{"id":50387,"date":"2016-11-08T06:30:36","date_gmt":"2016-11-07T22:30:36","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=50387"},"modified":"2017-03-18T21:54:29","modified_gmt":"2017-03-18T13:54:29","slug":"adv-energy-mater-%ef%bc%9acufes2%e4%b8%adzn%e5%a4%a7%e6%94%be%e5%bc%82%e5%bd%a9%ef%bc%8c%e5%8f%af%e6%8f%90%e9%ab%98cu1-xznxfes2%e7%83%ad%e7%94%b5%e7%89%b9%e6%80%a7","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=50387","title":{"rendered":"Adv. Energy Mater.\uff1aCuFeS2\u4e2dZn\u5927\u653e\u5f02\u5f69\uff0c\u53ef\u63d0\u9ad8Cu1\u2013xZnxFeS2\u70ed\u7535\u7279\u6027"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u6709\u6548\u89e3\u51b3\u4f59\u70ed\u6216\u662f\u5408\u7406\u5229\u7528\u80fd\u6e90\u65b9\u9762\uff0c\u70ed\u7535\u6750\u6599\u662f\u524d\u666f\u975e\u5e38\u53ef\u89c2\u7684\u6750\u6599\u3002\u7ec6\u6570\u8fd1\u6bb5\u65f6\u95f4\u5bf9\u4e8e\u70ed\u7535\u6750\u6599\u7684\u76f8\u5173\u6587\u732e\u62a5\u9053\uff0c\u53ef\u77e5\u8d8a\u6765\u8d8a\u591a\u7684\u7814\u7a76\u8005\u5f00\u59cb\u6d89\u53ca\u8fd9\u4e00\u9886\u57df\uff0c\u4ee5\u7814\u53d1\u51fa\u66f4\u4e3a\u9ad8\u70ed\u7535\u7279\u6027\u7684\u6750\u6599\uff0c\u70ed\u7535\u7279\u6027\u53ef\u7528ZT\uff08ZT = \u03b1<sup>2<\/sup>\u03c3T\/(\u03ba<sub>e<\/sub> + \u03ba<sub>L<\/sub>)\uff0c\u03b1-\u8d5b\u8d1d\u514b\u7cfb\u6570\uff0c\u03c3-\u7535\u5bfc\u7387\uff0c\u03ba<sub>e<\/sub>\u548c\u03ba<sub>L<\/sub>\u5206\u522b\u4e3a\u7535\u5b50\u548c\u6676\u683c\u70ed\u5bfc\u7387\uff09\u503c\u6765\u5224\u5b9a\u3002\u4eceZT\u516c\u5f0f\u53ef\u77e5\uff0c\u4f18\u5f02\u7684\u70ed\u7535\u6750\u6599\u9700\u8981\u5177\u5907\u9ad8\u8d5b\u8d1d\u514b\u7cfb\u6570\u3001\u9ad8\u7535\u5bfc\u7387\uff0c\u800c\u7535\u5b50\u548c\u6676\u683c\u7684\u70ed\u5bfc\u7387\u5219\u8981\u4f4e\u3002\u76ee\u524d\uff0c\u70ed\u7535\u6750\u6599\u96c6\u4e2d\u4e8eBi<sub>2<\/sub>Te<sub>3<\/sub>\u57fa\u6216PbTe\u57fa\u6750\u6599\uff0c\u4f46\u8fd9\u7c7b\u6750\u6599\u542b\u6709\u6709\u6bd2\u5143\u7d20\uff08Pb\uff09\u548c\u8d35\u5143\u7d20\uff08Te\uff09\u3002\u56e0\u6b64\uff0c\u9700\u8981\u8fdb\u4e00\u6b65\u52a0\u5f3a\u7814\u7a76\uff0c\u4ee5\u7814\u53d1\u51fa\u4e00\u4e9b\u65b0\u578b\u9ad8\u6548\u3001\u5ec9\u4ef7\u4e14\u73af\u5883\u53cb\u597d\u578b\u70ed\u7535\u6750\u6599\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u9ec4\u94dc\u77ff\uff08CuFeS<sub>2<\/sub>\uff09\u662f\u4e00\u79cd\u5e7f\u6cdb\u4f7f\u7528\u7684\u5929\u7136\u77ff\u7269\uff0c\u7ec4\u6210\u7684\u5143\u7d20\u4e0d\u4ec5\u6ca1\u6709\u6bd2\u6027\uff0c\u540c\u65f6\u5730\u7403\u5bcc\u542b\u91cf\u4e5f\u975e\u5e38\u9ad8\u3002\u56e0\u6b64\uff0cCuFeS<sub>2<\/sub>\u4e5f\u88ab\u8ba4\u4e3a\u662f\u4e00\u79cd\u5728\u70ed\u7535\u9886\u57df\u6bd4\u8f83\u5177\u6709\u53d1\u5c55\u524d\u666f\u7684n\u578b\u6750\u6599\u3002<strong>\u6b66\u6c49\u7406\u5de5\u5927\u5b66\u7684\u5510\u65b0\u5cf0\u548c\u82cf\u8d24\u793c\uff08\u5171\u540c\u901a\u8baf\u4f5c\u8005\uff09<\/strong>\u7b49\u4eba\u901a\u8fc7\u5c06\u771f\u7a7a\u7194\u878d\u548c\u7b49\u79bb\u5b50\u4f53\u6d3b\u5316\u70e7\u7ed3\uff08PAS\uff09\u76f8\u7ed3\u5408\u5408\u6210\u4e86\u4e00\u7cfb\u5217\u5177\u4e0d\u540cZn\u63ba\u6742\u91cf\u7684Cu<sub>1\u2013x<\/sub>Zn<sub>x<\/sub>FeS<sub>2<\/sub>\u6750\u6599\uff0c\u6765\u5206\u6790Zn\u5728\u6676\u683c\u4e2d\u7684\u6d53\u5ea6\u53ca\u4f4d\u7f6e\u5bf9CuFeS<sub>2<\/sub>\u70ed\u7535\u7279\u6027\u7684\u5f71\u54cd\u3002<\/p>\n<p>\u7814\u7a76\u8868\u660e\uff0cZn\u5728\u63d0\u9ad8\u6750\u6599\u8f7d\u6d41\u5b50\u6d53\u5ea6\u53caCuFeS<sub>2<\/sub>\u70ed\u7535\u7279\u6027\u4e0a\u53d1\u6325\u7740\u91cd\u8981\u4f5c\u7528\u3002\u5f53Zn\u7684\u63ba\u6742\u91cf\u8d85\u8fc7\u56fa\u6eb6\u9650\u5ea6\u65f6\uff0c\u90e8\u5206Zn\u539f\u5b50\u4f1a\u8fdb\u5165Cu\u4f4d\u70b9\u5e76\u5f62\u6210\u539f\u4f4dZnS\u7eb3\u7c73\u76f8\u3002\u8fd9\u4f1a\u6253\u7834\u539f\u6709\u9634\u79bb\u5b50\u548c\u9633\u79bb\u5b50\u95f4\u7684\u5e73\u8861\uff0c\u8fdb\u800c\u53c8\u901a\u8fc7\u5f62\u6210\u53cd\u4f4dFe\/Cu\u7f3a\u9677\u6765\u91cd\u5efa\u5e73\u8861\u3002\u5f62\u6210\u7684\u53cd\u4f4d\u7f3a\u9677\u9664\u4e86\u80fd\u7ef4\u6301\u7ed3\u6784\u7684\u7535\u8377\u4e2d\u6027\u5916\uff0c\u6709\u6548\u51cf\u5c0f\u4e86\u70b9\u9635\u95f4\u7684\u6676\u683c\u7578\u53d8\uff0c\u5e76\u8fdb\u4e00\u6b65\u63d0\u9ad8\u4e86Zn\u7684\u56fa\u6eb6\u5ea6\u3002\u800c630K\u4e0b\uff0cCu<sub>0.92<\/sub>Zn<sub>0.08<\/sub>FeS<sub>2<\/sub>\u7684\u6700\u9ad8ZT\u503c\u53ef\u8fbe\u52300.26\uff0c\u8fd9\u8f83\u65e0\u63ba\u6742\u7684CuFeS<sub>2<\/sub>\u6837\u54c1\u7684ZT\u503c\u63d0\u9ad8\u4e8680%\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe\u4e00\u3001CuFeS<sub>2<\/sub>\u7684\u6676\u4f53\u7ed3\u6784<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-50388\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/1-.jpg\" alt=\"\" width=\"600\" height=\"678\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/1-.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/1--265x300.jpg 265w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe\u4e8c\u3001Cu<sub>1\u2013x<\/sub>Zn<sub>x<\/sub>FeS<sub>2<\/sub>\u7684XRD\u8868\u5f81<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-50389\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/2-.jpg\" alt=\"\" width=\"600\" height=\"403\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/2-.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/2--300x202.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) PAS\u70e7\u7ed3\u5f97\u5230\u7684Cu<sub>1\u2013x<\/sub>Zn<sub>x<\/sub>FeS<sub>2<\/sub>\u6837\u54c1\uff08x=0\uff0c0.01\uff0c0.02\uff0c0.03\uff0c0.04\uff0c0.06\uff0c0.08\uff0c0.1\uff09\u7684XRD\u56fe\u8c31\u3002<\/p>\n<p>(b) Zn\u7ec4\u5206x\u7684\u6539\u53d8\u5f15\u8d77\u7684\u4e3b\u5cf0\u53d8\u5316\u3002<\/p>\n<p><strong>\u56fe\u4e09\u3001Cu<sub>1\u2013x<\/sub>Zn<sub>x<\/sub>FeS<sub>2<\/sub>\u7684\u5fae\u89c2\u5f62\u8c8c\u8868\u5f81<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-50390\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/3-.jpg\" alt=\"3-\" width=\"600\" height=\"331\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/3-.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/3--300x166.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) Cu<sub>1\u2013x<\/sub>Zn<sub>x<\/sub>FeS<sub>2<\/sub>\uff08x=0\uff0c0.01\uff0c0.02\uff0c0.03\uff0c0.04\uff0c0.06\uff0c0.08\uff0c0.1\uff09\u6837\u54c1\u65ad\u88c2\u9762FESEM\u56fe\u50cf\u3002\u901a\u8fc7EDS\u5206\u6790\u786e\u5b9a\u5149\u6591\u4e3aZnS\u3002<\/p>\n<p>(b) \u70e7\u7ed3\u524dCu<sub>0.92<\/sub>Zn<sub>0.08<\/sub>FeS<sub>2<\/sub>\u6837\u54c1\u7684\u65ad\u88c2\u9762FESEM\u56fe\u50cf\u3002<\/p>\n<p>(c) Cu<sub>0.92<\/sub>Zn<sub>0.08<\/sub>FeS<sub>2<\/sub>\u629b\u5149\u9762\u7684BSE\u56fe\u50cf\uff0c\u53ca\u5143\u7d20\u9762\u626b\u56fe\u3002<\/p>\n<p><strong>\u56fe\u56db\u3001Cu<sub>0.97<\/sub>Zn<sub>0.03<\/sub>FeS<sub>2<\/sub>\u4e0eCu<sub>0.92<\/sub>Zn<sub>0.08<\/sub>FeS<sub>2<\/sub>\u7684\u5fae\u89c2\u5f62\u8c8c\u8868\u5f81<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-50391\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/4-.jpg\" alt=\"4-\" width=\"600\" height=\"597\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/4-.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/4--150x150.jpg 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/4--300x300.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a)Cu<sub>0.97<\/sub>Zn<sub>0.03<\/sub>FeS<sub>2<\/sub>\u7684\u4f4e\u500dTEM\u56fe\u50cf\u8868\u660e\u6837\u54c1\u6709\u8f83\u9ad8\u6570\u5bc6\u5ea6\u7684ZnS\u7eb3\u7c73\u9897\u7c92\u3002<\/p>\n<p>(b) Cu<sub>0.97<\/sub>Zn<sub>0.03<\/sub>FeS<sub>2<\/sub>\u6837\u54c1\u4e2d\u5d4c\u5165\u7684ZnS\u7eb3\u7c73\u9897\u7c92\u7684HRTEM\u56fe\u50cf\u3002<\/p>\n<p>(c) \u548c(d)\u5206\u522b\u4e3aCu<sub>0.92<\/sub>Zn<sub>0.08<\/sub>FeS<sub>2<\/sub>\u6837\u54c1\u4e2dZnS\u7eb3\u7c73\u9897\u7c92\u7684\u4f4e\u500dTEM\u56fe\u50cf\u548cHRTEM\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe\u4e94\u3001Zn\u63ba\u6742\u91cf\u5bf9\u5404\u53c2\u6570\u7684\u5f71\u54cd<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-50392 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/5-.jpg\" alt=\"5-\" width=\"600\" height=\"169\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/5-.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/5--300x85.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) \u70b9\u9635\u4e2d\u6807\u79f0\u7684Zn\u542b\u91cf\u548c\u5b9e\u9645\u7684Zn\/Fe\u6469\u5c14\u6bd4\u95f4\u7684\u5173\u7cfb\uff1a\u7ea2\u7ebf\u548c\u84dd\u7ebf\u5206\u522b\u4ee3\u8868\u7740\u6807\u79f0\u7684\u548c\u7406\u8bba\u7684Zn\/Fe\u6469\u5c14\u6bd4\u3002<\/p>\n<p>(b) Cu<sub>1\u2013x<\/sub>Zn<sub>x<\/sub>FeS<sub>2<\/sub>\u7684\u6676\u683c\u5e38\u6570<\/p>\n<p>(c) \u6807\u79f0\u7684Zn\u542b\u91cf\u548c\u5ba4\u6e29\u4e0b\u7684\u8f7d\u6d41\u5b50\u6d53\u5ea6\u53ca\u8f7d\u6d41\u5b50\u8fc1\u79fb\u7387\u95f4\u7684\u5173\u7cfb\uff1a\u84dd\u7ebf\u8868\u793a\u4e86\u5b9e\u9645\u7684\u8f7d\u6d41\u5b50\u6d53\u5ea6\u66f2\u7ebf\uff0c\u84dd\u8272\u865a\u7ebf\u8868\u793a\u7684\u662f\u5f53Zn\u4ec5\u4f5c\u4e3a\u4e00\u4e2a\u63ba\u6742\u7269\u65f6\u9884\u671f\u7684\u8f7d\u6d41\u5b50\u6d53\u5ea6\u66f2\u7ebf\u3002<\/p>\n<p><strong>\u56fe\u516d\u3001Cu<sub>1\u2013x<\/sub>Zn<sub>x<\/sub>FeS<sub>2<\/sub>\u6837\u54c1\u7684\u5149\u7535\u5b50\u80fd\u8c31\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-50393\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/6-.jpg\" alt=\"6-\" width=\"600\" height=\"196\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/6-.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/6--300x98.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) Cu 2p<sub>1\/2<\/sub>\u548c2p<sub>3\/2<\/sub>\u7684\u80fd\u8c31\u56fe<\/p>\n<p>(b)\u00a0Fe 2p<sub>1\/2<\/sub>\u548c2p<sub>3\/2<\/sub>\u7684\u80fd\u8c31\u56fe<\/p>\n<p>(c) Cu<sub>1\u2013x<\/sub>Zn<sub>x<\/sub>FeS<sub>2<\/sub>\uff08x=0\uff0c0.02\uff0c0.08\uff09\u6837\u54c1Zn 2p<sub>3\/2<\/sub>\u7684\u5206\u5cf0\u56fe<\/p>\n<p><strong>\u56fe\u4e03\u3001\u6e29\u5ea6\u4e0eCu1\u2013xZnxFeS2\u6837\u54c1\u5404\u70ed\u7535\u53c2\u6570\u95f4\u7684\u5173\u7cfb<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-50394\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/7-.jpg\" alt=\"7-\" width=\"600\" height=\"184\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/7-.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/7--300x92.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>Cu<sub>1\u2013x<\/sub>Zn<sub>x<\/sub>FeS<sub>2<\/sub>\uff08x=0\uff0c0.01\uff0c0.02\uff0c0.03\uff0c0.04\uff0c0.06\uff0c0.08\uff0c0.1\uff09\u6837\u54c1\u7684\u5404\u9879\u53c2\u6570(a) \u7535\u5bfc\u7387\uff0c(b) \u8d5b\u8d1d\u514b\u7cfb\u6570\uff0c(c) \u529f\u7387\u7cfb\u6570\u968f\u6e29\u5ea6\u7684\u53d8\u5316\u66f2\u7ebf\u56fe\u3002<\/p>\n<p><strong>\u56fe\u516b\u3001Cu<sub>1\u2013x<\/sub>Zn<sub>x<\/sub>FeS<sub>2<\/sub>\u6837\u54c1\u8f7d\u6d41\u5b50\u4e0e\u6e29\u5ea6\u95f4\u7684\u5173\u7cfb<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-50395\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/8-.jpg\" alt=\"8-\" width=\"600\" height=\"279\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/8-.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/8--300x140.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>Cu<sub>1\u2013x<\/sub>Zn<sub>x<\/sub>FeS<sub>2<\/sub>\uff08x=0\uff0c0.01\uff0c0.02\uff0c0.03\uff0c0.04\uff0c0.06\uff0c0.08\uff0c0.1\uff09\u6837\u54c1\u7684(a) \u8f7d\u6d41\u5b50\u6d53\u5ea6\uff0c(b) \u8f7d\u6d41\u5b50\u8fc1\u79fb\u7387\u968f\u6e29\u5ea6\uff0810-300K\uff09\u7684\u53d8\u5316\u66f2\u7ebf\u56fe\u3002<\/p>\n<p><strong>\u56fe\u4e5d\u3001\u6e29\u5ea6\u4e0eCu<sub>1\u2013x<\/sub>Zn<sub>x<\/sub>FeS<sub>2<\/sub>\u6837\u54c1\u5404\u70ed\u7535\u53c2\u6570\u95f4\u7684\u5173\u7cfb<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-50396\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/9-.jpg\" alt=\"9-\" width=\"600\" height=\"186\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/9-.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/9--300x93.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>Cu<sub>1\u2013x<\/sub>Zn<sub>x<\/sub>FeS<sub>2<\/sub>\uff08x=0\uff0c0.01\uff0c0.02\uff0c0.03\uff0c0.04\uff0c0.06\uff0c0.08\uff0c0.1\uff09\u6837\u54c1\u7684(a) \u603b\u70ed\u5bfc\u7387\uff0c(b) \u6676\u683c\u70ed\u5bfc\u7387\uff0c(c) ZT\u503c\u968f\u6e29\u5ea6\u7684\u53d8\u5316\u66f2\u7ebf\u56fe\u3002<\/p>\n<p><strong>\u56fe\u5341\u3001Cu<sub>1\u2013x<\/sub>Zn<sub>x<\/sub>FeS<sub>2<\/sub>\u6837\u54c1\u7684\u70ed\u5bfc\u7387\u5206\u6790<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-50397\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/10-.jpg\" alt=\"10-\" width=\"600\" height=\"784\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/10-.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/10--230x300.jpg 230w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a-c) \u5206\u522b\u4e3aCu<sub>1\u2013x<\/sub>Zn<sub>x<\/sub>FeS<sub>2<\/sub>\uff08x=0\uff0c0.01\uff0c0.02\uff0c0.03\uff0c0.04\uff0c0.06\uff0c0.08\uff0c0.1\uff09\u6837\u54c1\u548cCu<sub>0.975<\/sub>Zn<sub>0.025<\/sub>FeS<sub>2 +x<\/sub>ZnS(x = 0.015, 0.035, 0.055, and 0.075)\u6837\u54c1\u5ba4\u6e29\u4e0b\u7684\u6676\u683c\u70ed\u5bfc\u7387\u3002\u5e95\u90e8\u66f2\u7ebf\u56fe\u4e2d\uff0c\u7ea2\u7ebf\u548c\u84dd\u7ebf\u5206\u522b\u57fa\u4e8eCallaway\u6a21\u578b\u548cEMA\u6a21\u578b\u8ba1\u7b97\u83b7\u5f97\u3002<\/p>\n<p><strong>\u56fe\u5341\u4e00\u3001Zn\u542b\u91cf\u4e0e\u6837\u54c1\u6563\u5c04\u80fd\u529b\u95f4\u7684\u5173\u7cfb<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-50398\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/11-.jpg\" alt=\"11-\" width=\"600\" height=\"565\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/11-.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/11--300x283.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>Zn\u542b\u91cf\u4e0e\u8d28\u91cf\u6d53\u5dee\u6563\u5c04\u53c2\u6570\u0393<sub>M<\/sub>\u548c\u5e94\u53d8\u6d53\u5dee\u6563\u5c04\u53c2\u6570\u0393<sub>S<\/sub>\u95f4\u7684\u5173\u7cfb\u56fe\u3002<\/p>\n<p><strong>\u56fe\u5341\u4e8c\u3001\u6837\u54c1\u6bd4\u70ed\u4e0e\u6e29\u5ea6\u7684\u5173\u7cfb<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-50399\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/12-.jpg\" alt=\"12-\" width=\"600\" height=\"547\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/12-.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/12--300x274.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>Cu<sub>0.98<\/sub>Zn<sub>0.02<\/sub>FeS<sub>2<\/sub>\u548cCu<sub>0.99<\/sub>Fe<sub>1.01<\/sub>S<sub>2<\/sub>\u7684\u4f4e\u6e29\u6bd4\u70edC<sub>p<\/sub>\uff0c\u5185\u5d4c\u56fe\u8868\u793a\u7684\u662fC<sub>p<\/sub>\/T-T<sup>2<\/sup>\u7684\u62df\u5408\u66f2\u7ebf\u3002<\/p>\n<p><strong>\u56fe\u5341\u4e09\u3001CuFeS<sub>2<\/sub>\uff0cCu<sub>0.98<\/sub>Zn<sub>0.02<\/sub>FeS<sub>2<\/sub>\uff0c\u53caCu<sub>0.99<\/sub>Fe<sub>1.01<\/sub>S<sub>2<\/sub>\u6837\u54c1\u5404\u70ed\u7535\u53c2\u6570\u4e0e\u6e29\u5ea6\u95f4\u7684\u5173\u7cfb<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-50400\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/13-.jpg\" alt=\"13-\" width=\"600\" height=\"577\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/13-.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/13--300x289.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>CuFeS<sub>2<\/sub>\uff0cCu<sub>0.98<\/sub>Zn<sub>0.02<\/sub>FeS<sub>2<\/sub>\uff0c\u53caCu<sub>0.99<\/sub>Fe<sub>1.01<\/sub>S<sub>2<\/sub>\u6837\u54c1\u7684(a) \u7535\u5bfc\u7387\uff0c(b) \u8d5b\u8d1d\u514b\u7cfb\u6570\uff0c(c) \u70ed\u5bfc\u7387\uff0c(d) ZT\u503c\u4e0e\u6e29\u5ea6\u95f4\u7684\u5173\u7cfb\u66f2\u7ebf\u3002<\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>Zn\u7684\u63ba\u6742\u5bf9\u9ec4\u94dc\u77ffCuFeS<sub>2<\/sub>\u6676\u683c\u5728\u7ed3\u6784\u548c\u7cfb\u7edf\u8f7d\u6d41\u5b50\u8fd0\u8f93\u6027\u4e0a\u5f71\u54cd\u90fd\u662f\u5f88\u5927\u7684\uff0c\u5f88\u5927\u7a0b\u5ea6\u4e0a\uff0cZn\u6709\u6548\u63d0\u9ad8\u4e86CuFeS<sub>2<\/sub>\u7684\u8f7d\u6d41\u5b50\u6d53\u5ea6\u548c\u70ed\u7535\u7279\u6027\u3002Zn\u63ba\u6742\u7684\u4f5c\u7528\u53ca\u539f\u4f4d\u5f62\u6210\u7684ZnS\u7eb3\u7c73\u76f8\u6240\u5e26\u6765\u7684\u5f71\u54cd\u4e5f\u53ef\u80fd\u8fdb\u4e00\u6b65\u5bf9\u5176\u4ed6\u7684Zn\u63ba\u6742\u3001\u786b\u57fa\u5316\u5408\u7269\u4e5f\u9002\u7528\u3002\u53e6\u5916\uff0c\u5f53\u4e0b\u7684\u5408\u6210\u65b9\u6cd5\u5728\u4e00\u5b9a\u7a0b\u5ea6\u4e0a\u9650\u5236\u4e86Zn\u5728\u9ec4\u94dc\u77ff\u7ed3\u6784\u4e2d\u7684\u6781\u9650\u6eb6\u89e3\u5ea6\u3002\u6b64\u7814\u7a76\u4eba\u5458\u7684\u4e0b\u4e00\u6b65\u7814\u7a76\u65b9\u5411\u7684\u901a\u8fc7\u4f7f\u7528\u66f4\u591a\u5feb\u901f\u5408\u6210\u7684\u65b9\u6cd5\u6253\u7834\u6eb6\u89e3\u6781\u9650\uff0c\u5e0c\u671b\u4ee5\u6b64\u663e\u8457\u63d0\u9ad8\u6676\u683c\u4e2d\u7684Zn\u56fa\u6eb6\u5ea6\uff0c\u6216\u662f\u8fdb\u4e00\u6b65\u6539\u53d8ZnS\u4e8c\u6b21\u76f8\u7684\u5f62\u6001\u3002\u82e5\u80fd\u6210\u529f\uff0c\u8fd9\u5c06\u5927\u5e45\u63a8\u8fdb\u5ec9\u4ef7\u3001\u73af\u5883\u53cb\u597d\u578b\u70ed\u7535\u6750\u6599\u7684\u70ed\u7535\u7279\u6027\u7684\u53d1\u5c55\uff01<\/p>\n<p>\u6587<strong>\u732e\u94fe\u63a5<\/strong>\uff1a<a href=\"http:\/\/onlinelibrary.wiley.com\/wol1\/doi\/10.1002\/aenm.201601299\/full\" target=\"_blank\">The Role of Zn in Chalcopyrite CuFeS2: Enhanced Thermoelectric Properties of Cu1\u2013xZnxFeS2 with In Situ Nanoprecipitates<\/a>\uff08Adv. Energy Mater.\uff0c2016\uff0cDOI\uff1a10.1002\/aenm.201601299\uff09<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u7535\u5b50\u7535\u5de5\u5b66\u672f\u7ec4\u5927\u9ed1\u5929\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u7f16\u8f91\u6574\u7406\u3002<\/p>\n<p>\u6750\u6599\u725b\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u8fd9\u91cc\u6c47\u96c6\u4e86\u5404\u5927\u9ad8\u6821\u7855\u535a\u751f\u3001\u4e00\u7ebf\u79d1\u7814\u4eba\u5458\u4ee5\u53ca\u884c\u4e1a\u4ece\u4e1a\u8005\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\">\u70b9\u6211\u52a0\u5165\u7f16\u8f91\u90e8<\/a>\u3002<\/p>\n<p>\u6750\u6599\u4eba\u7f51\u5c0a\u91cd\u6240\u6709\u8fdb\u884c\u77e5\u8bc6\u4f20\u64ad\u7684\u5a92\u4f53\uff0c\u8f6c\u8f7d\u8bf7\u8054\u7cfbtougao@cailiaoren.com\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u6709\u6548\u89e3\u51b3\u4f59\u70ed\u6216\u662f\u5408\u7406\u5229\u7528\u80fd\u6e90\u65b9\u9762\uff0c\u70ed\u7535\u6750\u6599\u662f\u524d\u666f\u975e\u5e38\u53ef\u89c2\u7684\u6750\u6599\u3002\u7ec6\u6570\u8fd1\u6bb5\u65f6\u95f4\u5bf9\u4e8e\u70ed\u7535\u6750\u6599\u7684\u76f8\u5173\u6587\u732e\u62a5\u9053\uff0c\u53ef\u77e5\u8d8a\u6765\u8d8a\u591a\u7684\u7814\u7a76\u8005\u5f00\u59cb\u6d89\u53ca\u8fd9\u4e00\u9886\u57df\uff0c\u4ee5\u7814\u53d1\u51fa&#8230;<\/p>\n","protected":false},"author":15,"featured_media":50397,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[1417,748],"class_list":["post-50387","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","tag-tangxinfeng","tag-redian"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/50387"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/15"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=50387"}],"version-history":[{"count":4,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/50387\/revisions"}],"predecessor-version":[{"id":50607,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/50387\/revisions\/50607"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/50397"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=50387"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=50387"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=50387"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}