{"id":46756,"date":"2016-10-19T06:30:10","date_gmt":"2016-10-18T22:30:10","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=46756"},"modified":"2016-10-17T22:05:29","modified_gmt":"2016-10-17T14:05:29","slug":"jasc%e5%8c%97%e4%ba%ac%e5%a4%a7%e5%ad%a6%e6%b7%b1%e5%9c%b3%e7%a0%94%e7%a9%b6%e7%94%9f%e9%99%a2%ef%bc%9a%e5%b1%82%e7%8a%b6linixmnycozo2-%e7%9a%84%e7%83%ad%e7%a8%b3%e5%ae%9a%e6%80%a7%e8%b0%83%e8%8a%82","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=46756","title":{"rendered":"\u5317\u5927\u6df1\u7814\u9662JACS\uff1a\u5c42\u72b6Li(NixMnyCoz)O2 \u7684\u70ed\u7a33\u5b9a\u6027\u8c03\u8282"},"content":{"rendered":"<p><span style=\"color: #ff0000;\"><strong>\u3010\u5f15\u8bed\u3011<\/strong><\/span><\/p>\n<p>\u53ef\u5145\u7535\u9502\u79bb\u5b50\u7535\u6c60\uff08LIBs\uff09\u88ab\u5e7f\u6cdb\u8fd0\u7528\u5728\u73b0\u4eca\u5927\u591a\u6570\u7684\u4fbf\u643a\u5f0f\u7535\u5b50\u4ea7\u54c1\u4e2d\uff0c\u4ee5\u53ca\u88ab\u8d8a\u6765\u8d8a\u591a\u7684\u7535\u52a8\u6c7d\u8f66\uff08EV\uff09\u548c\u7535\u7ad9\u5b58\u50a8\u6240\u9700\u6c42\u3002\u5728\u8fd9\u79cd\u53d1\u5c55\u8d8b\u52bf\u4e4b\u4e0b\uff0c\u6211\u4eec\u4e3b\u8981\u5173\u5fc3\u7684\u662f\u63d0\u9ad8\u4ed6\u4eec\u7684\u5b89\u5168\u6027\uff0c\u6210\u672c\u548c\u73af\u5883\u76f8\u5bb9\u6027\u3002\uff081\uff09\u9ad8\u80fd\u91cf\u548c\u9ad8\u529f\u7387\u5bc6\u5ea6\u7684\u5e94\u7528\uff08\u5982\u7535\u52a8\u6c7d\u8f66\uff09\uff0c\u5b89\u5168\u6027\u5c31\u53d8\u5f97\u5c24\u4e3a\u91cd\u8981\u3002\u7535\u6c60\u7684\u5b89\u5168\u6027\u901a\u5e38\u53d6\u51b3\u4e8e\u7531\u6b63\u6781\u6750\u6599\u7684\u70ed\u7a33\u5b9a\u6027\uff0c\u7531\u7ed3\u6784\u7684\u5206\u89e3\u548c\u76f8\u53d8\u6240\u53cd\u6620\u3002\u4e00\u822c\u6765\u8bf4\uff0c\u5206\u89e3\u53cd\u5e94\u4f34\u968f\u7740\u6c27\u7684\u91ca\u653e\u3002\uff082\uff09\u66f4\u5371\u9669\u7684\u662f\u6b63\u6781\u6750\u6599\u4e0e\u6709\u673a\u7535\u89e3\u8d28\u7684\u53cd\u5e94\u3002\u56e0\u6b64\uff0c\u6b63\u6781\u6750\u6599\u7684\u826f\u597d\u7684\u70ed\u7a33\u5b9a\u6027\u548c\u4e0d\u8f7b\u6613\u7684\u6c27\u91ca\u653e\u5bf9\u4e8e\u9ad8\u80fd\u91cf\u548c\u529f\u7387\u5bc6\u5ea6EV LIBS\u5e94\u7528\u5341\u5206\u91cd\u8981\u3002\u8fd1\u65e5\uff0c\u5317\u4eac\u5927\u5b66\u6df1\u5733\u7814\u7a76\u751f\u9662\u7684<span style=\"color: #ff0000;\"><strong>\u6f58\u5cf0\u6559\u6388<\/strong><\/span>\u8bfe\u9898\u7ec4\u5728<span style=\"color: #0000ff;\">J. Am. Chem. Soc<\/span>\u4e0a\u53d1\u6587\uff0c\u9898\u4e3a\u201c<span style=\"color: #0000ff;\"><em>Tuning of Thermal Stability in Layered Li(Ni<sub>x<\/sub>Mn<sub>y<\/sub>Co<sub>z<\/sub>)O<sub>2<\/sub><\/em><\/span>\u201d\u3002 \u672c\u6587\u5229\u7528\u4ece\u5934\u8ba1\u7b97\u4e0e\u5b9e\u9a8c\u7684\u65b9\u6cd5\u63a2\u7a76\u4e86\u5c42\u72b6Li(Ni<sub>x<\/sub>Mn<sub>y<\/sub>Co<sub>z<\/sub>)O<sub>2<\/sub>\u7684\u70ed\u7a33\u5b9a\u6027\u8c03\u6574\uff0c\u8fd9\u5bf9\u4e8e\u672a\u6765\u5b9e\u9a8c\u7814\u7a76\u5177\u6709\u6307\u5bfc\u6027\u610f\u4e49\u3002<\/p>\n<p><span style=\"color: #ff0000;\"><strong>\u3010\u4e3b\u8981\u5185\u5bb9\u3011<\/strong><\/span><\/p>\n<p>\u8be5\u7814\u7a76\u5c0f\u7ec4\u5c06\u4ece\u5934\u8ba1\u7b97\u65b9\u6cd5\u4e0e\u5b9e\u9a8c\u76f8\u7ed3\u5408\uff0c\u7814\u7a76\u4e86\u5982\u4f55\u8c03\u8282NMC\u6750\u6599\u7684\u70ed\u7a33\u5b9a\u6027\u3002\u7814\u7a76\u4eba\u5458\u5c06\u8be5\u6750\u6599\u5206\u4e3a\u4e24\u7ec4\uff1a\u201c\u5bcc\u954d\u201d\u7ec4\uff08\u6df7\u5408\u4ef7\u6001\u7684Ni<sup>2+<\/sup>\/Ni<sup>3+<\/sup>\uff09\u548c\u201cNi=Mn\u201d\u7ec4\uff08\u53ea\u6709Ni<sup>2+<\/sup>\u7684\u72b6\u6001\uff09\uff0c\u8fd9\u5c06\u6709\u5229\u4e8e\u7cfb\u7edf\u7684\u7814\u7a76\u3002\u7814\u7a76\u53d1\u73b0\uff0c\u6750\u6599\u70ed\u7a33\u5b9a\u6027\u4e0e\u6700\u4e0d\u7a33\u5b9a\u7684\u6c27\u5bc6\u5207\u76f8\u5173\uff0c\u8fd9\u662f\u7531\u5c40\u90e8\u642d\u914d\u7ed3\u6784\u5355\u5143\uff08LCSU\uff09\uff1aTM(Ni, Mn, Co)<sub>3<\/sub>-O-Li<sub>3\u2013<em>x<\/em><\/sub><sub>\u2032<\/sub>\u00a0(<em>x<\/em>\u2032= 0-3)\u6240\u51b3\u5b9a\u7684\u3002\u9502\u7684\u542b\u91cf\uff0c\u954d\u7684\u4ef7\u6001\uff0cNi\u3001Mn\u3001Co\u7684\u542b\u91cf\u4ee5\u53caNi\/Li\u7684\u6df7\u6392\u53ef\u4ee5\u901a\u8fc7\u5f71\u54cdNMC\u6750\u6599\u4e2d\u7684\u4f4d\u70b9\u3001\u542b\u91cf\u4ee5\u53ca\u6700\u4e0d\u7a33\u5b9a\u7684\u6c27\u91ca\u653e\u6e29\u5ea6\u6765\u8c03\u8282NMC\u6750\u6599\u7684\u70ed\u7a33\u5b9a\u6027\u3002\u53bb\u9502\u5316\u8fc7\u7a0b\u4e2d\uff0cLi\u7a7a\u4f4d\u548c\u9ad8\u4ef7\u6001\u954d\u5f62\u6210\u4e4b\u95f4\u7684\u534f\u540c\u6548\u5e94\u4f1a\u52a0\u91cd\u6c27\u7684\u4e0d\u7a33\u5b9a\uff0c\u4f46\u8fd9\u5bf9\u4e8e\u6240\u6709\u7684NMC\u6750\u6599\u7684\u4e2d\u95f4\u9502\u5316\u72b6\u6001\u7684\u70ed\u7a33\u5b9a\u6027\u6709\u5c11\u8bb8\u8d21\u732e\uff08\u4f8b\u5982\uff0c\u6750\u6599\u4ece25%\u523050%\u7684\u53bb\u9502\u5316\u8fc7\u7a0b\uff09\u3002\u5728\u4e00\u4e2a\u56fa\u5b9a\u7684\u53bb\u9502\u5316\u72b6\u6001\uff0c\u6c27\u642d\u914d\u66f4\u591a\u7684\u954d\uff08\u5c24\u5176\u662f\u9ad8\u4ef7\u6001\uff09\u6bd4\u5176\u4ed6\u79cd\u7c7b\u7684\u642d\u914d\u66f4\u4e0d\u7a33\u5b9a\u3002Ni\/Li\u6df7\u6392\u4f1a\u964d\u4f4e\u201cNi=Mn\u201d\u7ec4\u7684\u70ed\u7a33\u5b9a\u6027\u800c\u5229\u4e8e\u201c\u5bcc\u954d\u201d\u7ec4\u7684\u70ed\u7a33\u5b9a\u6027\uff0c\u56e0\u4e3a\u5728\u5bcc\u954dNMC\u6750\u6599\u4e2d\u7684Li\u5c42\u5185\u7684Ni\u4f1a\u5f62\u6210180\u00b0\u7684Ni\u2013O\u2013Ni\u8d85\u4ea4\u6362\u94fe\u3002\u8fd9\u9879\u5de5\u4f5c\u4e2d\u7684\u7406\u8bba\u8ba1\u7b97\u7ed3\u679c\u4e0e\u5b9e\u9a8c\u7ed3\u679c\u76f8\u4e00\u81f4\uff0c\u8fd9\u4e5f\u8bc1\u660e\u4e86\u8fd9\u4e00\u7b80\u5355\u6a21\u578b\u7684\u5408\u7406\u6027\uff0c\u5b83\u4e0d\u4ec5\u8003\u8651\u4e86\u6240\u6709\u7684\u5f71\u54cd\u56e0\u7d20\uff0c\u4e5f\u4ece\u539f\u5b50\u7684\u6c34\u5e73\u63d0\u4f9b\u4e86\u5bf9\u4e8eNMC\u6750\u6599\u70ed\u7a33\u5b9a\u6027\u7684\u4e00\u4e2a\u7b80\u5355\u4e14\u76f4\u63a5\u7684\u89e3\u91ca\u3002<\/p>\n<p><span style=\"color: #ff0000;\"><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/span><\/p>\n<p><span style=\"color: #ff6600;\"><strong>\u56fe\u4e00\uff1a NMC<\/strong><strong>\u6750\u6599\u6750\u6599\u7ed3\u6784\u5206\u6790<\/strong><\/span><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-46759 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/10\/1.jpeg\" alt=\"1\" width=\"600\" height=\"333\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/10\/1.jpeg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/10\/1-300x167.jpeg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u4e09\u89d2\u5f62\u8868\u660e\u5df2\u88ab\u7814\u7a76\u7684NMC\u6750\u6599\u3002<\/p>\n<p>\uff08b\uff09\uff08532\uff09\u7ed3\u6784\u6a21\u578b\u7684\u9876\u5c42\u89c6\u56fe\u548c\u4fa7\u89c6\u56fe\u3002\u63d2\u56fe\u663e\u793a\u4e86NMC\u6750\u6599\u4e2d\u6c27\u7684\u5c40\u90e8\u642d\u914d\u7ed3\u6784\u5355\u5143\u3002<\/p>\n<p>\uff08c\uff09\u5728NMC\u6750\u6599\u4e2d\u6c27\u76847\u4e2a\u5c40\u90e8\u642d\u914d\u7ed3\u6784\u5355\u5143\u3002<\/p>\n<p><span style=\"color: #ff6600;\"><strong>\u56fe\u4e8c\uff1a\u53bb\u9502\u5316\u8fc7\u7a0b\u4e2d\u70ed\u7a33\u5b9a\u6027\u8c03\u8282\u7684\u6574\u4f53\u89c6\u56fe<\/strong><\/span><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-46764 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/10\/\u6458\u8981.jpeg\" alt=\"\u6458\u8981\" width=\"600\" height=\"371\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/10\/\u6458\u8981.jpeg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/10\/\u6458\u8981-300x186.jpeg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>TG\uff1a\u7b2c\u4e00\u7ea7\u6c27\u635f\u5931\u7684\u6e29\u5ea6\u3002\u0394H\uff1a\u5728\u6700\u4e0d\u7a33\u5b9a\u7684LCSU\u8ba1\u7b97\u7684\u6c27\u7a7a\u4f4d\u5f62\u6210\u80fd\u3002\u7eff\u8272\uff1aLi\uff1b\u7ea2\u8272\uff1aO\uff1b\u94f6\uff1aNi\uff1b\u7d2b\u8272\uff1aMn\u548c\u84dd\u8272\uff1a Co\u3002<\/p>\n<p><span style=\"color: #ff6600;\"><strong>\u56fe\u4e09\uff1a\u6c27\u7a7a\u4f4d\u5f62\u6210\u80fd\uff08\u0394H<\/strong><strong>\uff09\u7684\u6bd4\u8f83\u548cTGA<\/strong><strong>\u66f2\u7ebf<\/strong><\/span><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-46765 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/10\/3-1.jpeg\" alt=\"3\" width=\"600\" height=\"215\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/10\/3-1.jpeg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/10\/3-1-300x108.jpeg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u5728SOC = 0.5\u65f6\uff0cTG\u548c\u6700\u4e0d\u7a33\u5b9a\u7684LCSU\u8ba1\u7b97\u7684\u6c27\u7a7a\u4f4d\u5f62\u6210\u80fd\uff08\u0394H\uff09\u7684\u6bd4\u8f83\u3002<\/p>\n<p>\uff08b\uff09Li<sub>1\u2212x<\/sub><sub>\u2033<\/sub>(Ni<sub>x<\/sub>Mn<sub>y<\/sub>Co<sub>z<\/sub>)O<sub>2<\/sub>\u5316\u5b66\u53bb\u9502\u5316\u8fc7\u7a0b\u7684TGA\u66f2\u7ebf\u3002<\/p>\n<p><span style=\"color: #ff6600;\"><strong>\u56fe\u56db\uff1a\u542b6.67%<\/strong><strong>\u7684Ni\/Li<\/strong><strong>\u6df7\u6392\u7684\uff08333<\/strong><strong>\uff09\u7ed3\u6784\u6a21\u578b<\/strong><\/span><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-46762 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/10\/4.jpeg\" alt=\"4\" width=\"600\" height=\"384\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/10\/4.jpeg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/10\/4-300x192.jpeg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u542b6.67%\u7684Ni\/Li\u6df7\u6392\u7684\uff08333\uff09\u7ed3\u6784\u6a21\u578b\u3002\u53f3\u8fb9\u7684\u9762\u677f\u663e\u793a\u4e86\u6709\u548c\u6ca1\u6709Ni\/Li\u9519\u6392\u7684\u8d85\u6676\u80de\u4e2d\u56db\u4e2a\u5177\u6709\u4ee3\u8868\u6027\u7684\u6c27\u7684LCSUs\u3002<\/p>\n<p><span style=\"color: #ff6600;\"><strong>\u56fe\u4e94\uff1a\u539f\u4f4dXRD<\/strong><strong>\u6d4b\u8bd5\u56fe<\/strong><\/span><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-46763 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/10\/5.jpeg\" alt=\"5\" width=\"600\" height=\"409\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/10\/5.jpeg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/10\/5-300x205.jpeg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u5728SOC = 0.5\u65f6\u7684\u52a0\u70ed\u8fc7\u7a0b\u4e2d\uff0871515\uff09\u7684\u539f\u4f4dX\u5c04\u7ebf\u884d\u5c04\u6d4b\u8bd5\u3002<\/p>\n<p>\uff08b\uff09\u6240\u6709NMC\u6750\u6599\u7684\uff08003\uff09<sub>R<\/sub>\u5cf0\u79fb\u4e0e\u6e29\u5ea6\u7684\u5173\u7cfb\u3002<\/p>\n<p>\uff08c\u3001d\uff09\uff08003\uff09R\u5cf0\u548c\uff08018\uff09<sub>R<\/sub>\/\uff08110\uff09<sub>R<\/sub>\u5bf9\u7684\u5185\u5377\u5316\u3002<\/p>\n<p><span style=\"color: #ff0000;\"><strong>\u3010\u603b\u7ed3\u3011<\/strong><\/span><\/p>\n<p>\u8be5\u7814\u7a76\u5c0f\u7ec4\u5c06\u4ece\u5934\u8ba1\u7b97\u65b9\u6cd5\u4e0e\u5b9e\u9a8c\u76f8\u7ed3\u5408\uff0c\u7814\u7a76\u4e86\u5982\u4f55\u8c03\u8282NMC\u6750\u6599\u7684\u70ed\u7a33\u5b9a\u6027\u3002\u7814\u7a76\u4eba\u5458\u5c06\u8be5\u6750\u6599\u5206\u4e3a\u4e24\u7ec4\uff1a\u201c\u5bcc\u954d\u201d\u7ec4\uff08\u6df7\u5408\u4ef7\u6001\u7684Ni<sup>2+<\/sup>\/Ni<sup>3+<\/sup>\uff09\u548c\u201cNi=Mn\u201d\u7ec4\uff08\u53ea\u6709Ni<sup>2+<\/sup>\u7684\u72b6\u6001\uff09\u3002\u7814\u7a76\u53d1\u73b0\uff0c\u6750\u6599\u70ed\u7a33\u5b9a\u6027\u4e0e\u6700\u4e0d\u7a33\u5b9a\u7684\u6c27\u5bc6\u5207\u76f8\u5173\uff0c\u8fd9\u662f\u7531\u5c40\u90e8\u642d\u914d\u7ed3\u6784\u5355\u5143\uff08LCSU\uff09\uff1aTM(Ni, Mn, Co)<sub>3<\/sub>-O-Li<sub>3\u2013<em>x<\/em><\/sub><sub>\u2032<\/sub>\u00a0(<em>x<\/em>\u2032= 0-3)\u6240\u51b3\u5b9a\u7684\u3002\u9502\u7684\u542b\u91cf\uff0c\u954d\u7684\u4ef7\u6001\uff0cNi\u3001Mn\u3001Co\u7684\u542b\u91cf\u4ee5\u53caNi\/Li\u7684\u6df7\u6392\u90fd\u53ef\u4ee5\u5f71\u54cdNMC\u6750\u6599\u7684\u70ed\u7a33\u5b9a\u6027\u3002\u5728\u8fd9\u9879\u5de5\u4f5c\u4e2d\u7684\u7406\u8bba\u8ba1\u7b97\u7ed3\u679c\u4e0e\u5b9e\u9a8c\u7ed3\u679c\u76f8\u4e00\u81f4\uff0c\u8fd9\u4e00\u7b80\u5355\u6a21\u578b\u4e0d\u4ec5\u8003\u8651\u4e86\u6240\u6709\u7684\u5f71\u54cd\u56e0\u7d20\uff0c\u4e5f\u4ece\u539f\u5b50\u7684\u6c34\u5e73\u4e3aNMC\u6750\u6599\u70ed\u7a33\u5b9a\u6027\u63d0\u4f9b\u4e86\u7684\u4e00\u4e2a\u7b80\u5355\u4e14\u76f4\u63a5\u7684\u89e3\u91ca\uff0c\u8fd9\u5bf9\u4e8e\u672a\u6765NMC\u6750\u6599\u7684\u5b9e\u9a8c\u7814\u7a76\u5177\u6709\u6307\u5bfc\u6027\u610f\u4e49\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a<\/strong><a href=\"http:\/\/xueshu.baidu.com\/s?wd=paperuri%3A%28379d4ca2f7e3985b32480f69ecc0ed04%29&amp;filter=sc_long_sign&amp;tn=SE_xueshusource_2kduw22v&amp;sc_vurl=http%3A%2F%2Fpubs.acs.org%2Fdoi%2Fabs%2F10.1021%2Fjacs.6b07771&amp;ie=utf-8&amp;sc_us=16286691280704637680\" target=\"_blank\">Tuning of Thermal Stability in Layered Li(Ni<sub>x<\/sub>Mn<sub>y<\/sub>Co<sub>z<\/sub>)O<sub>2<\/sub><\/a>\u00a0\uff08J. Am. Chem. Soc.\uff0c2016\uff0cDOI: 10.1021\/jacs. 6b07771\uff09<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u65b0\u80fd\u6e90\u5b66\u672f\u7ec4\u80cc\u9006\u65f6\u5149\u4f9b\u7a3f\uff0c\u70b9<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\">\u8fd9\u91cc\u52a0\u5165\u6750\u6599\u4eba\u7684\u5927\u5bb6\u5ead<\/a>\u3002<\/p>\n<p>\u53c2\u4e0e\u65b0\u80fd\u6e90\u8bdd\u9898\u8ba8\u8bba\u8bf7\u52a0\u5165\u201c\u6750\u6599\u4eba\u65b0\u80fd\u6e90\u6750\u6599\u4ea4\u6d41\u7fa4 422065952\u201d\uff0c\u82e5\u60f3\u53c2\u4e0e\u65b0\u80fd\u6e90\u6587\u732e\u89e3\u8bfb\u548c\u6587\u732e\u6c47\u603b\u3001\u65b0\u80fd\u6e90\u77e5\u8bc6\u79d1\u666e\u548c\u6df1\u5ea6\u6316\u6398\u65b0\u80fd\u6e90\u5b66\u672f\u4ea7\u4e1a\u4fe1\u606f\uff0c\u8bf7\u52a0qq 2728811768\u3002\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002\u6b22\u8fce\u5173\u6ce8\u5fae\u4fe1\u516c\u4f17\u53f7\uff0c\u5fae\u4fe1\u641c\u7d22\u201c\u65b0\u80fd\u6e90\u524d\u7ebf\u201d\u6216\u626b\u7801\u5173\u6ce8\u3002<img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-medium wp-image-37388 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/\u65b0\u80fd\u6e90\u524d\u7ebf-1-1-1-300x300.jpg\" alt=\"\u65b0\u80fd\u6e90\u524d\u7ebf-1-1\" width=\"300\" height=\"300\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/\u65b0\u80fd\u6e90\u524d\u7ebf-1-1-1-300x300.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/\u65b0\u80fd\u6e90\u524d\u7ebf-1-1-1-150x150.jpg 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/08\/\u65b0\u80fd\u6e90\u524d\u7ebf-1-1-1.jpg 340w\" sizes=\"(max-width: 300px) 100vw, 300px\" \/><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8bed\u3011 \u53ef\u5145\u7535\u9502\u79bb\u5b50\u7535\u6c60\uff08LIBs\uff09\u88ab\u5e7f\u6cdb\u8fd0\u7528\u5728\u73b0\u4eca\u5927\u591a\u6570\u7684\u4fbf\u643a\u5f0f\u7535\u5b50\u4ea7\u54c1\u4e2d\uff0c\u4ee5\u53ca\u88ab\u8d8a\u6765\u8d8a\u591a\u7684\u7535\u52a8\u6c7d\u8f66\uff08EV\uff09\u548c\u7535\u7ad9\u5b58\u50a8\u6240\u9700\u6c42\u3002\u5728\u8fd9\u79cd\u53d1\u5c55\u8d8b\u52bf\u4e4b\u4e0b\uff0c\u6211\u4eec\u4e3b\u8981\u5173&#8230;<\/p>\n","protected":false},"author":272,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[129],"class_list":["post-46756","post","type-post","status-publish","format-standard","hentry","category-jiedu","tag-battery"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/46756"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/272"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=46756"}],"version-history":[{"count":8,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/46756\/revisions"}],"predecessor-version":[{"id":47207,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/46756\/revisions\/47207"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=46756"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=46756"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=46756"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}