{"id":57116,"date":"2017-01-05T06:30:23","date_gmt":"2017-01-04T22:30:23","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=57116"},"modified":"2017-03-18T21:22:42","modified_gmt":"2017-03-18T13:22:42","slug":"nature%e5%ad%90%e5%88%8a%ef%bc%9a%e6%97%a0%e5%ba%8f%e7%9f%b3%e5%a2%a8%e7%83%af%e7%ba%a4%e7%bb%b4%e7%bb%84%e6%88%90%e5%a4%9a%e5%8a%9f%e8%83%bd%e7%9f%b3%e5%a2%a8%e7%83%af%e6%97%a0%e7%ba%ba%e5%b8%83","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=57116","title":{"rendered":"Nature\u5b50\u520a\uff1a\u65e0\u5e8f\u77f3\u58a8\u70ef\u7ea4\u7ef4\u7ec4\u6210\u591a\u529f\u80fd\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03"},"content":{"rendered":"<p style=\"padding-left: 30px;\"><strong><b>\u3010\u5f15\u8bed\u3011<\/b><\/strong><\/p>\n<p style=\"text-align: justify; padding-left: 30px;\">2016\u5e7411\u670816\u65e5\uff0cNat. Commun.\u00a0\u7f51\u7ad9\u5728\u7ebf\u53d1\u8868\u4e86\u9898\u4e3a\u201cMultifunctional non-woven fabrics of interfused graphene fibres\u201d\u7684\u6587\u7ae0\u3002<strong>\u8be5\u6587\u7ae0\u7684\u7b2c\u4e00\u4f5c\u8005\u4e3a\u6765\u81ea\u6d59\u6c5f\u5927\u5b66\u7684\u674e\u62ef\uff0c\u901a\u8baf\u4f5c\u8005\u4e3a\u6d59\u6c5f\u5927\u5b66\u7684\u9ad8\u8d85\u6559\u6388\u3002<\/strong>\u5728\u8fd9\u7bc7\u5feb\u8baf\uff08Communication\uff09\u6587\u7ae0\u4e2d\uff0c\u7814\u7a76\u4eba\u5458\u5728\u8fde\u7eed\u5316\u6e7f\u6cd5\u7eba\u4e1d\u6280\u672f\u7684\u57fa\u7840\u4e4b\u4e0a\u6210\u529f\u7814\u5236\u51fa\u4e86\u7b2c\u4e00\u5757\u7531\u7eaf\u77f3\u58a8\u70ef\u7ea4\u7ef4\u6784\u6210\u7684\u7ec7\u7269\u3002\u8be5\u77f3\u58a8\u70ef\u7ec7\u7269\u5b8c\u5168\u7531\u77f3\u58a8\u70ef\u7ea4\u7ef4\u6784\u6210\uff0c\u65e0\u9700\u6dfb\u52a0\u4efb\u4f55\u7c98\u63a5\u5242\uff0c\u4ec5\u5229\u7528\u6c27\u5316\u77f3\u58a8\u70ef\u7ea4\u7ef4\u95f4\u7684\u81ea\u878d\u5408\u73b0\u8c61\u4f7f\u5f97\u7ea4\u7ef4\u5728\u63a5\u89e6\u7ed3\u70b9\u5904\u878d\u4e3a\u4e00\u4f53\u3002<\/p>\n<p style=\"padding-left: 30px;\"><strong><b>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/b><\/strong><\/p>\n<p style=\"padding-left: 30px;\">\u78b3\u57fa\u7ea4\u7ef4\u7ec7\u7269\u4f5c\u4e3a\u4e00\u79cd\u9ad8\u6027\u80fd\u7684\u7279\u6b8a\u7ec7\u7269\u5728\u53ef\u7a7f\u6234\u5668\u4ef6\u548c\u80fd\u6e90\u7b49\u8bf8\u591a\u9886\u57df\u53d1\u6325\u7740\u91cd\u8981\u4f5c\u7528\u3002\u78b3\u57fa\u7ea4\u7ef4\u5177\u6709\u8010\u9ad8\u6e29\u3001\u4e0d\u6eb6\u4e14\u5f3a\u5206\u5b50\u95f4\u76f8\u4e92\u4f5c\u7528\u529b\u7684\u7279\u70b9\uff0c\u4f7f\u5f97\u78b3\u57fa\u7ea4\u7ef4\u7f16\u7ec7\u7269\u7684\u6574\u4f53\u6027\u80fd\u76f8\u5bf9\u78b3\u57fa\u7ea4\u7ef4\u6709\u660e\u663e\u7684\u4e0b\u964d\u3002\u4e00\u7ef4\u77f3\u58a8\u70ef\u7ea4\u7ef4\u662f\u7531\u7eb3\u7c73\u7ea7\u7684\u5355\u5c42\u6c27\u5316\u77f3\u58a8\u70ef\u7247\uff0c\u4e0d\u4f46\u5f3a\u5ea6\u9ad8\uff0c\u800c\u4e14\u97e7\u6027\u597d\uff0c\u53ef\u4ee5\u6253\u6210\u7ed3\u6216\u8005\u7f16\u7ec7\u6210\u5bfc\u7535\u7684\u7ea4\u7ef4\u7f16\u7ec7\u7269\u3002\u73b0\u6709\u5316\u5b66\u6c14\u76f8\u6c89\u79ef\u6cd5\u3001\u9759\u7535\u7eba\u4e1d\u6cd5\u7528\u4e8e\u5236\u5907\u77f3\u58a8\u70ef\u7f51\u72b6\u7f16\u5236\u7269\u3002\u4e3a\u5b9e\u73b0\u9ad8\u5bfc\u70ed\u7387\u548c\u5bfc\u7535\u7387\u7684\u77f3\u58a8\u70ef\u7f51\u72b6\u7f16\u7ec7\u7269\uff0c\u672c\u6587\u4e2d\u7684\u7814\u7a76\u4eba\u5458\u5728\u8fde\u7eed\u5316\u6e7f\u6cd5\u7eba\u4e1d\u6280\u672f\u7684\u57fa\u7840\u4e4b\u4e0a\u6210\u529f\u7814\u5236\u51fa\u4e86\u7b2c\u4e00\u5757\u7531\u7eaf\u77f3\u58a8\u70ef\u7ea4\u7ef4\u6784\u6210\u7684\u7ec7\u7269\u3002\u8be5\u77f3\u58a8\u70ef\u7ec7\u7269\u5b8c\u5168\u7531\u77f3\u58a8\u70ef\u7ea4\u7ef4\u6784\u6210\uff0c\u65e0\u9700\u6dfb\u52a0\u4efb\u4f55\u7c98\u63a5\u5242\uff0c\u4ec5\u5229\u7528\u6c27\u5316\u77f3\u58a8\u70ef\u7ea4\u7ef4\u95f4\u7684\u81ea\u878d\u5408\u73b0\u8c61\u4f7f\u5f97\u7ea4\u7ef4\u5728\u63a5\u89e6\u7ed3\u70b9\u5904\u878d\u4e3a\u4e00\u4f53\u3002\u56e0\u6b64\uff0c\u8be5\u77f3\u58a8\u70ef\u7ea4\u7ef4\u7ec7\u7269\u5728\u9ad8\u6e29\u77f3\u58a8\u5316\u540e\u8868\u73b0\u51fa\u6781\u9ad8\u7684\u7ed3\u6784\u7a33\u5b9a\u6027\u548c\u5bfc\u7535\u5bfc\u70ed\u6027\u80fd\u3002\u540c\u65f6\uff0c\u8be5\u7ec7\u7269\u501f\u7528\u4e86\u65e0\u7eba\u5e03\u7684\u7ed3\u6784\u5f62\u5f0f\uff0c\u4f7f\u77f3\u58a8\u70ef\u77ed\u7ea4\u7ef4\u968f\u673a\u53d6\u5411\u5e76\u642d\u63a5\u6210\u7f51\u7edc\u7ed3\u6784\uff0c\u5927\u5927\u7b80\u5316\u4e86\u5236\u5907\u8fc7\u7a0b\uff0c\u6709\u5229\u4e8e\u89c4\u6a21\u5316\u751f\u4ea7\u3002<\/p>\n<p style=\"padding-left: 30px;\"><strong><b>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/b><\/strong><\/p>\n<p style=\"padding-left: 30px;\"><strong><b>\u56fe1<\/b><\/strong><strong><b>.\u901a\u8fc7\u6e7f\u6cd5\u878d\u5408\u7ec4\u88c5\u6280\u672f\u5236\u5907\u77f3\u58a8\u70ef\u7ea4\u7ef4\u65e0\u7eba\u5e03<\/b><\/strong><\/p>\n<p style=\"padding-left: 30px;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-59810 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe1.jpg\" width=\"600\" height=\"262\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe1.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe1-300x131.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p style=\"padding-left: 30px;\">(a)\u6e7f\u6cd5\u7eba\u4e1d\u6cd5\u5236\u5907\u4eba\u9020\u6c27\u5316\u77f3\u58a8\u70ef\u77ed\u7ea4\u7ef4\u3002<\/p>\n<p style=\"padding-left: 30px;\">(b)\u521d\u6b65\u5e72\u71e5\u6c27\u5316\u77f3\u58a8\u70ef\u7ea4\u7ef4\u3002<\/p>\n<p style=\"padding-left: 30px;\">(c)\u5c06\u5e72\u71e5\u540e\u7684\u6c27\u5316\u77f3\u58a8\u70ef\u7ea4\u7ef4\u5206\u6563\u5728\u4e59\u9187\u548c\u6c34\u7684\u6df7\u5408\u6db2\u4e2d\u3002<\/p>\n<p style=\"padding-left: 30px;\">(d)\u8fc7\u6ee4\u5f97\u5230\u6e7f\u6cd5\u878d\u5408\u7ec4\u88c5\u7684\u3002<\/p>\n<p style=\"padding-left: 30px;\">(e)\u5e72\u71e5\u540e\u5f97\u5230\u8910\u8272\u7684\u6c27\u5316\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u3002<\/p>\n<p style=\"padding-left: 30px;\">(f)\u7ecf\u9ad8\u6e29\u6216\u5316\u5b66\u8fd8\u539f\u5f97\u5230\u7531\u6742\u4e71\u65e0\u5e8f\u7684\u77f3\u58a8\u70ef\u7ea4\u7ef4\u7ec4\u6210\u7684\u9ed1\u8272\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u3002<\/p>\n<p style=\"padding-left: 30px;\"><strong><b>\u00a0<\/b><\/strong><strong><b>\u56fe2\uff1a<\/b><\/strong><strong><b>\u6e7f\u6cd5\u878d\u5408\u7ec4\u88c5\u673a\u7406\u4ee5\u53ca\u6c27\u5316\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u548c\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u7684\u5f62\u8c8c<\/b><\/strong><\/p>\n<p style=\"padding-left: 30px;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-59811 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe2.jpg\" width=\"600\" height=\"470\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe2.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe2-300x235.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p style=\"padding-left: 30px;\">\u5728(a) \u5149\u5b66\u663e\u5fae\u955c\u548c(b) \u5149\u5b66\u663e\u5fae\u955c\u4e0b\uff0c\u6c27\u5316\u77f3\u58a8\u70ef\u7ea4\u7ef4\u5206\u6563\u5728\u4e59\u9187\u548c\u6c34\u7684\u6df7\u5408\u6db2\u4e2d\u7684\u5f62\u8c8c\u3002<\/p>\n<p style=\"padding-left: 30px;\">(c) \u6e7f\u6cd5\u878d\u5408\u540e\u7684\u6c27\u5316\u77f3\u58a8\u70ef\u7ea4\u7ef4\u5728\u5149\u5b66\u663e\u5fae\u955c\u548c\u5149\u5b66\u663e\u5fae\u955c\u4e0b\u7684\u5f62\u6001\u3002<\/p>\n<p style=\"padding-left: 30px;\">(d) \u5728\u53d1\u5149\u4e8c\u6781\u7ba1\u7167\u5c04\u4e0b\uff0c\u539a\u5ea6\u4e3a0.05 mm\u7684\u6c27\u5316\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u5448\u591a\u5b54\u6d45\u68d5\u8272\u3002<\/p>\n<p style=\"padding-left: 30px;\">(e) \u539a\u5ea6\u4e3a3 mm\u7684\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u5448\u9ed1\u68d5\u8272\u3002<\/p>\n<p style=\"padding-left: 30px;\">(f) \u8fdb\u9ad8\u6e29\u7145\u70e7\u8fd8\u539f\u7684\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u53ef\u7528\u4e8e\u5149\u548c\u7a7a\u6c14\u8fc7\u6ee4\u3002<\/p>\n<p style=\"padding-left: 30px;\">(g) \u6c27\u5316\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\uff08\u5de6\u56fe\uff09\u4e0e\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\uff08\u53f3\u56fe\uff09\u5bf9\u6bd4\u8868\u660e\uff1a\u8fd8\u539f\u540e\u65e0\u7eba\u5e03\u7684\u76f4\u5f84\u548c\u989c\u8272\u6709\u8f7b\u5fae\u7684\u53d8\u5316\u3002<\/p>\n<p style=\"padding-left: 30px;\">(h) \u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u5e03\u6761\u7f20\u7ed5\u5728\u73bb\u7483\u68d2\u4e0a\u3002<\/p>\n<p style=\"padding-left: 30px;\">(i) \u56db\u4e2a\u4e0d\u540c\u76f4\u5f84\u548c\u539a\u5ea6\u7684\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u3002<\/p>\n<p style=\"padding-left: 30px;\">\u5176\u4e2d\uff0c\u4e0a\u8ff0\u56fe\u7684\u6bd4\u4f8b\u5c3a\u5206\u522b\u4e3a\uff1a500 mm (a, b), 150 mm (c) and 20mm (d, f, h, i)\u3002<\/p>\n<p style=\"padding-left: 30px;\"><strong><b>\u00a0<\/b><\/strong><strong><b>\u56fe3\uff1a<\/b><\/strong><strong><b>\u6c27\u5316\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u548c\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u7684\u8868\u5f81<\/b><\/strong><\/p>\n<p style=\"padding-left: 30px;\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-59812 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe3.jpg\" alt=\"\" width=\"600\" height=\"508\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe3.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe3-300x254.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p style=\"padding-left: 30px;\">(a) \u6c27\u5316\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u3001\u6c34\u5408\u80bc\u8fd8\u539f\u7684\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u3001\u4e0d\u540c\u6e29\u5ea6\u7145\u70e7\u8fd8\u539f\u7684\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03(1000, 2000 \u548c3000 <sup>o<\/sup>C)\u7684XPS\u56fe\u3002<\/p>\n<p style=\"padding-left: 30px;\">(b) \u6c27\u5316\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u3001\u6c34\u5408\u80bc\u8fd8\u539f\u7684\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u3001\u4e0d\u540c\u6e29\u5ea6\u7145\u70e7\u8fd8\u539f\u7684\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u7684XRD\u56fe\u3002<\/p>\n<p style=\"padding-left: 30px;\">(c)\u00a0\u6c27\u5316\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u3001\u6c34\u5408\u80bc\u8fd8\u539f\u7684\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u3001\u4e0d\u540c\u6e29\u5ea6\u7145\u70e7\u8fd8\u539f\u7684\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u7684\u62c9\u66fc\u56fe\u3002<\/p>\n<p style=\"padding-left: 30px;\">(d) I<sub>D<\/sub>\/I<sub>G<\/sub>\u6bd4\u503c\u7684\u53d8\u5316\u3002<\/p>\n<p style=\"padding-left: 30px;\"><strong><b>\u00a0<\/b><\/strong><strong><b>\u56fe4\uff1a<\/b><\/strong><strong><b>\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u7684\u7535\u70ed\u6027\u548c\u5bfc\u7535\u6027 <\/b><\/strong><strong><b><br \/>\n<\/b><\/strong><\/p>\n<p style=\"padding-left: 30px;\"><strong><b><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-59813 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe4.jpg\" alt=\"\" width=\"600\" height=\"214\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe4.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe4-300x107.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p style=\"padding-left: 30px;\">(a) 130GFF\uff08\u9488\u5934\u76f4\u5f84\u4e3a130\u00b5m\u5236\u5f97\u7684\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\uff09\u4e0e200GFF\uff08\u9488\u5934\u76f4\u5f84\u4e3a130\u00b5m\u5236\u5f97\u7684\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\uff09\u7684\u5bfc\u70ed\u6027\u548c\u5bfc\u7535\u6027\u5bf9\u6bd4\u56fe\u3002<\/p>\n<p style=\"padding-left: 30px;\">(b) \u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u4e0e\u4e8c\u7ef4\u81ea\u7ec4\u88c5\u7684\u78b3\u7eb3\u7c73\u7ba1\u548c\u77f3\u58a8\u70ef\u5173\u4e8e\u6bd4\u5bfc\u70ed\u7387\u548c\u6bd4\u5bfc\u7535\u7387\u5bf9\u6bd4\u56fe\u3002<\/p>\n<p style=\"padding-left: 30px;\"><strong><b>\u00a0\u56fe5<\/b><\/strong><strong><b>\uff1a<\/b><\/strong><strong><b>\u6c27\u5316\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u548c\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u7684\u5fae\u89c2\u5f62\u8c8c <\/b><\/strong><\/p>\n<p style=\"padding-left: 30px;\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-59814 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe5.jpg\" alt=\"\" width=\"600\" height=\"455\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe5.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe5-300x228.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p style=\"padding-left: 30px;\">(a)-(c)\u5206\u522b\u4e3a130GFF\uff0c130GFF\u7145\u70e73000 <sup>o<\/sup>C (130GFF-3000)\u4e0e200GFF\u7684SEM\u56fe\u3002<\/p>\n<p style=\"padding-left: 30px;\">(d)-(f) \u5206\u522b\u4e3a130GFF\uff0c130GFF\u7145\u70e73000 <sup>o<\/sup>C\u4e0e200GFF\u7684\u9ad8\u500d\u7387SEM\u56fe\u3002<\/p>\n<p style=\"padding-left: 30px;\">(g) \u7145\u70e7\u8fd8\u539f\u524d\uff0c130GOFF\u8868\u73b0\u4e3aX\u578b\u4ea4\u53c9\u7ed3\u7ed3\u6784\u3002<\/p>\n<p style=\"padding-left: 30px;\">(h) 3000 <sup>o<\/sup>C\u4e0b\u7145\u70e7\u8fd8\u539f\u540e\uff0c130GFF-3000\u8868\u73b0\u4e3aY\u578b\u4ea4\u53c9\u7ed3\u7ed3\u6784\u3002<\/p>\n<p style=\"padding-left: 30px;\">(i) 130GFF-3000\u7834\u788e\u8fb9\u7f18\u90e8\u5206\u4ecd\u4fdd\u6301Y\u578b\u4ea4\u53c9\u7ed3\u7ed3\u6784\u3002<\/p>\n<p style=\"padding-left: 30px;\">\u5176\u4e2d\uff0c\u4e0a\u8ff0\u56fe\u7684\u6bd4\u4f8b\u5c3a\u5206\u522b\u4e3a\uff1a500 mm (a-c), 100 mm (d, e, f, i) and 50 mm (g, h).<\/p>\n<p style=\"padding-left: 30px;\"><strong><b>\u56fe6<\/b><\/strong><strong><b>\uff1a<\/b><\/strong><strong><b>\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u7684<\/b><\/strong><strong><b>\u7ed3\u6784\u7a33\u5b9a\u6027\u548c\u529b\u5b66\u6027\u80fd\u7814\u7a76<\/b><\/strong><\/p>\n<p style=\"padding-left: 30px;\"><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-59815 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe6.jpg\" alt=\"\" width=\"600\" height=\"406\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe6.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe6-300x203.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p style=\"padding-left: 30px;\">\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u7684\u7535\u963b\u7387\u7684\u53d8\u5316\uff1a\u5f2f\u66f2\u534a\u5f84\u8fbe\u52301.5mm (a), \u91cd\u590d\u5f2f\u66f21000\u5faa\u73af (b), \u5f2f\u66f2-\u6253\u5f00\u5faa\u73af10\u6b21\u3002<\/p>\n<p style=\"padding-left: 30px;\">(d) \u4e0e200GFF-3000\u7684\u5e94\u529b-\u5e94\u53d8\u66f2\u7ebf\u56fe\uff0c\u63d2\u56fe\u4e3a130GFF-3000\u7684\u5e94\u529b-\u5e94\u53d8\u653e\u5927\u56fe\u3002<\/p>\n<p style=\"padding-left: 30px;\">(e) \u5728\u5916\u5f20\u5e94\u529b\u4f5c\u7528\u4e0b\uff0c\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u7684\u65ad\u88c2\u8fc7\u7a0b\u56fe\u3002<\/p>\n<p style=\"padding-left: 30px;\">(f)-(g) \u5206\u522b\u4e3a\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u65ad\u88c2\u8fc7\u7a0b\u4e2d\uff0c\u7b2c\u4e8c\u9636\u6bb5\u548c\u7b2c\u4e09\u9636\u6bb5\u7684\u88c2\u7eb9\u6269\u5f20SEM\u56fe\uff0c\u6bd4\u4f8b\u5c3a\u4e3a100 \u00b5m\u3002<\/p>\n<p style=\"padding-left: 30px;\"><strong><b>\u00a0<\/b><\/strong><strong><b>\u56fe<\/b><\/strong><strong><b>7<\/b><\/strong><strong><b>\uff1a<\/b><\/strong><strong><b>\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u7684<\/b><\/strong><strong><b>\u7535\u70ed\u6027\u80fd<\/b><\/strong><strong><b>\u7814\u7a76<\/b><\/strong><strong><b><br \/>\n<\/b><\/strong><\/p>\n<p style=\"padding-left: 30px;\"><strong><b><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-59816 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe7.jpg\" alt=\"\" width=\"600\" height=\"555\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe7.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe7-300x278.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p style=\"padding-left: 30px;\">(a) \u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u7528\u4e8e\u7535\u52a0\u70ed\u7684\u88c5\u7f6e\u56fe\u3002<\/p>\n<p style=\"padding-left: 30px;\">(b) \u5728\u65bd\u52a0\u4e0d\u540c\u7535\u538b\u4e0b\uff0c\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03 (\u9762\u79ef\u4e3a4\u00d72 cm<sup>2<\/sup>) \u7684\u6e29\u5ea6\u66f2\u7ebf\u56fe\u3002<\/p>\n<p style=\"padding-left: 30px;\">(c) \u5347\u6e29\u901f\u7387\u4e0e\u964d\u6e29\u901f\u7387\u7684\u6700\u5927\u503c\u4e0e\u8f93\u5165\u529f\u7387\u6240\u80fd\u8fbe\u5230\u7684\u9971\u548c\u6e29\u5ea6\u7684\u5173\u7cfb\u56fe\u3002<\/p>\n<p style=\"padding-left: 30px;\">(d) \u65bd\u52a0\u4e0d\u540c\u9891\u7387\u7535\u538b\uff0c\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u7684\u6e29\u5ea6\u968f\u7740\u7535\u538b\u7684\u54cd\u5e94\u66f2\u7ebf\u56fe\u3002<\/p>\n<p style=\"padding-left: 30px;\">(e) \u4e0a\u534a\u90e8\u5206\u4e3a\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u5e73\u94fa\u3001\u5f2f\u66f2180<sup>o<\/sup>\u4ee5\u53ca\u5f2f\u66f2100\u5faa\u73af\u540e\u7684\u7535\u538b\u4e0e\u9971\u548c\u6e29\u5ea6\u5173\u7cfb\u56fe\uff0c\u4e0b\u534a\u90e8\u5206\u4e3a\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u5e73\u94fa\u548c\u5f2f\u66f2180<sup>o<\/sup>\u7684\u7ea2\u5916\u56fe\u3002<\/p>\n<p style=\"padding-left: 30px;\">(f) \u901a\u8fc7\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u4e2d\u5fc3\u6c34\u6ef4\u7684\u84b8\u53d1\u8fc7\u7a0b\u8868\u5f81\u53d8\u5316\uff0c\u4e0a\u534a\u90e8\u5206\u4e3a\u6e29\u5ea6\u6f14\u53d8\u548c\u65f6\u95f4\u7684\u5173\u7cfb\u56fe\uff0c\u4e0b\u534a\u90e8\u5206\u4e3a\u6db2\u6ef4\u6325\u53d1\u8fc7\u7a0b\u7684\u7ea2\u5916\u56fe\u3002<\/p>\n<p style=\"padding-left: 30px;\"><strong><b>\u00a0<\/b><\/strong><strong><b>\u56fe<\/b><\/strong><strong><b>8<\/b><\/strong><strong><b>\uff1a<\/b><\/strong><strong><b>\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u7684<\/b><\/strong><strong><b>\u5438\u6cb9<\/b><\/strong><strong><b>\u6027\u80fd\u7814\u7a76<\/b><\/strong><strong><b><br \/>\n<\/b><\/strong><\/p>\n<p style=\"padding-left: 30px;\"><strong><b><img loading=\"lazy\" decoding=\"async\" class=\"alignnone size-full wp-image-59817 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe8.jpg\" alt=\"\" width=\"600\" height=\"464\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe8.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/01\/\u56fe8-300x232.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p style=\"padding-left: 30px;\">(a) \u5bf9\u4e8e\u4e0d\u540c\u6709\u673a\u7269\uff0c\u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u7684\u5438\u9644\u603b\u91cf\u56fe\u3002<\/p>\n<p style=\"padding-left: 30px;\">(b)-(c) \u77f3\u58a8\u70ef\u65e0\u7eba\u5e03\u5728\u6c34\u4e2d\u7ecf\u8fc7\u5267\u70c8\u6405\u62cc\u4ecd\u65e7\u4fdd\u6301\u539f\u6765\u7684\u5f62\u72b6\u3002<\/p>\n<p style=\"padding-left: 30px;\">(d) \u77f3\u58a8\u70ef\u6c14\u51dd\u80f6\u5728\u6c34\u4e2d\u7ecf\u4e2d\u5ea6\u6405\u62cc\u4e0b\u53d8\u6210\u788e\u7247\u3002<\/p>\n<p style=\"padding-left: 30px;\">(e) \u5728\u5e9a\u70f7\u4e2d\u77f3\u58a8\u70ef\u5438\u6cb9\u6be1\u8868\u73b0\u6770\u51fa\u7684\u5feb\u5438\u80fd\u529b(\u4e0d\u8d85\u8fc71s)\u3002<\/p>\n<p style=\"padding-left: 30px;\">(f) \u77f3\u58a8\u70ef\u5438\u6cb9\u6be1\u7684\u5faa\u73af\u5438\u9644\u6027\u80fd\u56fe\u3002<\/p>\n<p style=\"padding-left: 30px;\">(g) \u77f3\u58a8\u70ef\u5438\u6cb9\u6be1\u7ecf\u8fc720\u6b21\u5438\u9644-\u71c3\u70e7\u5faa\u73af\uff0c\u5176\u5f62\u8c8c\u548c\u7ed3\u6784\u6ca1\u6709\u53d1\u751f\u53d8\u5316\uff0c\u6bd4\u4f8b\u5c3a\u4e3a50 \u00b5m\u3002<\/p>\n<p style=\"padding-left: 30px;\"><strong><b>\u3010\u5c0f\u7ed3\u3011<\/b><\/strong><\/p>\n<p style=\"padding-left: 30px;\">\u7efc\u4e0a\u6240\u8ff0\uff0c\u7814\u7a76\u4eba\u5458\u5728\u8fde\u7eed\u5316\u6e7f\u6cd5\u7eba\u4e1d\u6280\u672f\u7684\u57fa\u7840\u4e4b\u4e0a\u6210\u529f\u7814\u5236\u51fa\u4e86\u7b2c\u4e00\u5757\u7531\u7eaf\u77f3\u58a8\u70ef\u7ea4\u7ef4\u6784\u6210\u7684\u7ec7\u7269\u3002\u8fd9\u79cd\u77f3\u58a8\u70ef\u7ea4\u7ef4\u65e0\u7eba\u5e03\u5177\u6709\u975e\u5e38\u597d\u7684\u67d4\u6027\uff0c\u5bfc\u7535\u548c\u5bfc\u70ed\u6027\u80fd\u5206\u522b\u8fbe\u523028000 S\/m\u548c301 W\/mK\uff0c\u800c\u5bc6\u5ea6\u4ec5\u67090.22 \u514b\u6bcf\u7acb\u65b9\u5398\u7c73\uff0c\u5176\u6bd4\u5bfc\u7535\u7387\u548c\u6bd4\u5bfc\u70ed\u7387\u8fdc\u8fdc\u9ad8\u4e8e\u5df2\u62a5\u9053\u7684\u78b3\u57fa\u4e8c\u7ef4\u7ec7\u7269\u3001\u8584\u819c\u6750\u6599\u53ca\u5546\u4e1a\u5316\u7684\u78b3\u7ea4\u7ef4\u7eb8\u3002\u540c\u5546\u4e1a\u5316\u7684\u7535\u52a0\u70ed\u5143\u4ef6\u76f8\u6bd4\uff0c\u77f3\u58a8\u70ef\u7ea4\u7ef4\u65e0\u7eba\u5e03\u5177\u6709\u5feb\u901f\u70ed\u54cd\u5e94\u53ca\u9ad8\u5de5\u4f5c\u6e29\u5ea6\u7b49\u663e\u8457\u4f18\u52bf\u3002\u540c\u65f6\uff0c\u8be5\u65e0\u7eba\u5e03\u5bf9\u6709\u673a\u7269\u7684\u5438\u9644\u91cf\u548c\u5438\u9644\u901f\u5ea6\u660e\u663e\u4f18\u4e8e\u5546\u4e1a\u5316\u7684\u5438\u6cb9\u6be1\u3002\u57fa\u4e8e\u4ee5\u4e0a\u4f18\u5f02\u6027\u80fd\uff0c\u77f3\u58a8\u70ef\u7ea4\u7ef4\u65e0\u7eba\u5e03\u53ef\u88ab\u7528\u4f5c\u80fd\u6e90\u9886\u57df\u7684\u7535\u6781\u6750\u6599\u3001\u5feb\u901f\u9ad8\u6548\u7684\u7535\u70ed\u7ec7\u7269\u4ee5\u53ca\u5438\u9644\u6709\u673a\u7269\u7684\u5438\u6cb9\u7eb8\u3002<\/p>\n<p style=\"padding-left: 30px;\"><strong><b>\u6587\u732e\u94fe\u63a5\uff1a<\/b><\/strong><a href=\"http:\/\/www.nature.com\/articles\/ncomms13684\" target=\"_blank\"><u>Multifunctional non-woven fabrics of interfused graphene fibres<\/u><\/a>\u00a0\uff08<strong><b>Nat<\/b><\/strong><strong><b>.<\/b><\/strong><strong><b>\u00a0Commun<\/b><\/strong><strong><b>. <\/b><\/strong>2016, DOI: 10.1038\/ncomms13684\uff09<\/p>\n<p style=\"padding-left: 30px;\">\u8be5\u6587\u732e\u6c47\u603b\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u7eb3\u7c73\u5b66\u672f\u7ec4\u738b\u7545\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u7f16\u8f91\u6574\u7406\u3002<\/p>\n<p style=\"padding-left: 30px;\">\u6750\u6599\u725b\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u8fd9\u91cc\u6c47\u96c6\u4e86\u5404\u5927\u9ad8\u6821\u7855\u535a\u751f\u3001\u4e00\u7ebf\u79d1\u7814\u4eba\u5458\u4ee5\u53ca\u884c\u4e1a\u4ece\u4e1a\u8005\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\"><strong>\u70b9\u6211\u52a0\u5165\u7f16\u8f91\u90e8<\/strong><\/a>\u3002<\/p>\n<p style=\"padding-left: 30px;\">\u6750\u6599\u4eba\u7f51\u5c0a\u91cd\u6240\u6709\u8fdb\u884c\u77e5\u8bc6\u4f20\u64ad\u7684\u5a92\u4f53\uff0c\u8f6c\u8f7d\u8bf7\u8054\u7cfbtougao@cailiaoren.com<\/p>\n<p style=\"padding-left: 30px;\"><strong><b>\u6750\u6599\u6d4b\u8bd5\uff0c\u6570\u636e\u5206\u6790\uff0c\u4e0a<\/b><a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\"><b>\u6d4b\u8bd5\u8c37<\/b><\/a><b>\uff01<\/b><\/strong><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8bed\u3011 2016\u5e7411\u670816\u65e5\uff0cNat. Commun.\u00a0\u7f51\u7ad9\u5728\u7ebf\u53d1\u8868\u4e86\u9898\u4e3a\u201cMultifunctional non-woven fabrics of int&#8230;<\/p>\n","protected":false},"author":2338,"featured_media":59811,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[46],"class_list":["post-57116","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","tag-graphene"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/57116"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/2338"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=57116"}],"version-history":[{"count":8,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/57116\/revisions"}],"predecessor-version":[{"id":59869,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/57116\/revisions\/59869"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/59811"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=57116"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=57116"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=57116"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}