{"id":57923,"date":"2016-12-27T06:30:03","date_gmt":"2016-12-26T22:30:03","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=57923"},"modified":"2017-11-11T23:09:41","modified_gmt":"2017-11-11T15:09:41","slug":"%e5%ad%a6%e6%9c%af%e5%b9%b2%e8%b4%a7%e5%85%b3%e4%ba%8e%e5%8a%a8%e6%80%81%e5%8a%9b%e5%ad%a6%e5%88%86%e6%9e%90dmta%e4%bd%a0%e4%ba%86%e8%a7%a3%e5%a4%9a%e5%b0%91%ef%bc%9f","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=57923","title":{"rendered":"\u5b66\u672f\u5e72\u8d27|\u5173\u4e8e\u52a8\u6001\u529b\u5b66\u5206\u6790(DMTA)\u4f60\u4e86\u89e3\u591a\u5c11\uff1f"},"content":{"rendered":"<p>\u52a8\u6001\u529b\u5b66\u884c\u4e3a\u662f\u6307\u6750\u6599\u5728\u632f\u52a8\u6761\u4ef6\u4e0b\uff0c\u5373\u5728\u4ea4\u53d8\u5e94\u529b\uff08\u4ea4\u53d8\u5e94\u53d8\uff09\u4f5c\u7528\u4e0b\u505a\u51fa\u7684\u529b\u5b66\u54cd\u5e94\uff0c\u5373\u529b\u5b66\u6027\u80fd(\u6a21\u91cf\u3001\u5185\u8017)\u4e0e\u6e29\u5ea6\u3001\u9891\u7387\u7684\u5173\u7cfb\u3002\u6d4b\u5b9a\u6750\u6599\u5728\u4e00\u5b9a\u6e29\u5ea6\u8303\u56f4\u5185\u52a8\u6001\u529b\u5b66\u6027\u80fd\u7684\u53d8\u5316\u5c31\u662f\u52a8\u6001\u529b\u5b66\u70ed\u5206\u6790\uff08Dynamic Mechanical Thermal Analysis\uff0c\u7b80\u79f0DMTA\uff09\u6216\u52a8\u6001\u529b\u5b66\u5206\u6790\uff08 Dynamic Mechanical Analysis\uff0c\u7b80\u79f0DMA\uff09\u3002<\/p>\n<p><span style=\"color: #0000ff;\"><strong>\u52a8\u6001\u529b\u5b66\u6027\u80fd\u6d4b\u91cf\u539f\u7406\u00a0<\/strong><\/span><\/p>\n<p><strong>(1)\u805a\u5408\u7269\u7684\u7c98\u5f39\u884c\u4e3a \u00a0<\/strong><\/p>\n<p>\uff08a\uff09\u5f39\u6027\u53d8\u5f62\u4f53\u7cfb\uff1a\u5e94\u529b\u4e0e\u5e94\u53d8\u6210\u6b63\u6bd4\uff0c\u6ee1\u8db3\u80e1\u514b\u5b9a\u5f8b\uff1b\u5916\u529b\u53bb\u9664\u540e\uff0c\u53d8\u5f62\u53ef\u4ee5\u5b8c\u5168\u6062\u590d\u3002\u5916\u529b\u6240\u505a\u7684\u529f\u5b8c\u5168\u8f6c\u5316\u4e3a\u4f53\u7cfb\u7684\u52bf\u80fd\u3002<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-57925\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/\u5c4f\u5e55\u5feb\u7167-2016-12-20-\u4e0b\u53485.08.34.png\" alt=\"\" width=\"646\" height=\"41\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/\u5c4f\u5e55\u5feb\u7167-2016-12-20-\u4e0b\u53485.08.34.png 646w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/\u5c4f\u5e55\u5feb\u7167-2016-12-20-\u4e0b\u53485.08.34-300x19.png 300w\" sizes=\"(max-width: 646px) 100vw, 646px\" \/><\/p>\n<p>\uff08b\uff09\u7c98\u6027\u4f53\u7cfb\uff1a\u5916\u529b\u4f5c\u7528\u4e0b\u6240\u4ea7\u751f\u7684\u53d8\u5f62\u5b8c\u5168\u4e0d\u80fd\u6062\u590d\uff0c\u5916\u529b\u5bf9\u4f53\u7cfb\u6240\u505a\u7684\u529f\u5b8c\u5168\u8f6c\u5316\u4e3a\u70ed\u80fd\u6d88\u8017\u6389\u3002<\/p>\n<p>\uff08c\uff09\u7c98\u5f39\u6027\u4f53\u7cfb\uff1a\u5728\u5916\u529b\u4f5c\u7528\u4e0b\uff0c\u805a\u5408\u7269\u5206\u5b50\u94fe\u7531\u5377\u66f2\u72b6\u6001\u8f6c\u53d8\u4e3a\u4f38\u5c55\uff0c\u8be5\u8fc7\u7a0b\u6240\u53d1\u751f\u7684\u53d8\u5f62\u5c5e\u4e8e\u5f39\u6027\u53d8\u5f62\u3002<\/p>\n<p><strong>(2)\u632f\u52a8\u8d1f\u8377\u4e0b\u7684\u5e94\u529b\u4e0e\u5e94\u53d8\u00a0<\/strong><\/p>\n<p>\uff08a\uff09\u5b8c\u5168\u5f39\u6027\u4f53\u7cfb\uff1a\u5982\u56fe1\uff08a\uff09\u6240\u793a\u5f53\u6750\u6599\u53d7\u5230\u6b63\u5f26\u4ea4\u53d8\u5e94\u529b\u4f5c\u7528\u65f6\uff0c\u5e94\u53d8\u5bf9\u5e94\u529b\u7684\u54cd\u5e94\u662f\u77ac\u95f4\u7684\uff0c\u6bcf\u4e00\u5468\u671f\u80fd\u91cf\u65e0\u635f\u8017\uff0c\u6b64\u65f6\u6709\uff1a<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-57926\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/\u5c4f\u5e55\u5feb\u7167-2016-12-20-\u4e0b\u53485.09.52.png\" alt=\"\" width=\"218\" height=\"110\" \/><\/p>\n<p>(b) \u5b8c\u5168\u7c98\u6027\u4f53\u7cfb\uff0c\u5982\u56fe1\uff08b\uff09\u6240\u793a\uff0c\u5e94\u53d8\u54cd\u5e94\u6ede\u540e\u4e8e\u5e94\u529b90\u00b0\u76f8\u4f4d\u89d2\uff1b<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-57927\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/\u5c4f\u5e55\u5feb\u7167-2016-12-20-\u4e0b\u53485.10.19.png\" alt=\"\" width=\"217\" height=\"131\" \/><\/p>\n<p>\uff08c\uff09\u5bf9\u4e8e\u7c98\u5f39\u6027\u6750\u6599\uff0c\u5e94\u53d8\u5c06\u59cb\u7ec8\u6ede\u540e\u4e8e\u5e94\u529b0\u00b0-90\u00b0\u7684\u76f8\u4f4d\u89d2\u03b4\uff0c\u5982\u56fe1\uff08c\uff09\u6240\u793a\u5e76\u4e14\u5e94\u529b\u5e94\u53d8\u53ef\u4ee5\u7528\u4e0b\u5f0f\u6765\u8868\u8fbe\uff1a<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-57928\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/\u5c4f\u5e55\u5feb\u7167-2016-12-20-\u4e0b\u53485.10.53.png\" alt=\"\" width=\"240\" height=\"102\" \/><\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-57929\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/1-19.png\" alt=\"\" width=\"700\" height=\"500\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/1-19.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/1-19-300x214.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p style=\"text-align: center;\"><strong>\u56fe1\u5e94\u529b\uff08\u5e94\u53d8\uff09\u6b63\u5f26\u66f2\u7ebf\u66f2\u7ebf<\/strong><\/p>\n<p>\u5bf9\u4e8e\u805a\u5408\u7269\u7c98\u6027\u4f53\u7cfb\uff0c\u5e94\u529b\u4e0e\u5e94\u53d8\u5b58\u5728\u76f8\u4f4d\u5dee<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-57940\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/\u5c4f\u5e55\u5feb\u7167-2016-12-20-\u4e0b\u53485.12.46.png\" alt=\"\" width=\"605\" height=\"100\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/\u5c4f\u5e55\u5feb\u7167-2016-12-20-\u4e0b\u53485.12.46.png 605w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/\u5c4f\u5e55\u5feb\u7167-2016-12-20-\u4e0b\u53485.12.46-300x50.png 300w\" sizes=\"(max-width: 605px) 100vw, 605px\" \/><\/p>\n<p>\u5c06\uff083\uff09\u5c55\u5f00\uff0c\u53ef\u4ee5\u5f97\u5230\uff1a<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-57942\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/\u5c4f\u5e55\u5feb\u7167-2016-12-20-\u4e0b\u53485.13.17.png\" alt=\"\" width=\"617\" height=\"100\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/\u5c4f\u5e55\u5feb\u7167-2016-12-20-\u4e0b\u53485.13.17.png 617w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/\u5c4f\u5e55\u5feb\u7167-2016-12-20-\u4e0b\u53485.13.17-300x49.png 300w\" sizes=\"(max-width: 617px) 100vw, 617px\" \/><\/p>\n<p>\u7ed3\u5408\uff082\uff09\u3001\uff084\uff09\uff0c\u53ef\u4ee5\u5f97\u5230<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-57943\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/\u5c4f\u5e55\u5feb\u7167-2016-12-20-\u4e0b\u53485.13.41.png\" alt=\"\" width=\"675\" height=\"192\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/\u5c4f\u5e55\u5feb\u7167-2016-12-20-\u4e0b\u53485.13.41.png 675w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/\u5c4f\u5e55\u5feb\u7167-2016-12-20-\u4e0b\u53485.13.41-300x85.png 300w\" sizes=\"(max-width: 675px) 100vw, 675px\" \/><\/p>\n<p>\u5176\u4e2d\uff0c\u03c9\u662f\u89d2\u9891\u7387\uff0c\u03b4\u662f\u76f8\u4f4d\u89d2\uff0c\u03c3<sub>0<\/sub>\u662f\u5e94\u529b\u5cf0\u503c\uff0c\u03b5<sub>0<\/sub>\u662f\u5e94\u53d8\u5cf0\u503c\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-57944 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/\u5c4f\u5e55\u5feb\u7167-2016-12-20-\u4e0b\u53485.14.23.png\" alt=\"\" width=\"212\" height=\"54\" \/><\/p>\n<p>\u8d2e\u80fd\u6a21\u91cf\uff1a\u8868\u793a\u5728\u5e94\u529b\u4f5c\u7528\u4e0b\u80fd\u91cf\u5728\u6837\u54c1\u4e2d\u7684\u8d2e\u5b58\u80fd\u529b\uff0c\u540c\u65f6\u4e5f\u662f\u6750\u6599\u521a\u6027\u7684\u53cd\u6620\uff1b<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-57945 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/\u5c4f\u5e55\u5feb\u7167-2016-12-20-\u4e0b\u53485.14.28.png\" alt=\"\" width=\"220\" height=\"48\" \/><\/p>\n<p>\u635f\u8017\u6a21\u91cf\uff1a\u4e0e\u5e94\u53d8\u76f8\u4f4d\u5dee90\u5ea6\uff1b\u8868\u793a\u80fd\u91cf\u7684\u635f\u8017\u7a0b\u5ea6\uff0c\u662f\u6750\u6599\u8017\u6563\u80fd\u91cf\u7684\u80fd\u529b\u53cd\u6620\uff1b<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-57946 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/\u5c4f\u5e55\u5feb\u7167-2016-12-20-\u4e0b\u53485.14.34.png\" alt=\"\" width=\"162\" height=\"47\" \/><\/p>\n<p>\u5185\u8017\uff1a\u5e94\u529b\u5e94\u53d8\u76f8\u4f4d\u89d2\u4e4b\u6b63\u5207\u503c\uff0c\u662f\u6750\u6599\u8d2e\u80fd\u4e0e\u8017\u80fd\u80fd\u529b\u7684\u76f8\u5bf9\u5f3a\u5ea6\u3002<\/p>\n<p><strong><span style=\"color: #0000ff;\">\u52a8\u6001\u529b\u5b66\u5206\u6790\u6280\u672f<\/span><\/strong><\/p>\n<p>\u805a\u5408\u7269\u52a8\u6001\u529b\u5b66\u8bd5\u9a8c\u65b9\u6cd5\u5f88\u591a\uff0c\u6309\u7167\u5f62\u53d8\u6a21\u5f0f\u5206\u4e3a\u62c9\u4f38\u3001\u538b\u7f29\u3001\u5f2f\u66f2\u3001\u626d\u8f6c\u3001\u526a\u5207\u7b49\u3002\u6d4b\u5f97\u7684\u6a21\u91cf\u53d6\u51b3\u4e8e\u5f62\u53d8\u6a21\u5f0f\uff0c\u56e0\u800c\u5f39\u6027\u6a21\u91cf\u6709\u62c9\u4f38\u6a21\u91cf\u3001\u538b\u7f29\u6a21\u91cf\u3001\u526a\u5207\u6a21\u91cf\u7b49\u4e4b\u5206\uff1b\u6309\u7167\u632f\u52a8\u6a21\u5f0f\u5206\u4e3a\u81ea\u7531\u8870\u51cf\u632f\u52a8\u6cd5\u3001\u5f3a\u8feb\u5171\u632f\u6cd5\u3001\u5f3a\u8feb\u975e\u5171\u632f\u6cd5\u7b49\u3002<\/p>\n<p>DMA\u5de5\u4f5c\u539f\u7406\u2014\u2014\u5f3a\u8feb\u975e\u5171\u632f\u6cd5\uff1a\uff081\uff09\u8bd5\u6837\u5206\u522b\u4e0e\u9a71\u52a8\u5668\u3001\u5e94\u53d8\u4f4d\u79fb\u4f20\u611f\u5668\u76f8\u8fde\u63a5\uff1b\uff082\uff09\u9a71\u52a8\u5668\u5c06\u4e00\u5b9a\u9891\u7387\u7684\u6b63\u5f26\u4ea4\u53d8\u4f5c\u7528\u65bd\u52a0\u5230\u8bd5\u6837\u4e0a\uff1b\uff083\uff09\u7531\u5e94\u53d8\u4f4d\u79fb\u4f20\u611f\u5668\u68c0\u6d4b\u51fa\u5e94\u53d8\u7684\u6b63\u5f26\u4fe1\u53f7\uff1b\uff084\uff09\u901a\u8fc7\u5e94\u529b\u632f\u5e45\u4e0e\u5e94\u53d8\u632f\u5e45\u7684\u4f4d\u7f6e\u6bd4\u8f83\uff0c\u5f97\u5230\u5e94\u529b\u4e0e\u5e94\u53d8\u7684\u76f8\u4f4d\u5dee\uff1b\uff085\uff09\u7ecf\u8fc7\u4eea\u5668\u7684\u81ea\u52a8\u5904\u7406\uff0c\u5f97\u5230\u50a8\u80fd\u6a21\u91cfE\u00b4\u3001\u635f\u8017\u6a21\u91cfE&#8221;\u3001\u529b\u5b66\u635f\u8017tg\u03b4\u3002\u56fe2\u4e3aQ800 DMA\u4eea\u5668\u7ed3\u6784\u56fe\uff1a<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-57930\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/2-16.png\" alt=\"\" width=\"700\" height=\"520\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/2-16.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/2-16-300x223.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p style=\"text-align: center;\"><strong>\u56fe2 Q800 DMA\u4eea\u5668\u7ed3\u6784\u56fe<\/strong><\/p>\n<p>\u5b9e\u9a8c\u6280\u672f\uff1a\uff081\uff09\u4ea4\u53d8\u4f5c\u7528\u7cfb\u7edf\u2014\u2014\u5f2f\u66f2\u3001\u538b\u7f29\u3001\u62c9\u4f38\u3001\u526a\u5207\u3001\u626d\u8f6c\u3001\u5e73\u884c\u677f\u3001\u60ac\u81c2\u6881\u7b49\u591a\u79cd\u65b9\u5f0f\uff1b\uff082\uff09\u6837\u54c1\u8981\u6c42\u2014\u2014\u5f62\u72b6\u3001\u5c3a\u5bf8\u968f\u6d4b\u91cf\u7cfb\u7edf\u53d8\u5316\uff0c\u8981\u6c42\u5747\u5300\u3001\u8868\u9762\u5e73\u6574\u3001\u65e0\u6c14\u6ce1\u3001\u5404\u8fb9\u7cbe\u786e\u5e73\u884c\u548c\u5782\u76f4\uff0c\u6e7f\u5ea6\u5927\u7684\u5f0f\u6837\u5fc5\u987b\u5e72\u71e5\uff1b\uff083\uff09\u632f\u52a8\u9891\u7387\u4e0e\u632f\u52a8\u4f4d\u79fb\u2014\u2014\u4f4e\u9891(0.1~10Hz)\u6709\u5229\u4e8e\u68c0\u6d4b\u5c0f\u8fd0\u52a8\u5355\u5143\u7684\u677e\u9a70\uff1b\u968f\u9891\u7387\u589e\u52a0\uff0cE\u00b4\u548ctg\u03b4\u5411\u9ad8\u6e29\u533a\u79fb\u52a8\uff1b\u786c\u8bd5\u6837\u5c0f\u4f4d\u79fb\uff0c\u8f6f\u8bd5\u6837\u5927\u4f4d\u79fb\uff1b\uff084\uff09\u9759\u6001\u529b\u548c\u52a8\u6001\u529b\u2014\u2014\u4e3a\u4f7f\u8bd5\u6837\u4e0e\u9a71\u52a8\u5668\u548c\u4f20\u611f\u5668\u7d27\u5bc6\u63a5\u89e6\uff0c\u8981\u5bf9\u8bd5\u6837\u65bd\u52a0\u9759\u6001\u529b\u540e\u518d\u65bd\u52a0\u52a8\u6001\u529b\u8fdb\u884c\u68c0\u6d4b\uff0c\u5e76\u4e14\u9759\u6001\u529b\u9002\u5f53\u5927\u4e8e\u52a8\u6001\u529b\u3002<\/p>\n<p><span style=\"color: #0000ff;\"><strong>DMA\u8c31\u56fe\u2014\u2014\u52a8\u6001\u529b\u5b66\u6e29\u5ea6\u8c31\u548c\u9891\u7387\u8c31<\/strong><\/span><\/p>\n<p>\u6e29\u5ea6\u626b\u63cf\u6a21\u5f0f\u2014\u2014\u5728\u56fa\u5b9a\u9891\u7387\u4e0b\uff0c\u6d4b\u91cf\u52a8\u6001\u6a21\u91cf\u53ca\u529b\u5b66\u635f\u8017\u968f\u6e29\u5ea6\u7684\u53d8\u5316\u3002\u6240\u5f97\u66f2\u7ebf\u79f0\u52a8\u6001\u529b\u5b66\u6e29\u5ea6\u8c31\uff0c\u4e3a\u52a8\u6001\u529b\u5b66\u5206\u6790\u4e2d\u6700\u5e38\u4f7f\u7528\u7684\u6a21\u5f0f\uff0c\u5982\u56fe3\u6240\u793a\u3002<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-57931\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/3-17.png\" alt=\"\" width=\"700\" height=\"481\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/3-17.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/3-17-300x206.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p style=\"text-align: center;\"><strong>\u56fe3 \u805a\u5408\u7269\u7684DMA\u66f2\u7ebf\uff08\u6e29\u5ea6\u8c31\uff09\u00a0<\/strong><\/p>\n<p>\u9891\u7387\u626b\u63cf\u6a21\u5f0f\u2014\u2014\u5728\u56fa\u5b9a\u6e29\u5ea6\u4e0b\uff0c\u6d4b\u91cf\u52a8\u6001\u6a21\u91cf\u53ca\u529b\u5b66\u635f\u8017\u968f\u9891\u7387\u7684\u53d8\u5316\u3002\u6240\u5f97\u66f2\u7ebf\u79f0\u52a8\u6001\u529b\u5b66\u9891\u7387\u8c31\uff0c\u5982\u56fe4\u6240\u793a\u3002<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-57932\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/4-11.png\" alt=\"\" width=\"700\" height=\"474\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/4-11.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/4-11-300x203.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p style=\"text-align: center;\"><strong>\u56fe4\u805a\u5408\u7269\u7684DMA\u66f2\u7ebf\uff08\u9891\u7387\u8c31\uff09<\/strong><\/p>\n<p><strong><span style=\"color: #0000ff;\">DMA\u5206\u6790\u7684\u7279\u70b9 \u00a0 \u00a0<\/span> \u00a0<\/strong><\/p>\n<p>\uff08a\uff09 \u53ea\u9700\u5f88\u5c0f\u7684\u6837\u54c1\u5373\u53ef\u5728\u5f88\u5bbd\u7684\u6e29\u5ea6\u6216\u9891\u7387\u8303\u56f4\u6d4b\u5b9a\u6750\u6599\u7684\u52a8\u6001\u529b\u5b66\u6027\u80fd<\/p>\n<p>\uff08b\uff09 \u662f\u7814\u7a76\u9ad8\u5206\u5b50\u7ed3\u6784\u53d8\u5316\u2014\u2014\u8fd0\u52a8\u2014\u2014\u6027\u80fd\u4e09\u8005\u95f4\u5173\u7cfb\u7684\u7b80\u4fbf\u6709\u6548\u7684\u65b9\u6cd5<\/p>\n<p>\uff08c\uff09 \u975e\u5e38\u9002\u5408\u4e8e\u5728\u52a8\u6001\u8f7d\u8377\u4e0b\u5de5\u4f5c\u7684\u4ea7\u54c1\u7ed3\u6784\u3001\u914d\u65b9\u8bbe\u8ba1<\/p>\n<p><strong>D<span style=\"color: #0000ff;\">MA\u5728\u805a\u5408\u7269\u7814\u7a76\u4e2d\u7684\u5e94\u7528<\/span><\/strong><\/p>\n<p><strong>\uff081\uff09\u805a\u5408\u7269\u73bb\u7483\u5316\u8f6c\u53d8\u6e29\u5ea6\u7684\u6d4b\u5b9a\u00a0<\/strong><\/p>\n<p>Tg\u662f\u5ea6\u91cf\u9ad8\u5206\u5b50\u6750\u6599\u94fe\u6bb5\u8fd0\u52a8\u7684\u7279\u5f81\u6e29\u5ea6\uff0c\u5728Tg\u4ee5\u4e0b\uff0c\u9ad8\u5206\u5b50\u6750\u6599\u5904\u4e8e\u73bb\u7483\u6001\uff0cTg\u662f\u975e\u6676\u6001\u5851\u6599\u7684\u4f7f\u7528\u4e0a\u9650\uff0c\u662f\u6a61\u80f6\u7684\u4f7f\u7528\u6e29\u5ea6\u4e0b\u9650\uff0c\u6d4b\u5b9aTg\u65e0\u8bba\u5bf9\u975e\u6676\u5851\u6599\u548c\u6a61\u80f6\u90fd\u5177\u6709\u91cd\u8981\u7684\u610f\u4e49\u3002\u5c24\u5176\u662f\u5bf9\u4e8e\u73bb\u7483\u7ea4\u7ef4\u589e\u5f3a\u5851\u6599\uff0c\u7531\u4e8e\u91c7\u7528\u5dee\u793a\u626b\u63cf\u91cf\u70ed\u6cd5(DSC)\u6d4b\u8bd5\u65f6\u6240\u7528\u6837\u54c1\u91cf\u592a\u5c11\uff0c\u70ed\u6548\u5e94\u4e0d\u660e\u663e\uff0c\u6b64\u65f6\u7528DMA\u6cd5\u5c31\u80fd\u53cd\u6620\u51fa\u6bd4\u8f83\u660e\u663e\u7684Tg\uff0c\u5728\u73bb\u7483\u5316\u8f6c\u53d8\u9644\u8fd1\u805a\u5408\u7269\u7684\u529b\u5b66\u635f\u8017\u6709\u6700\u5927\u503c\u51fa\u73b0\uff0c\u636e\u6b64\u53ef\u6d4b\u5b9a\u805a\u5408\u7269\u7684\u73bb\u7483\u5316\u8f6c\u53d8\u6e29\u5ea6\u3002\u7531\u4e8e\u73bb\u7483\u5316\u8f6c\u53d8\u7684\u677e\u5f1b\u7279\u6027\uff0cTg\u5f3a\u70c8\u5730\u4f9d\u8d56\u4e8e\u6d4b\u8bd5\u4f5c\u7528\u529b\u7684\u9891\u7387\u548c\u5347\u6e29\u901f\u7387\u3002<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-57933\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/5-9.png\" alt=\"\" width=\"700\" height=\"547\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/5-9.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/5-9-300x234.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p style=\"text-align: center;\"><strong>\u56fe5 NBR\/CoCl<sub>2<\/sub>\u914d\u4f4d\u4ea4\u8054\u4f53\u7cfbDMA\u66f2\u7ebf \u00a0<\/strong><\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-57934\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/6-11.png\" alt=\"\" width=\"700\" height=\"521\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/6-11.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/6-11-300x223.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p style=\"text-align: center;\"><strong>\u56fe6 \u73af\u6c27\u6811\u8102\u5370\u5237\u7535\u8def\u677f\u7684DMA\u5206\u6790<\/strong><\/p>\n<p>\u4f8b\u5982\u4ece\u56fe5\u4e2d\u53ef\u4ee5\u6839\u636eDMA\u66f2\u7ebf\u6765\u7814\u7a76NBR\/CoCl<sub>2<\/sub>\u914d\u4f4d\u4ea4\u8054\u4f53\u7cfb\u73bb\u7483\u5316\u8f6c\u53d8\u6e29\u5ea6\u4e0e\u4ea4\u8054\u5242\u542b\u91cf\u7684\u5173\u7cfb\u3002\u5728\u52a8\u6001\u70ed\u673a\u68b0\u5206\u6790\u66f2\u7ebf\u4e0a\uff08\u56fe6\uff09\uff0c\u73bb\u7483\u5316\u8f6c\u53d8\u5448\u73b0\u5cf0\u5f62\uff0c\u56e0\u800c\u53ef\u975e\u5e38\u65b9\u4fbf\u51c6\u786e\u5730\u786e\u5b9a\u73bb\u7483\u5316\u8f6c\u53d8\u6e29\u5ea6\u3002<\/p>\n<p><strong>\u00a0\uff082\uff09\u9ad8\u5206\u5b50\u6750\u6599\u8010\u70ed\u6027\u8bc4\u4ef7 \u00a0<\/strong><\/p>\n<p>\u5728\u56fe7\u4e2d\uff0c\u901a\u8fc7\u52a8\u6001\u70ed\u673a\u68b0\u5206\u6790\u6280\u672f\uff0c\u53ef\u501f\u52a9\u5c11\u91cf\u6837\u54c1\u6d4b\u8bd5\u5373\u53ef\u83b7\u5f97\u5f88\u5bbd\u6e29\u5ea6\u8303\u56f4\u5185\u7684\u529b\u5b66\u6027\u80fd\u5982\u8d2e\u80fd\u6a21\u91cf\uff0c\u56e0\u800c\u53ef\u65b9\u4fbf\u800c\u53c8\u51c6\u786e\u5730\u5168\u9762\u8bc4\u4ef7\u6750\u6599\u7684\u8010\u70ed\u6027\u80fd\u3002<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-57935\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/7-6.png\" alt=\"\" width=\"628\" height=\"476\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/7-6.png 628w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/7-6-300x227.png 300w\" sizes=\"(max-width: 628px) 100vw, 628px\" \/><\/p>\n<p style=\"text-align: center;\"><strong>\u56fe7\u805a\u5408\u7269\u7684DMA\u66f2\u7ebf\uff08\u6e29\u5ea6\u8c31\uff09<\/strong><\/p>\n<p>\u4f8b\u5982\u56fe8\u4e2d\u867d\u7136\u70ed\u53d8\u5f62\u6e29\u5ea6\u7ed3\u679c\u8868\u660e\u786c\u8d28\u805a\u6c2f\u4e59\u70ef\u8010\u70ed\u6027\u80fd\u597d\u4e8e\u5c3c\u9f99\uff0c\u4f46\u52a8\u6001\u70ed\u673a\u68b0\u5206\u6790\u8868\u660e\u5728\u8f83\u9ad8\u6e29\u5ea6\u8303\u56f4\u540e\u8005\u8010\u70ed\u6027\u80fd\u8fdc\u8fdc\u4f18\u4e8e\u524d\u8005\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-57936\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/8-6.png\" alt=\"\" width=\"699\" height=\"540\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/8-6.png 699w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/8-6-300x232.png 300w\" sizes=\"(max-width: 699px) 100vw, 699px\" \/><\/p>\n<p style=\"text-align: center;\"><strong>\u56fe8 \u5c3c\u9f996\u548c\u786c\u8d28PVC\u7684E\u00b4-T\u5173\u7cfb\u66f2\u7ebf \u00a0 \u00a0<\/strong><\/p>\n<p><strong>(3)\u9ad8\u5206\u5b50\u6750\u6599\u8010\u5bd2\u6027\u8bc4\u4ef7 \u00a0 \u00a0<\/strong><\/p>\n<p>\u5de5\u4e1a\u4e0a\u5e38\u91c7\u7528\u843d\u9524\u5f0f\u51b2\u51fb\u8bd5\u9a8c\u6765\u8bc4\u4ef7\u9ad8\u5206\u5b50\u6750\u6599\u7684\u4f4e\u6e29\u97e7\u6027\u548c\u8010\u5bd2\u6027\uff0c\u8981\u6c42\u6837\u54c1\u6570\u91cf\u591a\u8fbe30\u4e2a\uff0c\u800c\u4e14\u6d4b\u8bd5\u524d\u987b\u5728-29\u2103\u4e0b\u8c03\u8282\u5904\u740624\u5c0f\u65f6\u3002\u56fe3\u4e2d\u6b21\u7ea7\u677e\u5f1b\u8f6c\u53d8\u6e29\u5ea6\u8d8a\u4f4e\u3001\u5cf0\u5f3a\u5ea6\u8d8a\u9ad8\uff0c\u8868\u660e\u805a\u5408\u7269\u94fe\u4e2d\u4f4e\u6e29\u8fd0\u52a8\u5355\u5143\u8d8a\u591a\uff0c\u56e0\u800c\u5177\u6709\u66f4\u597d\u7684\u4f4e\u6e29\u6027\u80fd\u3002\u8be5\u6cd5\u5177\u6709\u6837\u54c1\u5c11\u3001\u6d4b\u8bd5\u65b9\u4fbf\u4e4b\u4f18\u70b9\u3002\u56fe7\u4e3a\u6539\u6027\u805a\u4e19\u70ef\u4f4e\u6e29\u635f\u8017\u968f\u6e29\u5ea6\u53d8\u5316\u7684\u66f2\u7ebf\u4ee5\u53ca\u5728-29\u2103\u7684\u843d\u9524\u51b2\u51fb\u5f3a\u5ea6\uff0c\u7ed3\u679c\u663e\u793a\u968f\u7740\u6b21\u7ea7\u677e\u5f1b\u8f6c\u53d8\u5cf0\u5f3a\u5ea6\u4f9d\u6b21\u9012\u589e\uff0c\u6539\u6027\u805a\u4e19\u70ef\u7684\u4f4e\u6e29\u97e7\u6027\u9010\u6b65\u589e\u52a0\uff0c\u4e0e\u843d\u9524\u51b2\u51fb\u8bd5\u9a8c\u7ed3\u679c\u4e00\u81f4\u3002<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-57937\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/9-1.png\" alt=\"\" width=\"659\" height=\"499\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/9-1.png 659w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/9-1-300x227.png 300w\" sizes=\"(max-width: 659px) 100vw, 659px\" \/><\/p>\n<p style=\"text-align: center;\"><strong>\u56fe9 \u6539\u6027\u805a\u4e19\u70efDMA\u66f2\u7ebf<\/strong><\/p>\n<p>&nbsp;<\/p>\n<p><strong>\uff084\uff09\u9ad8\u5206\u5b50\u6750\u6599\u8010\u73af\u5883\u8001\u5316\u6027\u80fd\u8bc4\u4ef7\u00a0 \u00a0 \u00a0<\/strong><\/p>\n<p>\u9ad8\u5206\u5b50\u6750\u6599\u56e0\u5176\u51fa\u8272\u7684\u6bd4\u5f3a\u5ea6\u548c\u6bd4\u521a\u5ea6\u3001\u4f18\u826f\u7684\u8010\u75b2\u52b3\u6027\u53ca\u7075\u6d3b\u7684\u53ef\u8bbe\u8ba1\u6027\u5f97\u5230\u8d8a\u6765\u8d8a\u5e7f\u6cdb\u7684\u5e94\u7528\uff0c\u4f46\u662f\u5b83\u4eec\u5728\u70ed\u3001\u6e7f\u3001\u7d2b\u5916\u5149\u3001\u70df\u96fe\u7b49\u73af\u5883\u56e0\u7d20\u4e0b\u4f1a\u53d1\u751f\u8001\u5316\uff0c\u56e0\u6b64\u5bf9\u9ad8\u5206\u5b50\u6750\u6599\u8001\u5316\u673a\u7406\u53ca\u8001\u5316\u5bff\u547d\u7684\u9884\u4f30\u53d7\u5230\u5206\u5916\u5173\u6ce8\u3002\u8001\u5316\u540e\u9ad8\u5206\u5b50\u6750\u6599\u7684tan\u03b4\u548cTg\u90fd\u4f1a\u53d1\u751f\u53d8\u5316\u3002\u4f8b\u5982\u4ece\u56fe10\u4e2d\u7684\u5c3c\u9f9966\u5438\u6c34\u524d\u540e\u7684DMA\u66f2\u7ebf\u53ef\u4ee5\u770b\u51fa\u968f\u7740\u73af\u5883\u6e7f\u5ea6\u589e\u5927\uff0c\u5c3c\u9f99\u5438\u6536\u7a0b\u5ea6\u589e\u52a0\uff0c\u7531\u4e8e\u9170\u80fa\u57fa\u56e2\u6c34\u89e3\u5bfc\u81f4\u5206\u5b50\u65ad\u94fe\u4f7f\u5206\u5b50\u91cf\u4e0b\u964d\uff0c\u4ece\u800c\u4f7f\u635f\u8017\u5cf0\u4f4d\u7f6e\u6574\u4f53\u4f4e\u6e29\u504f\u79fb\u3002\u56fe11\u4e2d\u968f\u5149\u8001\u5316\u65f6\u95f4\u7684\u5ef6\u957f\uff0c\u786b\u9187\u6811\u8102\u5206\u5b50\u91cf\u4e0b\u964d\uff0c\u5bfc\u81f4\u635f\u8017\u5cf0\u4f4d\u7f6e\u6574\u4f53\u5411\u4f4e\u6e29\u65b9\u5411\u504f\u79fb\u3002<\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-57938\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/10-1.png\" alt=\"\" width=\"595\" height=\"489\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/10-1.png 595w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/10-1-300x247.png 300w\" sizes=\"(max-width: 595px) 100vw, 595px\" \/><\/p>\n<p style=\"text-align: center;\"><strong>\u56fe10 \u5c3c\u9f9966\u5438\u6c34\u524d\u540e\u7684DMA\u66f2\u7ebf \u00a0<\/strong><\/p>\n<p style=\"text-align: center;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-57939\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/11-1.png\" alt=\"\" width=\"642\" height=\"531\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/11-1.png 642w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/12\/11-1-300x248.png 300w\" sizes=\"(max-width: 642px) 100vw, 642px\" \/><\/p>\n<p style=\"text-align: center;\"><strong>\u56fe11 \u5149\u8001\u5316\u65f6\u95f4\u5bf9UV-\u56fa\u5316\u786b\u9187\u6811\u8102DMA\u7ed3\u679c\u7684\u5f71\u54cd<\/strong><\/p>\n<p><strong><span style=\"color: #0000ff;\">\u7ed3\u8bed<\/span><\/strong><\/p>\n<p>DMA\u6280\u672f\u662f\u7814\u7a76\u9ad8\u5206\u5b50\u6750\u6599\u7ed3\u6784\u53ca\u5176\u5316\u5b66\u4e0e\u7269\u7406\u529b\u5b66\u6027\u80fd\u5e38\u7528\u7684\u8868\u5f81\u65b9\u6cd5\u4e4b\u4e00\uff0c\u5176\u5728\u9ad8\u5206\u5b50\u6750\u6599\u6d4b\u8bd5\u548c\u8868\u5f81\u7684\u5404\u4e2a\u65b9\u9762\u90fd\u83b7\u5f97\u4e86\u5e7f\u6cdb\u7684\u5e94\u7528\uff0c\u76ee\u524d\u5df2\u6210\u4e3a\u7814\u7a76\u9ad8\u5206\u5b50\u6750\u6599\u6027\u80fd\u7684\u91cd\u8981\u65b9\u6cd5\u4e4b\u4e00\u3002<\/p>\n<p><span style=\"color: #0000ff;\"><strong>\u53c2\u8003\u6587\u732e<\/strong><\/span><\/p>\n<p>[1]\u738b\u96c1\u51b0, \u9ec4\u5fd7\u96c4, \u5f20\u8054\u76df. DMA\u5728\u9ad8\u5206\u5b50\u6750\u6599\u7814\u7a76\u4e2d\u7684\u5e94\u7528[J]. \u5efa\u6750\u4e16\u754c, 2004, 25(2):25-27.<\/p>\n<p>[2]\u5218\u6653. \u52a8\u6001\u70ed\u529b\u5b66\u5206\u6790\u5728\u9ad8\u5206\u5b50\u6750\u6599\u4e2d\u7684\u5e94\u7528[J]. \u5de5\u7a0b\u5851\u6599\u5e94\u7528, 2010, 38(7):84-86.<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u9ad8\u5206\u5b50\u6750\u6599\u7ec4\u5468\u5c0f\u51e4\u4f9b\u7a3f\uff0c\u6750\u6599\u4eba\u7f51\u7f16\u8f91\u6574\u7406\u3002<\/p>\n<p>\u6750\u6599\u725b\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u8fd9\u91cc\u6c47\u96c6\u4e86\u5404\u5927\u9ad8\u6821\u7855\u535a\u751f\u3001\u4e00\u7ebf\u79d1\u7814\u4eba\u5458\u4ee5\u53ca\u884c\u4e1a\u4ece\u4e1a\u8005\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\">\u70b9\u6211\u52a0\u5165\u6750\u6599\u4eba\u7f16\u8f91\u90e8<\/a>\u3002<\/p>\n<p>\u6750\u6599\u4eba\u7f51\u5411\u5404\u5927\u56e2\u961f\u8bda\u5fc3\u7ea6\u7a3f\uff0c\u8bfe\u9898\u7ec4\u6700\u65b0\u6210\u679c\u3001\u65b9\u5411\u603b\u7ed3\u3001\u56e2\u961f\u8bbf\u8c08\u3001\u5b9e\u9a8c\u6280\u80fd\u7b49\u7686\u53ef\u6295\u7a3f\uff0c\u8bf7\u8054\u7cfb\uff1a\u90ae\u7bb1tougao@cailiaoren.com \u6216 QQ\uff1a97482208\u3002<\/p>\n<p><span style=\"color: #ff0000;\"><strong>\u4eea\u5668\u8bbe\u5907\u3001\u8bd5\u5242\u8017\u6750\u3001\u6750\u6599\u6d4b\u8bd5\u3001\u6570\u636e\u5206\u6790\uff0c\u627e<a style=\"color: #ff0000;\" href=\"http:\/\/mai.cailiaoren.com\/\" target=\"_blank\">\u6750\u6599\u4eba<\/a>\u3001\u4e0a<a style=\"color: #ff0000;\" href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\">\u6d4b\u8bd5\u8c37<\/a>\uff01<\/strong><\/span><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u52a8\u6001\u529b\u5b66\u884c\u4e3a\u662f\u6307\u6750\u6599\u5728\u632f\u52a8\u6761\u4ef6\u4e0b\uff0c\u5373\u5728\u4ea4\u53d8\u5e94\u529b\uff08\u4ea4\u53d8\u5e94\u53d8\uff09\u4f5c\u7528\u4e0b\u505a\u51fa\u7684\u529b\u5b66\u54cd\u5e94\uff0c\u5373\u529b\u5b66\u6027\u80fd(\u6a21\u91cf\u3001\u5185\u8017)\u4e0e\u6e29\u5ea6\u3001\u9891\u7387\u7684\u5173\u7cfb\u3002\u6d4b\u5b9a\u6750\u6599\u5728\u4e00\u5b9a\u6e29\u5ea6\u8303\u56f4\u5185\u52a8\u6001\u529b\u5b66\u6027\u80fd&#8230;<\/p>\n","protected":false},"author":393,"featured_media":57930,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[4],"tags":[2513,42],"class_list":["post-57923","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-ganhuo","tag-refenxi","tag-gaofenzi"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/57923"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/393"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=57923"}],"version-history":[{"count":6,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/57923\/revisions"}],"predecessor-version":[{"id":59385,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/57923\/revisions\/59385"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/57930"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=57923"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=57923"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=57923"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}