{"id":50254,"date":"2016-11-07T06:30:30","date_gmt":"2016-11-06T22:30:30","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=50254"},"modified":"2016-11-06T21:05:17","modified_gmt":"2016-11-06T13:05:17","slug":"adv-mater%ef%bc%9afe-cop%e7%ba%b3%e7%b1%b3%e9%98%b5%e5%88%97-%e5%8d%95%e7%89%87%e5%a4%9a%e5%8a%9f%e8%83%bd%e9%ab%98%e6%95%88%e4%ba%a7%e6%b0%a2%e5%82%ac%e5%8c%96%e5%89%82","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=50254","title":{"rendered":"Adv. Mater\uff1aFe-CoP\u7eb3\u7c73\u9635\u5217-\u5355\u7247\u591a\u529f\u80fd\u9ad8\u6548\u4ea7\u6c22\u50ac\u5316\u5242"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u7535\u89e3\u6c34\u53cd\u5e94\u73b0\u5728\u5173\u6ce8\u5ea6\u6301\u7eed\u5347\u6e29\uff0c\u6790\u6c27\uff08OER\uff09\u53cd\u5e94\u548c\u6790\u6c22\uff08HER\uff09\u53cd\u5e94\uff0c\u662f\u7535\u89e3\u6c34\u4e2d\u4e24\u4e2a\u534a\u53cd\u5e94\u3002\u8d77\u59cb\u8fc7\u7535\u4f4d\uff08<em>\u03b7<\/em>\uff09\uff0c\u5854\u83f2\u5c14\u659c\u7387\uff08Tafel slope\uff09\u4e3a\u4e3b\u8981\u53c2\u6570\u3002\u76ee\u524d\u5df2\u88ab\u62a5\u9053\u7684Co-P\u53cc\u529f\u80fd\u50ac\u5316\u5242\u663e\u793a\u51fa\u8f83\u597d\u7684\u50ac\u5316\u6d3b\u6027<a href=\"http:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/anie.201501616\/abstract\"><sup>1<\/sup><\/a>\uff0c\u4f46\u5173\u4e8eNaBH<sub>4<\/sub>\u5206\u89e3\u4ea7\u6c22\u5374\u672a\u66fe\u7814\u7a76\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u6b64\u524d\uff0c\u787c\u6c22\u5316\u94a0\u4ea7\u6c22\u7684\u50ac\u5316\u5242\u4e3b\u8981\u96c6\u4e2d\u5728Co-B<a href=\"http:\/\/www.sciencedirect.com\/science\/article\/pii\/S0360319907003722\"><sup>2<\/sup><\/a><sup>, <\/sup><a href=\"http:\/\/www.sciencedirect.com\/science\/article\/pii\/S0378775307024500\"><sup>3<\/sup><\/a>\uff08ESI\u9ad8\u88ab\u5f15\u8bba\u6587\uff09\uff0cCo-P-B<sup><a href=\"http:\/\/www.sciencedirect.com\/science\/article\/pii\/S0378775308023070\">4<\/a><\/sup>\uff08ESI\u9ad8\u88ab\u5f15\u8bba\u6587\uff09\u548cNi-Co-B<a href=\"http:\/\/www.sciencedirect.com\/science\/article\/pii\/S0378775307008166\"><sup>5<\/sup><\/a>\uff08ESI\u9ad8\u88ab\u5f15\u8bba\u6587\uff09\u7b49\u975e\u8d35\u91d1\u5c5e\u50ac\u5316\u5242\u4e0a\uff1b\u94c2\u7cfb\u50ac\u5316\u5242\u96c6\u4e2d\u5728Pt\/CeO<sub>2<\/sub><a href=\"http:\/\/pubs.acs.org\/doi\/abs\/10.1021\/ja4069134\"><sup>6<\/sup><\/a>\uff08ESI\u9ad8\u88ab\u5f15\u8bba\u6587\uff09\u548cRu\/Pd<a href=\"http:\/\/www.sciencedirect.com\/science\/article\/pii\/S0360319909009446\"><sup>7<\/sup><\/a>\uff08ESI\u9ad8\u88ab\u5f15\u8bba\u6587\uff09\u3002<\/p>\n<p>10\u670831\u65e5\uff0cAdvanced Materials\u5728\u7ebf\u53d1<strong>\u8868\u56db\u5ddd\u5927\u5b66\u5316\u5de5\u5b66\u9662\u5b59\u65ed\u5e73\u6559\u6388\u8bfe\u9898\u7ec4<\/strong>\uff0c\u9898\u4e3a\u201cFe-CoP\u7eb3\u7c73\u9635\u5217\uff1a\u5355\u7247\u591a\u529f\u80fd\u9ad8\u6548\u4ea7\u6c22\u50ac\u5316\u5242\u201d\uff08Fe-Doped CoP Nanoarray: A Monolithic Multifunctional Catalyst for Highly Efficient Hydrogen Generation\uff09\u7684\u7814\u7a76\u8bba\u6587<a href=\"http:\/\/onlinelibrary.wiley.com\/wol1\/doi\/10.1002\/adma.201602441\/abstract\"><sup>8<\/sup><\/a>\u3002\u672c\u6587\u4eae\u70b9\uff1a\u5728\u78b1\u6027\u6761\u4ef6\u4e0b\uff0cFe\u63ba\u6742Co-P\u50ac\u5316\u5242\u53ef\u5e94\u7528\u4e8eHER\uff0cOER\u548cNaBH<sub>4<\/sub>\u5206\u89e3\u4ea7\u6c22\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe1.Fe\u63ba\u6742Co-P\u50ac\u5316\u5242\u7684\u6c34\u89e3\u4ea7\u6c22\u901f\u7387\u5feb\uff0c\u6d3b\u5316\u80fd\u4e3a43.4kJ\/mol\uff0c\u7ecf\u8fc75\u6b21\u5faa\u73af\u6d4b\u8bd5\u65e0\u660e\u663e\u8870\u51cf<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-50255 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/\u56fe\u72471-2.jpg\" alt=\"\u56fe\u72471\" width=\"650\" height=\"509\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/\u56fe\u72471-2.jpg 650w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/\u56fe\u72471-2-300x235.jpg 300w\" sizes=\"(max-width: 650px) 100vw, 650px\" \/><\/p>\n<p>a\uff09Ti\u7b94\uff08\u5de6\uff09\u548cFe-CoP\/Ti\uff08\u53f3\uff09\u4e0a\u50ac\u5316\u7684NaBH<sub>4<\/sub>\u6c34\u89e3\u7684\u5149\u5b66\u7167\u7247\u3002<\/p>\n<p>b\uff09\u5728\u4e0d\u540cNaBH<sub>4<\/sub>\u6d53\u5ea6\u4e0bFe-CoP\/Ti\u50ac\u5316\u7684NaBH<sub>4<\/sub>\u6c34\u89e3\uff081wt\uff05NaOH\uff09\u4ea7\u6c14\u4f53\u79ef\u56fe(1.03mg Fe-CoP\uff0c25\u2103)\u3002<\/p>\n<p>c\uff09\u57283mL\u6eb6\u6db2\uff081wt\uff05NaBH<sub>4<\/sub>\u548c1wt\uff05NaOH\uff09\u4e0b\u5728\u4e0d\u540c\u6e29\u5ea6\u4e0b\uff0cFe-CoP\/Ti\u50ac\u5316\u7684NaBH<sub>4<\/sub>\u6c34\u89e3\u7684\u6c22\u6c14\u4f53\u79ef\u5bf9\u65f6\u95f4\u7684\u56fe\uff08\u63d2\u56fe\uff1a\u76f8\u5e94\u7684Arrhenius\u56fe\uff09\u3002<\/p>\n<p>d\uff09\u57283mL\u53cd\u5e94\u6eb6\u6db2(1wt\uff05NaBH<sub>4<\/sub>\u4e0e1wt\uff05NaOH)\u4e2d\uff0cFe-CoP\/Ti\u6c34\u89e3NaBH<sub>4<\/sub>\u7684\u53ef\u91cd\u590d\u6027\u3002<\/p>\n<p><strong>\u56fe2. HER\u8fc7\u7535\u4f4d78 mV\uff0810 mA cm<sup>\u22122<\/sup>\uff09\u63a5\u8fd1Pt\/C\uff0cOER\u8fc7\u7535\u4f4d230 mV\uff0810 mA cm<sup>\u22122<\/sup>\uff09\u4f18\u4e8eRuO<sub>2<\/sub>\u3002<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-50260 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/\u56fe\u72472-1.jpg\" alt=\"\u56fe\u72472\" width=\"680\" height=\"505\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/\u56fe\u72472-1.jpg 680w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/\u56fe\u72472-1-300x223.jpg 300w\" sizes=\"(max-width: 680px) 100vw, 680px\" \/><\/p>\n<p>\uff08a\uff09HER\u7ebf\u6027\u626b\u63cf\u4f0f\u5b89\u66f2\u7ebf \u00a0 \u00a0 \u00a0\uff08b\uff09HER\u5bf9\u5e94\u7684\u5854\u83f2\u5c14\u659c\u7387\uff1b<\/p>\n<p>\uff08c\uff09OER\u7ebf\u6027\u626b\u63cf\u4f0f\u5b89\u66f2\u7ebf \u00a0 \u00a0 \uff08d\uff09OER\u5bf9\u5e94\u7684\u5854\u83f2\u5c14\u659c\u7387\u3002<\/p>\n<p><strong>\u56fe3. Fe\u63ba\u6742Co-P\u7eb3\u7c73\u9635\u5217\u8868\u5f81<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-50261 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/\u56fe\u72473-1.jpg\" alt=\"\u56fe\u72473\" width=\"680\" height=\"761\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/\u56fe\u72473-1.jpg 680w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/\u56fe\u72473-1-268x300.jpg 268w\" sizes=\"(max-width: 680px) 100vw, 680px\" \/><\/p>\n<p>\u9488\u72b6\u5f62\u8c8c\u4e3aCo-P\u7eb3\u7c73\u7ebf\uff0c\u5143\u7d20Mapping\u56fe\u663e\u793aFe\u5747\u5300\u63ba\u6742\u5728\u7eb3\u7c73\u7ebf\u8868\u9762\uff0cFe-CoP\u7684XPS\u8c31\uff0c\u5728712.5\u548c725.3 eV\u5904\u4e24\u4e2a\u5cf0\uff0c\u5206\u522b\u5bf9\u5e94Fe2p<sub>3\/2<\/sub>\u548cFe2p<sub>1\/2<\/sub>\u7684\u7ed3\u5408\u80fd\u4f4d\u7f6e\uff0c\u8bc1\u5b9eFe<sup>3+<\/sup>\u7684\u5b58\u5728\u3002<\/p>\n<p>\u56fe3 Fe\u63ba\u6742Co-P\u7eb3\u7c73\u9635\u5217\u7684\uff08a\uff09SEM\u56fe\uff0c\uff08b\uff09\u5c40\u90e8\u653e\u5927SEM\u56fe\u50cf\uff0c\uff08c\uff09\u5143\u7d20Mapping\u5206\u6790\u4ee5\u53ca\uff08d\uff09XPS\u56fe\u8c31\u3002<\/p>\n<p><strong>\u3010\u5c55\u671b\u3011<\/strong><\/p>\n<p>\u8fd9\u9879\u7814\u7a76\u5728\u8bbe\u8ba1\u4e09\u5143\u6216\u63ba\u6742\u8fc7\u6e21\u91d1\u5c5e\u78f7\u5316\u7269\u7eb3\u7c73\u9635\u5217\u4f5c\u4e3a\u6210\u672c\u4f4e\u3001\u9ad8\u6548\u3001\u575a\u56fa\u7684\u591a\u529f\u80fd\u6750\u6599\u7684\u5e94\u7528\u65b9\u9762\u5177\u6709\u53c2\u8003\u610f\u4e49\u3002\u5229\u7528\u5728Ti\u7b94\u4e0a\u751f\u957f\u7684Fe-CoP\u7eb3\u7c73\u9635\u5217\u50ac\u5316\u5242\u663e\u793a\u4f18\u826f\u7684\u7535\u5316\u5b66\u6c34\u5206\u89e3\u7684\u50ac\u5316\u6027\u80fd\uff0c\u5728\u78b1\u6027\u6761\u4ef6\u4e0bNaBH<sub>4<\/sub>\u7684\u6c34\u89e3\u8131\u6c22\u4e5f\u5448\u73b0\u4e86\u8f83\u4f4e\u7684\u6d3b\u5316\u80fd\uff0839.6 kJ mol<sup>-1<\/sup>\uff09\u3002<\/p>\n<p><strong>\u539f\u6587\u94fe\u63a5<\/strong>\uff1a<a href=\"http:\/\/onlinelibrary.wiley.com\/wol1\/doi\/10.1002\/adma.201602441\/abstract\">Fe-Doped CoP Nanoarray: A Monolithic Multifunctional<\/a>\u00a0<a href=\"http:\/\/onlinelibrary.wiley.com\/wol1\/doi\/10.1002\/adma.201602441\/abstract\" target=\"_blank\">Catalyst for Highly Efficient Hydrogen Generation<\/a>\u00a0\u00a0(Adv. Mater.\uff0c2016\uff0cDOI:10.1002\/adma.201602441)<\/p>\n<p><strong>\u3010\u5b59\u65ed\u5e73\u6559\u6388\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u5b59\u65ed\u5e73\u6559\u6388\uff0c1997\u5e74\u672c\u79d1\u6bd5\u4e1a\u4e8e\u897f\u534e\u5e08\u8303\u5927\u5b66\u5316\u5b66\u5316\u5de5\u5b66\u9662\uff0c2005\u5e74\u4e8e\u4e2d\u79d1\u9662\u957f\u6625\u5e94\u5316\u6240\u83b7\u5206\u6790\u5316\u5b66\u535a\u58eb\u5b66\u4f4d\uff0c2008\u5e74\u83b7\u5168\u56fd\u767e\u7bc7\u4f18\u79c0\u535a\u58eb\u8bba\u6587\u30022006-2009\u5e74\u5148\u540e\u5728\u5fb7\u56fd\u5eb7\u65af\u5766\u8328\u5927\u5b66\u3001\u52a0\u62ff\u5927\u591a\u4f26\u591a\u5927\u5b66\u53ca\u7f8e\u56fd\u666e\u6e21\u5927\u5b66\u4ece\u4e8b\u535a\u58eb\u540e\u7814\u7a76\u5de5\u4f5c\uff0c2010\u5e741\u6708\u8058\u4e3a\u957f\u6625\u5e94\u5316\u6240\u7814\u7a76\u5458\uff0c2011\u5e74\u8058\u4e3a\u6c99\u7279\u56fd\u738b\u5927\u5b66\u517c\u804c\u6559\u6388\uff0c2015\u5e7410\u6708\u4ece\u5e94\u5316\u6240\u5168\u804c\u5f15\u5165\u56db\u5ddd\u5927\u5b66\u3002\u76ee\u524d\uff0c\u5df2\u5728J. Am. Chem. Soc.\u3001Angew. Chem.\u3001Adv. Mater.\u3001Nucleic Acids Res.\u3001Chem. Mater.\u3001ACS Catal.\u3001ChemSusChem\u3001Anal. Chem.\u7b49\u520a\u7269\u53d1\u8868\u7814\u7a76\u8bba\u6587260\u4f59\u7bc7\uff0c22\u7bc7\u8bba\u6587\u5165\u9009ESI\u6570\u636e\u5e93\u9ad8\u88ab\u5f15\u8bba\u6587\uff0c5\u7bc7\u8bba\u6587\u5165\u9009ESI\u6570\u636e\u5e93\u70ed\u70b9\u8bba\u6587\uff0c2\u7bc7\u8bba\u6587\u5165\u90092014\u5e74\u4e2d\u56fd\u767e\u7bc7\u6700\u5177\u5f71\u54cd\u56fd\u9645\u5b66\u672f\u8bba\u6587\uff1b\u8bba\u6587\u4ed6\u5f156000\u4f59\u6b21\uff0cH-index 49\u3002<\/p>\n<p><strong>\u53c2\u8003\u6587\u732e\uff1a<\/strong><\/p>\n<ol>\n<li>Jiang N, You B, Sheng M, Sun Y. Electrodeposited Cobalt-Phosphorous-Derived Films as Competent Bifunctional Catalysts for Overall Water Splitting. <em>Angewandte Chemie International Edition<\/em> 2015, <strong>54<\/strong>(21)<strong>:<\/strong> 6251-6254.\u88ab\u5f15\u9891\u6b21: <a title=\"\u67e5\u770b\u5f15\u7528\u672c\u6587\u7684\u6240\u6709\u6587\u732e\" href=\"http:\/\/apps.webofknowledge.com\/CitingArticles.do?product=WOS&amp;SID=V2pnKECzabR2zx8BgPn&amp;search_mode=CitingArticles&amp;parentProduct=WOS&amp;parentQid=7&amp;parentDoc=1&amp;REFID=486946749&amp;excludeEventConfig=ExcludeIfFromNonInterProduct\">88<\/a><\/li>\n<\/ol>\n<ol start=\"2\">\n<li>Zhao J, Ma H, Chen J. <a href=\"http:\/\/www.sciencedirect.com\/science\/article\/pii\/S0360319907003722\" target=\"_blank\">Improved hydrogen generation from alkaline solution using carbon-supported as catalysts<\/a>. <em>International Journal of Hydrogen Energy<\/em> 2007, <strong>32<\/strong>(18)<strong>:<\/strong> 4711-4716. \u88ab\u5f15\u9891\u6b21: 117<\/li>\n<\/ol>\n<ol start=\"3\">\n<li>Dai H-B, Liang Y, Wang P, Cheng H-M. <a href=\"http:\/\/www.sciencedirect.com\/science\/article\/pii\/S0378775307024500\" target=\"_blank\">Amorphous cobalt\u2013boron\/nickel foam as an effective catalyst for hydrogen generation from alkaline sodium borohydride solution<\/a>. <em>Journal of Power Sources<\/em> 2008, <strong>177<\/strong>(1)<strong>:<\/strong> 17-23. \u88ab\u5f15\u9891\u6b21: 117<\/li>\n<\/ol>\n<ol start=\"4\">\n<li>Patel N, Fernandes R, Miotello A. <a href=\"http:\/\/www.sciencedirect.com\/science\/article\/pii\/S0378775308023070\" target=\"_blank\">Hydrogen generation by hydrolysis of NaBH4 with efficient Co-P-B catalyst: A kinetic study<\/a>. <em>Journal of Power Sources<\/em> 2009, <strong>188<\/strong>(2)<strong>:<\/strong> 411-420.\u88ab\u5f15\u9891\u6b21: <a title=\"\u67e5\u770b\u5f15\u7528\u672c\u6587\u7684\u6240\u6709\u6587\u732e\" href=\"http:\/\/apps.webofknowledge.com\/CitingArticles.do?product=WOS&amp;SID=V2pnKECzabR2zx8BgPn&amp;search_mode=CitingArticles&amp;parentProduct=WOS&amp;parentQid=1&amp;parentDoc=1&amp;REFID=265249788&amp;excludeEventConfig=ExcludeIfFromNonInterProduct\">93<\/a><\/li>\n<\/ol>\n<ol start=\"5\">\n<li>Ingersoll JC, Mani N, Thenmozhiyal JC, Muthaiah A. <a href=\"http:\/\/www.sciencedirect.com\/science\/article\/pii\/S0378775307008166\" target=\"_blank\">Catalytic hydrolysis of sodium borohydride by a novel nickel\u2013cobalt\u2013boride catalyst<\/a>. <em>Journal of Power Sources<\/em> 2007, <strong>173<\/strong>(1)<strong>:<\/strong> 450-457.\u88ab\u5f15\u9891\u6b21: <a title=\"\u67e5\u770b\u5f15\u7528\u672c\u6587\u7684\u6240\u6709\u6587\u732e\" href=\"http:\/\/apps.webofknowledge.com\/CitingArticles.do?product=WOS&amp;SID=V2pnKECzabR2zx8BgPn&amp;search_mode=CitingArticles&amp;parentProduct=WOS&amp;parentQid=2&amp;parentDoc=3&amp;REFID=80100007&amp;excludeEventConfig=ExcludeIfFromNonInterProduct\">139<\/a><\/li>\n<\/ol>\n<ol start=\"6\">\n<li>Wang X, Liu DP, Song SY, Zhang HJ. <a href=\"http:\/\/pubs.acs.org\/doi\/abs\/10.1021\/ja4069134\" target=\"_blank\">Pt@CeO2 Multicore@Shell Self-Assembled Nanospheres: Clean Synthesis, Structure Optimization, and Catalytic Applications<\/a>. <em>Journal of the American Chemical Society<\/em> 2013, <strong>135<\/strong>(42)<strong>:<\/strong> 15864-15872.\u88ab\u5f15\u9891\u6b21: <a title=\"\u67e5\u770b\u5f15\u7528\u672c\u6587\u7684\u6240\u6709\u6587\u732e\" href=\"http:\/\/apps.webofknowledge.com\/CitingArticles.do?product=WOS&amp;SID=V2pnKECzabR2zx8BgPn&amp;search_mode=CitingArticles&amp;parentProduct=WOS&amp;parentQid=5&amp;parentDoc=1&amp;REFID=460123425&amp;excludeEventConfig=ExcludeIfFromNonInterProduct\">106<\/a><\/li>\n<\/ol>\n<ol start=\"7\">\n<li>Metin O, Sahin S, Ozkar S. <a href=\"http:\/\/www.cailiaoniu.com\/50010.html\" target=\"_blank\">Water-soluble poly(4-styrenesulfonic acid-co-maleic acid) stabilized ruthenium(0) and palladium(0) nanoclusters as highly active catalysts in hydrogen generation from the hydrolysis of ammonia-borane<\/a>. <em>International Journal of Hydrogen Energy<\/em> 2009, <strong>34<\/strong>(15)<strong>:<\/strong> 6304-6313.\u88ab\u5f15\u9891\u6b21: <a title=\"\u67e5\u770b\u5f15\u7528\u672c\u6587\u7684\u6240\u6709\u6587\u732e\" href=\"http:\/\/apps.webofknowledge.com\/CitingArticles.do?product=WOS&amp;SID=V2pnKECzabR2zx8BgPn&amp;search_mode=CitingArticles&amp;parentProduct=WOS&amp;parentQid=6&amp;parentDoc=1&amp;REFID=274161387&amp;excludeEventConfig=ExcludeIfFromNonInterProduct\" target=\"_blank\">135<\/a><\/li>\n<\/ol>\n<ol start=\"8\">\n<li>Tang C, Zhang R, Lu W, He L, Jiang X, Asiri AM<em>, et al.<\/em> <a href=\"http:\/\/onlinelibrary.wiley.com\/wol1\/doi\/10.1002\/adma.201602441\/abstract\" target=\"_blank\">Fe-Doped CoP Nanoarray: A Monolithic Multifunctional Catalyst for Highly Efficient Hydrogen Generation<\/a>. <em>Advanced Materials<\/em><strong>:<\/strong> <strong>2016,<\/strong> DOI: 10.1002\/adma.201602441.<\/li>\n<\/ol>\n<p>&nbsp;<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u65b0\u80fd\u6e90\u5b66\u672f\u7ec4 pamperhey \u6574\u7406\u3002<\/p>\n<p>\u6750\u6599\u725b\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u8fd9\u91cc\u6c47\u96c6\u4e86\u5404\u5927\u9ad8\u6821\u7855\u535a\u751f\u3001\u4e00\u7ebf\u79d1\u7814\u4eba\u5458\u4ee5\u53ca\u884c\u4e1a\u4ece\u4e1a\u8005\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\">\u70b9\u6211\u52a0\u5165\u6750\u6599\u4eba\u7f16\u8f91\u90e8<\/a>\u3002<\/p>\n<p>\u53c2\u4e0e\u65b0\u80fd\u6e90\u8bdd\u9898\u8ba8\u8bba\u8bf7\u52a0\u5165\u201c\u6750\u6599\u4eba\u65b0\u80fd\u6e90\u6750\u6599\u4ea4\u6d41\u7fa4 422065952\u201d\u3002\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002\u6b22\u8fce\u5173\u6ce8\u5fae\u4fe1\u516c\u4f17\u53f7\uff0c\u5fae\u4fe1\u641c\u7d22\u201c\u65b0\u80fd\u6e90\u524d\u7ebf\u201d\u6216\u626b\u7801\u5173\u6ce8\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-48816 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/10\/\u65b0\u80fd\u6e90\u524d\u7ebf-\u9ad8\u6e05.jpg\" alt=\"\u65b0\u80fd\u6e90\u524d\u7ebf-\u9ad8\u6e05\" width=\"340\" height=\"340\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/10\/\u65b0\u80fd\u6e90\u524d\u7ebf-\u9ad8\u6e05.jpg 340w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/10\/\u65b0\u80fd\u6e90\u524d\u7ebf-\u9ad8\u6e05-150x150.jpg 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/10\/\u65b0\u80fd\u6e90\u524d\u7ebf-\u9ad8\u6e05-300x300.jpg 300w\" sizes=\"(max-width: 340px) 100vw, 340px\" \/><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u7535\u89e3\u6c34\u53cd\u5e94\u73b0\u5728\u5173\u6ce8\u5ea6\u6301\u7eed\u5347\u6e29\uff0c\u6790\u6c27\uff08OER\uff09\u53cd\u5e94\u548c\u6790\u6c22\uff08HER\uff09\u53cd\u5e94\uff0c\u662f\u7535\u89e3\u6c34\u4e2d\u4e24\u4e2a\u534a\u53cd\u5e94\u3002\u8d77\u59cb\u8fc7\u7535\u4f4d\uff08\u03b7\uff09\uff0c\u5854\u83f2\u5c14\u659c\u7387\uff08Tafel slope\uff09\u4e3a\u4e3b&#8230;<\/p>\n","protected":false},"author":1311,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[81],"class_list":["post-50254","post","type-post","status-publish","format-standard","hentry","category-jiedu","tag-clearenergy"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/50254"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/1311"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=50254"}],"version-history":[{"count":10,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/50254\/revisions"}],"predecessor-version":[{"id":50497,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/50254\/revisions\/50497"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=50254"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=50254"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=50254"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}