{"id":50857,"date":"2016-11-13T14:00:07","date_gmt":"2016-11-13T06:00:07","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=50857"},"modified":"2016-11-12T19:10:23","modified_gmt":"2016-11-12T11:10:23","slug":"%e9%92%a8%e9%93%9c%e5%90%88%e9%87%91%e7%9a%84%e6%95%b4%e4%bd%93%e8%bf%9e%e6%8e%a5%e6%8a%80%e6%9c%af","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=50857","title":{"rendered":"\u94a8\u94dc\u5408\u91d1\u7684\u6574\u4f53\u8fde\u63a5\u6280\u672f"},"content":{"rendered":"<p><strong>\u6750\u6599\u725b\u6ce8\uff1a<\/strong>\u957f\u671f\u4ee5\u6765\uff0c\u94a8\u548c\u94dc\u5408\u91d1\u7684\u6574\u4f53\u8fde\u63a5\u6280\u672f\u5c31\u5236\u7ea6\u7740\u6838\u805a\u53d8\u53cd\u5e94\u4e2d\u504f\u6ee4\u5668\u88c5\u7f6e\u7684\u53d1\u5c55\u3002\u600e\u6837\u5728\u4e0d\u6dfb\u52a0\u4e2d\u95f4\u6750\u6599\u7684\u60c5\u51b5\u4e0b\u5c06\u4e8c\u8005\u5408\u4e8c\u4e3a\u4e00\u4e00\u76f4\u662f\u4ee4\u79d1\u5b66\u5bb6\u4eec\u5934\u75bc\u7684\u95ee\u9898\u3002\u8fd1\u671f\uff0c\u65e5\u672c\u4e1c\u4eac\u7684\u79d1\u5b66\u5bb6\u6210\u529f\u7814\u5236\u51fa\u89e3\u51b3\u8fd9\u4e00\u96be\u9898\u7684\u6280\u672f\uff0c\u8ba9\u6211\u4eec\u4e00\u7779\u4e3a\u5feb\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-50858\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/161102132335_1_540x360.jpg\" alt=\"161102132335_1_540x360\" width=\"540\" height=\"229\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/161102132335_1_540x360.jpg 540w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/11\/161102132335_1_540x360-300x127.jpg 300w\" sizes=\"(max-width: 540px) 100vw, 540px\" \/><\/p>\n<p>\uff08a\uff09\u4e09\u70b9\u5f2f\u66f2\u8bd5\u9a8c\u4e2dBNi-6\u8fde\u63a5\u5c42\u7684\u53d8\u5f62\u539f\u7406\u56fe\u3002\u8fde\u63a5\u5c42\u53d1\u751f\u5c40\u90e8\u53d8\u5f62\u3002\uff08b\uff09\u7ea2\u5b9e\u7ebf\u4ee3\u8868\u7684\u662f\u94a2\u5316\u8fde\u63a5\u5c42\u7684\u5e94\u529b\u5e94\u53d8\u66f2\u7ebf\u3002\uff081\uff09\u70b9\u4e3a\u660e\u663e\u5c48\u670d\u70b9\u3002\u7eff\u8272\u865a\u7ebf\u4ee3\u8868\u7684\u662f\u4e0d\u540c\u94dc\u5408\u91d1\u548c\u710a\u63a5\u6750\u6599\u5236\u5907\u7684\u6837\u54c1\u5728\u710a\u63a5\u5931\u8d25\u65f6\u7684\u5f62\u6001\u3002<\/p>\n<p>\u6301\u7eed\u4ece\u6838\u805a\u53d8\u7b49\u79bb\u5b50\u4f53\u4e2d\u5438\u6536\u9ad8\u70ed\u91cf\u548c\u7c92\u5b50\u6d41\u7684\u88c5\u7f6e\u662f\u4e00\u4e2a\u504f\u6ee4\u5668\u3002\u7531\u4e8e\u5728\u70ed\u8f6c\u79fb\u65b9\u9762\u7684\u8868\u73b0\u4f18\u826f\u4e14\u53ef\u9760\uff0c\u8fd9\u4e00\u504f\u6ee4\u88c5\u7f6e\u5728\u4e16\u754c\u8303\u56f4\u5185\u6380\u8d77\u4e00\u80a1\u7814\u7a76\u5b83\u7684\u70ed\u6f6e\u3002\u5757\u72b6\u91d1\u5c5e\u94a8\u53ef\u7528\u4f5c\u504f\u6ee4\u5668\u88c5\u7532\u6750\u6599\uff0c\u5b83\u5177\u6709\u4f4e\u6c22\u540c\u4f4d\u7d20\u4fdd\u7559\u53ca\u4f4e\u6e85\u5c04\u6548\u7387\u7684\u4f18\u52bf\u3002\u5728\u94a8\u88c5\u7532\u6750\u6599\u7684\u80cc\u9762\u8fde\u63a5\u7740\u94dc\u5408\u91d1\u505a\u7684\u6c34\u51b7\u6563\u70ed\u5668\uff0c\u5728\u70ed\u4f20\u9012\u8fc7\u7a0b\u4e2d\uff0c\u8fd9\u4e00\u88c5\u7f6e\u4f1a\u81a8\u80c0\u4f38\u957f\u3002\u4ed6\u4eec\u8003\u8651\u5728\u65cb\u8f6c\u53cd\u5e94\u5806(FFHR-d1)\u4e2d\u52a0\u5165\u540c\u6837\u7684\u7ed3\u6784\uff0cNIFS\u5728\u8003\u8651\u8303\u56f4\u3002\u8fd9\u4e48\u8bf4\u6765\uff0c\u8fde\u63a5\u94a8\u548c\u94dc\u7684\u6280\u672f\u5c31\u5fc5\u4e0d\u53ef\u5c11\u4e86\u3002\u7136\u800c\uff0c\u8fd9\u4e24\u79cd\u91d1\u5c5e\u5e76\u4e0d\u4f1a\u5f62\u6210\u5408\u91d1\u3002\u5728\u4e24\u79cd\u91d1\u5c5e\u4e2d\uff0c\u52a0\u5165\u586b\u5145\u6750\u6599\u4f5c\u4e3a\u8fde\u63a5\u6750\u6599\uff0c\u5e76\u5c06\u8fd9\u4e00\u6750\u6599\u52a0\u70ed\u81f3900\u2103\u4ee5\u4e0a\u3002\u7531\u4e8e\u94dc\u548c\u94a8\u7684\u70ed\u81a8\u80c0\u7387\u5927\u4e0d\u76f8\u540c\uff0c\u7528\u4e8e\u5438\u6536\u70ed\u81a8\u80c0\u7684\u4e2d\u95f4\u6750\u6599\u9700\u8981\u548c\u586b\u5145\u6750\u6599\u4e00\u8d77\u6dfb\u52a0\u8fdb\u53bb\u3002\u76f4\u5230\u73b0\u5728\u4eba\u4eec\u4e5f\u6ca1\u6709\u53d1\u73b0\u4e0d\u7528\u4e2d\u95f4\u6750\u6599\u5c31\u80fd\u8fde\u63a5\u4e8c\u8005\u7684\u6280\u672f\u3002\u4f46\u52a0\u5165\u4e2d\u95f4\u6750\u6599\uff0c\u53c8\u4f1a\u589e\u52a0\u8fde\u63a5\u754c\u9762\u548c\u8fde\u63a5\u9762\u79ef\uff0c\u4ece\u800c\u51cf\u5f31\u7ed3\u6784\u5f3a\u5ea6\uff0c\u5bfc\u81f4\u6210\u672c\u589e\u52a0\u3001\u6392\u70ed\u6027\u80fd\u4e0b\u964d\u7b49\u95ee\u9898\u3002<\/p>\n<p><span style=\"color: #ff0000;\"><strong>\u7814\u7a76\u7ed3\u679c\u548c\u610f\u4e49<\/strong><\/span><\/p>\n<p>\u65e5\u672c\u6838\u878d\u5408\u79d1\u5b66\u7814\u7a76\u6240\u7684\u7814\u7a76\u9662Masayuki Tokitani\u53ca\u5176\u7814\u7a76\u56e2\u961f\u7814\u5236\u51fa\u4e00\u79cd\u76f4\u63a5\u8fde\u63a5\u94a8\u548c\u94dc\u5408\u91d1\u7684\u6280\u672f\uff0c\u867d\u7136\u6709\u70b9\u56f0\u96be\u3002\u4ed6\u4eec\u5c06\u8fde\u63a5\u6750\u6599\u7528\u4f5c\u7f13\u51b2\uff0c\u4ece\u800c\u51cf\u5c11\u4e86\u4e2d\u95f4\u6750\u6599\u7684\u4f7f\u7528\u3002\u5229\u7528\u8fd9\u4e00\u6280\u672f\uff0c\u4ed6\u4eec\u6210\u529f\u5236\u5907\u51fa\u5728\u53cd\u5e94\u5806\u6761\u4ef6(~15 MW\/m2)\u4e0b\u90fd\u5177\u6709\u4f18\u5f02\u70ed\u8f6c\u79fb\u5bb9\u91cf\u7684\u5c0f\u578b\u504f\u6ee4\u5668\u3002<\/p>\n<p>\u8be5\u504f\u6ee4\u5668\u5fc5\u987b\u80fd\u591f\u627f\u53d7\u5f97\u4f4f\u6781\u5f3a\u7684\u70ed\u6d41\u51b2\u51fb\uff0c\u751a\u81f3\u5728\u710a\u63a5\u70ed\u5904\u7406\u9636\u6bb5\uff0c\u56e0\u4e3a\u5728\u8fd9\u4e00\u9636\u6bb5\uff0c\u8fd9\u4e2a\u5143\u5668\u4ef6\u4f1a\u88ab\u52a0\u70ed\u81f3900\u2103\uff0c\u518d\u51b7\u5374\u81f3\u5ba4\u6e29\u3002\u6240\u4ee5\uff0c\u88c5\u7532\u6750\u6599\u548c\u70ed\u6c89\u6750\u6599\u8fde\u63a5\u754c\u9762\u4e0a\u5c31\u4f1a\u4ea7\u751f\u70ed\u5e94\u529b\u3002\u8fd9\u79cd\u70ed\u5e94\u529b\u5e94\u88ab\u5c3d\u53ef\u80fd\u5feb\u5730\u9664\u53bb\u3002\u8fd9\u4e00\u6b21\uff0c\u4e3a\u4e86\u540c\u65f6\u6ee1\u8db3\u79cd\u79cd\u9700\u6c42\uff0c\u7814\u7a76\u56e2\u961f\u7684\u6210\u5458\u4f7f\u7528BNi-6 (Ni-11%P)\u3001\u6c27\u5316\u7269\u5f25\u6563\u5f3a\u5316\u94dc\u5408\u91d1(ODS-Cu)\u548cGlidCop\u00ae (Cu-0.3wt%Al2O3)\u4f5c\u4e3a\u586b\u5145\u6750\u6599\uff0c\u4ee5\u8fbe\u5230\u6700\u4f18\u710a\u63a5\u6761\u4ef6\u3002<\/p>\n<p>\u66f4\u7279\u522b\u7684\u662f\uff0cTokitani\u6559\u6388\u7684\u7814\u7a76\u56e2\u961f\u5c06\u710a\u63a5\u6750\u6599\u7684\u539a\u5ea6\u5b9a\u4e3a38 ?m\uff0c\u70ed\u5904\u7406\u6e29\u5ea6\u548c\u65f6\u95f4\u5206\u522b\u662f960\u2103\u548c10min\uff0c\u5728\u6b64\u671f\u95f4\u8fdb\u884c\u710a\u63a5\u64cd\u4f5c\u3002\u63a5\u4e0b\u6765\uff0c\u4ed6\u4eec\u5728\u4ece960\u2103\u5230100\u2103\u7684\u51b7\u5374\u8fc7\u7a0b\u4e2d\u91c7\u7528\u4e86\u6781\u7f13\u6162\u7684\u81ea\u7136\u51b7\u5374\uff0c\u5728100\u2103\u5230\u5ba4\u6e29\u8fd9\u6bb5\u51b7\u5374\u8fc7\u7a0b\u4e2d\uff0c\u91c7\u7528\u6c2e\u6c14\u51b7\u5374\u3002\u710a\u63a5\u5b8c\u6210\u540e\uff0c\u91c7\u53d6\u4e09\u70b9\u5f2f\u66f2\u8bd5\u9a8c\u6765\u6d4b\u8bd5\u8fde\u63a5\u7684\u5f3a\u5ea6\u3002\u4ee4\u4eba\u5403\u60ca\u7684\u662f\uff0c\u8fde\u63a5\u5c42\u5177\u6709\u4f18\u826f\u7684\u97e7\u6027\uff0c\u5176\u5c48\u670d\u5f3a\u5ea6\u8fbe200 MPa\u3002\u65e2\u7136\u94a8\u548cGlidCop\u00ae\u6750\u6599\u5728\u710a\u63a5\u5904\u7406\u540e\u7684\u5c48\u670d\u5f3a\u5ea6\u90fd\u5728300 MPa\u4ee5\u4e0a\uff0c\u90a3\u4e48\u53d8\u5f62\u533a\u57df\u5fc5\u7136\u5728\u710a\u63a5\u533a\u4ee5\u5185\u3002\u5f53\u5f20\u529b\u4e3a0.2%\u65f6\uff0c\u8fd9\u4e00\u533a\u57df\u4e5f\u4e0d\u592a\u53ef\u80fd\u662f\u4ea7\u751f\u5927\u5851\u6027\u53d8\u5f62\u7684\u5730\u65b9\u3002\u65e2\u7136\u5b9e\u9645\u7684\u5851\u6027\u53d8\u5f62\u533a\u57df\u90fd\u7279\u522b\u8584\uff08\u6bd4\u5982\u51e0\u5341\u5fae\u7c73\uff09\uff0c\u90a3\u4e48\u5b9e\u9645\u7684\u5f20\u529b\u5e94\u8fdc\u5927\u4e8e0.2%\u3002\u8fd9\u771f\u662f\u4e00\u4e2a\u4ee4\u4eba\u60ca\u8bb6\u7684\u7ed3\u679c\u3002<\/p>\n<p>\u8fd9\u8868\u660e\u8fde\u63a5\u5c42\u6709\u97e7\u6027\uff0c\u710a\u63a5\u4ea7\u751f\u7684\u70ed\u81a8\u80c0\u5728\u8fd9\u4e00\u533a\u57df\u88ab\u5438\u6536\u6b86\u5c3d\u3002\u8fd9\u79cd\u65bd\u52a0\u5e94\u529b\u7684\u91ca\u653e\u529f\u80fd\u5177\u6709\u5f3a\u5927\u7684\u4f18\u52bf\uff0c\u80fd\u6709\u6548\u53bb\u9664\u53cd\u5e94\u5806\u6761\u4ef6\u4e0b\u5de5\u4f5c\u7684\u504f\u6ee4\u5668\u4e2d\u7684\u968f\u673a\u70ed\u81a8\u80c0\u3002\u53e6\u5916\uff0c\u710a\u63a5\u5931\u8d25\u7684\u6837\u54c1\u4e2d\u7eff\u8272\u865a\u7ebf\u8868\u793a\u4e0d\u540c\u94dc\u5408\u91d1\u548c\u710a\u63a5\u6750\u6599\u3002\u5728\u8fd9\u4e9b\u5931\u8d25\u4e86\u7684\u710a\u63a5\u6837\u54c1\u4e2d\uff0c\u8fde\u63a5\u5c42\u8106\u6027\u592a\u5927\uff0c\u4ec5\u57281\/4\u6240\u9700\u5f20\u529b\u7684\u60c5\u51b5\u4e0b\u5c31\u53d1\u751f\u65ad\u88c2\u3002W\/BNi-6\/GlidCop\u00ae\u5c0f\u578b\u504f\u6ee4\u5668\u7684\u6210\u529f\u5236\u5907\u8981\u5f52\u56e0\u4e8e\u5148\u8fdb\u7684\u710a\u63a5\u6280\u672f\u3002\u5bf9\u8fd9\u4e00\u504f\u6ee4\u5668\uff0c\u4ed6\u4eec\u5728NIFS\u4e0b\u5229\u7528ACT2\u7535\u5b50\u675f\u88c5\u7f6e\uff0c\u5728\u53cd\u5e94\u5806\u76f8\u5173\u6761\u4ef6\u4e0b\u8fdb\u884c\u4e86\u70ed\u8d1f\u8377\u5b9e\u9a8c\u3002650\u2103\u7684\u6e29\u5ea6\u8fdc\u4f4e\u4e8eBNi-6\u7684\u7194\u70b9\uff08875\u2103\uff09\u548c\u94a8\u7684\u518d\u7ed3\u6676\u6e29\u5ea6\uff08~1500\u2103\uff09\u3002\u4e3a\u4ec0\u4e48\u5b83\u5177\u6709\u5982\u6b64\u4f18\u826f\u7684\u70ed\u8f6c\u79fb\u5bb9\u91cf\u5462\uff1f\u539f\u56e0\u5728\u4e8e\uff0c\u65e2\u7136\u8981\u4e0d\u52a0\u4e2d\u95f4\u6750\u6599\u5730\u76f4\u63a5\u7ed3\u5408\uff0c\u5c31\u5e94\u5f53\u5c06\u88c5\u7532\u5c42\u5230\u6563\u70ed\u5668\u7684\u70ed\u963b\u51cf\u81f3\u6700\u5c0f\u3002<\/p>\n<p>\u8fd9\u4e00\u7814\u7a76\u6210\u679c\u63d0\u51fa\u7684\u5148\u8fdb\u710a\u63a5\u6280\u672f\u4e0d\u4ec5\u53ef\u4ee5\u5236\u5907\u5148\u8fdb\u7684\u504f\u6ee4\u5668\uff0c\u800c\u4e14\u53ef\u4ee5\u51cf\u5c11\u805a\u53d8\u53cd\u5e94\u5806\u6574\u4f53\u504f\u6ee4\u5668\u7ed3\u6784\u7684\u5236\u9020\u6210\u672c\u3002\u5728\u672a\u6765\u7684\u5de5\u4f5c\u4e2d\uff0c\u5229\u7528\u8fd9\u4e00\u6280\u672f\uff0c\u6211\u4eec\u53ef\u4ee5\u5236\u5907\u548c\u8fd9\u4e00\u5c0f\u578b\u504f\u6ee4\u5668\u7ed3\u6784\u76f8\u540c\u7684\u5927\u578b\u504f\u6ee4\u88c5\u7f6e\uff0c\u5e76\u7528\u4e8e\u6838\u805a\u53d8\u53cd\u5e94\u4e2d\u3002\u6211\u4eec\u7684\u76ee\u6807\u5728\u4e8e\u4f7f\u504f\u6ee4\u88c5\u7f6e\u7684\u8fdc\u7a0b\u64cd\u4f5c\u548c\u5b89\u5168\u4f7f\u7528\u6210\u4e3a\u53ef\u80fd\u3002<\/p>\n<p>\u8be5\u7814\u7a76\u7ed3\u679c\u53d1\u8868\u57282016\u5e74\u5341\u670817~22\u65e5\u671f\u95f4\u4e8e\u65e5\u672c\u4e1c\u4eac\u53ec\u5f00\u7684\u7b2c26\u6b21\u56fd\u9645\u539f\u5b50\u80fd\u673a\u6784\u7684\u805a\u53d8\u80fd\u6e90\u4f1a\u8bae\u7eaa\u5f55\u4e0a\u3002<\/p>\n<p>\u539f\u6587\u94fe\u63a5\uff1a<a href=\"https:\/\/www.sciencedaily.com\/releases\/2016\/11\/161102132335.htm\" target=\"_blank\">Establishing an advanced bonding technique for tungsten and copper alloys<\/a><\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"https:\/\/www.nins.jp\/english\/\" target=\"_blank\">National Institutes of Natural Sciences<\/a><\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u6768\u6811\u63d0\u4f9b\u7d20\u6750\uff0c\u5f20\u6587\u626c\u7f16\u8bd1\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\">\u70b9\u6211\u52a0\u5165\u6750\u6599\u4eba\u7f16\u8f91\u90e8<\/a>\u3002<\/p>\n<p>\u6750\u6599\u6d4b\u8bd5\uff0c\u6570\u636e\u5206\u6790\uff0c\u4e0a<a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\">\u6d4b\u8bd5\u8c37<\/a>\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u6750\u6599\u725b\u6ce8\uff1a\u957f\u671f\u4ee5\u6765\uff0c\u94a8\u548c\u94dc\u5408\u91d1\u7684\u6574\u4f53\u8fde\u63a5\u6280\u672f\u5c31\u5236\u7ea6\u7740\u6838\u805a\u53d8\u53cd\u5e94\u4e2d\u504f\u6ee4\u5668\u88c5\u7f6e\u7684\u53d1\u5c55\u3002\u600e\u6837\u5728\u4e0d\u6dfb\u52a0\u4e2d\u95f4\u6750\u6599\u7684\u60c5\u51b5\u4e0b\u5c06\u4e8c\u8005\u5408\u4e8c\u4e3a\u4e00\u4e00\u76f4\u662f\u4ee4\u79d1\u5b66\u5bb6\u4eec\u5934\u75bc\u7684\u95ee\u9898\u3002\u8fd1\u671f\uff0c\u65e5&#8230;<\/p>\n","protected":false},"author":635,"featured_media":50858,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[2],"tags":[54],"class_list":["post-50857","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-keji","tag-making"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/50857"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/635"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=50857"}],"version-history":[{"count":5,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/50857\/revisions"}],"predecessor-version":[{"id":51423,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/50857\/revisions\/51423"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/50858"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=50857"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=50857"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=50857"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}