\u7a76\u8fdb\u5165\u4e86\u4e00\u4e2a\u74f6\u9888\u65f6\u671f\u3002<\/p>\n<p>\u6709\u673a\u7535\u6781\u6750\u6599\u7684\u7814\u7a76\u6709\u6548\u5730\u6539\u5584\u4e86\u8fd9\u4e2a\u95ee\u9898\uff0c\u76f8\u5bf9\u4e8e\u65e0\u673a\u7535\u6781\u6750\u6599\u800c\u8a00\uff0c\u6709\u673a\u6b63\u6781\u6750\u6599\u53ef\u4ee5\u53d1\u751f\u591a\u7535\u5b50\u53cd\u5e94\uff0c\u4ece\u800c\u5177\u6709\u8f83\u9ad8\u7684\u7406\u8bba\u5bb9\u91cf\u3002\u6b64\u5916\uff0c\u5b83\u8fd8\u5177\u6709\u5206\u5b50\u91cf\u4f4e\uff0c\u7ed3\u6784\u591a\u6837\uff0c\u6c27\u5316\u8fd8\u539f\u7535\u4f4d\u53ef\u8c03\u6574\u7684\u72ec\u7279\u4f18\u52bf\uff1b\u66f4\u91cd\u8981\u7684\u662f\uff0c\u6709\u673a\u6b63\u6781\u6750\u6599\u53ef\u4ee5\u76f4\u63a5\u4ece\u4e30\u5bcc\u7684\u53ef\u518d\u751f\u7684\u751f\u7269\u8d28\u524d\u9a71\u4f53\u4e2d\u5236\u5907\u5f97\u5230\uff0c\u7ecf\u8fc7\u5149\u5408\u4f5c\u7528\u53ef\u8fdb\u884c\u5faa\u73af\uff0c\u7b26\u5408\u9502\u79bb\u5b50\u7535\u6c60\u201c\u7eff\u8272\u3001\u53ef\u6301\u7eed\u7684\u201d\u7684\u53d1\u5c55\u7406\u5ff5\u3002<\/p>\n<p>\u4e3a\u4e86\u5bfb\u6c42\u9ad8\u6027\u80fd\u7684\u6709\u673a\u7535\u6781\u6750\u6599\uff0c\u542b\u6709\u4e00\u4e2a\u6216\u591a\u4e2a\u7535\u5316\u5b66\u6d3b\u6027\u7fb0\u57fa\u7684\u6709\u673a\u7fb0\u57fa\u5316\u5408\u7269\u56e0\u5176\u9ad8\u5bb9\u91cf\u548c\u5feb\u901f\u7684\u52a8\u529b\u5b66\u5f97\u5230\u7684\u5e7f\u6cdb\u7684\u7814\u7a76\u3002\u5176\u4e2d\uff0c\u6bcf\u4e00\u4e2a\u7fb0\u57fa\u5728\u5145\u653e\u7535\u8fc7\u7a0b\u90fd\u53ef\u4ee5\u53d1\u751f\u4e00\u7535\u5b50\u53ef\u9006\u8f6c\u79fb\u53cd\u5e94\u3002\u5373\uff0c\u5355\u7535\u5b50\u8fd8\u539f\u5f62\u6210\u4e00\u4e2a\u5355\u9634\u79bb\u5b50\uff0c\u7136\u540e\u5355\u7535\u5b50\u6c27\u5316\u8f6c\u6362\u56de\u5230\u7fb0\u57fa\u3002\u6709\u673a\u7fb0\u57fa\u5316\u5408\u7269\u7684\u7814\u7a76\u53ef\u8ffd\u6eaf\u52301969\u5e74\u65e9\u671f\uff0c\u4f46\u662f\u7edd\u5927\u591a\u6570\u6709\u673a\u7fb0\u57fa\u6b63\u6781\u6750\u6599\u5728\u7535\u89e3\u8d28\u4e2d\u6eb6\u89e3\u4e25\u91cd\u4f7f\u5176\u5bb9\u91cf\u8870\u51cf\u8fc5\u901f\uff0c\u5176\u5bfc\u7535\u6027\u5dee\u4e5f\u4f7f\u5f97\u5176\u500d\u7387\u6027\u80fd\u8f83\u5dee\u3002\u4e3a\u4e86\u89e3\u51b3\u4e0a\u8ff0\u95ee\u9898\uff0c\u8fc4\u4eca\u4e3a\u6b62\u5df2\u7ecf\u91c7\u53d6\u4e86\u4e00\u7cfb\u5217\u7684\u63aa\u65bd\uff1a1\u3001\u4f18\u5316\u5206\u5b50\u7ed3\u6784\uff1b2\u3001\u5c06\u7fb0\u57fa\u5316\u5408\u7269\u56fa\u5b9a\u5728\u5bfc\u7535\u7684\u57fa\u8d28\u4e0a\uff1b3\u3001\u5c06\u7fb0\u57fa\u5c0f\u5206\u5b50\u805a\u5408\u5f62\u6210\u805a\u5408\u7269\uff1b4\u3001\u4f7f\u7528\u56fa\u4f53\u7535\u89e3\u8d28\u3002\u5176\u4e2d\uff0c\u5236\u5907\u78b3\u590d\u5408\u6750\u6599\u6210\u4e3a\u6784\u5efa\u9ad8\u6027\u80fd\u6709\u673a\u6b63\u6781\u6750\u6599\u7684\u4e00\u79cd\u6709\u6548\u65b9\u6cd5\u3002\u4f5c\u4e3a\u53ef\u4ee5\u4ece\u690d\u7269\u4e2d\u63d0\u53d6\u6216\u8005\u5408\u6210\u7684\u7fb0\u57fa\u7c7b\u67d3\u6599\uff0c\u8fc4\u4eca\u4e3a\u6b62\uff0c\u8fd8\u6ca1\u6709\u5173\u4e8e\u5176\u53ef\u7528\u4f5c\u9502\u79bb\u5b50\u7535\u6c60\u6b63\u6781\u6750\u6599\u7684\u76f8\u5173\u7814\u7a76\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u4ecb\u7ecd\u3011<\/strong><\/p>\n<p><strong>\u5357\u4eac\u5de5\u4e1a\u5927\u5b66\u9ec4\u7ef4\u9662\u58eb<\/strong>\u548c<strong>\u5357\u6d0b\u7406\u5de5\u5927\u5b66Ting Yu\u6559\u6388\uff08\u5171\u540c\u901a\u8baf\u4f5c\u8005\uff09\u7b49<\/strong>\u63d0\u4f9b\u4e86\u4e00\u79cd\u7b80\u5355\u901a\u7528\u7684\u8fd8\u539f\u67d3\u6599\/\u77f3\u58a8\u590d\u5408\u6750\u6599\u5236\u5907\u65b9\u6cd5\u3002\u5c06\u8d85\u58f0\u5904\u7406\u548c\u6c34\u70ed\u6cd5\u76f8\u7ed3\u5408\u53ef\u5236\u5907\u51fa\u591a\u79cd\u8fd8\u539f\u67d3\u6599\/\u77f3\u58a8\u590d\u5408\u6750\u6599\uff0c\u7528\u6765\u505a\u9ad8\u6027\u80fd\u9502\u79bb\u5b50\u7535\u6c60\u6b63\u6781\u6750\u6599\u3002\u4f8b\u5982\uff0c\u901a\u8fc7\u8fd8\u539f\u7eff8\u548c\u77f3\u58a8\u70ef\u7247\u4e4b\u95f4\u7684\u03c0-\u03c0\u76f8\u4e92\u4f5c\u7528\u7814\u7a76\u4eba\u5458\u5f97\u5230\u4e86\u7a33\u5b9a\u7684\u590d\u5408\u7ed3\u6784\uff0c\u5b83\u4e0d\u4ec5\u53ef\u4ee5\u6709\u6548\u5730\u6291\u5236\u6d3b\u6027\u7269\u8d28\u7684\u6eb6\u89e3\u73b0\u8c61\uff0c\u5728\u7535\u5316\u5b66\u53cd\u5e94\u671f\u95f4\u8fd8\u53ef\u4ee5\u4fdd\u8bc1\u7535\u5b50\u7684\u5feb\u901f\u4f20\u8f93\u3002\u56e0\u6b64\uff0c\u8fd8\u539f\u7eff8 \/\u77f3\u58a8\u70ef\uff08VG8 \/ G\uff09\u7684\u590d\u5408\u6750\u6599\u8868\u73b0\u51fa\u826f\u597d\u7684\u5faa\u73af\u7a33\u5b9a\u6027\u548c\u4f18\u5f02\u7684\u9ad8\u500d\u7387\u6027\u80fd\u3002\u8fd9\u79cd\u7b80\u5355\u901a\u7528\u7684\u65b9\u6cd5\u8fd8\u53ef\u4ee5\u7528\u6765\u5236\u5907\u8fd8\u539f\u68d5BR\/\u77f3\u58a8\u70ef\uff08VB BR\/ G\uff09\u548c\u8fd8\u539f\u6a44\u6984T \/\u77f3\u58a8\u70ef\uff08VO T \/ G\uff09\u590d\u5408\u6750\u6599\uff0c\u90fd\u8868\u73b0\u51fa\u4f18\u5f02\u7684\u7535\u5316\u5b66\u6027\u80fd\uff0c\u4e3a\u9ad8\u6027\u80fd\u9502\u79bb\u5b50\u7535\u6c60\u6b63\u6781\u6750\u6599\u7684\u5f00\u53d1\u63d0\u4f9b\u4e86\u65b0\u7684\u65b9\u5411\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u89e3\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe\u4e00\u3001VG 8\/G\u590d\u5408\u6750\u6599\u5408\u6210\u793a\u610f\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-44150 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72471-30.jpg\" alt=\"\u56fe\u72471\" width=\"500\" height=\"115\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72471-30.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72471-30-300x69.jpg 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p>VG8\/ G\u590d\u5408\u6750\u6599\u7684\u5408\u6210\u8fc7\u7a0b\uff1a1\u3001\u8fd8\u539f\u7eff8\u6676\u4f53\u7ed3\u6784\u5206\u89e3\uff1b2\u3001\u8fd8\u539f\u7eff8\u5728\u77f3\u58a8\u70ef\u7247\u4e0a\u91cd\u65b0\u8fdb\u884c\u7ec4\u88c5\u3002\u8fd8\u539f\u7eff8\u548c\u77f3\u58a8\u70ef\u7247\u4e4b\u95f4\u7684\u03c0-\u03c0\u76f8\u4e92\u4f5c\u7528\u662f\u5f62\u6210VG 8\/ G\u590d\u5408\u7ed3\u6784\u7684\u4e3b\u8981\u9a71\u52a8\u529b\u3002<\/p>\n<p><strong>\u56fe\u4e8c\u3001\u8fd8\u539f\u7eff8\u548cVG 8\/G-0.5\u590d\u5408\u6750\u6599<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-44151 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72472-24.jpg\" alt=\"\u56fe\u72472\" width=\"500\" height=\"203\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72472-24.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72472-24-300x122.jpg 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p>a\u3001b\uff1a\u50a8\u9502\u7ed3\u6784\u793a\u610f\u56fe\uff1b \u00a0 \u00a0 \u00a0 \u00a0 \u00a0 \u00a0 \u00a0 \u00a0 c\u3001d\uff1aFESEM\u56fe\uff1b<\/p>\n<p>e\u3001f\uff1aTEM\u56fe\uff1b\u5176\u4e2d\uff0c\u63d2\u56fe\u5747\u4e3a\u76f8\u5e94\u6837\u54c1\u66f4\u9ad8\u500d\u7387\u7684FESEM\u56fe\u548cTEM\u56fe\u3002<\/p>\n<p><strong>\u56fe\u4e09\u3001GO\u3001VG 8\/G-0.25\u3001VG 8\/G-0.5\u3001VG 8\/G-1<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-44152 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72473-23.jpg\" alt=\"\u56fe\u72473\" width=\"500\" height=\"410\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72473-23.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72473-23-300x246.jpg 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p>a\uff09XPS\u8c31\uff1b \u00a0 \u00a0 \u00a0b\uff09\u9ad8\u500d\u7387C 1s XPS\u5149\u8c31\uff1b<\/p>\n<p>c\uff09\u7ec4\u4efd\u65e0GO\u7684\u9ad8\u500d\u7387N 1s XPS\u5149\u8c31\u3002<\/p>\n<p><strong>\u56fe\u56db\u3001VG 8\/G\u590d\u5408\u6750\u6599<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-44153 size-large\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72474-22-459x1024.jpg\" alt=\"\u56fe\u72474\" width=\"459\" height=\"1024\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72474-22-459x1024.jpg 459w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72474-22-135x300.jpg 135w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72474-22.jpg 500w\" sizes=\"(max-width: 459px) 100vw, 459px\" \/><\/p>\n<p>a\uff09VG8\u4e0e\u77f3\u58a8\u7684XRD\u8c31\u56fe\uff1b<\/p>\n<p>b\uff09\u4e0erGO\u4f7f\u7528532nm\u6fc0\u53d1\u5149\u65f6\u7684RGO\u62c9\u66fc\u5149\u8c31\uff1b<\/p>\n<p>c\uff09\u4e0e\u8fd8\u539f\u7eff8\u5728N<sub>2<\/sub>\u6c14\u6c1b\u4e0b\u7684TGA\u66f2\u7ebf\u3002<\/p>\n<p><strong>\u56fe\u4e94\u3001VG 8\/G\u590d\u5408\u6750\u6599<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-44154 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72475-15.jpg\" alt=\"\u56fe\u72475\" width=\"500\" height=\"562\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72475-15.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72475-15-267x300.jpg 267w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p>a\uff09\u5355\u4e00\u7684VG 8\/G\u5355\u5143\u7684\u7535\u5316\u5b66\u50a8\u9502\u673a\u5236\uff1b<\/p>\n<p>b\uff09\u626b\u63cf\u901f\u5ea6\u4e3a0.5 mV s<sup>\u22121<\/sup>\u65f6\uff0c\u4e0d\u540c\u7535\u6781\u7684CV\u66f2\u7ebf\uff1b<\/p>\n<p>c\uff09VG 8\/G-0.5\u7535\u6781\u5728\u4e0d\u540c\u7535\u6d41\u5bc6\u5ea6\u4e0b\u7684\u5145\u653e\u7535\u66f2\u7ebf\uff1b<\/p>\n<p>d\uff09100 mA g<sup>\u22121<\/sup>\u65f6\uff0c\u4e0d\u540c\u7535\u6781\u6750\u6599\u7684\u5faa\u73af\u6027\u80fd\uff1b<\/p>\n<p>e\uff09\u4e0d\u540c\u7535\u6781\u5728\u4e0d\u540c\u7535\u6d41\u5bc6\u5ea6\u4e0b\u7684\u500d\u7387\u6027\u80fd\u3002<\/p>\n<p><strong>\u56fe\u516d\u3001\u8fd8\u539f\u7eff8\u3001VG 8\/G-0.25\u3001VG 8\/G-0.5\u3001VG 8\/G-1\u7535\u6781\u963b\u6297\u6d4b\u8bd5\u53ca\u5176\u7b49\u6548\u7535\u8def\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-44155 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72476-13.jpg\" alt=\"\u56fe\u72476\" width=\"500\" height=\"267\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72476-13.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72476-13-300x160.jpg 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p>a\uff09\u5404\u7535\u6781Nyquist\u56fe\uff1b<\/p>\n<p>b\uff09EIS\u7b49\u6548\u7535\u8def\u6a21\u578b\u56fe\uff1b<\/p>\n<p>c\uff09\u4e0d\u540c\u7535\u6781\u7684\u62df\u5408\u7ed3\u679c\u3002<\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u8fd9\u9879\u5de5\u4f5c\u63d0\u4f9b\u4e86\u4e00\u79cd\u7528\u6765\u5236\u5907\u9502\u79bb\u5b50\u7535\u6c60\u6b63\u6781\u6750\u6599\u2014\u8fd8\u539f\u67d3\u6599\/\u77f3\u58a8\u70ef\u590d\u5408\u6750\u6599\u7684\u7b80\u5355\u65b9\u6cd5\u3002\u5176\u539f\u7406\u662f\u67d3\u6599\u5206\u5b50\u6676\u4f53\u7ed3\u6784\u7684\u5206\u89e3\uff0c\u7136\u540e\u901a\u8fc7\u03c0\u2013\u03c0\u8d85\u5f3a\u76f8\u4e92\u4f5c\u7528\u5728\u77f3\u58a8\u70ef\u4e0a\u91cd\u65b0\u7ec4\u88c5\uff0c\u8fd9\u79cd\u8bbe\u8ba1\u53ef\u4ee5\u4f7f\u5f97\u5177\u6709\u7535\u5316\u5b66\u6d3b\u6027\u7684\u8fd8\u539f\u67d3\u6599\u5206\u5b50\u5bf9Li<sup>+<\/sup>\u7684\u76f8\u4e92\u505a\u4f5c\u7528\u663e\u8457\u589e\u5f3a\uff0c\u540c\u65f6\u4f7f\u5176\u5728\u7535\u89e3\u8d28\u4e2d\u7684\u6eb6\u89e3\u95ee\u9898\u5f97\u5230\u6291\u5236\u3002\u8fd9\u79cd\u72ec\u7279\u7684\u7ed3\u6784\u6709\u5229\u4e8e\u7535\u5b50\u7684\u6709\u6548\u4f20\u8f93\uff0c\u5e76\u7f29\u77ed\u91ccLi<sup>+<\/sup>\u6269\u6563\u7684\u957f\u5ea6\u3002\u6b64\u5916\uff0c\u83b7\u5f97\u4e86VG 8\/G\u3001VB BR\/G\u548cVO T\/G\u7b49\u591a\u79cd\u7c7b\u578b\u7684\u8fd8\u539f\u67d3\u6599\/\u77f3\u58a8\u70ef\u590d\u5408\u6750\u6599\uff0c\u5e76\u5df2\u7528\u4f5c\u9502\u79bb\u5b50\u7535\u6c60\u6b63\u6781\u6750\u6599\u7684\u7814\u7a76\uff0c\u5747\u5177\u6709\u5f88\u9ad8\u7684\u9502\u5b58\u50a8\u5bb9\u91cf\uff0c\u8868\u73b0\u51fa\u826f\u597d\u7684\u7535\u5316\u5b66\u6027\u80fd\u3002\u4e3a\u9ad8\u50a8\u9502\u6709\u673a\u7535\u6781\u6750\u6599\u7684\u53d1\u5c55\u63d0\u4f9b\u4e86\u826f\u597d\u7684\u65b9\u6cd5\uff0c\u5bf9\u4e8e\u6709\u673a\u57fa\u7535\u6781\u6750\u6599\u7684\u5b9e\u9645\u5e94\u7528\u4e5f\u5177\u6709\u6307\u5bfc\u6027\u7684\u610f\u4e49\u3002<\/p>\n<p><strong>\u9ec4\u7ef4\u7b80\u4ecb\uff1a<\/strong><br \/>\n\u4e2d\u56fd\u79d1\u5b66\u9662\u9662\u58eb\uff0c\u5357\u4eac\u5de5\u4e1a\u5927\u5b66\u6821\u957f\u3001\u6559\u6388\u3001\u535a\u5bfc\uff0c\u6709\u673a\u5149\u7535\u5b50\u5b66\u5bb6\u3002\u6559\u80b2\u90e8\u201c\u957f\u6c5f\u5b66\u8005\u201d\u7279\u8058\u6559\u6388\uff0c\u56fd\u5bb6\u6770\u51fa\u9752\u5e74\u79d1\u5b66\u57fa\u91d1\u83b7\u5f97\u8005\uff0c\u4e2d\u7ec4\u90e8\u201c\u5343\u4eba\u8ba1\u5212\u201d\u56fd\u5bb6\u7279\u8058\u4e13\u5bb6\uff0c\u79d1\u6280\u90e8\u201c973\u201d\u9879\u76ee\u9996\u5e2d\u79d1\u5b66\u5bb6\u3002\u4e3b\u8981\u7814\u7a76\u65b9\u5411\u662f\u81f4\u529b\u4e8e\u5efa\u6709\u673a\u5149\u7535\u5b50\u5b66\u79d1\u7684\u7406\u8bba\u4f53\u7cfb\u6846\u67b6\u3001\u5b9e\u73b0\u6709\u673a\u534a\u5bfc\u4f53\u7684\u9ad8\u6027\u80fd\u5316\u4e0e\u591a\u529f\u80fd\u5316\u3001\u63a8\u8fdb\u79d1\u6280\u6210\u679c\u8f6c\u5316\u4e0e\u4ea7\u4e1a\u5316\u65b9\u9762\u7684\u53d1\u5c55\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5<\/strong>\uff1a<a href=\"http:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/adfm.201603603\/full\" target=\"_blank\">Toward High Energy Organic Cathodes for Li-Ion Batteries:A Case Study of Vat Dye\/Graphene Composites<\/a>\u00a0\uff08Adv. Funct. Mater.\uff0c2016\uff0cDOI: 10.1002\/adfm.201603603\uff09<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u65b0\u80fd\u6e90\u5b66\u672f\u7ec4 <strong>NeverSayBye<\/strong> \u4f9b\u7a3f\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\">\u70b9\u8fd9\u91cc\u52a0\u5165\u6750\u6599\u4eba\u7684\u5927\u5bb6\u5ead<\/a>\u3002\u53c2\u4e0e\u65b0\u80fd\u6e90\u8bdd\u9898\u8ba8\u8bba\u8bf7\u52a0\u5165\u201c\u6750\u6599\u4eba\u65b0\u80fd\u6e90\u6750\u6599\u4ea4\u6d41\u7fa4 422065952\u201d,\u6b22\u8fce\u5173\u6ce8\u5fae\u4fe1\u516c\u4f17\u53f7\uff0c\u5fae\u4fe1\u641c\u7d22\u201c\u65b0\u80fd\u6e90\u524d\u7ebf\u201d\u6216\u626b\u7801\u5173\u6ce8\u3002<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-44156 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72477-12.jpg\" alt=\"\u56fe\u72477\" width=\"341\" height=\"341\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72477-12.jpg 341w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72477-12-150x150.jpg 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/09\/\u56fe\u72477-12-300x300.jpg 300w\" sizes=\"(max-width: 341px) 100vw, 341px\" \/><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u50a8\u80fd\u662f\u5f53\u4eca21\u4e16\u7eaa\u6700\u91cd\u8981\u7684\u8bdd\u9898\u4e4b\u4e00\u3002\u81ea20\u4e16\u7eaa90\u5e74\u4ee3\u9502\u79bb\u5b50\u7535\u6c60\u8bde\u751f\u4ee5\u6765\uff0c\u5b83\u5df2\u7ecf\u5728\u4fbf\u643a\u5f0f\u7535\u5b50\u4ea7\u54c1\u9886\u57df\u5360\u636e\u4e86\u4e3b\u8981\u5e02\u573a\uff0c\u6210\u4e3a\u4e86\u6700\u6709\u6f5c\u529b\u7684\u50a8\u80fd\u65b9\u5f0f\u3002\u7136\u800c\uff0c\u9502&#8230;<\/p>\n","protected":false},"author":174,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[54,46,1399],"class_list":["post-44147","post","type-post","status-publish","format-standard","hentry","category-jiedu","tag-making","tag-graphene","tag-huangwei"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/44147"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/174"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=44147"}],"version-history":[{"count":8,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/44147\/revisions"}],"predecessor-version":[{"id":44804,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/44147\/revisions\/44804"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=44147"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=44147"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=44147"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}